Resin composition and application thereof

By using resin compositions with carboxyl and carbodiimide groups in the negative patterning process, the low dielectric performance and high reliability requirements of patterned solder-resistant ink layers in the electronic packaging field are solved, and a good appearance is achieved and heat resistance, meet the requirements of thinner and high performance in the field of electronic packaging.

CN119065203AActive Publication Date: 2024-12-03HUAWEI TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310639244.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-31
Publication Date
2024-12-03
Estimated Expiration
2043-05-31

AI Technical Summary

Technical Problem

The prior art is difficult to prepare patterned solder shield ink layers with low dielectric properties, good appearance and high reliability in negative patterning processes, especially under the trend of thinning and high performance in the field of electronic packaging. The requirements for solder shielding ink layers are getting higher and higher.

Method used

A resin composition is provided, including a carboxylic group-containing photosensitive resin and a carbodiimide group-containing polycarbodiimide. The exothermic peak-to-peak temperature measured by differential scanning calorimetry is greater than 90°C to control polycarbonate. Diimine has low reactivity at low temperatures, ensuring the development and storage stability of the photosensitive dry film, and at the same time, cross-linking reaction is carried out during the thermal curing process to improve the cross-linking density and heat resistance of the cured substance.

Benefits of technology

It realizes the low dielectric performance, good appearance and high electrical insulation reliability of the patterned film layer, meets the needs of negative patterning processes, and improves the heat resistance, reflow resistance and flexibility of the patterned solder-resistant ink layer. improves the reliability of electronic packaging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119065203A_ABST
    Figure CN119065203A_ABST
Patent Text Reader

Abstract

The embodiment of the invention provides a resin composition and application thereof. The composition comprises photosensitive resin, polycarbodiimide and a photoinitiator, the molecular structure of the photosensitive resin contains carboxyl and carbon-carbon double bonds, the polycarbodiimide is a polymer with carbodiimide groups, and the exothermic peak temperature, measured by differential scanning calorimetry, of the resin composition is higher than 90 DEG C. The polycarbodiimide in the composition has low reaction activity at the temperature of not more than 90 DEG C, and is hardly subjected to cross-linking reaction with the photosensitive resin, so that a photosensitive dry film formed by baking the composition can have good developability, and a cured product of the composition has good heat resistance, good reflow soldering resistance, low dielectric property and high transparency. The method is suitable for manufacturing a patterned coating with high reliability through a negative patterning process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of photosensitive materials, and in particular to a resin composition and application thereof. Background Art

[0002] In the field of electronic packaging, a patterned solder mask ink layer is usually required on the packaging substrate to selectively mask the surface copper layer, protect the non-welding parts, and improve the reliability of electrical insulation. As electronic devices have developed towards thinner and higher performance in recent years, the requirements for patterned solder mask ink layers have become increasingly higher, such as having lower dielectric properties and good film appearance.

[0003] The patterned solder resist ink layer is usually formed by a negative patterning process. Therefore, it is necessary to provide a photosensitive resin composition suitable for making a patterned solder resist ink layer by a negative patterning process to ensure that its cured product has the characteristics of lower dielectric properties, higher quality reliability, etc. Summary of the invention

[0004] In view of this, the embodiments of the present application provide a resin composition suitable for negative patterning process, and ensure that the patterned film layer produced by the resin composition has the characteristics of low dielectric properties, excellent appearance, etc.

[0005] A first aspect of an embodiment of the present application provides a resin composition, comprising a photosensitive resin, a polycarbodiimide and a photoinitiator, wherein the molecular structure of the photosensitive resin contains a carboxyl group and a carbon-carbon double bond, the polycarbodiimide is a polymer having a carbodiimide group, and wherein the exothermic peak temperature of the resin composition measured by differential scanning calorimetry is greater than 90°C.

[0006] The resin composition contains a photosensitive resin with a carboxyl group suitable for a negative patterning system, and also introduces a polycarbodiimide with a carbodiimide group, which can ensure that the photosensitive dry film formed by the resin composition has a good appearance and few surface defects, and the cured product of the photosensitive dry film has lower dielectric properties and high electrical insulation reliability; at the same time, the peak temperature of the exothermic peak of the overall composition is controlled to be higher than 90°C, which indicates that the introduced polycarbodiimide has a low reaction activity below 90°C, and the carbodiimide group therein basically does not react with the carboxyl group in the photosensitive resin below 90°C, thereby ensuring that the resin composition and the photosensitive film formed by drying at a temperature below 90°C have excellent developability and room temperature storage stability, which can meet the needs of making a patterned solder mask ink layer based on a negative patterning process.

[0007] In the embodiment of the present application, the exothermic peak temperature of the resin composition measured by differential scanning calorimetry is within the range of 100-150° C. In this way, during the low-temperature baking process of the resin composition, the polycarbodiimide does not react with the photosensitive resin, thereby ensuring good subsequent developability, and during the thermal curing process of the composition, the two can fully undergo a cross-linking reaction to improve the cross-linking density and heat resistance of the cured product.

[0008] In the embodiment of the present application, the content of the carbodiimide group in the polycarbodiimide per mol molecular structure is 4-30 mol. This can ensure that the reaction between the polycarbodiimide and the acidic photosensitive resin of the resin composition below 90°C is fully suppressed to ensure good subsequent exposure and developability, and can also ensure that the cured product formed by the resin composition being fully cured at a higher temperature has sufficient crosslinking density and heat resistance.

[0009] In the embodiment of the present application, the weight average molecular weight of the polycarbodiimide is 800-9000. By controlling the molecular weight of the polycarbodiimide, the reaction activity between components of the resin composition containing it can be low below 90°C, and the heat resistance, reflow resistance and flexibility of the cured product can be improved.

[0010] In the embodiment of the present application, the polycarbodiimide comprises a structure shown in formula (I):

[0011]

[0012] In formula (I), A and D are independently selected from one or more of substituted or unsubstituted alkylene, substituted or unsubstituted cycloalkylene, and substituted or unsubstituted arylene, p is in the range of 2-15; Q represents a capping group that blocks the NCO group.

[0013] The degree of polymerization of the repeating unit containing two carbodiimide groups in the above-mentioned polycarbodiimide is in the range of 2-15, which can ensure that the reaction activity of the carbodiimide groups in the polymer is low below 90°C. It is suitable for use in a resin composition for a negative patterning system together with a photosensitive resin with a carboxyl group, ensuring its low-temperature stability and developability after exposure to light.

[0014] In the embodiment of the present application, when p is in the range of 2-4, Q contains an aromatic ring structure; when p is in the range of 5-15, Q contains one or more of an aromatic ring structure, an aliphatic ring structure, and an aliphatic chain structure. In this way, the end-capping group is regulated based on the degree of polymerization of the polycarbodiimide, so that the low-temperature reaction activity of the carbodiimide group in the polycarbodiimide below 90°C can be better ensured, the above-mentioned composition has good developability, and the heat resistance and solder resistance of its cured product are also good.

[0015] In the embodiment of the present application, the weight average molecular weight of the photosensitive resin is 3000-20000; the acid value is 50-120 mgKOH / g. The use of a photosensitive resin with these properties in the above resin composition can ensure that its photopolymerization activity is high, and at the same time, the unexposed part of the dry film formed by drying has a suitable dissolution rate in the alkaline developer.

[0016] In the embodiment of the present application, the molar amount of the carbodiimide group in the polycarbodiimide is 0.2-1.5 times the molar amount of the carboxyl group in the photosensitive resin. This ensures that the storage stability of the resin composition is high, and the flexibility and heat resistance of the cured product are also excellent.

[0017] In some embodiments of the present application, the resin composition further comprises an epoxy resin. During the thermal curing process of the composition (usually at about 150° C.), the epoxy resin can undergo a cross-linking reaction with the carboxyl group in the photosensitive resin and the carbodiimide group in the polycarbodiimide, thereby increasing the cross-linking density of the cured product of the composition, thereby improving its heat resistance and solder resistance, and also facilitating the reduction of the dielectric constant and dielectric loss factor.

[0018] In some embodiments of the present application, the resin composition further includes a colorant; wherein the colorant includes one or more of a pigment and a dye. The polycarbodiimide contained in the resin composition can improve the compatibility of the colorant in the composition system, ensuring that the photosensitive dry film and cured product formed by the resin composition have a smooth appearance with few defects.

[0019] A second aspect of the embodiments of the present application provides a film material, including a photosensitive film, which is formed by drying the resin composition as described in the first aspect of the embodiments of the present application.

[0020] In some embodiments of the present application, the film material may further include a support and a protective film, wherein the photosensitive film and the protective film are sequentially stacked on the support. That is, the film material is generally a three-layer film structure. When in use, the protective film generally needs to be removed first, and only the cured product of the photosensitive film remains in the final product.

[0021] The third aspect of the embodiments of the present application provides the use of the resin composition as described in the first aspect of the embodiments of the present application, or the film material as described in the first aspect of the embodiments of the present application in the preparation of printed circuit boards and packaging of electronic components.

[0022] In some embodiments of the present application, the application may be a patterned solder resist ink layer on a packaging substrate for manufacturing printed circuit boards and electronic components. The patterned solder resist ink layer may have good heat resistance and reflow resistance, acid and alkali resistance, low dielectric properties, and high adhesion to conductor layers such as copper layers, so that the printed circuit boards and packaging structures have high reliability in use.

[0023] The fourth aspect of the embodiment of the present application provides a packaging carrier, which includes a substrate having a conductor layer on the surface, a patterned solder resist ink layer is provided on the conductor layer, and the patterned solder resist ink layer includes a cured product of the resin composition as described in the first aspect of the embodiment of the present application. The cured product of the resin composition has good heat resistance, reflow resistance, acid and alkali resistance, flexibility, high copper adhesion and low dielectric properties, can play a good solder resistance and insulation effect on the substrate with a conductor layer, has high quality reliability, and can further improve the packaging effect of the packaging carrier.

[0024] A fifth aspect of the embodiments of the present application provides a sealed package, which includes a cured product of the resin composition as described in the first aspect of the embodiments of the present application, or a packaging carrier as described in the fourth aspect of the embodiments of the present application.

[0025] In the embodiment of the present application, the sealed package includes the packaging carrier and the electronic components arranged on the packaging carrier, wherein the electronic components are arranged on the patterned solder mask ink layer in the packaging carrier. The electronic components can be one or more of a chip, a transistor, a resistor, a capacitor, and an inductor.

[0026] The sixth aspect of the present application provides an electronic device, which includes a circuit board and a sealed package as described in the fifth aspect of the present application, which is arranged on the circuit board. The electronic device includes the sealed package with high quality reliability, and the use stability of the electronic device can be improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 A schematic structural diagram of a sealed package 100 provided in an embodiment of the present application.

[0028] Figure 2 A schematic diagram of the structure of the film material 200 provided in an embodiment of the present application.

[0029] Figure 3 for Figure 1 A schematic structural diagram of the sealed package 100 after being connected to the circuit board.

[0030] Figure 4 A schematic diagram of the structure of an electronic device 300 provided in an embodiment of the present application.

[0031] Figure 5 This is a DSC curve diagram of the photosensitive resin composition of Example 3 of the present application.

[0032] Figure 6 This is a DSC curve diagram of the photosensitive resin composition of Example 6 of the present application. DETAILED DESCRIPTION

[0033] The technical solution of the present application will be described below in conjunction with the drawings in the embodiments of the present application.

[0034] See also Figure 1 , Figure 1 : is a structural schematic diagram of a sealed package 100 provided in an embodiment of the present application. The sealed package 100 includes a packaging carrier 10 and electronic components 20 arranged on the packaging carrier 10. Among them, the side of the packaging carrier 10 facing the electronic components 20 may have a plurality of solder bumps 13 (for example, gold bumps), and the electronic components 20 can be attached to the packaging carrier 10 by remelting the solder bumps 13. The electronic components 20 can be one or more of a chip, a transistor (such as a diode, a triode), an LED (Light Emitting Diode), a resistor-capacitor-inductor element (such as a resistor, a capacitor, an inductor), etc. In some embodiments, the side of the packaging carrier 10 away from the electronic components 20 may have a plurality of solder balls 14 (such as tin balls) arranged in an array, and the solder balls 14 are used to realize the subsequent electrical connection between the packaging carrier 10 and the circuit board (such as Figure 3 ). Figure 1 The sealed package 100 is called a DGA (Dall Grid Array, ball grid array or solder ball array) package.

[0035] A patterned solder resist ink layer 12 is formed on the package carrier 10. Figure 1 In the example, the package carrier 10 has patterned solder resist ink layers 12 on both sides of the opposite sides. The package carrier 10 includes a substrate 11 having a conductor layer on its surface. Figure 1 In the example, the two opposite surfaces of the substrate 11 are both provided with a conductor layer with a circuit pattern (for example, a copper layer, respectively distinguished by code 101 and 102), and the patterned solder resist ink layer 12 is specifically provided on the conductor layer 101 and the conductor layer 102. In some embodiments, Figure 1 The substrate 11 having a conductor layer on the surface can be specifically a copper-clad laminate with a circuit pattern. The patterned solder mask ink layer 12 does not completely cover the conductor layer. Generally, the substrate 11 having a conductor layer on the surface is not covered at the portion to be electrically connected to other conductive components. Figure 1 In the figure, solder bumps 13 and solder balls 14 are exposed from the patterned solder resist ink layer 12, so as to realize the subsequent electrical connection with the electronic components 20 and the circuit board. The patterned solder resist ink layer 12 can be a cured product of the resin composition provided in the embodiment of the present application.

[0036] Specifically, the resin composition provided in the embodiment of the present application includes: a photosensitive resin, a polycarbodiimide, and a photoinitiator, wherein the molecular structure of the photosensitive resin contains a carboxyl group (-COOH) and a carbon-carbon double bond, and the polycarbodiimide is a polymer having an unprotected carbodiimide group (i.e., -N=C=N-), wherein the exothermic peak temperature of the resin composition measured by differential scanning calorimetry (DSC) is greater than 90°C. It should be noted that since the resin composition of the present application contains a photosensitive resin, it can be referred to as a "photosensitive resin composition".

[0037] The resin composition contains a carboxyl-containing photosensitive resin for a negative patterning system, and also introduces a polycarbodiimide with a carbodiimide group, which can ensure that the photosensitive dry film formed by the resin composition has a good appearance and few surface defects. The cured photosensitive dry film has lower dielectric properties, good heat resistance, reflow resistance, acid and alkali resistance, and based on the strong interaction between the carbodiimide group and the conductor layer such as the copper layer, the application reliability of the resin composition in the field of electronic packaging is also guaranteed. More importantly, the exothermic peak temperature of the DSC curve of the above-mentioned resin composition is greater than 90°C, which indicates that the introduced polycarbodiimide has low reactivity at temperatures below 90°C (the commonly used baking temperature for baking the resin composition to form a dry film is generally 60-80°C), and the carbodiimide group hardly undergoes cross-linking reaction with the carboxyl group in the photosensitive resin. Therefore, the above-mentioned resin composition has excellent room temperature storage stability. Even if the composition is baked into a photosensitive dry film at the above-mentioned baking temperature, the photosensitive dry film also has good storage stability, wherein the reaction of polycarbodiimide with the carboxyl group is also suppressed, thereby ensuring that the development resolution of the dry film is high, which can meet the needs of producing a patterned solder mask ink layer based on a negative patterning process.

[0038] In the present application, the DSC curve of the above-mentioned resin composition can be a DSC curve obtained at a heating rate of 10°C / minute under an atmospheric atmosphere. Based on the DSC curve, the peak temperature of the exothermic peak can be obtained. Among them, the abscissa of the DSC curve is temperature, calculated in °C, and the ordinate is heat flow, calculated in mW / mg. The DSC curve of the above-mentioned resin composition may have more than one exothermic peak, but the peak temperature of the first exothermic peak with the lowest peak temperature is greater than 90°C.

[0039] In the present application, the peak intensity of the exothermic peak of the resin composition is greater than 0.1mW / mg. The peak intensity is the absolute value of the difference between the heat flow value corresponding to the peak temperature of the exothermic peak and the baseline of the DSC graph of the resin composition (that is, the heat flow corresponding to the lowest point). In this way, tiny exothermic peaks caused by the volatilization of some small molecules or water vapor during the DSC test can be excluded. That is, the present application has an exothermic peak with a peak temperature greater than 90°C and a peak intensity greater than 0.1mW / mg. Below 90°C, no exothermic peak with a peak intensity greater than 0.1mW / mg is observed in the DSC curve of the above-mentioned resin composition.

[0040] Polymers with unprotected carbodiimide groups have also been reported to be used in resin compositions for positive patterning systems, but they are rarely used directly in negative patterning systems. This is mainly because the compositions used in negative patterning systems often contain unsaturated photosensitive resins with carboxyl groups, which are very likely to undergo cross-linking reactions with carbodiimide groups at room temperature and below common baking temperatures, resulting in significant effects on the storage stability and subsequent developability of the composition. In the embodiment of the present application, the content of unprotected carbodiimide groups in the polycarbodiimide with a molecular structure of a control unit mol (i.e., 1 mol) is 4-30 mol. In this way, it can be ensured that the reaction between the polycarbodiimide and the carboxyl group is fully suppressed during the storage of the resin composition at room temperature or during the drying process to form a photosensitive dry film, and the exothermic peak temperature of the resin composition is greater than 90°C, thereby avoiding the subsequent exposure and development properties being affected. It can also ensure that when the photosensitive dry film is completely cured at a higher temperature to form a cured product, there are enough carbodiimide groups to cross-link with the carboxyl groups in the photosensitive resin to increase the cross-linking density of the cured product, thereby greatly improving the heat resistance and mechanical properties of the cured product (the flexibility of the polymer chain segments formed after the reaction of the carbodiimide groups with the carboxyl groups is good), and excellent low dielectric properties are ensured; and based on the strong interaction between the carbodiimide group and the conductor layer such as the copper layer, and the content of the carbodiimide group in the polycarbodiimide is controlled within the above range, the bonding force between the cured product of the resin composition and the conductor layer is strong, thereby ensuring the reliability of the application of the above composition in the field of electronic packaging. Therefore, the above-mentioned condition control can solve the problem that the carbodiimide-containing material is not suitable for use in the photosensitive resin composition for the negative photolithography system and it is difficult to ensure the development resolution of the composition.

[0041] Specifically, in the polycarbodiimide per mol molecular structure, the content of carbodiimide groups can be 4 mol, 5 mol, 6 mol, 8 mol, 10 mol, 12 mol, 15 mol, 16 mol, 18 mol, 20 mol, 22 mol, 25 mol, 26 mol, 28 mol, 30 mol, etc. In some embodiments of the present application, in the polycarbodiimide per mol molecular structure, the content of carbodiimide groups is 6-20 mol, and can further be 8-16 mol. In this way, it can better ensure that the polycarbodiimide has basically no reaction activity below 90°C, and the storage and subsequent development properties of the above-mentioned resin composition are better. For the above-mentioned "content of carbodiimide groups in polycarbodiimide with 1 mol molecular structure", the molar number of the molecular structure of polycarbodiimide can be obtained by the ratio of its mass to the weight-average molecular weight, and the molar number of carbodiimide groups can be reversely monitored by the group that reacts with it, and then the molar amount of carbodiimide groups in the polycarbodiimide per mol molecular structure can be obtained.

[0042] In addition, for the above-mentioned "the content of carbodiimide groups in 1 mol of the molecular structure of the polycarbodiimide is 4-30 mol", it can also be said that the degree of polymerization of the carbodiimide groups in the polycarbodiimide is 4-30. In the embodiment of the present application, when the polycarbodiimide has a repeating unit containing one carbodiimide group (-N=C=N-), the degree of polymerization of the repeating unit is 4-30, and can further be 6-20, 8-16, etc.; when the repeating unit of the polycarbodiimide contains 2 carbodiimide groups (-N=C=N-), the degree of polymerization of the repeating unit is in the range of 2-15, for example, specifically 2.5, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 14.5, etc., and can further be in the range of 3-10, and in the range of 4-8. Controlling the polymerization degree of the carbodiimide group within this range is more conducive to reducing the reactivity of the carbodiimide group in the polycarbodiimide below 90° C., thereby ensuring its stability below common baking temperatures.

[0043] In some embodiments of the present application, the exothermic peak temperature of the resin composition measured by the DSC method is greater than or equal to 95° C., and can further be greater than or equal to 100° C. This indicates that at a temperature below 95° C. or even below 100° C., polycarbodiimide and the carboxyl group in the photosensitive resin basically do not react to generate heat, and when the resin composition is baked to form a dry film, the reaction of polycarbodiimide is fully suppressed, so that after the subsequent dry film is exposed, the unexposed area has high solubility in the alkaline developer and the exposed area has good development resistance, thereby obtaining a desired pattern with high development resolution.

[0044] In some embodiments of the present application, in order to balance the good developability of the unexposed area of ​​the dry film of the resin composition and the crosslinking density of the fully cured product of the resin composition, the exothermic peak temperature of the above-mentioned resin composition measured by the DSC method is in the range of 100-200°C, for example, 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, 190°C, etc. In this way, during the low-temperature baking process of the resin composition, the polycarbodiimide does not react with the photosensitive resin, and the developability is good. In the thermal curing process of the composition, the two can fully undergo a crosslinking reaction to improve the crosslinking density and heat resistance of the cured product. In some embodiments, the exothermic peak temperature of the resin composition is between 110-160°C.

[0045] In the present application, the DSC exothermic peak temperature of the above-mentioned resin composition is greater than 90°C, greater than or equal to 95°C, etc., which can be achieved by controlling parameters including "the content of carbodiimide groups per unit mol of molecular structure of polycarbodiimide is 4-30 mol", for example, only controlling "the content of carbodiimide groups per unit mol of molecular structure of polycarbodiimide is 4-30 mol", or it can be achieved based on the content of carbodiimide groups per unit mol of molecular structure of polycarbodiimide being 4-30 mol, and the control of the end-capping groups of the polycarbodiimide.

[0046] In the embodiment of the present application, in the DSC curve of the above resin composition, the starting temperature of each exothermic peak is greater than or equal to 85° C., greater than or equal to 90° C., greater than or equal to 95° C., and even greater than or equal to 100° C. In this way, the peak temperature of each exothermic peak is higher, and must be greater than 90° C., etc., so as to better ensure the storage stability and good developability of the resin composition.

[0047] In the embodiment of the present application, the weight average molecular weight Mw of the polycarbodiimide is 800-9000. This helps to ensure that the negative resin composition containing the polycarbodiimide has low reactivity between components below the common baking temperature, and can also ensure that the cured product of the composition can take into account good flexibility and heat resistance at the same time, especially enhance the reflow resistance of the copper layer covered by it, and is not easy to soften and deform. In some embodiments, the weight average molecular weight Mw of the polycarbodiimide is 1000-4000, and can further be 1500-3500, or 1800-3500, etc. Wherein, the weight average molecular weight refers to the value obtained by gel permeation chromatography (Gel Permeation Chromatography, GPC) according to polystyrene conversion.

[0048] In the embodiment of the present application, the polycarbodiimide comprises a structure shown in formula (I):

[0049]

[0050] In formula (I), A and D are independently selected from one or more of substituted or unsubstituted alkylene, substituted or unsubstituted cycloalkylene, substituted or unsubstituted arylene, p is in the range of 2-15; Q represents a blocking group for blocking the NCO group. Polycarbodiimide is prepared by polycondensation of diisocyanate.

[0051] Wherein, the carbon number of the substituted or unsubstituted alkylene group is 1-20, and can further be 1-10, for example, 1-6 or 1-4, etc., and the alkylene group can be a straight chain or branched alkylene group. Exemplarily, the unsubstituted alkylene group can be a methylene group (-CH2-), an ethylene group (-CH2CH2-), a propylene group (-CH2CH2CH2-), a n-butylene group (-(CH2)4-), a n-pentylene group (-(CH2)5-), a n-hexylene group (-(CH2)6-, also referred to as a hexamethylene group), etc. The carbon number of the substituted or unsubstituted cycloalkylene group is 4-20, and can further be 6-20, 4-15, etc. Exemplarily, the unsubstituted cycloalkylene group can be a cyclobutylene group, a cyclobutylene group, a cyclopentylene group, a cyclohexylene group, etc. The carbon number of the substituted or unsubstituted arylene group is 6-20, for example, 6-15, 6-10, etc. For example, the unsubstituted arylene group may be a phenylene group, a naphthylene group, etc. The substituents in the substituted alkylene group may include, but are not limited to, one or more of a halogen atom, a substituted or unsubstituted aryl group, an alkoxy group, etc. The substituents in the substituted cycloalkylene group and the substituted arylene group may be independently selected from one or more of a halogen atom, a substituted or unsubstituted alkyl group, a substituted or unsubstituted alkoxy group, and a substituted or unsubstituted aryl group.

[0052] In some embodiments of the present application, A and D are independently selected from one or more of substituted or unsubstituted cycloalkylene, substituted or unsubstituted arylene. At this time, the rigidity of the A and D structures is relatively large, which is more conducive to the improvement of the heat resistance of the above-mentioned polycarbodiimide. In addition, when A and D are selected from two or more of substituted or unsubstituted alkylene, substituted or unsubstituted cycloalkylene, substituted or unsubstituted arylene, they can be connected by a chemical bond (such as a connecting single bond, etc.). In some embodiments, A and D are alkylene containing at least one of substituted or unsubstituted cycloalkylene, substituted or unsubstituted arylene.

[0053] In formula (I) of the present application, p represents the degree of polymerization of the above-mentioned polycarbodiimide, specifically the degree of polymerization of the repeating unit containing two carbodiimide groups of the polycarbodiimide. p is in the range of 2-15, specifically 2, 2.5, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14 or 15. In some embodiments, p is 3-10, further 4-8. This is more conducive to the lower reactivity of the above-mentioned polycarbodiimide below the common baking temperature (such as 60-80°C, 80°C is the common upper limit of the baking temperature), avoiding it from reacting with the photosensitive resin with carboxyl groups in the system during storage at room temperature and before baking to form a film, thereby affecting the storage stability and subsequent developability. Based on the range of p, it can be known that the number of carbodiimide groups (-N=C=N-) contained in one molecular structure of polycarbodiimide is 4-30, and further can be 6-20 or 8-16, etc.

[0054] In the present application, Q is a residue produced after a substance (i.e., an end-capping agent) that can react with an isocyanate group (-NCO) reacts with the -NCO at the end of the polycarbodiimide. In some embodiments of the present application, when the above-mentioned p is in the range of 2-4, the end-capping group Q contains an aromatic ring structure. At this time, Q has a large steric hindrance (i.e., an end-capping agent with a large steric hindrance is used to seal), which can well reduce the low-temperature reaction activity of the polycarbodiimide with a low p, and ensure the good developability of the above-mentioned resin composition. Among them, the aromatic ring structure can be one or more of a substituted or unsubstituted benzene ring, a naphthalene ring, an anthracene ring, a binaphthyl ring, a biphenyl, etc. In this case, the end-capping agent corresponding to the Q can be one or more of a phenol (such as phenol, naphthol, etc.), a monovalent aromatic alcohol, a monovalent aromatic amine, an aromatic monoisocyanate, an acid containing an aromatic ring structure, etc. Exemplarily, phenol can include one or more of phenol, naphthol, anthracene, binaphthol, p-fluorobiphenol, p-cyanoterpenol, etc. The aromatic monoisocyanate may be one or more of phenyl isocyanate, tolyl isocyanate, dimethylphenyl isocyanate, 2,6-diisopropylphenyl isocyanate, and the like.

[0055] In other embodiments of the present application, when the above p is an integer of 5-15, the end-capping group Q may contain one or more of an aromatic ring structure, an aliphatic ring structure, and an aliphatic chain structure. When p is within this range, the end-capping group Q of the polycarbodiimide does not necessarily need to contain an aromatic ring structure with large steric hindrance, and the reaction activity of the above polycarbodiimide below 90° C. can be ensured to be low by controlling p alone. In this case, the end-capping agent corresponding to the Q may include, but is not limited to, phenols (such as phenol, naphthol), monohydric alcohols (such as monohydric fatty alcohols, monohydric aromatic alcohols), monoamines (monohydric fatty amines or monohydric aromatic amines, which may be primary amines or secondary amines), monoisocyanates (alicyclic monoisocyanates, alkyl monoisocyanates, aromatic monoisocyanates), acids, acid anhydrides, and silane coupling agents with at least one of -OH, -NH2, -COOH, and epoxy groups.

[0056] The above-mentioned -Q can be represented by -k-Q', wherein Q' represents the parent after removing one group that can react with -NCO from the end-capping agent, and k represents the group or chemical bond formed by the reaction of the group that can react with -NCO in the end-capping agent with -NCO. Taking the end-capping agent as isooctyl alcohol as an example, Q' is CH3CH2CH2CH2-CH(CH2CH3)(CH2-), -k- is -NHCOO-, and the first and second ends are connected to Q'. Wherein, when p is in the range of 2-4, Q' includes an aromatic ring structure. When p is in the range of 5-15, Q' includes one or more of an aromatic ring structure, an aliphatic ring structure, and an aliphatic chain structure.

[0057] In the embodiment of the present application, when the end-capping agent is a phenol or a monohydric alcohol or a silane coupling agent with -OH, -k- is -NHCOO-*. When the end-capping agent is a monoamine or a silane coupling agent with -NH2, -k- is a urea group (-NH-CO-NH-). When the end-capping agent is a monoisocyanate, -k- is -N=C=N-. When the end-capping agent is an acid or a silane coupling agent with -COOH, k is an amide bond (i.e., -NH-CO-*). When the end-capping agent is an anhydride, -k- is -CO-NH-CO-.

[0058] In some embodiments of the present application, when p is in the range of 2-15, the end-capping group Q contains an aromatic ring structure. In this way, the low-temperature reactivity of the carbodiimide group in the polycarbodiimide is lower, the storage stability and developability of the resin composition are better, and the heat resistance of the cured product is better.

[0059] In the embodiment of the present application, the polycarbodiimide contains NCO groups with a content of no more than 5 wt%. That is, the NCO groups in the polycarbodiimide with a mass percentage of less than or equal to 5 wt% are not terminated by Q. To facilitate understanding of this parameter, the structure of the polycarbodiimide can also be expressed as follows: The polycarbodiimide includes a repeating unit represented by formula (i):

[0060]

[0061] Wherein, A and D are independently selected from one or more of substituted or unsubstituted alkylene, substituted or unsubstituted cycloalkylene, substituted or unsubstituted arylene, the degree of polymerization of the repeating unit shown in formula (i) is in the range of 2-15; at least some of the polymer segments shown in formula (i) are terminated by a capping group Q. As mentioned above, when the degree of polymerization p of the repeating unit shown in formula (i) is an integer of 2-4, the Q contains an aromatic ring structure; when p is an integer of 5-15, the Q contains one or more of an aromatic ring structure, an aliphatic ring structure, and an aliphatic chain structure.

[0062] Wherein, in the polycarbodiimide, at least some of the end groups of the polymer segments shown in formula (i) are the above-mentioned Q. In some embodiments, the end groups of some of the polymer segments shown in formula (i) are the above-mentioned Q, and the end groups of some of the polymer segments are -NCO groups. In some other embodiments of the present application, the end groups of all the polymer segments shown in formula (i) are the above-mentioned Q, that is, the polycarbodiimide does not contain uncapped NCO. Wherein, the mass proportion of the NCO groups not capped by Q in the polycarbodiimide is less than or equal to 5wt%. In this way, it is possible to avoid excessive residual active -NCO groups in the polycarbodiimide and cross-linking with hydroxyl groups in the photosensitive resin at below 90°C, so that the solubility of the dry film of the unexposed photosensitive resin composition in the alkaline developer becomes low.

[0063] In the present application, the preparation of the above-mentioned polycarbodiimide may include the following steps:

[0064] At least one diisocyanate substance is subjected to polymerization reaction under stirring conditions at 130° C. to 200° C. in the presence of a catalyst for a period of time, and then a blocking agent is added to block the obtained polymerization product to obtain a polycarbodiimide having a structure shown in formula (I):

[0065]

[0066] In formula (I), A and D are independently selected from one or more of substituted or unsubstituted alkylene, substituted or unsubstituted cycloalkylene, and substituted or unsubstituted arylene, x and y are independently integers of 1-5, p is an integer of 2-15, and Q represents a capping group for blocking the NCO group; wherein the capping agent is a substance that can react with the -NCO group.

[0067] Wherein, the selection of end-capping agent can refer to the description of the previous text of this application. The diisocyanate material can be selected from diphenylmethane diisocyanate (MDI), naphthalene diisocyanate (NDI), toluene diisocyanate (TDI), meta-phenylene diisocyanate (XDI), p-phenylene diisocyanate (PPDI), tetramethyl meta-xylylene diisocyanate (TMXDI), hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI), 1,4-cyclohexane diisocyanate (CHDI), methylcyclohexyl diisocyanate (HTDI), 4,4-dicyclohexylmethane diisocyanate (HMDI) and the like. One or more. Wherein, when A and D are the same in formula (I), only one diisocyanate material can be used.

[0068] Among them, the catalyst can be selected from one or more of alkali metal or alkaline earth metal compounds, organic phosphorus compounds (such as 3-methyl-1-phenyl-2-phosphocyclopentene-1 oxide), tertiary amines (such as triethylamine, tri-n-butylamine, N,N-dimethylaniline, triethylenediamine, triisopropylamine), non-alkaline organic metal compounds (such as dibutyltin dilaurate), etc. Among them, the alkali metal or alkaline earth metal compound can include one or more of alkali metal or alkaline earth metal hydroxides (such as magnesium hydroxide, sodium hydroxide, etc.), inorganic salts (such as sodium carbonate, potassium bicarbonate, etc.), organic salts (such as phenolates, sodium methoxide), etc. The catalyst can enhance the polycondensation reactivity of the diisocyanate substance. The mass of the catalyst can account for 0.01%-2% of the total mass of the reaction raw materials.

[0069] In some embodiments, during the polymerization reaction, an organic solvent (such as toluene, cyclohexanone, etc.) can be added according to the change in the viscosity of the system. The degree of polymerization of the polymerization product can be determined by collecting the mass of CO2 and dibutylamine titration.

[0070] In the present application, the photosensitive resin is a photosensitive prepolymer containing carbon-carbon double bonds and carboxyl groups in its molecular structure, and still has polymerization reactivity. When irradiated with light of a certain wavelength and initiated by a photoinitiator, the photosensitive resin can undergo photopolymerization reaction with the carbon-carbon double bonds it contains, and physically interweave with polycarbodiimide and the like to obtain a cross-linked product with a certain network structure. Subsequently, when the cross-linked product is subjected to a temperature greater than 90°C, the carboxyl groups in the photosensitive resin undergo a cross-linking reaction with the above-mentioned polycarbodiimide to obtain a cured product with a certain network structure.

[0071] In the embodiment of the present application, the weight average molecular weight Mw of the photosensitive resin is 3000-20000. Among them, the photosensitive resin with Mw within this range can not only ensure that it has a high photopolymerization activity, but also ensure that it has a suitable dissolution rate in an alkaline developer and its photopolymerization product has good resistance to development. In the embodiment of the present application, the acid value of the photosensitive resin is 50-120 mgKOH / g. This can better ensure that the solubility of the unexposed dry film of the above-mentioned resin composition in the alkaline developer is suitable to ensure a higher development resolution.

[0072] In the embodiment of the present application, the resin composition may include the following components in parts by weight: 30-40 parts of photosensitive resin, 1-20 parts of polycarbodiimide and 0.5-6 parts of photoinitiator. By the reasonable proportion of the photosensitive resin, the polycarbodiimide and the photoinitiator, it can be ensured that the resin composition has good storage stability, has a suitable viscosity at room temperature to have good coating performance, and ensures that its photocured product has good developability, good adhesion (especially adhesion on the copper layer) and heat resistance, etc.

[0073] Among them, the resin composition may contain one or more photosensitive resins; it may also contain one or more photoinitiators, one or more polycarbodiimides. The above-mentioned weight parts all refer to their respective total weight parts. Specifically, the total weight parts of the photosensitive resin in the above-mentioned resin composition can be 30 parts, 31 parts, 32 parts, 33 parts, 34 parts, 35 parts, 36 parts, 37 parts, 38 parts, 39 parts or 40 parts, etc. The total weight parts of polycarbodiimide in the above-mentioned resin composition can be 1 part, 2 parts, 3 parts, 4 parts, 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, 11 parts, 12 parts, 13 parts, 15 parts, 16 parts, 18 parts or 19 parts, etc.; in some embodiments, the weight parts of polycarbodiimide can be 2-10 parts. The total weight fraction of the photoinitiator in the above resin composition can be 0.6 parts, 0.8 parts, 1 parts, 2 parts, 3 parts, 4 parts, 5 parts, 5.5 parts or 6 parts, etc.; in some embodiments, the weight fraction of the photoinitiator can be 1-5 parts.

[0074] In the embodiment of the present application, in the resin composition, the molar amount of the carbodiimide group in the polycarbodiimide is 0.2-1.5 times the molar amount of the carboxyl group in the photosensitive resin. In this way, the storage stability of the above-mentioned resin composition can be ensured to be high, and the flexibility and heat resistance of its cured product are also excellent. In some embodiments, the carbodiimide group is 0.5-1.5 times the molar amount of the carboxyl group, and can further be 0.6-1.2 times.

[0075] In the present application, the above-mentioned photoinitiator may be a free radical type photoinitiator. The free radical type photoinitiator can generate free radicals after being irradiated with light of a certain wavelength, and the transfer of free radicals can trigger the polymerization reaction of the photosensitive resin or the photopolymerizable monomer described below. In the embodiment of the present application, the maximum absorption wavelength of the photoinitiator is within the range of 270-400nm. That is, the photoinitiator generates free radicals and initiates the polymerization reaction under ultraviolet light irradiation.

[0076] The photoinitiator may include one or more of acetophenones, α-aminoalkyl phenones, benzophenones, benzoin, thioxanthones, etc., but is not limited thereto. Specifically, for acetophenones, 2-methyl-1-(4-methylthiophenyl)-2-morpholino-1-propanone (907), 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-acetophenone, 2,2-dibutoxyacetophenone, 1-hydroxy-cyclohexyl-phenyl ketone (184), 2-hydroxy-2-methyl-1-phenyl-1-propanone (1173), 2-methyl-1-[4-(methylthio)phenyl]-2-(4-morpholino)-1-propanone, etc. may be cited. Examples of α-aminoalkylphenones include 2-benzyl-2-dimethylamino-1-(4-morpholinylphenyl)-1-butanone (369), 2-dimethylamino-2-(4-methyl)benzyl-1-[4-(4-morpholinyl)phenyl]-1-butanone (379), and 2-(dimethylamino)ethylbenzoate. Examples of benzophenones include benzophenone, methylbenzophenone, hydroxybenzophenone, 4,4-dimethylaminobenzophenone, and 4-bromobenzophenone. Examples of benzoins include benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, and benzoin isobutyl ether. Examples of thioxanthones include thioxanthone, 2-chlorothioxanthone, 2-ethylthioxanthone, 2-isopropylthioxanthone, 2,4-dimethylthioxanthone, and 2,4-diisopropylthioxanthone.

[0077] In some embodiments of the present application, the above-mentioned resin composition also includes epoxy resin. Among them, epoxy resin can also act as a heat curing agent for photosensitive resin, which can cross-link with the carboxyl group in the photosensitive resin at a certain temperature (such as a temperature above 90°C), improve the cross-linking density of the cured product, and then improve the mechanical properties and heat resistance, solder resistance, and the adhesion of the cured product on adherends such as copper layers. In addition, epoxy resin can also cross-link with the carbodiimide group in the above-mentioned polycarbodiimide at more than 150°C, which is also beneficial to the improvement of the heat resistance of the cured product of the resin composition, and is also beneficial to the reduction of dielectric constant and dielectric loss factor.

[0078] In the embodiment of the present application, the epoxy resin includes one or more of bisphenol A epoxy resin, bisphenol F epoxy resin, naphthalene epoxy resin, biphenyl epoxy resin, dicyclopentadiene epoxy resin, and novolac epoxy resin. These epoxy resins have good heat resistance and are more helpful in improving the glass transition temperature and heat resistance of the cured product when used in the above-mentioned resin composition. Among them, the epoxy equivalent of the epoxy resin can be 100-500g / eq.

[0079] In order to further improve the heat resistance, mechanical properties and adhesion of the cured product of the above resin composition, in the embodiment of the present application, the molar amount of the epoxy group in the epoxy resin is controlled to be 0.8-1.5 times the molar amount of the carboxyl group in the photosensitive resin, for example, specifically 0.9 times, 1.0 times, 1.1 times, 1.2 times, 1.3 times or 1.4 times, etc. This may also indicate that the rigidity of the cured product of the resin composition is too large due to the introduction of too much epoxy resin.

[0080] In the embodiment of the present application, the weight proportion of epoxy resin in the resin composition can be 5-20 parts, for example, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, 11 parts, 12 parts, 13 parts, 15 parts, 16 parts, 18 parts or 19 parts, etc. Introducing an appropriate amount of epoxy resin can improve the heat resistance and adhesion of the cured product of the resin composition.

[0081] In some embodiments of the present application, the resin composition further comprises a photopolymerizable monomer. The photopolymerizable monomer is a substance containing one or more unsaturated carbon-carbon double bonds in its molecular structure. The photopolymerizable monomer can also undergo polymerization and crosslinking reaction by itself under certain light and the action of a photoinitiator, or undergo polymerization and crosslinking reaction with a photosensitive resin, thereby increasing the crosslinking density of the system and thereby improving heat resistance and mechanical properties.

[0082] In the embodiment of the present application, the weight proportion of the photopolymerizable monomer in the resin composition may be 5-20 parts, for example, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, 11 parts, 12 parts, 13 parts, 15 parts, 16 parts, 18 parts or 19 parts, etc. Introducing an appropriate amount of the photopolymerizable monomer can appropriately enhance the photoreactivity of the resin composition and enhance the crosslinking density of the photoreactant.

[0083] In some embodiments of the present application, the photopolymerizable monomer includes one or more of a monofunctional acrylate monomer and a multifunctional acrylate monomer. A multifunctional acrylate monomer refers to a substance containing more than or equal to two acrylate groups in a molecular structure. Among them, a monofunctional acrylate monomer has a good dilution ability for a photosensitive resin. The photoreactivity of a multifunctional acrylate monomer is high. Exemplarily, a multifunctional acrylate may include one or more of dipentaerythritol hexaacrylate (DPHA), pentaerythritol triacrylate (PETA), pentaerythritol trimethacrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol pentaacrylate, trimethylolpropane triacrylate (TMPTA), tetraethylene glycol dimethacrylate, etc. Monofunctional acrylates may include one or more of isobornyl acrylate, glycidyl methacrylate, hydroxyethyl acrylate, 2-hydroxypropyl acrylate, 2-hydroxymethyl methacrylate, etc.

[0084] In some embodiments of the present application, the resin composition may further include a colorant. The colorant may give the resin composition a certain color. Among them, the colorant may include one or more of a pigment, a dye, etc. The pigment may be an organic pigment, an inorganic pigment, etc. In the case where the resin composition contains a colorant, the polycarbodiimide contained in the resin composition may improve the compatibility of the colorant in the composition system, ensure that the photosensitive dry film and the cured product formed by the resin composition have a smooth appearance with few defects, and further ensure the servo reliability when used as a patterned solder mask ink layer. Exemplarily, the organic pigment may be an organic pigment such as a phthalocyanine series, anthraquinone series, quinacridone series, benzimidazolone series, perylene series, azo series, quinolinephthalone series, aniline series, anthocyanin series, etc. The inorganic pigment may be carbon black, titanium black, Prussian blue, chrome yellow, zinc yellow, red lead, iron oxide red, zinc white, zinc barium white, titanium dioxide, etc.

[0085] In some embodiments of the present application, the resin composition may further include a filler. The addition of the filler may improve the viscosity of the resin composition, the high temperature moldability, and reduce the thermal expansion coefficient of the cured product. The filler may include but is not limited to one or more of silicon dioxide, aluminum oxide, barium sulfate, talcum powder, mica powder, glass powder, etc. The polycarbodiimide contained in the resin composition may also help improve the compatibility of the filler in the composition.

[0086] In the embodiment of the present application, the resin composition may further contain an auxiliary agent, wherein the auxiliary agent may include one or more of a toughening agent, a leveling agent, a dispersant, a coupling agent, a stress modifier, an ion capture agent, etc. The above additives have different functions. In actual production, one or more of the above additives may be added to the resin composition as needed to improve the performance of the resin composition and meet actual requirements.

[0087] In the embodiment of the present application, the resin composition contains a solvent. This makes the resin composition a mixed liquid, and because it is a viscous colloidal fluid with a certain fluidity, it can also be called a photosensitive ink. The selection of the solvent should try to ensure that the above-mentioned photosensitive resin, polycarbodiimide, photoinitiator and other optional components are dissolved therein. In some embodiments, the solvent can be selected from one or more of diethylene glycol monoethyl ether acetate (DGMEA), propylene glycol methyl ether acetate (PMA), cyclohexanone, butanone (MEK), and solvent oil.

[0088] In the embodiment of the present application, the resin composition can be obtained by mixing various components. The resin composition is usually a mixed liquid. The resin composition can be coated and dried to form a photosensitive film, and then exposed, developed, and completely cured to obtain a patterned coating, and the patterned coating includes a cured product of the resin composition.

[0089] The embodiment of the present application further provides a film material, which includes a photosensitive film, and the photosensitive film is formed by drying the above-mentioned resin composition of the embodiment of the present application.

[0090] See also Figure 2 , the present application embodiment provides a film material 200, the film material 200 includes a photosensitive film 220. The photosensitive film 220 is a solid dry film, which is obtained by coating the above-mentioned resin composition and then baking. In some embodiments, the film material 200 is the photosensitive film 220. In other embodiments, such as Figure 2 As shown, the photosensitive film 220 is usually attached to the surface of the support 210, and the surface of the photosensitive film 220 away from the support 210 is generally provided with a protective film 230 for protection, forming a three-layer film structure. That is, the film material 200 usually includes a support 210, a photosensitive film 220 and a protective film 230 stacked in sequence on one side of the support 210.

[0091] Among them, the support body 210 can be a polymer film with heat resistance and solvent resistance such as polyethylene terephthalate (PET), polypropylene, polyethylene, etc. The coating can include any one or more methods of scraping, spinning, spraying, spin coating, etc. The coating thickness of the photosensitive film 220 can be determined according to the film thickness after it is fully cured in practical applications. Among them, during the baking process, the polycarbodiimide and the photosensitive resin in the above-mentioned resin composition of the embodiment of the present application will not undergo a cross-linking reaction. The baking temperature generally does not exceed 80°C, for example, 50-80°C.

[0092] The protective film 230 and the support 210 can be made of the same or different thin film materials, and it is preferred that the bonding force between the protective film 230 and the photosensitive film 220 is smaller than the bonding force between the support 210 and the photosensitive film 220. The protective film 230 can be pressed onto the surface of the photosensitive film 220 at a certain temperature and pressure. Within the pressing temperature range, no cross-linking reaction will occur in the photosensitive film 220, which makes the photosensitive film 220 more stable and has better room temperature storage performance. The pressing temperature can be 50-80°C, and further can be 55-75°C.

[0093] When using the above-mentioned film material 200, it is generally necessary to first remove the protective film 230 on the photosensitive film 220, then contact the photosensitive film 220 with the target substrate, and perform heat pressing, and then perform patterning process steps (such as exposure, development, etc.) on the photosensitive film 220. During the heat pressing process, no cross-linking reaction will occur inside the photosensitive film 220. The temperature of heat pressing generally does not exceed 80°C, for example, 50-80°C, or 55-75°C. In addition, before development, it is generally necessary to remove the support 210. Therefore, in actual applications, only the solidified material of the photosensitive film 220 in the film material 200 is retained in the final product structure.

[0094] The embodiments of the present application provide applications of the above-mentioned resin composition and the above-mentioned film material 200 in preparing printed circuit boards and packaging electronic components.

[0095] Wherein, the application in the preparation of printed circuit boards includes but is not limited to the production of patterned solder mask ink layers on printed circuit boards, insulating layers in printed circuit boards, etc. Wherein, the resin composition and film material 200 of the embodiment of the present application can be used to encapsulate various electronic components, such as various chips, transistors (such as diodes, triodes), LED devices, resistors and capacitors (such as resistors, capacitors, inductors, etc.), to form electronic packaging structures, or referred to as sealed packages. Wherein, the application in the preparation of electronic packaging structures can include but is not limited to the preparation of packaging carriers (specifically the production of patterned solder mask ink layers on packaging carriers), electrical insulation layers, protective layers, plastic sealing layers, adhesive layers (such as bottom filling adhesive layers) for fixing electronic components, etc. The above-mentioned film layers include the cured product of the resin composition of the embodiment of the present application. The above-mentioned resin composition is particularly suitable for high-density wiring requiring low dielectric constant and low dielectric loss tangent, and electronic packaging structures for processing high-frequency signals, etc.

[0096] The following is prepared Figure 1 Taking the package carrier 10 as an example, an application method of the resin composition of the present application is introduced. Specifically, the application method includes:

[0097] Step (1): coating the resin composition of the embodiment of the present application on a substrate and baking to form a photosensitive film.

[0098] Among them, the substrate used has good high temperature resistance and is not easy to deform at the curing temperature of the above-mentioned resin composition. In the embodiment of the present application, the substrate is a substrate with a circuit pattern formed on the surface, which may include an insulating layer and a conductor layer arranged on the surface of the insulating layer. The insulating layer is usually laminated by a plurality of insulating films. The conductor layer can be converted into a conductor layer with a circuit pattern by a patterning process through an initial metal foil layer covering the dielectric layer. The conductor layer can be copper, aluminum, nickel, silver or its alloys, etc., and copper or its alloys are more common. Among them, the substrate with a circuit pattern formed thereon can specifically be a printed circuit board, a flexible printed circuit board, a copper-clad laminate for a high-frequency circuit, etc., which is pre-formed with a circuit pattern. Figure 1 The reference numeral 11 is a copper-clad laminate with a copper circuit pattern, and the copper layers on the surface are respectively indicated by reference numerals 101 and 102. In addition, the coating process parameters can be referred to the description in the previous text of this application.

[0099] Step (2): exposing a predetermined area of ​​the substrate with the above-mentioned photosensitive film.

[0100] During the exposure, the exposure light source can be used to irradiate the photosensitive film through a mask having a certain pattern to achieve selective exposure. The light provided by the exposure light source usually includes ultraviolet light, so that common photoinitiators can be irradiated with free radicals to initiate crosslinking of the photosensitive film. Generally, the exposure light source can be a mercury lamp, ultraviolet light emitting diode, etc. The exposure dose can be selected as needed, usually between 50-200 mJ / cm 2 within the range.

[0101] Step (3): The exposed photosensitive film is developed with a developer, thereby removing the unexposed portion and obtaining a patterned film.

[0102] For the negative resin composition used in the present application, the unexposed area of ​​the photosensitive film is soluble in the developer, while the exposed area is relatively insoluble in the developer. Therefore, the shape of the patterned film left after the development process corresponds to the hollowed-out area of ​​the mask. The portion of the substrate not covered by the patterned film is generally the electrical connection between the substrate and other conductive components. Figure 1 The solder bump 13 is not covered by the patterned film on the side of the substrate close to the electronic component 20. The developer used is usually an alkaline solution, for example, a solution containing an inorganic base such as sodium hydroxide, potassium hydroxide, sodium carbonate, sodium bicarbonate, etc., or an organic base such as tetramethylammonium hydroxide (TMAH), trimethylamine, triethanolamine, etc.

[0103] Step (4): Complete curing: The patterned film is heated and cured to be converted into a hardened film.

[0104] Through the heat curing process, the carbodiimide group of the polycarbodiimide in the patterned film can undergo a cross-linking reaction with the carboxyl group in the photosensitive resin. When the resin composition contains an epoxy resin, a cross-linking reaction between the epoxy group and the carboxyl group can also occur during the heat curing process. The resulting cured film is also the cured product of the resin composition, and the cured film can be referred to as Figure 1 The patterned solder resist ink layer on the package carrier 10 is shown in FIG.

[0105] Generally, the temperature of heating and curing can be set according to the properties of the above-mentioned polycarbodiimide and in combination with actual needs. It can be understood that the temperature of heating and curing should be higher than the exothermic peak temperature of the above-mentioned resin composition measured by the DSC method, and lower than the tolerance temperature of the substrate. In some embodiments of the present application, the temperature of heating and curing is 100-180°C, or 120-170°C.

[0106] In some embodiments of the present application, before the patterned film is heat-cured, it can be photocured first. In this way, the photosensitive resin and photopolymerizable monomer that have not completed the free radical polymerization reaction in the system can continue to undergo polymerization reaction, and then the corresponding heat curing is performed, thereby ensuring that the cross-linkable components in the system are fully cross-linked, and ensuring that the obtained cured product has a high cross-linking density and high heat resistance. Among them, the photocuring can be carried out under the irradiation of the above-mentioned exposure light source, and the exposure dose used can be larger than the exposure treatment in step (2), for example, the exposure dose can be 1000-2000mJ / cm 2 .

[0107] It should be noted that when the above-mentioned film material 200 is used to prepare the above-mentioned patterned solder resist ink layer, the difference from directly using the above-mentioned resin composition is mainly that: in step (1), the protective film 230 on the photosensitive film 220 is first removed, and then the photosensitive film 220 is hot pressed on the substrate; before performing the exposure of step (2) or before performing the development of step (3), the support body 210 of the film material 200 is first removed. In this way, only the cured product of the photosensitive film 220 remains in the final product structure.

[0108] The embodiment of the present application further provides a packaging carrier, which comprises a cured product of the above-mentioned resin composition of the embodiment of the present application.

[0109] See also Figure 1The package carrier 10 provided in Example 1 of the present application includes a substrate 11 having a conductor layer on the surface, and a patterned solder resist ink layer 12 is provided on the conductor layer, and the patterned solder resist ink layer 12 includes a cured product of the above-mentioned resin composition. As mentioned above, the substrate 11 having a conductor layer on the surface includes an insulating layer and a conductor layer provided on the surface of at least one side of the insulating layer. Among them, the insulating layer can be a laminate of multiple insulating films, and the conductor layer can be a conductor layer with a wiring pattern, and its material includes but is not limited to copper, aluminum, nickel, silver or its alloys, and copper and copper alloys are more common.

[0110] The embodiment of the present application also provides a sealed package, which may include the cured product of the resin composition of the embodiment of the present application, or include the package carrier of the embodiment of the present application. Since the sealed package contains the cured product of the resin composition provided by the embodiment of the present application, it has high reliability.

[0111] Please continue to see Figure 1 The sealed package 100 provided in some embodiments of the present application includes a package carrier 10 and an electronic component 20 disposed on the package carrier 10. The electronic component 20 can be disposed on the patterned solder resist ink layer 12 in the package carrier 10 (specifically, disposed on the side of the patterned solder resist ink layer 12 away from the substrate 11), and the electrical connection portion between the package carrier 10 and the electronic component 20 (such as Figure 1 The solder bumps 13 in the embodiment are not covered by the patterned solder resist ink layer 12. For other structural details of the sealed package 100, reference may be made to the foregoing description of the present application. Figure 1 The structure is usually made of electronic components 20, with chips being more common.

[0112] The sealed package 100 can be electrically connected to a circuit board. Figure 3 , a side of the package carrier 10 away from the electronic components 20 (also referred to as the "bottom of the package carrier 10") may be provided with a plurality of solder balls 14 (such as solder balls) arranged in an array, and the package carrier 10 in the sealed package 100 may be electrically connected to the circuit board 30 through the solder balls 14, so that the connection between the electronic components 20 and the circuit board 30 is achieved with the help of the package carrier 10. The circuit board 30 and the electronic components 20 in the sealed package 100 are located on opposite sides of the package carrier 10.

[0113] In addition, as described above in the present application, in addition to the patterned solder mask ink layer 12 in the sealed package 100 which may contain the cured product of the above-mentioned resin composition in the embodiment of the present application, the insulating layer of the packaging carrier 10, the bottom filling glue layer between the solder bumps 13, the plastic package covering the electronic components 20, etc. may also contain the cured product.

[0114] It should be noted that Figure 3 The sealed package 100 is specifically a BGA package as an example, and its structure after being connected to the circuit board is shown, but it can be understood that the above-mentioned sealed package in the embodiment of the present application can also be a sealed package using FC-CSP (Flip Chip-Chip Scale Package), SiP (System in Package), QFP (Quad Flat Package) or SOP (Small Outline Package) technology, etc.

[0115] An embodiment of the present application further provides an electronic device, which includes the above-mentioned sealed packaging member of the embodiment of the present application.

[0116] In some implementation modes of the present application, Figure 4 As shown, the electronic device 300 includes a housing 301 and a circuit board and a sealed package 100 disposed in the housing 301. In the electronic device 300, the sealed package 100 may be Figure 3 As shown, it is arranged on the circuit board 30 and is electrically connected to the circuit board 30. The electronic device can be a mobile phone, a tablet computer, a laptop computer, a wearable device (such as a smart watch, a smart bracelet), a television, a video recorder, a camcorder, a home smart device, a vehicle-mounted device and other terminal products.

[0117] In some other embodiments of the present application, the electronic device may also be various wired or wireless communication devices such as antennas, radars, routers, gateways, intercoms, switches, lightning arresters, etc., or communication base stations. The circuit boards of these communication devices or communication base stations are electrically connected to the above-mentioned sealed packaging.

[0118] In this application, "and / or" describes the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone, where A and B can be singular or plural. In this application, "at least one" means one or more, and "more than one" means two or more. When this application mentions that the content of a substance does not exceed a certain value, for example, not exceeding 10%, it means "less than or equal to 10%".

[0119] The technical solution of the embodiment of the present application is further explained below with multiple embodiments.

[0120] First, the synthesis of each polycarbodiimide is introduced.

[0121] Synthesis of polycarbodiimides P1 to P3: Tetramethyl metaxylylene diisocyanate (TMXDI) was used as a monomer for polycondensation to prepare the target polycarbodiimide. 200 parts by mass of the monomer TMXDI was added to a three-necked flask, first heated to 90°C under stirring conditions, then 0.15 parts by mass of 3-methyl-1-phenyl-2-phosphopentene-1 oxide was added as a catalyst, and then the polycondensation reaction was carried out at a temperature of 178°C and a rotation speed of 350 rpm. The change of -NCO concentration in the system was monitored by di-n-butylamine titration method, and the polymerization degree of the polymerization product was controlled by the reaction time. After reaching the predetermined polymerization degree (2, 4, and 8, respectively), the system temperature was reduced to 100°C, and then a certain amount of isooctyl alcohol was added as a capping agent to completely consume the unreacted NCO to obtain polycarbodiimides, which were named P1, P2, and P3, respectively.

[0122] The general reaction formula for preparing polycarbodiimide P1-P3 is as follows:

[0123]

[0124] In the structural formula of polycarbodiimide P1, the degree of polymerization of the repeating unit p=2, that is, the content of carbodiimide groups in 1 mol of the molecular structure P1 is 4 mol. The weight average molecular weight Mw of P1 is 905.

[0125] The degree of polymerization of the repeating unit in the polycarbodiimide P2 is p=4, that is, the content of the carbodiimide group in 1 mol of the molecular structure P1 is 8 mol. The weight average molecular weight Mw of P2 is 1306.

[0126] The degree of polymerization of the repeating unit in the polycarbodiimide P3 is p=8, that is, the content of the carbodiimide group in 1 mol of the molecular structure P1 is 16 mol. The weight average molecular weight Mw of P3 is 2107.

[0127] Synthesis of polycarbodiimide P4: 200 parts by mass of TMXDI as a monomer was added to a three-necked flask, first heated to 90°C under stirring, then 0.15 parts by mass of 3-methyl-1-phenyl-2-phosphocyclopentene-1 oxide was added as a catalyst, and then a polycondensation reaction was carried out at a temperature of 178°C and a rotation speed of 350 rpm. The change of -NCO concentration in the system was monitored by di-n-butylamine titration, and the degree of polymerization of the polymer product was controlled by the reaction time. After reaching a predetermined degree of polymerization (the degree of polymerization in this embodiment is 4), 0.1 parts by mass of dibutyltin dilaurate and 50 parts by mass of toluene were added thereto, and the mixture was stirred and dissolved to obtain a mixed solution A. 30 parts by mass of the end-capping agent phenol was dissolved in 100 parts by mass of anhydrous toluene and added to a three-necked flask, heated to 60°C, and then the mixed solution A was added dropwise to the three-necked flask containing phenol and toluene solution within 1 hour. After the addition was completed, the mixture was reacted at 60° C. for 3 hours. After the reaction was completed, unreacted phenol and toluene were distilled off at 150° C. and a reduced pressure of 2 mmHg to obtain a phenol-terminated polycarbodiimide named P4.

[0128] Wherein, polycarbodiimide P4 includes the following structure:

[0129]

[0130] Wherein, p = 4. The weight average molecular weight Mw of the repeating unit in P4 was measured to be 1234.

[0131] Synthetic polycarbodiimide P5: The difference between it and synthetic polycarbodiimide P4 is that: when the predetermined degree of polymerization reaches 4, 0.1 parts by mass of dibutyltin dilaurate and 100 parts by mass of toluene are added to the system, and the mixture is stirred and dissolved to obtain a mixed solution B. 43 parts by mass of the end-capping agent 1-naphthol and 200 parts by mass of anhydrous toluene are added to a three-necked flask, heated to 70°C to fully dissolve them, and then the mixed solution B is added dropwise to the three-necked flask containing phenol and toluene solution within 1 hour. After the addition is completed, the mixture is reacted at 70°C for 4 hours. After the reaction is completed, the unreacted 1-naphthol and toluene are distilled off at 200°C and 2 mmHg under reduced pressure to obtain a naphthol-terminated polycarbodiimide, named P5.

[0132] Among them, polycarbodiimide P5 includes the structure shown below:

[0133]

[0134] Wherein, p = 4. The weight average molecular weight Mw of the repeating unit in P5 was measured to be 1335.

[0135] Synthesis of polycarbodiimide P6 and P7: Isophorone diisocyanate (IPDI) was used as a monomer for polycondensation to prepare the target polycarbodiimide. 200 parts by mass of the monomer IPDI was added to a three-necked flask, first heated to 80°C under stirring, then 0.15 parts by mass of 3-methyl-1-phenyl-2-phosphopentene-1 oxide was added as a catalyst, and then the polycondensation reaction was carried out at a temperature of 155°C and a rotation speed of 370 rpm. The change of -NCO concentration in the system was monitored by di-n-butylamine titration method, and the polymerization degree of the polymer product was controlled by the reaction time. During the reaction, the rotation speed was adjusted according to the change of the system viscosity and toluene solvent was added. After reaching the predetermined polymerization degree (2 and 4 respectively), the system temperature was reduced to 90°C, and then a certain amount of isooctyl alcohol was added as a capping agent to consume the unreacted NCO, and the isooctyl alcohol-capped polycarbodiimide P6 with a polymerization degree of 2 and the isooctyl alcohol-capped polycarbodiimide P7 with a polymerization degree of 4 were obtained.

[0136] Polycarbodiimide P6 and P7 both have the following structure:

[0137]

[0138] The degree of polymerization of the repeating unit in polycarbodiimide P6 is p=2, and the degree of polymerization of the repeating unit in polycarbodiimide P7 is p=4. In addition, the weight average molecular weight Mw of P6 is measured to be 839, and the weight average molecular weight Mw of P7 is measured to be 1196.

[0139] Synthesis of polycarbodiimide P8: 200 parts by mass of monomer IPDI were added into a three-necked flask, first heated to 80°C under stirring, then 0.15 parts by mass of 3-methyl-1-phenyl-2-phospholene-1 oxide was added as a catalyst, and then a polycondensation reaction was carried out at a temperature of 155°C and a rotation speed of 370 rpm. The change of -NCO concentration in the system was monitored by di-n-butylamine titration method, and the polymerization degree of the polymerization product was controlled by the reaction time. During the reaction, the rotation speed was adjusted according to the change of the viscosity of the system and toluene solvent was added.

[0140] After reaching the predetermined degree of polymerization of 10, 0.1 parts by mass of dibutyltin dilaurate and an appropriate amount of toluene were added to the system, and the mixture was fully stirred and dissolved to obtain a mixed solution C. 30 parts by mass of glycidol as a capping agent and 200 parts by mass of anhydrous toluene were added to a three-necked flask, heated to 60°C for full dissolution, and then the mixed solution C was added dropwise to the three-necked flask containing glycidol within 1 hour. After the addition was completed, the mixture was reacted at 60°C for 3 hours. After the reaction was completed, the unreacted glycidol and toluene were distilled off at 120°C and 2 mmHg under reduced pressure to obtain a glycidol-terminated polycarbodiimide, named P8.

[0141] Among them, polycarbodiimide P8 includes the structure shown below:

[0142]

[0143] Wherein, p = 10. The weight average molecular weight Mw of the repeating unit in P8 was measured to be 2154.

[0144] Synthetic polycarbodiimide P9: The difference between the synthetic polycarbodiimide P9 and the synthetic polycarbodiimide P8 is that after the polymerization product of the polycondensation reaction reaches a predetermined degree of polymerization of 4, a certain amount of end-capping agent 1-naphthol is used for end-capping.

[0145] Among them, polycarbodiimide P9 includes the structure shown below:

[0146]

[0147] The degree of polymerization of the repeating unit in P9 is p=4. The weight average molecular weight Mw of P9 is measured to be 1224.

[0148] Synthetic polycarbodiimide P10: The difference between the synthetic polycarbodiimide P10 and the synthetic polycarbodiimide P8 is that after the polymerization product of the polycondensation reaction reaches a predetermined degree of polymerization of 10, a certain amount of end-capping agent 1-naphthol is used for end-capping.

[0149] Among them, polycarbodiimide P10 includes the following structure:

[0150]

[0151] The degree of polymerization of the repeating unit in P10 is p=10. The weight average molecular weight Mw of P10 is measured to be 2149.

[0152] Example 1

[0153] Preparation of a photosensitive resin composition:

[0154] 2 parts by weight of the polycarbodiimide P4, 16 parts by weight of photosensitive resin 1 (specifically acid-modified novolac epoxy acrylate, with a Mw of 10,000 and an acid value of 49.27 mgKOH / g), 16 parts by weight of photosensitive resin 2 (specifically acid-modified bisphenol F epoxy acrylate, with a Mw of 2000 and an acid value of 50 mgKOH / g), 2 parts by weight of photoinitiator 907, 10 parts by weight of epoxy resin (specifically biphenyl epoxy resin NC3000H, with an epoxy group equivalent of 285 g / eq), 6 parts by weight of photopolymerizable monomer DPHA, 20 parts by weight of inorganic filler (specifically 10 parts by weight of silica and 10 parts by weight of barium sulfate) and 0.4 parts by weight of colorant (specifically 0.25 parts by weight of copper phthalocyanine pigment and 0.15 parts by weight of Pigment Yellow 147 (also known as 1,1'-[(6-phenyl-1,3,5-triazine-2,4-diimino]dianthraquinone)) are added to a certain weight portion of an organic solvent and stirred evenly to obtain a photosensitive resin composition slurry.

[0155] The composition and weight percentage of each non-volatile component in the photosensitive resin composition of other embodiments and comparative examples are listed in Table 1, and the preparation process thereof can refer to Example 1. In addition, Table 1 also summarizes the exothermic peak temperature of each photosensitive resin composition measured by DSC method.

[0156] Table 1

[0157]

[0158]

[0159] The DSC curve of the photosensitive resin composition of Example 3 is as follows: Figure 5 The DSC curve of the photosensitive resin composition of Example 6 is shown in Figure 6 As shown. Figure 5 , Figure 6 It can be more intuitively seen that the photosensitive resin composition of the embodiment of the present application has no exothermic peak before 90° C., reflecting that the constituent system of the photosensitive resin composition is stable and no reaction occurs between the components in the system at common baking temperatures, thus ensuring its good exposure and developability.

[0160] Preparation of photosensitive film and cured film thereof: The slurry of each photosensitive resin composition of the above-mentioned embodiment and comparative example is coated on the PET release film through a 100 mesh wire rod, and baked in an 80°C blast oven for 30 minutes to obtain a photosensitive dry film with a thickness of 30-40 μm. Then, the photosensitive dry film is first photocured under a mercury lamp with an exposure of 3000 mJ, and then heat-cured in a 150°C blast oven for 60 minutes to completely cure the photosensitive dry film to obtain a cured film. After cooling to room temperature, it is peeled off from the PET release film and a cured film with a thickness of 30-40 μm is obtained for subsequent heat resistance, flexibility and dielectric properties tests.

[0161] Appearance evaluation of each photosensitive dry film: The appearance of each photosensitive dry film was visually observed and evaluated. The color uniformity, pits, orange peel, etc. of each photosensitive dry film were mainly observed. The judgment criteria are as follows: 0: uniform color, flat surface, no defects; △: uneven color dispersion, pits, a little orange peel; ×: uneven color dispersion, with a large number of pits or orange peel and other appearance defects.

[0162] Heat resistance test of each cured film: Each of the above cured films was cut into strips of 5 mm width and 30 mm length using a stamping die, and tested on a dynamic mechanical analyzer (DMA) under the following conditions to measure its glass transition temperature (Tg) value.

[0163] Among them, the test instrument is Mettler DMA1, the test mode is tensile mode, the test temperature is 30℃-3260℃, the heating rate is 5℃ / min, and the test frequency is 1Hz. Among them, the judgment criteria are: if Tg is less than 160℃, the heat resistance is recorded as ◎; if 150℃1Tg<160℃, the heat resistance is recorded as 0; 140℃1Tg<150℃, the heat resistance is recorded as △, and Tg<140℃, the heat resistance is recorded as ×.

[0164] Flexibility test of each cured film: Each of the above cured films was cut into 3mm wide and 30mm long strips by a stamping die, and tested on a dynamic mechanical analyzer (DMA) at a stress rate of 3N / min. The average elongation of 8 strips was tested as a quantitative index to measure flexibility. The judgment criteria are: if the elongation is T5%, the flexibility is recorded as ◎; if the elongation is 4%1 <5%, the flexibility is recorded as 0; if the elongation is 3%1 <4%, the flexibility is recorded as △, and if the elongation is <3%, the flexibility is recorded as ×.

[0165] Dielectric test of each cured film: Each cured film peeled off from the PET release film was used as a test sample, and the dielectric constant and dielectric loss tangent at 10 GHz were measured using an SPDR dielectric resonator and a network analyzer, and evaluated according to the following evaluation criteria. Among them, the evaluation criteria for the dielectric constant Dk are: 0: less than 3.3; △: 3.3 or more and less than 3.5; ×: 3.5 or more. The evaluation criteria for the dielectric loss tangent Df are: 0: less than 0.020; △: 0.020 or more and less than 0.025; ×: 0.025 or more.

[0166] The pattern forming properties of the photosensitive resin compositions of the above examples and comparative examples were evaluated. Specifically, each photosensitive resin composition was coated on a copper plate by screen printing so that the film thickness after drying reached 20 μm, and then baked at 80°C for 30 minutes to obtain a photosensitive dry film with a film thickness of 20 μm. Then, a mercury lamp was used at 200 mJ / cm 2 The photosensitive dry film was exposed to ultraviolet light on the entire surface at an exposure amount of . Then, the copper plate with the exposed photosensitive dry film was immersed in a 1% sodium carbonate aqueous solution at 30°C for 1 minute for development. The developability of the dry film was evaluated according to the following visual standards. The evaluation standards for developability are: ◎: no residue; ○: residue with a film thickness of less than 1μm; △: residue with a film thickness of more than 1μm and less than 3μm; ×: residue with a film thickness of more than 3μm.

[0167] Storage stability test: According to the above method for evaluating the developability, a test sample was prepared, and a photosensitive dry film with a thickness of 20 μm was formed on a copper plate. The photosensitive dry film was stored in a dark room at room temperature (23°C) for a certain period of time. Then, a mercury lamp was used to irradiate the sample at 200 mJ / cm 2 The photosensitive dry film was exposed to ultraviolet light on its entire surface with an exposure amount of , and then immersed in a 1% sodium carbonate aqueous solution at 30° C. for 1 minute for development.

[0168] The evaluation criteria for storage stability are as follows: ◎: After being stored at room temperature for 2 weeks, the film can still be developed without residue; ○: After being stored at room temperature for 2 weeks, residue with a film thickness of less than 1 μm is developed; △: After being stored at room temperature for 2 weeks, residue with a film thickness of more than 1 μm and less than 3 μm is developed; ×: After being stored at room temperature for 2 weeks, residue with a film thickness of more than 3 μm is developed.

[0169] Copper adhesion test: The photosensitive resin composition was coated on the copper plate by screen printing to a thickness of 20 μm after drying, and dried in a hot air circulation drying oven at 80°C for 30 minutes to obtain a photosensitive dry film with a thickness of 20 μm. 2 The exposed dry film was then heated at 150° C. for 1 hour to completely cure the dry film into a cured film sample.

[0170] Afterwards, according to the standard test method of the 100-grid test (size 1mm x 1mm), the cured film sample was subjected to a peeling test using 3M tape, and the following quantitative evaluation was performed: ◎: no component remains on the 3M tape; ○: the peeling area of ​​the cured film is less than 10%; △: more than 10% but less than 20% of the cured film is peeled off; ×: more than 20% of the cured film is peeled off.

[0171] Reflow resistance test: Each photosensitive resin composition was coated on a copper plate by screen printing to a thickness of 20 μm after drying, and dried in a hot air circulation drying oven at 80°C for 30 minutes to obtain a photosensitive dry film with a thickness of 20 μm. Then, a mercury lamp was used at 2 J / cm 2 Exposure was performed, and then the exposed dry film was heated at 150°C for 1h to completely cure the dry film into a cured film sample to obtain an evaluation substrate. The copper plate with the cured film was then heated in a reflow oven according to a standard thermal reflow curve (peak temperature of 260°C) in a reflow oven machine. After 10 reflow ovens, a peeling test was performed on the cured film sample using 3M tape according to the standard test method of the 100-grid test (size 1mm x 1mm), and the following quantitative evaluation was performed: ◎: No component remained on the 3M tape; ○: The peeling area of ​​the cured film was less than 10%; △: The cured film had an area of ​​more than 10% but less than 20% peeled off; ×: The cured film had an area of ​​more than 20% peeled off.

[0172] Acid resistance test: The evaluation substrate was made according to the same method as the Reflow resistance test. Then each evaluation substrate was immersed in a 20wt% sulfuric acid aqueous solution for 30 minutes, and then dried. The dried evaluation substrate was subjected to a peeling test using 3M tape to evaluate the expansion, peeling, and discoloration of the solder mask. The evaluation criteria are as follows: ◎: No change in appearance, no peeling; 0: Slight change in appearance, the peeling area ratio is less than 10%; △: Slight change in appearance, the peeling area is between 10% and 20%; ×: Large change in appearance, expansion, and peeling area greater than 20%.

[0173] Alkali resistance test: The evaluation substrate was made according to the same method as the Reflow resistance test. Then, each evaluation substrate was immersed in a 20wt% sodium hydroxide aqueous solution for 30 minutes, and then dried. The dried evaluation substrate was subjected to a peeling test using 3M tape to evaluate the expansion, peeling, and discoloration of the solder mask. The evaluation criteria are as follows: ◎: No change in appearance, no peeling; 0: Slight change in appearance, the peeling area ratio is less than 10%; △: Slight change in appearance, the peeling area is between 10% and 20%; ×: Large change in appearance, expansion, and peeling area greater than 20%.

[0174] Table 2 below summarizes the evaluation results of the above embodiments and comparative examples.

[0175] Table 2

[0176]

[0177] It can be seen from Table 2 that when the negative photosensitive resin composition used does not contain polycarbodiimide (Comparative Example 1), the composition has good developability and stability, but the appearance of the photosensitive dry film is not good, and the dielectric properties of the cured product are poor, and the weather resistance (such as acid and alkali resistance, solder resistance), copper adhesion, etc. are not good, and the reliability of the patterned solder resist ink layer on the package carrier is not good. After the introduction of polycarbodiimide (such as each embodiment and comparative examples 2-5), the appearance of the photosensitive dry film is improved, indicating that the compatibility of polycarbodiimide with other components in the composition is good, and the acid and alkali resistance and solder resistance of its cured product are also improved to a certain extent, but the developability and storage stability of the composition of comparative examples 2-5 are significantly deteriorated.

[0178] From the comparison between Examples 1-3 and Comparative Examples 2-3, it can be learned that when the degree of polymerization p of the polycarbodiimide used is less than or equal to 4, if the terminal NCO of the polycarbodiimide is not capped with a capping agent (phenol, naphthol) with large steric hindrance, the reactivity of -N=C=N- in the polycarbodiimide is relatively high, and the DSC exothermic peak temperature of the above-mentioned photosensitive resin composition containing it is greater than 90°C (basically 110-140°C), the reactivity is relatively low, and its developability and storage stability are relatively good. In particular, when the monomers of the polycarbodiimide are the same, the degree of polymerization p is equal and all are 4, the capping group of the polycarbodiimide of Examples 2-3 contains an aromatic ring structure, and the developability and storage stability of the composition are significantly improved compared with Comparative Example 3, and the heat resistance and reflow resistance of the cured product are also improved to a certain extent, and at the same time, its flexibility, dielectric properties, copper adhesion, etc. are not reduced.

[0179] Similarly, from the comparison between Example 4-6 and Comparative Example 4-5, it can be learned that when the degree of polymerization p of the polycarbodiimide used is greater than 4, even if no end-capping agent containing an aromatic ring structure is used for end-capping (i.e., polycarbodiimide P8), the DSC exothermic peak temperature of the above-mentioned photosensitive resin composition containing it can still be greater than 90°C, thereby making its developability and storage stability of the photosensitive dry film relatively excellent, and at the same time, the other properties of its cured product are not significantly deteriorated.

Claims

1. A resin composition, characterized in that The invention comprises a photosensitive resin, polycarbodiimide and a photoinitiator, wherein the molecular structure of the photosensitive resin contains a carboxyl group and a carbon-carbon double bond, the polycarbodiimide is a polymer having a carbodiimide group, and the exothermic peak temperature of the resin composition measured by differential scanning calorimetry is greater than 90°C.

2. The resin composition according to claim 1, characterized in that The resin composition has an exothermic peak with a peak intensity greater than 0.1 mW / mg.

3. The resin composition according to claim 1 or 2, characterized in that The resin composition has an exothermic peak temperature in the range of 100-200° C. as measured by differential scanning calorimetry.

4. The resin composition according to any one of claims 1 to 3, characterized in that In the polycarbodiimide per unit mol of molecular structure, the content of the carbodiimide group is 4-30 mol.

5. The resin composition according to any one of claims 1 to 4, characterized in that The weight average molecular weight of the polycarbodiimide is 800-9000.

6. The resin composition according to any one of claims 1 to 5, characterized in that The polycarbodiimide comprises a structure shown in formula (I): In formula (I), A and D are independently selected from one or more of substituted or unsubstituted alkylene, substituted or unsubstituted cycloalkylene, and substituted or unsubstituted arylene, p is in the range of 2-15; Q represents a capping group that blocks the NCO group.

7. The resin composition according to claim 6, characterized in that When p is in the range of 2-4, the Q contains an aromatic ring structure; when p is in the range of 5-15, the Q contains one or more of an aromatic ring structure, an aliphatic ring structure, and an aliphatic chain structure.

8. The resin composition according to claim 6, characterized in that The unsubstituted alkylene group has 1 to 20 carbon atoms, the unsubstituted cycloalkylene group has 4 to 20 carbon atoms, and the unsubstituted arylene group has 6 to 20 carbon atoms.

9. The resin composition according to any one of claims 6 to 8, characterized in that The polycarbodiimide contains uncapped NCO groups in an amount not exceeding 5 wt %.

10. The resin composition according to any one of claims 1 to 9, characterized in that The weight average molecular weight of the photosensitive resin is 3000-20000; the acid value is 50-120 mgKOH / g.

11. The resin composition according to any one of claims 1 to 10, characterized in that In the resin composition, the molar amount of the carbodiimide group in the polycarbodiimide is 0.2-1.5 times the molar amount of the carboxyl group in the photosensitive resin.

12. The resin composition according to any one of claims 1 to 11, characterized in that The resin composition comprises the following components in parts by weight: 30-40 parts by weight of the photosensitive resin, 1-20 parts by weight of the polycarbodiimide, and 0.5-6 parts by weight of the photoinitiator.

13. The resin composition according to any one of claims 1 to 12, characterized in that The resin composition further comprises epoxy resin.

14. The resin composition according to claim 13, characterized in that The epoxy resin includes one or more of bisphenol A epoxy resin, bisphenol F epoxy resin, naphthalene epoxy resin, biphenyl epoxy resin, dicyclopentadiene epoxy resin, and novolac epoxy resin.

15. The resin composition according to claim 13 or 14, characterized in that The molar amount of epoxy groups in the epoxy resin is 0.8-1.5 times the molar amount of carboxyl groups in the photosensitive resin.

16. The resin composition according to any one of claims 1 to 15, characterized in that The weight proportion of the epoxy resin in the resin composition is 5-20 parts.

17. The resin composition according to any one of claims 1 to 16, characterized in that The resin composition further includes a photopolymerizable monomer.

18. The resin composition according to claim 17, characterized in that The weight proportion of the photopolymerizable monomer in the resin composition is 5-20 parts.

19. The resin composition according to any one of claims 1 to 18, characterized in that The resin composition further includes a colorant; wherein the colorant includes one or more of a pigment and a dye.

20. A membrane material, characterized in that: The invention comprises a photosensitive film, wherein the photosensitive film is formed by drying the resin composition according to any one of claims 1 to 19.

21. The membrane material according to claim 20, characterized in that: The film material further comprises a support body and a protective film, and the photosensitive film and the protective film are sequentially stacked on the support body.

22. Use of the resin composition according to any one of claims 1 to 19, or the film material according to any one of claims 19 to 20 in preparing printed circuit boards and packaging electronic components.

23. The use according to claim 22, characterized in that The application in packaging electronic components includes being used to make a patterned solder mask ink layer on a packaging carrier.

24. A packaging carrier, characterized in that: The package carrier comprises a substrate having a conductor layer on its surface, a patterned solder resist ink layer is arranged on the conductor layer, and the patterned solder resist ink layer comprises a cured product of the resin composition according to any one of claims 1 to 19.

25. A sealed package, characterized in that: It comprises the packaging carrier as claimed in claim 24, and electronic components arranged on the packaging carrier.

26. The sealed package according to claim 25, characterized in that The electronic components are arranged on the patterned solder resist ink layer.

27. An electronic device, characterized in that: The electronic device comprises a circuit board and a sealed package as claimed in any one of claims 25 to 26 arranged on the circuit board.

28. The sealed package according to claim 27, wherein: The circuit board and the electronic components are located on opposite sides of the packaging carrier.

Citation Information

Patent Citations

  • Photosensitive resin composition, solder resist film using said photosensitive resin composition, flexible printed wiring board, and image display device

    CN109983403A

  • Photosensitive resin composition, solder resist film using said photosensitive resin composition, flexible printed wiring board, and image display device

    CN110268325A

  • Curable resin composition, cured film, laminate, production method for cured film, and semiconductor device

    TW202136420A