IBC battery positive grid line aluminum paste and IBC battery

By adding boron nitride and gallium powder to the positive gate line aluminum slurry of IBC cells to form a thicker aluminum-silicon alloy layer and a higher doping slurry concentration, the problem of low photoelectric conversion efficiency of the battery in the prior art is solved. Achieve more efficient battery performance.

CN119069155AActive Publication Date: 2024-12-03DAS SOLAR CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310613000.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-25
Publication Date
2024-12-03
Estimated Expiration
2043-05-25

AI Technical Summary

Technical Problem

The positive gate line aluminum paste of existing IBC batteries cannot effectively improve the photoelectric conversion efficiency of the battery, mainly because the aluminum-silicon alloy layer is thinner and the doping concentration on the silicon surface is smaller.

Method used

Using an aluminum paste containing organic additives, boron nitride powder, aluminum powder, gallium powder and glass powder, by adding boron nitride and gallium powder to the aluminum paste, the superconductivity and permeability of gallium and aluminum grains are utilized. Inter-permeability forms a thicker aluminum-silicon alloy layer and a higher doping concentration, improving conductivity.

Benefits of technology

It improves the photoelectric conversion efficiency of IBC batteries, reduces the slurry cost, and achieves more efficient battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069155A_ABST
    Figure CN119069155A_ABST
Patent Text Reader

Abstract

The embodiment of the invention provides an IBC battery positive electrode grid line aluminum paste and an IBC battery, and the aluminum paste provided by the embodiment of the invention comprises an organic auxiliary agent, boron nitride powder, aluminum powder, gallium powder, an organic binder and glass powder. Boron carbide has the characteristic of boron, gallium and aluminum are third main group elements and have chemical characteristics similar to those of aluminum, and gallium has superconductivity and permeability, so that boron nitride and gallium powder are added into the aluminum paste, not only can form a good aluminum-silicon alloy layer and P + layer doping with silicon, but also can permeate among aluminum grains to improve the structure of the material, so that the performance of the aluminum paste is improved, and the service life of the aluminum paste is prolonged. The conductivity of the battery is improved, so that the efficiency of the battery is improved, and the problem that the photoelectric conversion efficiency of the battery cannot be effectively improved by the existing IBC battery positive electrode grid line aluminum paste is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of crystalline silicon solar cell manufacturing, and in particular to an IBC battery positive grid line aluminum paste and an IBC battery. Background Art

[0002] The interdigitated back contact (IBC) battery is a new type of battery in which the contact electrodes of the P / N junction, substrate and emitter region are made in an interdigitated shape on the back of the battery. Its core technology is to prepare high-quality p-regions and n-regions arranged in an interdigitated shape on the back of the battery.

[0003] At present, in order to increase the doping concentration of the P region to improve the photoelectric conversion efficiency of the cell, the existing P-type IBC cell needs to laser groove the P+ region and print the positive electrode grid line aluminum paste doped with boron to form the positive electrode grid line.

[0004] However, the above method of using boron-doped positive electrode grid line aluminum paste forms a thin aluminum-silicon alloy layer after sintering, and the doping concentration on the silicon surface is slightly increased, so it cannot effectively improve the photoelectric conversion efficiency of the battery. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide an IBC battery positive electrode grid line aluminum paste and an IBC battery, so as to solve the problem that the existing IBC battery positive electrode grid line aluminum paste cannot effectively improve the photoelectric conversion efficiency of the battery.

[0006] In order to solve the above problems, the present invention is achieved through the following technical solutions:

[0007] The present invention provides an IBC battery positive electrode grid line aluminum paste, wherein the components constituting the aluminum paste include organic additives, boron nitride powder, aluminum powder, gallium powder, organic adhesive and glass powder.

[0008] Furthermore, in the aluminum paste, the mass fractions of the organic additive, boron nitride powder, aluminum powder, gallium powder, organic binder and glass powder are 0.2-0.4%, 0.1-0.4%, 72-78%, 0.2-0.5%, 19.4-26.3% and 1.2-1.4% respectively.

[0009] Furthermore, in the aluminum paste, the organic additive includes one or more of fatty alcohol ether phosphate, aluminate coupling agent, silane coupling agent, zirconium aluminate coupling agent, and laurel phosphate.

[0010] Furthermore, in the aluminum paste, the gallium powder is micron-sized single-element gallium.

[0011] Furthermore, in the aluminum paste, the aluminum powder includes micron-sized spherical aluminum powder and nano-sized spherical aluminum powder.

[0012] Furthermore, in the aluminum paste, the aluminum powder includes 88 to 95 parts by mass of micron-sized spherical aluminum powder and 5 to 12 parts by mass of nano-sized spherical aluminum powder.

[0013] Furthermore, in the aluminum paste, the organic binder includes a high molecular polymer resin and an organic solvent;

[0014] The mass fraction of the high molecular weight polymer in the organic binder is 6 to 8%;

[0015] The mass fraction of the organic solvent in the organic binder is 92-94%.

[0016] Furthermore, in the aluminum paste, the high molecular polymer is ethyl cellulose-N100;

[0017] The organic solvent includes at least four of benzyl alcohol, diethyl phthalate, terpineol, butyl carbitol, butyl carbitol acetate, tributyl citrate, Span 85 and alcohol ester twelve.

[0018] Furthermore, in the aluminum paste, the glass powder includes Bi2O3 with a mass fraction of 15-25%, SiO2 with a mass fraction of 6-10%, Pb2O5 with a mass fraction of 10-15%, ZnO with a mass fraction of 5-15%, Sb2O5 with a mass fraction of 15-25%, V2O5 with a mass fraction of 15-25%, TiO2 with a mass fraction of 15-22%, and BaO with a mass fraction of 5-15%.

[0019] The present invention also provides an IBC battery, wherein a positive electrode grid line is attached to the back of the IBC, and the positive electrode grid line is prepared from the above-mentioned aluminum paste.

[0020] Compared with the prior art, the embodiments of the present invention have the following advantages:

[0021] In the embodiment of the present invention, the aluminum paste for positive gate lines of IBC batteries provided comprises organic additives, boron nitride powder, aluminum powder, gallium powder, organic adhesive and glass powder. Because boron carbide has the characteristic of containing boron elements, and gallium and aluminum are both third main group elements, and have similar chemical properties to aluminum, and gallium has superconductivity and permeability, adding boron nitride and gallium powder to the aluminum paste can not only form a good aluminum-silicon alloy layer and P+ layer doping with silicon, but also penetrate into the aluminum grains, improve the material structure, and improve the conductivity of the battery, thereby improving the efficiency of the battery, thereby solving the problem that the existing aluminum paste for positive gate lines of IBC batteries cannot effectively improve the photoelectric conversion efficiency of the battery.

[0022] It should be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a flow chart of a method for preparing an IBC battery positive grid line aluminum paste provided by an embodiment of the present invention;

[0024] Figure 2 It is a flow chart of the method for preparing an IBC battery provided in an embodiment of the present invention. DETAILED DESCRIPTION

[0025] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0026] The applicant of the present invention has found that in order to increase the doping concentration of the P region to improve the photoelectric conversion efficiency of the cell, the existing P-type IBC cell needs to laser groove the P+ region and print the positive grid line aluminum paste doped with boron to form the positive grid line.

[0027] However, the above method of using boron-doped positive electrode grid line aluminum paste forms a thin aluminum-silicon alloy layer after sintering, and the doping concentration on the silicon surface is slightly increased, so it cannot effectively improve the photoelectric conversion efficiency of the battery.

[0028] In order to solve the above problems, an embodiment of the present invention provides an IBC battery positive electrode grid line aluminum paste, wherein the components constituting the above aluminum paste include organic additives, boron nitride powder, aluminum powder, gallium powder, organic binder and glass powder.

[0029] Among them, aluminum powder is the main component; glass powder is an inorganic adhesive, which will melt into liquid under high temperature conditions and condense when cooled to play a bonding role; organic adhesives can ensure the overall bonding effect, and organic additives can reduce the overall viscosity of the aluminum paste, while making the components in the aluminum paste uniform and stable; boron nitride has the characteristic of containing boron elements and is low in cost; and gallium powder and aluminum belong to the third main group and have similar chemical characteristics. By adding gallium powder to the slurry, the above-mentioned doping substances can be used to penetrate into the aluminum grains without affecting the formation of the aluminum-silicon alloy layer and the P+ layer, thereby improving the material structure and improving the conductivity of the battery, thereby improving the photoelectric conversion efficiency of the battery.

[0030] In the embodiment of the present invention, boron nitride and gallium powder are added to the aluminum paste, which not only reduces the paste cost by using boron nitride instead of elemental boron, but also improves the thickness of the aluminum-silicon alloy formed by the paste and the silicon substrate and the doping concentration on the silicon surface, thereby improving the photoelectric conversion efficiency of the battery, thereby solving the problem that the existing IBC battery positive grid line aluminum paste cannot effectively improve the photoelectric conversion efficiency of the battery.

[0031] The IBC battery positive electrode grid line aluminum paste provided in the embodiment of the present invention is an IBC battery positive electrode grid line aluminum paste doped with boron nitride instead of elemental boron and doped with gallium powder, which is suitable for printing on the surface of the silicon wafer on the back of the IBC battery by screen printing to form a positive electrode fine grid.

[0032] Optionally, in one embodiment, in the aluminum paste, the mass fractions of the organic additive, boron nitride powder, aluminum powder, gallium powder, organic binder and glass powder are 0.2-0.4%, 0.1-0.3%, 72-78%, 0.2-0.5%, 19.4-26.3% and 1.2-1.4%, respectively. That is, in parts by mass, the aluminum paste comprises 0.2-0.4 parts of organic additive, 0.1-0.3 parts of boron nitride powder, The aluminum paste is prepared by mixing 72 to 78 parts of aluminum powder, 0.2 to 0.5 parts of gallium powder, 19.4 to 26.3 parts of organic binder and 1.2 to 1.4 parts of glass powder, so that the mass fractions of organic additive, boron nitride powder, aluminum powder, gallium powder, organic binder and glass powder in the aluminum paste are 0.2 to 0.4%, 0.1 to 0.4%, 72 to 78%, 0.2 to 0.5%, 19.4 to 26.3% and 1.2 to 1.4% respectively.

[0033] Optionally, in some embodiments, the mass fractions of organic additive, boron nitride powder, aluminum powder, gallium powder, organic binder and glass powder are 0.25-0.35%, 0.15-0.25%, 73-75%, 0.3-0.4%, 23-25% and 1.25-1.35%, respectively.

[0034] For example, the mass fractions of the organic additive, boron nitride powder, aluminum powder, gallium powder, organic binder and glass powder in the aluminum paste are 0.2%, 0.3%, 72%, 0.5%, 25.6% and 1.4%, respectively.

[0035] For example, the mass fractions of the organic additive, boron nitride powder, aluminum powder, gallium powder, organic binder and glass powder in the aluminum paste are 0.4%, 0.1%, 78%, 0.2%, 20.1% and 1.2%, respectively.

[0036] For example, the mass fractions of the organic additive, boron nitride powder, aluminum powder, gallium powder, organic binder and glass powder in the aluminum paste are 0.2%, 0.1%, 72%, 0.2%, 26.3% and 1.2%, respectively.

[0037] For example, the mass fractions of the organic additive, boron nitride powder, aluminum powder, gallium powder, organic binder and glass powder in the aluminum paste are 0.4%, 0.3%, 78%, 0.5%, 19.4% and 1.4%, respectively.

[0038] For example, the mass fractions of the organic additive, boron nitride powder, aluminum powder, gallium powder, organic binder and glass powder in the aluminum paste are 0.3%, 0.3%, 75%, 0.3%, 23.2% and 1.2%, respectively.

[0039] For example, the mass fractions of the organic additive, boron nitride powder, aluminum powder, gallium powder, organic binder and glass powder in the aluminum paste are 0.4%, 0.4%, 77%, 0.4%, 20.6% and 1.2%, respectively.

[0040] Optionally, the organic auxiliary agent may be one or more of an aluminate coupling agent, a silane coupling agent, a zirconium aluminate coupling agent, a phosphate ester, a lauryl alcohol phosphate ester, Digo 655, and BYK109.

[0041] Optionally, the purity of the boron nitride powder is more than 1 9 micron-grade boron nitride powder. In the embodiment of the present invention, the purity of the boron nitride used for doping the P region only needs to reach 1 9 to achieve effective doping, which can effectively reduce the slurry cost.

[0042] Optionally, in one embodiment, the gallium powder is micron-sized single-element gallium, specifically micron-sized single-element gallium with a purity of 2 nines.

[0043] Optionally, in one embodiment, the aluminum powder includes micron-sized spherical aluminum powder and nano-sized spherical aluminum powder. Since there is a gap between the micron-sized aluminum powder and the aluminum powder, and the nano-sized aluminum powder and the micron-sized aluminum powder are graded, the nano-sized aluminum powder can be used to fill the gap between the micron-sized aluminum powder.

[0044] Optionally, in a specific embodiment, in an embodiment of the present invention, the aluminum powder includes 88 to 95 parts of micron-sized spherical aluminum powder and 5 to 12 parts of nano-sized spherical aluminum powder, measured by mass. That is, the above-mentioned aluminum powder includes 88 to 95% of micron-sized spherical aluminum powder and 5 to 12% of nano-sized spherical aluminum powder by mass.

[0045] For example, the aluminum powder includes 88 parts of micron-sized spherical aluminum powder and 12 parts of nano-sized spherical aluminum powder by mass.

[0046] For example, the aluminum powder includes 90 parts by mass of micron-sized spherical aluminum powder and 10 parts by mass of nano-sized spherical aluminum powder.

[0047] For example, the aluminum powder includes 92 parts of micron-sized spherical aluminum powder and 8 parts of nano-sized spherical aluminum powder by mass.

[0048] For example, the aluminum powder includes 95 parts of micron-sized spherical aluminum powder and 5 parts of nano-sized spherical aluminum powder by mass.

[0049] Optionally, in one embodiment, the organic binder includes 6-8 parts of a polymer resin and 92-94 parts of an organic solvent, by weight. The organic binder includes a polymer resin and an organic solvent; that is, the mass fraction of the polymer in the organic binder is 6-8%, and the mass fraction of the organic solvent in the organic binder is 92-94%. The polymer is dissolved in the organic solvent, so that the organic solvent can be used as an organic binder, that is, the slurry can play a role in bonding the powder after drying.

[0050] Among them, the above-mentioned high molecular polymer resin can be one or more of ethyl cellulose, acrylic resin, nitrocellulose, phenolic resin, rosin resin, cellulose acetate, epoxy resin, and polymethacrylate; the above-mentioned organic solvent can be at least three of phenylmethyl alcohol, terpineol, diethyl phthalate, terpineol, butyl carbitol, butyl carbitol acetate, tributyl citrate, and Span 85.

[0051] In the embodiment of the present invention, the glass powder includes Bi2O3, SiO2, Pb2O5, ZnO, Sb2O5, V2O5, TiO2 and BaO, that is, the glass powder is obtained by sintering and crushing Bi2O3, SiO2, Pb2O5, ZnO, Sb2O5, V2O5, TiO2 and BaO. Among them, Bi2O3 is the main network structure, ZnO can break the network structure and promote glass crystallization, Sb2O5 is used to clarify and uniform the glass liquid; SiO2 is a glass network former, which promotes glass stability and improves the melting point of glass; Pb2O5 reacts with silicon nitride to generate lead, nitrogen and silicon dioxide; V2O5 and TiO2 can assist Pb2O5 and silicon nitride to react; BaO is used for local crystallization.

[0052] Optionally, in one embodiment, the glass powder includes Bi2O3 with a mass fraction of 15-25%, SiO2 with a mass fraction of 6-10%, Pb2O5 with a mass fraction of 10-15%, ZnO with a mass fraction of 5-15%, Sb2O5 with a mass fraction of 15-25%, V2O5 with a mass fraction of 5-15%, TiO2 with a mass fraction of 15-22%, and BaO with a mass fraction of 5-15%, and the D50 of the glass powder is 1-1.6μm.

[0053] For example, the glass powder includes, by mass, 15% Bi2O3, 10% SiO2, 10% Pb2O5, 15% ZnO, 15% Sb2O5, 15% V2O5, 15% TiO2, and 5% BaO.

[0054] For example, the glass powder includes, by mass, 25% Bi2O3, 6% SiO2, 10% Pb2O5, 5% ZnO, 15% Sb2O5, 15% V2O5, 15% TiO2, and 9% BaO.

[0055] For example, in terms of mass fraction, the glass powder includes 22% Bi2O3, 6% SiO2, 12% Pb2O5, 10% ZnO, 18% Sb2O5, 7% V2O5, 15% TiO2, and 10% BaO.

[0056] The present invention also provides a method for preparing aluminum paste for positive grid lines of an IBC battery, such as Figure 1 As shown, it includes steps 101 to 103:

[0057] Step 101, mixing boron nitride powder, aluminum powder, gallium powder, an organic binder and glass powder to obtain a mixture;

[0058] Step 102: Grind the mixture, add an organic additive, and obtain aluminum paste for positive grid lines of IBC batteries.

[0059] In the above step 101, 0.1-0.3% of boron nitride powder, 72-78% of aluminum powder, 0.2-0.5% of gallium powder, 19.4-26.3% of organic binder, and 1.2-1.4% of glass powder, which account for 0.1-0.3% of the total mass of the raw materials, are weighed and mixed, and dispersed by a disperser to obtain the above mixture.

[0060] Optionally, in one embodiment, in the above step 101, the organic binder, nano-sized aluminum powder, boron nitride powder and gallium powder are first mixed and dispersed using a disperser, and then micron-sized aluminum powder is added, dispersed again using a disperser, and then ground to obtain the above mixture.

[0061] In the above step 102, the above mixture is ground and then an organic additive accounting for 0.2-0.4% of the total mass of the raw materials is added, and after high-speed dispersion, an IBC battery positive electrode grid line aluminum paste that can be formed without laser grooving and can effectively improve the photoelectric conversion efficiency of the battery is obtained.

[0062] In the embodiment of the present invention, because boron carbide has the characteristic of containing boron elements, and gallium and aluminum are both third main group elements, have similar chemical properties to aluminum, and gallium has superconductivity and permeability, adding boron nitride and gallium powder to the aluminum paste can not only form a good aluminum-silicon alloy layer and P+ layer doping with silicon, but also penetrate into between aluminum grains, improve the material structure, and improve the conductivity of the battery, thereby improving the efficiency of the battery, thereby solving the problem that the existing IBC battery positive grid line aluminum paste cannot effectively improve the photoelectric conversion efficiency of the battery.

[0063] Optionally, in the preparation method provided in the embodiment of the present invention, the organic auxiliary agent includes one or more of fatty alcohol ether phosphate, aluminate coupling agent, silane coupling agent, zirconium aluminate coupling agent, and laurel phosphate.

[0064] Optionally, in the preparation method provided in an embodiment of the present invention, the gallium powder is micron-sized single-element gallium.

[0065] Optionally, in the preparation method provided in an embodiment of the present invention, the aluminum powder includes micron-sized spherical aluminum powder and nano-sized spherical aluminum powder.

[0066] Optionally, in the preparation method provided in the embodiment of the present invention, the aluminum powder includes 88 to 95 parts by mass of micron-sized spherical aluminum powder and 5 to 12 parts by mass of nano-sized spherical aluminum powder.

[0067] Optionally, in the preparation method provided in the embodiment of the present invention, the organic binder comprises a high molecular polymer resin and an organic solvent;

[0068] The mass fraction of the high molecular weight polymer in the organic binder is 6 to 8%;

[0069] The mass fraction of the organic solvent in the organic binder is 92-94%.

[0070] Optionally, in the preparation method provided in the embodiment of the present invention, the high molecular polymer is ethyl cellulose-N100;

[0071] The organic solvent includes at least four of benzyl alcohol, diethyl phthalate, terpineol, butyl carbitol, butyl carbitol acetate, tributyl citrate, Span 85 and alcohol ester twelve.

[0072] Optionally, in the preparation method provided in an embodiment of the present invention, the glass powder includes Bi2O3 with a mass fraction of 15-25%, SiO2 with a mass fraction of 6-10%, Pb2O5 with a mass fraction of 10-15%, ZnO with a mass fraction of 5-15%, Sb2O5 with a mass fraction of 15-25%, V2O5 with a mass fraction of 15-25%, TiO2 with a mass fraction of 15-22%, and BaO with a mass fraction of 5-15%.

[0073] The present invention also provides a method for preparing an IBC battery, wherein: Figure 2 As shown, it includes steps 201 to 203:

[0074] Step 201, after forming interdigitated n+ doped regions and p+ doped regions on the back side of the silicon wafer, a passivation layer is formed on the surfaces of the n+ doped regions and the p+ doped regions;

[0075] Step 202, printing aluminum paste on the first area of ​​the passivation layer after laser grooving, and printing silver paste on the second area of ​​the passivation layer; the projection of the first area is within the range of the p+ doped area, and the projection of the second area is within the range of the n+ doped area; wherein the components constituting the aluminum paste include organic additives, boron nitride powder, aluminum powder, gallium powder, organic adhesive and glass powder;

[0076] Step 203: high-temperature sintering the P-type silicon wafer with aluminum paste printed on the first region and silver paste printed on the second region to obtain an IBC battery.

[0077] In the above step 201, the silicon wafer is firstly subjected to alkali texturing, and then an n+ doped region and a p+ doped region arranged in a finger-like manner are formed on the back of the silicon wafer, and then a silicon oxide layer or a silicon nitride layer is deposited to cover the entire back of the silicon wafer as the above passivation layer.

[0078] In the above step 202, the silicon wafer after forming the passivation layer is laser grooved and then screen printed to prepare the electrode grid lines. Specifically, the aluminum paste is printed on the first area of ​​the passivation layer on the back of the silicon wafer after laser grooves are made, and the projection of the first area is within the p+ doped area to form a positive grid line that is conductive with the p+ doped area; at the same time, silver paste is also required to be printed on the second area of ​​the back passivation layer, and the projection of the second area is within the n+ doped area to form a negative grid line spaced from the positive grid line, wherein the silver paste can be a traditional silver paste.

[0079] In the above step 203, boron nitride and gallium powder are added to the aluminum paste, which not only reduces the paste cost by using boron nitride instead of elemental boron, but also improves the thickness of the aluminum-silicon alloy formed by the paste and the silicon substrate and the doping concentration on the silicon surface, thereby improving the photoelectric conversion efficiency of the battery; and gallium powder and aluminum belong to the third main group and have similar chemical characteristics. By adding gallium powder to the paste, the above-mentioned doping substances can be used to penetrate between the aluminum grains without affecting the doping formation of the aluminum-silicon alloy layer and the P+ layer, thereby improving the material structure and improving the conductivity of the battery, thereby further improving the photoelectric conversion efficiency of the battery.

[0080] Therefore, the embodiments of the present invention solve the problem that the existing aluminum paste for the positive grid line of an IBC battery cannot effectively improve the photoelectric conversion efficiency of the battery.

[0081] The silicon wafer may be an N-type silicon wafer or a P-type silicon wafer.

[0082] For example, when the silicon wafer is a P-type silicon wafer, step 101 specifically includes:

[0083] (1) Take a P-type original silicon wafer, and use low pressure chemical vapor deposition (LPCVD) to form an ultra-thin silicon oxide layer on the back of the P-type silicon wafer as an ultra-thin tunneling oxide layer, and then prepare a polysilicon layer with a thickness that can meet the passivation effect on both sides; because the double-sided preparation of the polysilicon layer is conducive to the subsequent removal of the front polysilicon layer, it is not easy to have the two extreme situations of excessive removal or insufficient removal, and the yield is better controlled;

[0084] (2) After the polysilicon layer is prepared, the silicon wafer is fed into a furnace tube to dope the polysilicon layer with phosphorus to form an n+ doped region;

[0085] (3) laser grooving the back of the silicon wafer to expose the p+ doped region, forming n+ doped regions and p+ doped regions arranged in an interdigitated manner, and then removing the front polysilicon layer by a wet method;

[0086] (4) Atomic layer deposition (ALD) is used to plate a passivation layer on the entire front and back of the product to form field passivation; after the aluminum oxide film is formed, an anti-reflection film is first plated on the front of the battery, and then on the back to further enhance the passivation effect of the battery cell.

[0087] The present invention further provides an IBC battery, wherein a positive electrode grid line is attached to the back of the IBC, and the positive electrode grid line is prepared from the aluminum paste.

[0088] The present invention is described in detail below by way of examples.

[0089] Example 1

[0090] (1) Preparation of glass powder: 22 parts of Bi2O3, 6 parts of SiO2, 12 parts of Pb2O5, 10 parts of ZnO, 18 parts of Sb2O5, 7 parts of V2O5, 15 parts of TiO2, and 10 parts of BaO were weighed by mass, mixed evenly with a mixer, loaded into a porcelain crucible, placed in a muffle furnace, and kept at 950°C for 120 minutes. The melted glass powder particles were quenched with deionized water, ball-milled for 4 hours, and sieved through a 300-mesh sieve to obtain glass powder with a particle size D50 of 1 to 1.6 μm;

[0091] (2) Preparation of organic binder: 6 parts of ethyl cellulose-N100 and 94 parts of organic solvent were weighed by weight, mixed and dispersed on a large disperser for 40 to 50 minutes to obtain a transparent and uniform organic binder; wherein, by weight, the organic solvent includes 0.5 parts of phenylmethyl alcohol, 62 parts of butyl carbitol, 32.7 parts of butyl carbitol acetate, 0.3 parts of tributyl citrate, 0.5 parts of Span 85 and 4 parts of alcohol ester dodecahydrate;

[0092] (3) Preparation of aluminum powder: Weigh 90 parts by mass of micron-grade aluminum powder and 10 parts by mass of nano-grade aluminum powder, and mix them to obtain mixed aluminum powder;

[0093] (4) Preparation of aluminum paste: 0.3 parts of boron nitride powder, 75 parts of aluminum powder, 0.3 parts of elemental gallium powder, 23.2 parts of organic binder, and 1.2 parts of glass powder were weighed by mass and mixed. After mixing evenly with a disperser, the mixture was ground to less than 20 μm with a three-roll grinder. Then, 0.1 parts of zirconium aluminate coupling agent and 0.2 parts of lauryl phosphate were added and stirred thoroughly to obtain aluminum paste.

[0094] The sample aluminum paste prepared as above was used to form a positive electrode fine grid on the back side of a P-type single crystal silicon wafer with a size of 182mm×182mm by 380 mesh screen printing, and then sintered in a sintering furnace with a peak temperature of 766°C.

[0095] After sintering, the electrical properties tested were: open circuit voltage of 0.719 V, short circuit current of 13.845 A, fill factor of 83.45, and photoelectric conversion efficiency of 25.16%.

[0096] Example 2

[0097] (1) Preparation of glass powder: 22 parts of Bi2O3, 6 parts of SiO2, 12 parts of Pb2O5, 10 parts of ZnO, 18 parts of Sb2O5, 7 parts of V2O5, 15 parts of TiO2, and 10 parts of BaO were weighed by mass, mixed evenly with a mixer, loaded into a porcelain crucible, placed in a muffle furnace, and kept at 950°C for 120 minutes. The melted glass powder particles were quenched with deionized water, ball-milled for 4 hours, and sieved through a 300-mesh sieve to obtain glass powder with a particle size D50 of 1 to 1.6 μm;

[0098] (2) Preparation of organic binder: 9 parts of ethyl cellulose-N100 and 91 parts of organic solvent were weighed by weight, mixed and dispersed on a large disperser for 40 to 50 minutes to obtain a transparent and uniform organic binder; wherein, by weight, the organic solvent includes 0.5 parts of phenylmethyl alcohol, 62 parts of butyl carbitol, 32.7 parts of butyl carbitol acetate, 0.3 parts of tributyl citrate, 0.5 parts of Span 85 and 4 parts of alcohol ester dodecahydrate;

[0099] (3) Preparation of aluminum powder: Weigh 92 parts by mass of micron-grade aluminum powder and 8 parts by mass of nano-grade aluminum powder, and mix them to obtain mixed aluminum powder;

[0100] (4) Preparation of aluminum paste: 0.4 parts of boron nitride powder, 77 parts of aluminum powder, 0.4 parts of elemental gallium powder, 20.6 parts of organic binder, and 1.2 parts of glass powder were weighed by mass and mixed. After mixing evenly with a disperser, the mixture was ground to less than 20 μm with a three-roll grinder. