Thermal shock resistance test method for aluminum electrolysis anode carbon block
By performing thermal shock resistance test methods for pretreatment and insulation treatment in an inert atmosphere, the problem of thermal shock resistance of aluminum electrolytic anode carbon block cannot be effectively measured in the prior art, and the thermal resistance of aluminum electrolytic anode carbon block is realized Accurate evaluation of earthquake performance reduces cracks and block loss, and improves the stability and efficiency of aluminum electrolytic cells.
Patent Information
- Application Number
- CN202411399092.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-09
- Publication Date
- 2024-12-03
AI Technical Summary
The prior art cannot effectively determine the thermal shock resistance of aluminum electrolytic anode carbon blocks, resulting in cracks and blocks falling off during replacement, affecting the normal operation of the aluminum electrolytic cell.
The thermal shock resistance test method is adopted for pretreatment and insulation treatment in an inert atmosphere. By simulating the process of rapid rise of the anode carbon block from low temperature to high temperature, and cooling in an inert atmosphere, the number of fractures is recorded to evaluate the thermal shock resistance level. .
This method can accurately and safely evaluate the thermal shock resistance of aluminum electrolytic anode carbon blocks, reduce cracks and block loss, and improve the stable operation and efficiency of aluminum electrolytic cells.
Smart Images

Figure CN119064203A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of aluminum electrolysis anode carbon blocks, and in particular to a thermal shock resistance test method for aluminum electrolysis anode carbon blocks. Background Art
[0002] Aluminum electrolytic anode is one of the main raw materials for aluminum electrolytic production, and plays an important role in aluminum electrolytic production. The quality of aluminum electrolytic anode directly affects the normal operation of aluminum electrolytic production and various technical and economic indicators, so it is called the "heart" of aluminum electrolytic cell. Aluminum electrolytic anode is constantly consumed when it is operating normally on the aluminum electrolytic cell, and needs to be replaced at regular intervals. When replacing aluminum electrolytic anode, since the temperature of the anode is at room temperature or reaches a certain temperature after preheating, and the normal operating temperature in the aluminum electrolytic cell is about 950℃, the temperature difference between the two is large, so cracks and blocks often occur when replacing the anode. Some anode carbon blocks have good conventional indicators, but when used in aluminum electrolytic cells, cracks and blocks are serious. Cracks and blocks often lead to disordered operation of aluminum electrolytic cells, and even electrolytic cell accidents, which greatly increase the consumption of electricity and materials, sharply reduce the current efficiency, and even lead to serious accidents such as cell shutdown. Based on the above, the reason is that the thermal shock resistance of aluminum electrolytic anode is poor. Thermal shock resistance is the ability of a material to resist damage under conditions of rapid temperature changes, and is a comprehensive expression of its mechanical and thermal properties under temperature changes. When a material is subjected to rapid temperature changes, new cracks may form, and the extension of new cracks and existing cracks may cause cracking, peeling, and breaking.
[0003] At present, the quality index of aluminum electrolysis anode does not involve the detection of thermal shock resistance. The existing methods for thermal shock resistance of other materials are mainly: water quenching method, air quenching method and water quenching-crack determination method. Considering that aluminum electrolysis anode is a carbon material, it is easy to oxidize at high temperature, and there are many technical problems in the above-mentioned thermal shock resistance detection technologies. Water quenching method, air quenching method and water quenching-crack determination method, these three methods are to heat the sample to the set temperature, keep it for a certain time, and then use water or air for rapid cooling, so as to determine the quality of the material's thermal shock resistance. Aluminum electrolysis anode is a carbon material. Due to its particularity, using water as a cooling medium, carbon will react with water to produce flammable and explosive gases such as carbon monoxide and hydrogen, which will bring great safety hazards to the experimental operation; using air as a cooling medium, carbon will undergo oxidation reaction when it encounters air at high temperature, which will have a great impact on the accuracy of the experimental data. More importantly, these three methods all measure the thermal shock resistance of the material by cooling the sample, which cannot truly reflect the condition of the aluminum electrolytic anode on the electrolytic cell. When replacing the anode, the aluminum electrolytic cell is prone to cracks and block drop, which is caused by the anode rapidly rising from low temperature to high temperature. In summary, there is an urgent need for a thermal shock resistance test method for aluminum electrolytic anode carbon blocks. Summary of the invention
[0004] The present application provides a method for testing the thermal shock resistance of an aluminum electrolysis anode carbon block to solve the following technical problem: how to efficiently measure the thermal shock resistance of an aluminum electrolysis anode carbon block.
[0005] The present application provides a method for testing the thermal shock resistance of an aluminum electrolysis anode carbon block, the method comprising:
[0006] S1. Sampling is performed at a set position of the aluminum electrolysis anode carbon block to be tested to obtain a sample to be tested having a set size;
[0007] S2, pre-treating the sample to be tested;
[0008] S3, placing the pretreated sample to be tested in an inert atmosphere and performing a heat preservation treatment at a set temperature;
[0009] S4, cooling the test sample after the heat preservation treatment to room temperature in the inert atmosphere;
[0010] S5, determining whether the sample to be tested is broken after being cooled to room temperature; if not, looping steps S2 to S4 until the sample to be tested is broken; if broken, recording the number of tests when the break occurs;
[0011] S6. According to the number of tests, the thermal shock resistance grade of the aluminum electrolysis anode carbon block to be tested is obtained.
[0012] Optionally, obtaining the thermal shock resistance grade of the aluminum electrolysis anode carbon block to be tested according to the number of tests includes:
[0013] According to the test times, the thermal shock resistance grade of the aluminum electrolysis anode carbon block to be tested is obtained; wherein,
[0014] When the test number is ≥5 times, the thermal shock resistance grade of the aluminum electrolysis anode carbon block to be tested is grade A;
[0015] When the test number is 2 to 4 times, the thermal shock resistance grade of the aluminum electrolysis anode carbon block to be tested is Class B;
[0016] When the test number is 1, the thermal shock resistance grade of the aluminum electrolysis anode carbon block to be tested is grade C;
[0017] Among them, grade A is better than grade B, and grade B is better than grade C.
[0018] Optionally, the set dimensions include: a diameter of 10 mm to 100 mm and a length of 20 mm to 200 mm.
[0019] Optionally, the set position is the bottom or side of the aluminum electrolysis anode carbon block to be tested.
[0020] Optionally, pre-processing the sample to be tested includes:
[0021] The test sample is dried to perform pretreatment.
[0022] Optionally, the drying temperature is 100° C. to 300° C., and the drying time is 0.5 h to 2 h.
[0023] Optionally, the set temperature is 900°C to 1000°C.
[0024] Optionally, the insulation treatment time is 5 minutes to 30 minutes.
[0025] Optionally, the interval between placing the pretreated sample to be tested in the inert atmosphere and subjecting the pretreated sample to the heat preservation treatment is 2 minutes to 5 minutes.
[0026] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:
[0027] The present application provides a method for testing the thermal shock resistance of an aluminum electrolytic anode carbon block, comprising: S1, sampling at a set position of the aluminum electrolytic anode carbon block to be tested to obtain a test sample with a set size; S2, pre-treating the test sample; S3, placing the pre-treated test sample in an inert atmosphere, and performing a heat preservation treatment at a set temperature; S4, cooling the test sample after the heat preservation treatment to room temperature in the inert atmosphere; S5, determining whether the test sample after cooling to room temperature is broken; if no break occurs, looping steps S2 to S4 until the test sample is broken; if break occurs, recording the number of tests when the break occurs; S6, obtaining the thermal shock resistance grade of the aluminum electrolytic anode carbon block to be tested according to the number of tests. First, through accurate sampling and pretreatment, the representativeness of the samples to be tested is ensured; secondly, the process of rapid rise from low temperature to high temperature of the anode carbon block during electrolysis is simulated by heat preservation treatment at a set temperature; rapid and stable cooling is used to simulate the rapid cooling process that the anode carbon block may encounter during electrolysis; the atmosphere of heat preservation treatment and cooling is limited to an inert atmosphere to avoid oxidation of the samples to be tested; finally, the thermal shock resistance is evaluated according to the number of fractures. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.
[0029] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0030] Figure 1 A schematic flow chart of a method for testing the thermal shock resistance of an aluminum electrolysis anode carbon block provided in an embodiment of the present application. DETAILED DESCRIPTION
[0031] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0032] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0033] In addition, in the description of the specification of the present application, the terms "including", "comprising", etc. mean "including but not limited to". In this article, relational terms such as "first" and "second", etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A and B can be singular or plural. In this article, "at least one" means one or more, and "plurality" means two or more. "At least one", "the following at least one item (items)" or similar expressions refer to any combination of these items, including any combination of single items (items) or plural items (items). For example, "at least one of a, b, or c", or "at least one of a, b and c", can both mean: a, b, c, ab (i.e. a and b), ac, bc or abc, where a, b, c can be single or plural, respectively.
