High-wear-resistance anti-reflection anti-dazzle film and display device

By adopting a three-layer structure high wear-resistant and anti-glare film in the anti-glare film, the wet coating process is used to simplify the preparation process, reduce costs, and improve the anti-glare performance of the film, solving the existing solutions The problem of cumbersome preparation process and high cost in the technology.

CN119065035APending Publication Date: 2024-12-03JIANGSU RIJIU OPTOELECTRONICS LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411352535.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-26
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The preparation process of the existing anti-glare and impermeable film is cumbersome and expensive. It is necessary to first apply the anti-glare coating by wet method, then magnetron sputter the impermeable layer, and finally spray the anti-glare layer.

Method used

High wear-resistance and anti-glare film with three-layer structure, including hardened anti-glare UV barrier layer, high refractive optical layer and low fold wear-resistant layer, prepared by wet coating process, high refractive optical layer and low fold resistance The grinding layer cooperates to form an optical anti-reverse structure to improve the anti-reverse effect, and improve anti-glare and mechanical properties by adding a hardened anti-glare ultraviolet barrier layer.

Benefits of technology

The preparation process is simplified, the cost is reduced, and the film is significantly improved. The film has anti-reflection, wear resistance and anti-glare properties are ensured, ensuring excellent visual effects and mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119065035A_ABST
    Figure CN119065035A_ABST
Patent Text Reader

Abstract

The invention discloses a high-wear-resistance anti-reflection anti-dazzle film and a display device, and the high-wear-resistance anti-reflection anti-dazzle film comprises a base material layer, a hardened anti-dazzle ultraviolet blocking layer, a hard anti-dazzle ultraviolet blocking layer, a transparent anti-dazzle layer and a transparent anti-dazzle ultraviolet blocking layer, the high-refractive-index optical layer is arranged on the side, away from the base material layer, of the hardened anti-dazzle ultraviolet blocking layer; the low-refractive-index wear-resistant layer is arranged on the surface, deviating from the base material layer, of the high-refractive-index The refractive index of the high-refractive-index optical layer is 1.68-1.70, the refractive index of the low-refractive-index wear-resistant layer is 1.33-1.42, and the high-refractive-index optical layer and the low-refractive-index wear-resistant layer are matched to form an optical anti-reflection structure. A three-layer coating structure is adopted, the high-refractive-index optical layer and the low-refractive-index wear-resistant layer are matched to form an optical anti-reflection structure, the anti-reflection effect is improved, the anti-dazzle performance and the mechanical performance are improved through the first hardened anti-dazzle ultraviolet blocking layer, on the other hand, the anti-reflection effect is further improved, and it is guaranteed that the high-wear-resistant anti-reflection anti-dazzle film has excellent anti-reflection, anti-dazzle, mechanical and wear-resistant performance; the coating can be prepared through a wet coating process, the preparation process is simple, and the cost is relatively low.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of optical films, and specifically relates to a highly wear-resistant anti-reflection and anti-glare film and a display device. Background Art

[0002] In order to improve the visual experience and reduce user eye fatigue, monitors are now beginning to use anti-glare and anti-reflection films on the screen surface. Anti-glare and anti-reflection films can reduce reflected and scattered light on the screen surface, change the transmission and refraction rules of light, and reduce the generation of glare; scattered light can be evenly dispersed on the screen surface, reducing the light directly shining on the user's eyes, providing a clearer and more comfortable viewing experience, especially in bright outdoor environments or under strong light, it can effectively reduce the interference of glare on vision; reduce external interference light, better display its original color, and improve visual effects.

[0003] In order to achieve the anti-glare and anti-reflection effects, the existing anti-glare and anti-reflection films generally adopt a structure in which an anti-glare coating and an anti-reflection layer are superimposed. The anti-reflection layer must be prepared using a magnetron sputtering process. The preparation process requires first wet coating of the anti-glare coating, then magnetron sputtering of the anti-reflection layer, and finally spraying of the anti-fouling layer. The process is cumbersome and costly. Summary of the invention

[0004] The purpose of the present application is to provide a highly wear-resistant anti-reflection and anti-glare film and display device to solve the technical problem that the anti-glare and anti-reflection film in the prior art needs to first be wet-coated with an anti-glare coating, then magnetron sputtered with an anti-reflection layer, and finally sprayed with an anti-fouling layer, which is a cumbersome and costly process.

