Flexible pressure sensor and preparation method and application thereof
By using flexible pressure sensors prepared by bio-based materials, the problem of insufficient sensitivity and inorganic compatibility of traditional sensors is solved, and high sensitivity and self-powered are achieved. It is suitable for pressure and physiological monitoring, and is suitable for smart wearable devices.
Patent Information
- Application Number
- CN202310622214.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-30
- Publication Date
- 2024-12-03
AI Technical Summary
Traditional wearable pressure sensors have insufficient sensitivity, poor flexibility, need external power supply and inorganic materials, which limit their application in human-computer interaction and health monitoring.
The flexible pressure sensor is prepared using bio-based materials, including the encapsulation layer, intermediate layer and encapsulation layer of the sandwich structure. The intermediate layer is composed of polyvinyl alcohol, inorganic salts and keratin. Self-generating power is achieved through triboelectric phenomenon, and the encapsulation layer is tensile. Excellent aliphatic aromatic random copolyester, the electrode area is smaller than the intermediate layer, achieving single electrode self-power supply.
It improves the sensitivity and linearity of the flexible pressure sensor, enhances biocompatibility and tensile performance, realizes self-powered, is suitable for pressure monitoring and smart wearable devices, with a strain of up to 200%, and is widely used in pressure and physiological monitoring.
Smart Images

Figure CN119063881A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of pressure sensors, and in particular to a flexible pressure sensor and a preparation method and application thereof. Background Art
[0002] Wearable pressure sensors are widely used in human-computer interaction, machine recognition, and health monitoring. Traditional wearable pressure sensors are usually not sensitive enough and lack flexibility, which seriously limits the application of such sensors in various fields. In addition, existing sensors require external power supply and are dual-electrode, which greatly reduces the working life and system integration of the wearable system. Traditional materials used for sensors are basically polymers or metals, which makes wearable sensors lack biocompatibility and flexibility and cannot fit safely with human skin. Summary of the invention
[0003] In order to solve the above problems, the object of the present invention is to provide a flexible pressure sensor and a preparation method and application thereof. The flexible pressure sensor is based on bio-based materials and can be used for pressure detection.
[0004] To achieve the above object, the present invention provides a flexible pressure sensor, which comprises a first packaging layer, an intermediate layer, and a second packaging layer stacked in sequence; the first packaging layer and the second packaging layer seal the intermediate layer inside, a lead electrode is provided between the intermediate layer and any packaging layer, and microstructures are distributed on the inner surfaces of the first packaging layer and the second packaging layer;
[0005] Wherein, in terms of weight, the raw materials of the middle layer include: 1-2 parts of polyvinyl alcohol, 1-3 parts of inorganic salt, 1-4 parts of keratin, and 1-20 parts of water.
[0006] In the above-mentioned flexible pressure sensor, preferably, in parts by weight, the raw materials of the intermediate layer include: 2 parts of polyvinyl alcohol, 1 part of inorganic salt, 4 parts of keratin, and 20 parts of water.
[0007] The flexible pressure sensor of the present invention has a sandwich structure of "packaging layer-middle layer-packaging layer", which can realize the functions of pressure sensing and self-power generation, and realizes the self-power supply of the single-electrode sensor through the frictional electricity phenomenon between the different materials of the middle layer and the packaging layer. In the above-mentioned flexible pressure sensor, the area of the electrode layer is smaller than the area of the middle layer, that is, the middle layer can directly contact the packaging layers on both sides.
[0008] The present invention improves the linearity and sensitivity of the flexible pressure sensor by optimizing the raw material components and ratio of the intermediate layer, wherein the increase in keratin content can effectively enhance the output voltage of triboelectricity.
[0009] In the above-mentioned flexible pressure sensor, preferably, the inorganic salt is calcium chloride and / or sodium chloride.
[0010] In the above-mentioned flexible pressure sensor, preferably, the material of the encapsulation layer is aliphatic aromatic random copolyester (Ecoflex). In the present invention, the encapsulation layer can generate electricity by friction with the intermediate layer; the encapsulation layer is made of a polymer with excellent tensile properties and good biocompatibility, and has an electronic sensing function.
[0011] In the above-mentioned flexible pressure sensor, preferably, the microstructure is a rectangular parallelepiped protrusion.
[0012] In the above-mentioned flexible pressure sensor, preferably, the size of the microstructure is (0.2-1) mm×(0.2-1) mm×(0.2-1) mm, and the thickness of the packaging layer is 0.2-1 mm; more preferably, the size of the microstructure is 0.4 mm×0.4 mm×0.2 mm, and the thickness of the packaging layer is 0.6 mm.
[0013] The present invention also provides a method for preparing the above-mentioned flexible pressure sensor, which comprises the following steps:
[0014] (1) dissolving calcium chloride or sodium chloride in water, then adding polyvinyl alcohol to dissolve under heating conditions, cooling, then adding keratin, stirring evenly, obtaining a stock solution for preparing an intermediate layer, and pouring the stock solution into an intermediate layer mold, freezing and solidifying, and obtaining the intermediate layer after thawing;
[0015] (2) pouring the liquid aliphatic aromatic random copolyester into the encapsulation layer mold, and after curing, obtaining a first encapsulation layer and a second encapsulation layer respectively;
[0016] (3) Attach any packaging layer and the middle layer, adhere the electrode to the surface of the middle layer with a conductive paste, cover the middle layer with another packaging layer, and then use liquid aliphatic aromatic random copolyester to adhere the edges of the two packaging layers, and obtain the flexible pressure sensor after curing.
[0017] In the above-mentioned method for preparing the flexible pressure sensor, preferably, the temperature when adding and dissolving polyvinyl alcohol in step (1) is 75-90°C.
[0018] In the method for preparing the flexible pressure sensor, preferably, the temperature during the adding and stirring of keratin in step (1) is 30-60°C.
[0019] In the above-mentioned method for preparing the flexible pressure sensor, preferably, in step (1), the freezing temperature is -10°C to -20°C, and the freezing time is 24-48h.
[0020] In the above-mentioned method for preparing the flexible pressure sensor, preferably, the packaging layer mold is in the shape of a rectangular groove, and microstructure holes are evenly distributed on the inner surface of the groove.
[0021] The present invention also provides an application of the above-mentioned flexible pressure sensor in pressure monitoring sensing, physiological monitoring sensing or the preparation of intelligent wearable electronic devices.
[0022] The intermediate layer and the packaging layer both have good stretchability, and the pressure sensor of the present invention has good flexibility, so it is suitable for wearable pressure detection. In addition, the flexible pressure sensor can also be used for finger movement tracking to achieve recognition of gestures and object shapes.
[0023] The technical solution provided by the present invention has the following beneficial effects:
[0024] The present invention effectively improves the sensitivity and linearity of the flexible pressure sensor by adding keratin to the middle layer, and optimizes the bio-based material formula of the middle layer so that it has good biocompatibility and excellent tensile properties. In some specific embodiments, the strain of the prepared flexible pressure sensor is as high as 200%.
[0025] In the preparation of the flexible pressure sensor, the encapsulation layer and the intermediate layer can be prepared by 3D printing, and the thickness and raw material content are adjustable and controllable. The preparation method of the flexible pressure sensor of the present invention is simple and has broad application prospects in the fields of pressure monitoring, intelligent wearable electronics and physiological monitoring sensors. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 A schematic diagram of the sensor structure designed for the present invention;
[0027] Figure 2 This is an optical micrograph of the encapsulation layer obtained in Example 1 of the present invention;
[0028] Figure 3 This is a scanning electron microscope image of the intermediate layer obtained in Example 2 of the present invention;
[0029] Figure 4 This is a gesture recognition signal diagram of the flexible pressure sensor obtained in Example 3 of the present invention, wherein the thumb (P), index finger (I), middle finger (M), ring finger (A) and little finger (X) correspond to fingertip position sensors respectively;
[0030] Figure 5a The finger fixing position of the flexible pressure sensor in the embodiment 4 of the present invention in the gesture recognition test;
[0031] Figure 5b This is a gesture recognition signal diagram of the flexible pressure sensor according to Embodiment 4 of the present invention;
[0032] Figure 5c This is a gesture recognition signal diagram of the flexible pressure sensor according to Embodiment 4 of the present invention;
[0033] Figure 5d This is a gesture recognition signal diagram of the flexible pressure sensor according to Embodiment 4 of the present invention;
[0034] Figure 6 These are the output voltage test results of the flexible pressure sensors of Examples 1-4 of the present invention.
[0035] Description of Figure Numbers:
[0036] 1. First packaging layer, 2. Second packaging layer, 3. Intermediate layer, 4. Lead electrode, 5. Microstructure. DETAILED DESCRIPTION
[0037] In order to have a clearer understanding of the technical features, purposes and beneficial effects of the present invention, the technical solution of the present invention is now described in detail below, but it should not be construed as limiting the applicable scope of the present invention.
[0038] Example 1
[0039] This embodiment provides a flexible pressure sensor, such as Figure 1 As shown, the flexible pressure sensor includes a first packaging layer 1, an intermediate layer 3, and a second packaging layer 2 which are stacked in sequence; the first packaging layer 1 and the second packaging layer 2 seal the intermediate layer 3 inside, a lead-out electrode 4 is provided between the intermediate layer 3 and the first packaging layer 1, the thickness of the first packaging layer 1 and the second packaging layer 2 is 0.6 mm, and the inner surfaces of the first packaging layer 1 and the second packaging layer 2 are distributed with rectangular raised microstructures 5 with a size of 0.4 mm×0.4 mm×0.2 mm;
[0040] The method for preparing the flexible pressure sensor of this embodiment includes the following steps:
[0041] (1) Preparation of the intermediate layer
[0042] 1 g of calcium chloride powder was added to 20 mL of water, and the mixture was stirred at room temperature for 1 h to obtain a calcium chloride solution, which was placed at room temperature for later use; 2 g of polyvinyl alcohol powder was added to the calcium chloride solution, and the mixture was heated to 80° C. until the polyvinyl alcohol was completely dissolved, and the mixture was cooled to 60° C. for later use; 1 g of keratin powder was added to the solution containing polyvinyl alcohol and calcium chloride until the keratin was completely dissolved to obtain a stock solution for preparing the intermediate layer, which was placed at 60° C. for later use;
[0043] The intermediate layer preparation solution was poured into a 3D printing mold, placed in a -20°C environment for 24 hours, and then thawed at room temperature to obtain the intermediate layer.
[0044] (2) Preparation of microstructure encapsulation layer
[0045] Liquid aliphatic aromatic random copolyester material (Ecoflex) is poured into a 3D printed encapsulation layer mold and solidified to obtain a first encapsulation layer and a second encapsulation layer with a microstructure; wherein the encapsulation layer mold is in the shape of a rectangular groove with a thickness of 0.6 mm, and microstructure holes are evenly distributed on the inner surface of the groove, and the microstructure holes are rectangular holes of 0.4 mm×0.4 mm×0.2 mm.
[0046] Figure 2 This is an optical micrograph of the obtained encapsulation layer, and it can be seen that microstructures are distributed on the encapsulation layer.
[0047] (3) Assembly
[0048] The second packaging layer and the middle layer are attached, the electrodes are adhered to the surface of the middle layer with a conductive paste, and then the first packaging layer is covered to cover the middle layer, and liquid Ecoflex is used to adhere the edges of the two packaging layers. After curing, a flexible pressure sensor is obtained.
[0049] In order to conduct a stretch test on the flexible pressure sensor prepared in this embodiment, the strain is as high as 200%.
[0050] Example 2
[0051] This embodiment provides a flexible pressure sensor, whose structure is the same as that of Embodiment 1.
[0052] The preparation method of the flexible pressure sensor in this embodiment is the same as that in Embodiment 1, except that the amount of keratin used is 2 g.
[0053] Figure 3 This is a scanning electron microscope image of the intermediate layer prepared in Example 2 of the present invention.
[0054] Example 3
[0055] This embodiment provides a flexible pressure sensor, whose structure is the same as that of Embodiment 1.
[0056] The preparation method of the flexible pressure sensor in this embodiment is the same as that in Embodiment 1, except that the amount of keratin used is 3 g.
[0057] Take 5 flexible pressure sensors of Example 3 and fix them on the tips of five fingers respectively, connect the electrodes of the sensors to the ESP32 microcontroller system, and transmit them to the mobile app via Bluetooth to collect the following information: Figure 4 The results show that the flexible pressure sensor of the present invention can be used for gesture recognition.
[0058] Example 4
[0059] This embodiment provides a flexible pressure sensor, whose structure is the same as that of Embodiment 1.
[0060] The preparation method of the flexible pressure sensor in this embodiment is the same as that in Embodiment 1, except that the amount of keratin used is 4 g.
[0061] Take 10 flexible pressure sensors of Example 4 and fix them in the palm of your hand. Figure 5a As shown above, the electrodes of the sensor are connected to the ESP32 microcontroller system and transmitted to the mobile app via Bluetooth. Figure 5b , Figure 5c , Figure 5d The results show that the flexible pressure sensor of the present invention can be used for gesture recognition.
[0062] Example 5
[0063] This embodiment provides a flexible pressure sensor, whose structure is the same as that of Embodiment 1.
[0064] The preparation method of the flexible pressure sensor in this embodiment is the same as that in Embodiment 1, except that the amount of calcium chloride powder used is 2 g, and the amount of keratin used is 4 g.
[0065] The maximum output voltage of the flexible pressure sensor prepared in the above examples 1-4 was tested, and the results were as follows: Figure 6 As shown. Figure 6 It can be seen that the increase in keratin content can effectively enhance the output voltage of triboelectricity.
[0066] Comparative Example 1
[0067] This comparative example provides a flexible pressure sensor, whose structure is the same as that of Example 4.
[0068] The preparation method of the flexible pressure sensor is the same as that of Example 4, except that the raw materials of the middle layer are 2 g of polyvinyl alcohol and 20 ml of water, and do not contain calcium chloride and keratin.
[0069] The method for preparing the intermediate layer of this comparative example is as follows: add 2 g of polyvinyl alcohol powder to 20 ml of water, heat to 80°C until the polyvinyl alcohol is completely dissolved, cool to 60°C for standby use, and obtain a stock solution for preparing the intermediate layer; pour the stock solution for preparing the intermediate layer into a 3D printing mold, place it in an environment of -20°C for 24 hours, and then thaw it at room temperature to obtain the intermediate layer.
[0070] Comparative Example 2
[0071] This comparative example provides a flexible pressure sensor, whose structure is the same as that of Example 4.
[0072] The preparation method of the flexible pressure sensor is also the same as that of Example 4, except that the raw materials of the intermediate layer are 2 g of polyvinyl alcohol, 1 g of calcium chloride powder and 20 ml of water, and keratin is not included.
[0073] The preparation method of the intermediate layer of this comparative example is as follows: 1 g of calcium chloride powder is added to 20 mL of water, stirred at room temperature for 1 hour to obtain a calcium chloride solution, and placed at room temperature for use; 2 g of polyvinyl alcohol powder is added to the calcium chloride solution, heated to 80°C until the polyvinyl alcohol is completely dissolved, to obtain an intermediate layer preparation solution, which is placed at 60°C for use; the intermediate layer preparation solution is poured into a 3D printing mold, placed in an environment of -20°C for 24 hours, and then thawed at room temperature to obtain an intermediate layer.
[0074] Comparative Example 3
[0075] This comparative example provides a flexible pressure sensor, whose structure is the same as that of Example 4.
[0076] The preparation method of the flexible pressure sensor is also the same as that of Example 4, except that the raw materials of the middle layer are 2 g of polyvinyl alcohol, 4 g of keratin and 20 ml of water, and calcium chloride is not included.
[0077] The preparation method of the intermediate layer of this comparative example is as follows: 2 g of polyvinyl alcohol powder is added to 20 mL of water, heated to 80° C. until the polyvinyl alcohol is completely dissolved, and cooled to 60° C. for use; 4 g of keratin powder is added to a solution containing polyvinyl alcohol until the keratin is completely dissolved to obtain an intermediate layer preparation solution, which is placed at 60° C. for use; the intermediate layer preparation solution is poured into a 3D printing mold, placed in an environment of -20° C. for 24 hours, and then thawed at room temperature to obtain an intermediate layer.
[0078] The sensitivity and linearity of the flexible pressure sensors of Example 4 and Comparative Examples 1-3 were tested, wherein the sensitivity was calculated by the output voltage corresponding to the forces of different magnitudes applied by the linear motor, and the linearity was calculated by linearly fitting the results of the force and voltage. The test results are shown in Table 1.
[0079] Table 1 Test results of sensitivity and linearity of flexible pressure sensor
[0080] Group Middle layer raw material Sensitivity, V / KPa <![CDATA[Correlation coefficient (R 2 )]]> Example 4 Polyvinyl alcohol + calcium chloride + keratin 0.225 0.988 Comparative Example 1 Polyvinyl alcohol 0.081 0.762 Comparative Example 2 Polyvinyl alcohol + calcium chloride 0.011 0.921 Comparative Example 3 Polyvinyl alcohol + keratin 0.132 0.898
[0081] The results shown in Table 1 show that the flexible pressure sensor prepared in Example 4 of the present invention has good sensitivity and linearity. According to the results of Comparative Example 2, the present invention greatly improves the sensitivity of the flexible pressure sensor by adding keratin, and the linearity is also improved. According to the results of Comparative Example 3, the addition of calcium chloride in the present invention also significantly improves the sensitivity of the flexible pressure sensor.
Claims
1. A flexible pressure sensor, comprising a first packaging layer, an intermediate layer and a second packaging layer stacked in sequence; the first packaging layer and the second packaging layer seal the intermediate layer inside, a lead electrode is provided between the intermediate layer and any packaging layer, and microstructures are distributed on the inner surfaces of the first packaging layer and the second packaging layer; in, In terms of weight, the raw materials of the middle layer include: 1-2 parts of polyvinyl alcohol, 1-3 parts of inorganic salt, 1-4 parts of keratin, and 1-20 parts of water.
2. The flexible pressure sensor according to claim 1, wherein: The raw materials of the middle layer include: 2 parts of polyvinyl alcohol, 1 part of inorganic salt, 4 parts of keratin and 20 parts of water.
3. The flexible pressure sensor according to claim 1, wherein: The inorganic salt is calcium chloride and / or sodium chloride.
4. The flexible pressure sensor according to claim 1, wherein: The material of the encapsulation layer is aliphatic aromatic random copolyester.
5. The flexible pressure sensor according to claim 1, wherein: The microstructure is a rectangular parallelepiped protrusion.
6. A method for preparing the flexible pressure sensor according to any one of claims 1 to 5, comprising the following steps: (1) dissolving calcium chloride or sodium chloride in water, then adding polyvinyl alcohol to dissolve under heating conditions, cooling, then adding keratin, stirring evenly, obtaining a stock solution for preparing an intermediate layer, and pouring the stock solution into an intermediate layer mold, freezing and solidifying, and obtaining the intermediate layer after thawing; (2) pouring the liquid aliphatic aromatic random copolyester into the encapsulation layer mold, and after curing, obtaining a first encapsulation layer and a second encapsulation layer respectively; (3) Attach any packaging layer and the middle layer, adhere the electrode to the surface of the middle layer with a conductive paste, cover the middle layer with another packaging layer, and then use liquid aliphatic aromatic random copolyester to adhere the edges of the two packaging layers, and obtain the flexible pressure sensor after curing.
7. The method for preparing a flexible pressure sensor according to claim 6, wherein: The temperature when adding polyvinyl alcohol and dissolving it in step (1) is 75-90°C.
8. The method for preparing a flexible pressure sensor according to claim 6, wherein: The temperature when adding keratin and stirring in step (1) is 30-60°C.
9. The method for preparing a flexible pressure sensor according to claim 6, wherein: In step (1), the freezing temperature is -10°C to -20°C, and the freezing time is 24-48h.
10. Application of the flexible pressure sensor according to any one of claims 1 to 5 in pressure monitoring sensing, physiological monitoring sensing or preparation of smart wearable electronic devices.