[0034] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.
[0035] Figure 1 A schematic flow chart of a method for testing the thermal shock resistance of an aluminum electrolysis anode carbon block provided in an embodiment of the present application.
[0036] See also Figure 1 The present application provides a method for testing the thermal shock resistance of an aluminum electrolysis anode carbon block, the method comprising:
[0037] The present application provides a method for testing the thermal shock resistance of an aluminum electrolysis anode carbon block, the method comprising:
[0038] S1. Sampling is performed at a set position of the aluminum electrolysis anode carbon block to be tested to obtain a sample to be tested having a set size;
[0039] The test sample with set size is obtained from the aluminum electrolysis anode carbon block to ensure the consistency and repeatability of the test.
[0040] In some embodiments, sampling at a set position of the aluminum electrolysis anode carbon block to be tested to obtain a sample to be tested having a set size includes:
[0041] A hollow drill bit is used to drill a sample at a set position of the aluminum electrolysis anode carbon block to be tested, and then processed to form a sample to be tested with a set size.
[0042] Using a hollow drill bit to drill the sample can accurately control the drilling position and depth and reduce damage to other parts of the carbon block during the sampling process.
[0043] In some embodiments, the set size includes: a diameter of 10 mm to 100 mm and a length of 20 mm to 200 mm.
[0044] The sample to be tested is a cylinder, and the diameter of the sample to be tested is limited to 10mm to 100mm and the length is 20mm to 200mm, so as to more comprehensively reflect the performance of the carbon block and reduce the complexity and cost of the test. For example, the diameter of the sample to be tested can be 10mm, 20mm, 40mm, 60mm, 80mm, 100mm, etc., and the length can be 20mm, 40mm, 60mm, 80mm, 100mm, 120mm, 150mm, 180mm, 200mm, etc.
[0045] In some embodiments, the set position is the bottom or side of the aluminum electrolysis anode carbon block to be tested.
[0046] The bottom and sides of the anode carbon block for aluminum electrolysis are the areas where the anode carbon block is most affected by force and temperature in the electrolytic cell. Therefore, selecting samples at these locations can more representatively reflect the performance of the carbon block.
[0047] S2, pre-treating the sample to be tested;
[0048] Pretreatment can eliminate stress and moisture inside the test sample to ensure the accuracy of the test results.
[0049] In some embodiments, the pre-treating the sample to be tested comprises:
[0050] The sample to be tested is dried for pretreatment.
[0051] In some embodiments, the drying temperature is 100° C. to 300° C., and the drying time is 0.5 h to 2 h.
[0052] The drying temperature is limited to 100°C to 300°C, and the drying time is 0.5h to 2h, so as to ensure that the moisture inside the sample is fully removed, and at the same time, avoid oxidation of the surface of the carbon block or damage to the structure. Exemplarily, the drying temperature can be 100°C, 120°C, 150°C, 180°C, 200°C, 250°C, 280°C, 300°C, etc., and the drying time can be 0.5h, 0.8h, 1h, 1.2h, 1.4h, 1.6h, 1.8h, 2h, etc.
[0053] In some embodiments, after pre-treating the sample to be tested, the method further comprises:
[0054] The pre-treated sample to be tested is mounted on a sample holder.
[0055] It should be noted that the sample holder is a device specially used to fix the experimental sample. Through its specific clamp or support structure, the sample is firmly fixed in a certain position for subsequent experiments or analysis. In order to ensure the stability and safety of the test sample in subsequent tests, it is usually necessary to install it on the sample holder. This step is of great significance to reduce adverse phenomena such as movement, rotation or falling off of the sample during thermal shock. At the same time, it is necessary to select a suitable sample holder based on factors such as the size, shape and weight of the sample. The holder should have good high temperature resistance and sufficient mechanical strength to withstand the thermal and mechanical stresses during the test.
[0056] In some embodiments, the number of samples to be tested mounted on the sample holder may be determined to be one or more according to the size of the furnace of the heating device, and the samples to be tested may be from the same batch or different batches.
[0057] S3, placing the pretreated sample to be tested in an inert atmosphere and performing a heat preservation treatment at a set temperature;
[0058] It should be noted that the insulation treatment uses a heating device, which usually refers to a high-temperature furnace or similar heating equipment. It should have the ability to accurately control the temperature to ensure that the sample can be evenly and stably heated to the required temperature.
[0059] The sample to be tested is placed directly in the heating device and is kept warm until it reaches the set temperature, thereby simulating the process of the anode carbon block rapidly rising from low temperature to high temperature during electrolysis. At the same time, the introduction of inert atmosphere (such as nitrogen, argon, etc.) is to prevent the sample from reacting with oxygen in the air at high temperature, causing oxidation or other unnecessary chemical changes, thereby ensuring the accuracy of the test results.
[0060] In some embodiments, the set temperature is 900°C to 1000°C.
[0061] In some embodiments, the heat preservation treatment time is 5 minutes to 30 minutes.
[0062] The actual working temperature of the anode carbon block during the electrolysis process is usually between 900°C and 1000°C. The temperature of the heating furnace is limited to 900°C to 1000°C, and the insulation treatment time is 5min to 30min, so as to better simulate the working environment of the anode carbon block in the electrolytic cell. Exemplarily, the set temperature of the heating furnace is 900°C, 920°C, 940°C, 950°C, 960°C, 980°C, 990°C, 1000°C, etc., and the insulation treatment time can be 5min, 8min, 10min, 15min, 20min, 25min, 30min, etc.
[0063] In some embodiments, the interval between placing the pretreated sample to be tested in the inert atmosphere and subjecting the pretreated sample to the heat preservation treatment is 2 min to 5 min.
[0064] After the pre-treated test sample is placed in the heating device, the heating device needs a certain amount of time to recover to the set temperature. This time is usually 2 minutes to 5 minutes, depending on the heating efficiency of the heating device and the initial temperature of the sample. A shorter recovery time helps to reduce energy loss and unnecessary waiting time during the test and improve test efficiency. Exemplarily, the time it takes for the temperature of the heating device to recover to the set temperature can be 2 minutes, 2.5 minutes, 3 minutes, 3.5 minutes, 4 minutes, 4.5 minutes, 5 minutes, etc.
[0065] S4, cooling the test sample after the heat preservation treatment to room temperature in the inert atmosphere;
[0066] Step S4 may specifically include: placing the test sample after the heat preservation treatment in a cooling device filled with inert gas to cool it to room temperature.
[0067] By cooling the sample to be tested to room temperature, the cooling process of the anode carbon block suddenly encountering cold air or electrolyte during electrolysis is simulated. At the same time, cooling under an inert atmosphere can prevent the sample from coming into contact with oxygen in the air, thereby avoiding oxidation reactions. Oxidation reactions may change the properties of the sample and affect the accuracy of the test results.
[0068] S5, determining whether the sample to be tested is broken after being cooled to room temperature; if not, looping steps S2 to S4 until the sample to be tested is broken; if broken, recording the number of tests when the break occurs;
[0069] The fracture condition of the specimens was observed through cyclic tests to evaluate their thermal shock resistance.
[0070] S6. According to the number of tests, the thermal shock resistance grade of the aluminum electrolysis anode carbon block to be tested is obtained.
[0071] The thermal shock resistance grade of the anode carbon block is evaluated according to the number of tests. Specifically, the thermal shock resistance grade of the anode carbon block can be determined by comparing the recorded number of tests with the standard according to a predetermined evaluation standard or grading standard.
[0072] In some embodiments, obtaining the thermal shock resistance grade of the aluminum electrolysis anode carbon block to be tested according to the number of tests includes:
[0073] According to the test times, the thermal shock resistance grade of the aluminum electrolysis anode carbon block to be tested is obtained; wherein,
[0074] When the test number is ≥5 times, the thermal shock resistance grade of the aluminum electrolysis anode carbon block to be tested is grade A;
[0075] When the test number is 2 to 4 times, the thermal shock resistance grade of the aluminum electrolysis anode carbon block to be tested is Class B;
[0076] When the test number is 1, the thermal shock resistance grade of the aluminum electrolysis anode carbon block to be tested is grade C;
[0077] Among them, grade A is better than grade B, and grade B is better than grade C.
[0078] The thermal shock resistance grade of the anode carbon block is determined by comparing the number of tests when the sample breaks under specific test conditions with the predetermined evaluation criteria. The specific grading standards may vary due to different application requirements, but can generally follow similar logic as follows: Grade A: When the sample can withstand higher temperature changes without breaking during the test, that is, the number of tests when the break occurs is ≥5 times, the anode carbon block is considered to have excellent thermal shock resistance and is rated as Grade A. Grade B: If the sample shows good thermal shock resistance in the test, but is slightly worse than Grade A, that is, the number of tests when the break occurs is between 2 and 4 times (including 2 and 4 times), it is rated as Grade B. Grade C: When the sample breaks quickly during the test, that is, the number of tests when the break occurs is only 1, it indicates that the thermal shock resistance of the anode carbon block is poor and is rated as Grade C.
[0079] In some embodiments, if no fracture occurs and cracks appear in the test sample, the number and length, width and depth of the cracks are recorded.
[0080] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to industry standards. If there is no corresponding industry standard, then the conditions recommended by the manufacturer are followed.
[0081] Example 1
[0082] This embodiment provides a method for testing the thermal shock resistance of an aluminum electrolysis anode carbon block, wherein the testing process comprises the following steps:
[0083] S11. Use a hollow drill bit with an inner diameter of 110 mm to drill a sample with a length of 210 mm on the aluminum electrolysis anode carbon block to be tested. The sampling position is at the bottom of the aluminum electrolysis anode carbon block. Process the drilled sample into a cylinder with a diameter of 100 mm and a length of 200 mm to obtain a sample to be tested;
[0084] S21, drying the sample to be tested at 300°C for 2h;
[0085] S31, installing the dried test sample on the sample holder, placing the installed test sample in a heating furnace set at 1000°C for 30 minutes, restoring the furnace temperature to the set temperature within 5 minutes, and continuously filling the heating furnace with argon gas;
[0086] S41, placing the test sample after the heat preservation treatment into a cooling device filled with argon gas, and cooling it to room temperature after a certain period of time;
[0087] S51, take out the sample to be tested that has been cooled to room temperature from the cooling device, and observe whether the sample has cracks or breaks. If the sample to be tested has not broken or cracked, then loop through steps S11 to S41. If the sample to be tested breaks after two cycles, then the test process ends;
[0088] S61. The sample to be tested broke after three tests, indicating that the thermal shock resistance grade of the aluminum electrolysis anode carbon block to be tested is Class B, and the thermal shock resistance is good.
[0089] Example 2
[0090] This embodiment provides a method for testing the thermal shock resistance of an aluminum electrolysis anode carbon block, wherein the testing process comprises the following steps:
[0091] S12, use a hollow drill bit with an inner diameter of 15 mm to drill a sample with a length of 25 mm on the aluminum electrolysis anode carbon block to be tested, and the sampling position is at the bottom of the aluminum electrolysis anode carbon block, and the drilled sample is processed into a cylinder with a diameter of 10 mm and a length of 20 mm to obtain a sample to be tested;
[0092] S22, drying the sample to be tested at 100°C for 0.5h;
[0093] S32, installing the dried test sample on the sample holder, placing the installed test sample in a heating furnace set at 900°C for 5 minutes, and returning the furnace temperature to the set temperature within 3.5 minutes. The heating furnace is filled with helium and continuously supplied with helium;
[0094] S42, placing the test sample after the heat preservation treatment into a cooling device filled with helium, and cooling it to room temperature after a certain period of time;
[0095] S52, take out the test sample cooled to room temperature from the cooling device, and observe whether the sample has cracks and breaks. If the test sample breaks and has cracks, record the number of cracks and their length, width and depth, and the test process ends;
[0096] S62. The test sample broke after one test, indicating that the thermal shock resistance grade of the aluminum electrolysis anode carbon block to be tested is C, which is very poor.
[0097] Example 3
[0098] This embodiment provides a method for testing the thermal shock resistance of an aluminum electrolysis anode carbon block, wherein the testing process comprises the following steps:
[0099] S13, use a hollow drill bit with an inner diameter of 55 mm to drill a sample with a length of 110 mm on the aluminum electrolysis anode carbon block to be tested, the sampling position is at the bottom of the aluminum electrolysis anode carbon block, and the drilled sample is processed into a cylinder with a diameter of 50 mm and a length of 100 mm to obtain a sample to be tested;
[0100] S23, drying the sample to be tested at 200°C for 1.5h;
[0101] S33, installing the dried test sample on the sample holder, placing the installed test sample in a heating furnace set at 950°C for 20 minutes, and returning the furnace temperature to the set temperature within 2 minutes. The heating furnace is filled with xenon gas and continuously supplied;
[0102] S43, placing the test sample after the heat preservation treatment into a cooling device filled with xenon gas, and cooling it to room temperature after a certain period of time;
[0103] S53, take out the sample to be tested that has been cooled to room temperature from the cooling device, and observe whether the sample has cracks or breaks. If the sample to be tested has not broken or cracked, then loop through steps S11 to S41. If the sample to be tested breaks after four cycles, then the test process ends;
[0104] S63. The sample to be tested broke after 5 tests, indicating that the thermal shock resistance grade of the aluminum electrolysis anode carbon block to be tested is A, and the thermal shock resistance is excellent.
[0105] In addition, one or more technical solutions in the embodiments of the present invention have at least the following technical effects or advantages:
[0106] In the embodiments of the present invention, the thermal shock resistance test method of aluminum electrolysis anode carbon blocks provided can fill the gap in the prior art for thermal shock resistance test methods of aluminum electrolysis anode carbon blocks, thereby reducing the occurrence of cracks and block falling of the anode in the aluminum electrolysis cell, which is beneficial to the stable operation of the aluminum electrolysis cell.
[0107] In the embodiment of the present invention, by directly sampling and testing the aluminum electrolysis anode carbon block to be tested, the actual thermal shock resistance of the carbon block can be reflected more directly and accurately. This test method avoids the performance deviation that may be caused by using simulated materials or alternative materials.
[0108] In the embodiment of the present invention, the process of multiple cycles of heating, heat preservation and cooling can simulate the thermal shock cycle that the anode carbon block may experience under long-term working conditions, so as to more comprehensively evaluate its thermal shock resistance. This method is helpful to discover the performance degradation or failure problems that may occur in the anode carbon block during long-term use.
[0109] In the embodiment of the present invention, by accurately controlling the test conditions such as the temperature of the heating device, the holding time, and the cooling method, the consistency and repeatability of each test can be ensured, thereby improving the accuracy of the test results. In addition, the use of an inert atmosphere for heating and cooling avoids the reaction of the sample with oxygen in the air, further ensuring the accuracy of the test results.
[0110] In the embodiment of the present invention, the thermal shock resistance test method of the aluminum electrolysis anode carbon block provided is relatively simple to operate and easy to control. In addition, by recording the number of tests when the fracture occurs as an evaluation index, the thermal shock resistance grade of the anode carbon block can be quickly and intuitively obtained, thereby improving the efficiency of the test.
[0111] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.
Claims
1. A thermal shock resistance test method for aluminum electrolysis anode carbon blocks, characterized in that: The method comprises: S1. Sampling is performed at a set position of the aluminum electrolysis anode carbon block to be tested to obtain a sample to be tested having a set size; S2, pre-treating the sample to be tested; S3, placing the pretreated sample to be tested in an inert atmosphere and performing a heat preservation treatment at a set temperature; S4, cooling the test sample after the heat preservation treatment to room temperature in the inert atmosphere; S5, determining whether the sample to be tested is broken after being cooled to room temperature; if not, looping steps S2 to S4 until the sample to be tested is broken; if broken, recording the number of tests when the break occurs; S6. According to the number of tests, the thermal shock resistance grade of the aluminum electrolysis anode carbon block to be tested is obtained.
2. The method according to claim 1, characterized in that The step of obtaining the thermal shock resistance grade of the aluminum electrolysis anode carbon block to be tested according to the number of tests comprises: According to the test times, the thermal shock resistance grade of the aluminum electrolysis anode carbon block to be tested is obtained; wherein, When the test number is ≥5 times, the thermal shock resistance grade of the aluminum electrolysis anode carbon block to be tested is grade A; When the test number is 2 to 4 times, the thermal shock resistance grade of the aluminum electrolysis anode carbon block to be tested is Class B; When the test number is 1, the thermal shock resistance grade of the aluminum electrolysis anode carbon block to be tested is grade C; Among them, grade A is better than grade B, and grade B is better than grade C.
3. The method according to claim 1, characterized in that The set dimensions include: a diameter of 10 mm to 100 mm and a length of 20 mm to 200 mm.
4. The method according to claim 1, characterized in that: The set position is the bottom or side of the aluminum electrolysis anode carbon block to be tested.
5. The method according to claim 1, characterized in that The pre-processing of the sample to be tested comprises: The test sample is dried to perform pretreatment.
6. The method according to claim 5, characterized in that The drying temperature is 100° C. to 300° C., and the drying time is 0.5 h to 2 h.
7. The method according to claim 1, characterized in that The set temperature is 900°C to 1000°C.
8. The method according to claim 1, characterized in that The time of the heat preservation treatment is 5 minutes to 30 minutes.
9. The method according to claim 1, characterized in that: The interval time between placing the pretreated sample to be tested in the inert atmosphere and subjecting the pretreated sample to the heat preservation treatment is 2 minutes to 5 minutes.