[0005] In order to achieve the above-mentioned object, the first aspect of the present application provides a highly wear-resistant anti-reflection and anti-glare film, comprising:

[0006] Substrate layer:

[0007] A hardened anti-glare UV blocking layer is arranged on one side of the substrate layer;

[0008] A high refractive index optical layer is arranged on a side of the hardened anti-glare UV blocking layer away from the substrate layer;

[0009] A low-refractive wear-resistant layer is arranged on a side of the high-refractive optical layer away from the substrate layer;

[0010] The refractive index of the high-refractive optical layer is 1.68-1.70, the refractive index of the low-refractive wear-resistant layer is 1.33-1.42, and the high-refractive optical layer and the low-refractive wear-resistant layer cooperate to form an optical anti-reflection structure.

[0011] In one or more embodiments, the thickness of the high refractive index optical layer is 130-180 nm, and the thickness of the low refractive index wear-resistant layer is 90-130 nm.

[0012] In one or more embodiments, the hardened anti-glare UV blocking layer has a refractive index of 1.50 to 1.54 and a thickness of 3 to 5 μm.

[0013] In one or more embodiments, the substrate layer is a PET substrate layer or a SRF substrate layer.

[0014] In one or more embodiments, the coating liquid of the hardened anti-glare UV blocking layer comprises the following components in parts by weight: 40 to 50 parts of a first acrylic resin; 15 to 25 parts of inorganic hard particles; 1 to 2 parts of a UV blocking agent; 3 to 6 parts of a photoinitiator; and 50 to 100 parts of an organic solvent.

[0015] Wherein, the refractive index of the first acrylic resin is 1.50 to 1.54; and / or,

[0016] The first acrylic resin includes one or more combinations of pentaerythritol triacrylate, trimethylolpropane triacrylate, trimethylolpentane trimethacrylate, dipentaerythritol acrylate, trimethylolpropane triacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, and dipentaerythritol hexaacrylate.

[0017] In one or more embodiments, the inorganic hardening particles include aluminum oxide particles having a diameter of 3 to 4 μm.

[0018] In one or more embodiments, the coating solution of the high refractive optical layer includes the following components in parts by weight: 10 to 20 parts of a second acrylic resin; 3 to 6 parts of a photoinitiator; 50 to 100 parts of an organic solvent;

[0019] Wherein, the refractive index of the second acrylic resin is 1.68 to 1.70; and / or,

[0020] The second acrylic resin includes one or a combination of isobutyl methacrylate, ethylene glycol dimethacrylate, trimethylolpropane trimethacrylate, 2-hydroxypropyl acrylate, and pentanediol diacrylate.

[0021] In one or more embodiments, the coating liquid of the low-fold wear-resistant layer includes the following components in parts by weight: 10 to 20 parts of a third acrylic resin; 0.5 to 2 parts of an AF additive; 2 to 5 parts of inorganic wear-resistant particles; 3 to 5 parts of a photoinitiator; and 50 to 100 parts of an organic solvent.

[0022] Wherein, the refractive index of the third acrylic resin is 1.33 to 1.42; and / or,

[0023] The third acrylic resin includes one or a combination of pentaerythritol diacrylate, dipentaerythritol pentaacrylate, ethylene glycol diacrylate, pentanediol diacrylate, 2-hydroxyethyl methacrylate, trimethylolpentane trimethacrylate, pentaerythritol tetraacrylate, and dipentaerythritol acrylate.

[0024] In one or more embodiments, the inorganic wear-resistant particles include reactant particles of dimethylhydroxyl-terminated siloxane and silicon dioxide, and have a diameter of 100 to 150 nm.

[0025] In order to achieve the above objectives, the second aspect of the present application provides a display device, including a screen and the high wear-resistant anti-reflection and anti-glare film described in any of the above embodiments, wherein the substrate layer of the high wear-resistant anti-reflection and anti-glare film is adhered to the surface of the screen.

[0026] Different from the prior art, the beneficial effects of this application are:

[0027] The high wear-resistant anti-reflection and anti-glare film of the present application adopts a three-layer coating structure, wherein the high refractive index optical layer and the low refractive index wear-resistant layer cooperate to form an optical anti-reflection structure to improve the anti-reflection effect. The low refractive index wear-resistant layer significantly improves the wear resistance of the film layer. The hardened anti-glare UV blocking layer improves the anti-glare and mechanical properties of the film layer on the one hand, and further improves the anti-reflection effect on the other hand, thereby ensuring that the high wear-resistant anti-reflection and anti-glare film has excellent anti-reflection performance, anti-glare performance, mechanical performance and wear resistance.

[0028] The high wear-resistant anti-reflection and anti-glare film of the present application can be prepared by a wet coating process, and the preparation process is simple and the cost is low. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0030] Figure 1 It is a schematic structural diagram of an embodiment of a highly wear-resistant anti-reflection and anti-glare film of the present application. DETAILED DESCRIPTION

[0031] In order to enable those skilled in the art to better understand the technical solutions in the present application, the technical solutions in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without creative work should fall within the scope of protection of the present application.

[0032] In order to solve the technical problem that the anti-reflection layer of the existing anti-glare anti-reflection film must be prepared by a magnetron sputtering process, and the preparation process requires first wet coating of the anti-glare coating, then magnetron sputtering of the anti-reflection layer, and finally spraying of the anti-fouling layer, the process is cumbersome and costly, the applicant has developed a new type of highly wear-resistant anti-reflection anti-glare film, the film layer can be prepared entirely by a wet coating process, the preparation process is simple, the cost is low, and it has excellent anti-reflection, wear resistance and anti-glare properties.

[0033] Specifically, see Figure 1 , Figure 1 It is a schematic structural diagram of an embodiment of a highly wear-resistant anti-reflection and anti-glare film of the present application.

[0034] like Figure 1 As shown, the highly wear-resistant anti-reflection and anti-glare film comprises a substrate layer 100, a hardened anti-glare UV blocking layer 200, a high-refractive optical layer 300 and a low-refractive wear-resistant layer 400 which are stacked in sequence.

[0035] The refractive index of the high refractive index optical layer 300 is 1.68-1.70, and the refractive index of the low refractive index wear-resistant layer 400 is 1.33-1.42, so that the high refractive index optical layer 300 and the low refractive index wear-resistant layer 400 can cooperate to form an optical anti-reflection structure.

[0036] In order to optimize optical matching and improve the anti-reflection effect, in one embodiment, the thickness of the high-refractive optical layer 300 may be 130-180 nm, and the thickness of the low-refractive wear-resistant layer 400 may be 90-130 nm.

[0037] In order to further improve the anti-reflection effect, in one embodiment, the refractive index of the hardened anti-glare UV blocking layer 200 may be 1.50-1.54, and the thickness may be 3-5 μm.

[0038] Based on the above three-layer structure, the anti-reflection optical effect of the film is significantly improved, and at the same time the mechanical properties of the film are improved.

[0039] The material composition of each layer of the present application is described in detail below. In one embodiment, the material of the substrate layer 100 can be PET or SRF, and its thickness can be adjusted based on actual working conditions, for example, it can be 125μm, 100μm, etc., and the effect of this embodiment can be achieved under the premise of transmittance.

[0040] In one embodiment, the hardened anti-glare UV blocking layer 200 is obtained by coating and curing, and its coating liquid may include the following components in parts by weight: 40 to 50 parts of a first acrylic resin; 15 to 25 parts of inorganic hardening particles; 1 to 2 parts of a UV blocker; 3 to 6 parts of a photoinitiator; and 50 to 100 parts of an organic solvent.

[0041] The refractive index of the first acrylic resin may be 1.50-1.54, so as to control the refractive index of the hardened anti-glare UV blocking layer 200 .

[0042] Specifically, the first acrylic resin may include one or more combinations of pentaerythritol triacrylate trimethylolpropane triacrylate, trimethylolpentane trimethacrylate, dipentaerythritol acrylate, trimethylolpropane triacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, and dipentaerythritol hexaacrylate.

[0043] In one embodiment, the inorganic hardening particles can be aluminum oxide particles with a diameter of 3 to 4 μm, which can improve the hardness on the one hand, and on the other hand, the aluminum oxide particles can be stacked on the resin surface to form an uneven structure, which can reflect external light back in the form of diffuse reflection to achieve an anti-glare effect.

[0044] In one embodiment, the high refractive optical layer 300 can be obtained by coating and curing, and the coating liquid thereof may include the following components in parts by weight: 10 to 20 parts of a second acrylic resin; 3 to 6 parts of a photoinitiator; and 50 to 100 parts of an organic solvent.

[0045] The refractive index of the second acrylic resin is 1.68-1.70, so as to control the refractive index of the high refractive index optical layer 300 .

[0046] Specifically, the second acrylic resin may include one or a combination of isobutyl methacrylate, ethylene glycol dimethacrylate, trimethylolpropane trimethacrylate, 2-hydroxypropyl acrylate, and pentylene glycol diacrylate.

[0047] In one embodiment, the low-fold wear-resistant layer 400 can be obtained by coating and curing, and its coating liquid may include the following components in parts by weight: 10 to 20 parts of a third acrylic resin; 0.5 to 2 parts of an AF additive; 2 to 5 parts of inorganic wear-resistant particles; 3 to 5 parts of a photoinitiator; and 50 to 100 parts of an organic solvent.

[0048] The refractive index of the third acrylic resin is 1.33-1.42, so as to control the refractive index of the low-reflection wear-resistant layer 400 .

[0049] Specifically, the third acrylic resin may include one or a combination of pentaerythritol diacrylate, dipentaerythritol pentaacrylate, ethylene glycol diacrylate, p-pentanediol diacrylate, 2-hydroxyethyl methacrylate, trimethylolpentane trimethacrylate, pentaerythritol tetraacrylate, and dipentaerythritol acrylate.

[0050] In one embodiment, the inorganic wear-resistant particles may include reactant particles of dimethylhydroxyl-terminated siloxane and silicon dioxide, with a diameter of 100 to 150 nm, thereby significantly improving the wear resistance.

[0051] It should be noted that in the material composition of each of the above layers, the UV blocker, the photoinitiator and the organic solvent may be any UV blocker, photoinitiator and organic solvent commonly used in the art.

[0052] Exemplarily, the UV blocker can be Jedewin UV 571, the photoinitiator can be BASF 184, and the organic solvent can be one or more combinations of butanone, methyl isobutyl ketone, acetone or cyclopentanone, propylene glycol methyl ether, ethyl acetate, butyl acetate, amyl acetate, methanol, ethanol, n-propanol, butanol, ethylene glycol ethyl ether, ethylene glycol butyl ether, and diethylene glycol ethyl ether.

[0053] The present application also provides a display device, comprising a screen and a highly wear-resistant anti-reflection and anti-glare film of any of the above-mentioned embodiments, wherein the substrate layer 100 of the highly wear-resistant anti-reflection and anti-glare film is adhered to the surface of the screen, thereby improving the visual effect of the screen and providing a clearer and more comfortable viewing experience.

[0054] The beneficial effects of the technical solution of the present application are described in detail below in conjunction with specific embodiments.

[0055] Embodiment 1:

[0056] A highly wear-resistant anti-reflection and anti-glare film is prepared by the following method:

[0057] 1. Preparation of hardened anti-glare UV blocking layer: Take 18 parts of aluminum oxide (4μm) particles and dissolve them in a mixed solvent of 20 parts of butanone and 30 parts of propylene glycol methyl ether, and stir them at room temperature for 4 hours using a magnetic stirrer; after stirring, add 45 parts of Halima UVH-D-ZR-174-1 (the first acrylic resin) successively, and then stir them at room temperature for 2 hours using a magnetic stirrer, and finally add 4 parts of BASF 184 and 1.5 parts of Jedewin UV 571 and stir evenly; use a 12# wire rod to spin-coat the coating liquid on a 125μm PET, put it in an oven at 80℃ and bake it for 2 minutes, and then put the baked sample into a UV machine for curing, and the curing conditions are 300mJ / cm 2 Curing under ultraviolet light conditions to prepare a 4 μm thick hardened anti-glare ultraviolet barrier layer;

[0058] 2. Preparation of high refractive index optical layer: Dissolve 12 parts of TYZ70-RA01-CN (second acrylic resin) in a mixed solvent of 35 parts of butanone and 45 parts of propylene glycol methyl ether, and stir at room temperature for 4 hours using a magnetic stirrer; after stirring, add 4 parts of BASF 184 and stir evenly; use a 4# wire rod to spin-coat the coating liquid on the above-mentioned hardened anti-glare UV blocking layer, bake it in an oven at 80°C for 2 minutes, and then put the baked sample into a UV machine for curing. The curing conditions are 300mJ / cm 2 Curing under ultraviolet light conditions to prepare a 170nm thick high refractive index optical layer;

[0059] 3. Preparation of low-refractive wear-resistant layer: 3 parts of dimethylhydroxyl-terminated siloxane and silicon dioxide reactant particles (120 nm) were dissolved in a mixed solvent of 30 parts of butanone and 45 parts of propylene glycol methyl ether, and stirred at room temperature for 4 hours using a magnetic stirrer; after stirring, 10 parts of Ningbo Tianxuan New Materials SPC-1410 (third acrylic resin) were added, and then stirred at room temperature for 2 hours using a magnetic stirrer, and finally 4 parts of BASF 184 and 1 part of Shin-Etsu KY1203 were added and stirred evenly; using a 3# wire rod, the coating liquid was spin-coated on the above-mentioned high-refractive optical layer, and placed in an 80°C oven for baking for 2 minutes, and then the baked sample was placed in a UV machine for curing, and the curing conditions were 500mJ / cm 2 The film was cured under ultraviolet light to prepare a 110 nm thick low-fold wear-resistant layer, thereby obtaining a highly wear-resistant anti-reflection and anti-glare film.

[0060] Embodiment 2:

[0061] A highly wear-resistant anti-reflection and anti-glare film, the preparation method of which is substantially the same as that of Example 1, except that:

[0062] The thickness of the hardened anti-glare UV blocking layer of this embodiment is 5 μm, and the amount of aluminum oxide particles added to the coating liquid of the hardened anti-glare UV blocking layer is 25 parts.

[0063] Embodiment 3:

[0064] A highly wear-resistant anti-reflection and anti-glare film, the preparation method of which is substantially the same as that of Example 1, except that:

[0065] The amount of the reaction product particles of dimethylhydroxyl-terminated siloxane and silicon dioxide added to the coating solution of the low-fold wear-resistant layer of this embodiment is 5 parts.

[0066] Embodiment 4:

[0067] A highly wear-resistant anti-reflection and anti-glare film, the preparation method of which is substantially the same as that of Example 1, except that:

[0068] In this embodiment, the thickness of the hardened anti-glare UV blocking layer is 3 μm; the thickness of the high-refractive optical layer is 130 nm; and the thickness of the low-refractive wear-resistant layer is 90 nm.

[0069] Embodiment 5:

[0070] A highly wear-resistant anti-reflection and anti-glare film, the preparation method of which is substantially the same as that of Example 1, except that:

[0071] In this embodiment, the thickness of the high refractive index optical layer is 180 nm; the thickness of the low refractive index wear-resistant layer is 130 nm.

[0072] Comparative Example 1:

[0073] A highly wear-resistant anti-reflection and anti-glare film, the preparation method of which is substantially the same as that of Example 1, except that:

[0074] The coating liquid of the low-fold wear-resistant layer of Comparative Example 1 does not contain particles of the reactant of dimethylhydroxyl-terminated siloxane and silicon dioxide.

[0075] Comparative Example 2:

[0076] A highly wear-resistant anti-reflection and anti-glare film, the preparation method of which is substantially the same as that of Example 1, except that:

[0077] The amount of aluminum oxide particles added to the coating solution of the hardened anti-glare UV blocking layer of Comparative Example 1 is 5 parts.

[0078] Comparative Example 3:

[0079] A highly wear-resistant anti-reflection and anti-glare film, the preparation method of which is substantially the same as that of Example 1, except that:

[0080] The thickness of the low-fold wear-resistant layer of this comparative example is 200 nm.

[0081] Comparative Example 4:

[0082] A highly wear-resistant anti-reflection and anti-glare film, the preparation method of which is substantially the same as that of Example 1, except that:

[0083] The thickness of the high refractive index optical layer in this comparative example was 80 nm.

[0084] Effect example:

[0085] The films of Examples 1 to 3 and Comparative Examples 1 to 4 were tested for optical properties, hardness and wear resistance. The specific test items are as follows:

[0086] 1. Transmittance: Use a transmittance tester to test the transmittance of 380-780nm light incident from the low-reflection wear-resistant layer side, and the transmittance of 380nm light incident from the substrate layer side;

[0087] 2. Haze: Use a haze meter to test the haze of the film;

[0088] 3. Glossiness: Use a gloss meter to test the glossiness of the film surface at an angle of 60°;

[0089] 4. Hardness: Use a graphite pencil to test the surface hardness of the diaphragm according to ASTM D3363 standard;

[0090] 5. Wear resistance: Steel wool wear resistance test method is used, square head: 2cmx2cm, SW: Bon star#0000, load 1kg.

[0091] The test results are shown in the following table:

[0092]

[0093] As shown in the table above, the high wear-resistant anti-reflection and anti-glare films of Examples 1 to 3 have an average reflectivity of more than 94% for light of 380 to 780 nm incident on the low-refractive wear-resistant layer side, a haze of about 10.5%, a glossiness of less than 25.6, a pencil hardness of 4H, and can withstand 5,000 wear cycles with excellent anti-reflection, anti-glare, mechanical and wear-resistant properties.

[0094] Comparing Example 1 with Comparative Example 1, the coating liquid of the low-fold wear-resistant layer of Comparative Example 1 does not contain reactant particles of dimethylhydroxyl-terminated siloxane and silicon dioxide, resulting in poor wear resistance.

[0095] Comparing Example 1 and Comparative Example 2, the amount of aluminum oxide particles added in the coating liquid of the hardened anti-glare UV blocking layer of Comparative Example 2 is 5 parts, the amount added is small, the haze and hardness are low, the glossiness reaches 98.2, and the anti-glare performance and mechanical properties are poor.

[0096] Comparing Example 1 with Comparative Example 3, the thickness of the low-reflection wear-resistant layer of Comparative Example 3 is too large, which affects the optical matching, resulting in low transmittance and poor anti-reflection performance;

[0097] Comparing Example 1 with Comparative Example 4, the thickness of the high refractive index optical layer in Comparative Example 4 is too small, which affects the optical matching, resulting in lower transmittance and poor anti-reflection performance.

[0098] It is obvious to those skilled in the art that the present application is not limited to the details of the exemplary embodiments described above, and that the present application can be implemented in other specific forms without departing from the spirit or essential features of the present application. Therefore, the embodiments should be regarded as exemplary and non-limiting in all respects, and the scope of the present application is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present application. Any reference numeral in a claim should not be regarded as limiting the claim to which it relates.

[0099] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A highly wear-resistant anti-reflection and anti-glare film, characterized in that: include: Substrate layer: A hardened anti-glare UV blocking layer is arranged on one side of the substrate layer; A high refractive index optical layer is arranged on a side of the hardened anti-glare UV blocking layer away from the substrate layer; A low-refractive wear-resistant layer is arranged on a side of the high-refractive optical layer away from the substrate layer; The refractive index of the high-refractive optical layer is 1.68-1.70, the refractive index of the low-refractive wear-resistant layer is 1.33-1.42, and the high-refractive optical layer and the low-refractive wear-resistant layer cooperate to form an optical anti-reflection structure.

2. The highly wear-resistant anti-reflection and anti-glare film according to claim 1, characterized in that: The thickness of the high-refractive optical layer is 130-180 nm, and the thickness of the low-refractive wear-resistant layer is 90-130 nm.

3. The highly wear-resistant anti-reflection and anti-glare film according to claim 1, characterized in that: The hardened anti-glare UV blocking layer has a refractive index of 1.50 to 1.54 and a thickness of 3 to 5 μm.

4. The highly wear-resistant anti-reflection and anti-glare film according to claim 1, characterized in that: The substrate layer is a PET substrate layer or a SRF substrate layer.

5. The highly wear-resistant anti-reflection and anti-glare film according to claim 1, characterized in that: The coating liquid of the hardened anti-glare UV blocking layer comprises the following components by weight: 40-50 parts of a first acrylic resin; 15-25 parts of inorganic hard particles; 1-2 parts of a UV blocking agent; 3-6 parts of a photoinitiator; and 50-100 parts of an organic solvent. Wherein, the refractive index of the first acrylic resin is 1.50 to 1.54; and / or, The first acrylic resin includes one or more combinations of pentaerythritol triacrylate, trimethylolpropane triacrylate, trimethylolpentane trimethacrylate, dipentaerythritol acrylate, trimethylolpropane triacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, and dipentaerythritol hexaacrylate.

6. The highly wear-resistant anti-reflection and anti-glare film according to claim 5, characterized in that: The inorganic hardening particles include aluminum oxide particles with a diameter of 3 to 4 μm.

7. The highly wear-resistant anti-reflection and anti-glare film according to claim 1, characterized in that: The coating liquid of the high refractive optical layer comprises the following components by weight: 10 to 20 parts of a second acrylic resin; 3 to 6 parts of a photoinitiator; and 50 to 100 parts of an organic solvent. Wherein, the refractive index of the second acrylic resin is 1.68 to 1.70; and / or, The second acrylic resin includes one or a combination of isobutyl methacrylate, ethylene glycol dimethacrylate, trimethylolpropane trimethacrylate, 2-hydroxypropyl acrylate, and pentanediol diacrylate.

8. The highly wear-resistant anti-reflection and anti-glare film according to claim 1, characterized in that: The coating liquid of the low-fold wear-resistant layer includes the following components by weight: 10-20 parts of the third acrylic resin; 0.5-2 parts of the AF auxiliary agent; 2-5 parts of the inorganic wear-resistant particles; 3-5 parts of the photoinitiator; 50-100 parts of the organic solvent; Wherein, the refractive index of the third acrylic resin is 1.33 to 1.42; and / or, The third acrylic resin includes one or a combination of pentaerythritol diacrylate, dipentaerythritol pentaacrylate, ethylene glycol diacrylate, pentanediol diacrylate, 2-hydroxyethyl methacrylate, trimethylolpentane trimethacrylate, pentaerythritol tetraacrylate, and dipentaerythritol acrylate.

9. The highly wear-resistant anti-reflection and anti-glare film according to claim 8, characterized in that: The inorganic wear-resistant particles include reactant particles of dimethylhydroxyl-terminated siloxane and silicon dioxide, and have a diameter of 100 to 150 nm.

10. A display device, characterized in that: The invention comprises a screen and the highly abrasion-resistant anti-reflection and anti-glare film according to any one of claims 1 to 9, wherein the substrate layer of the highly abrasion-resistant anti-reflection and anti-glare film is attached to the surface of the screen.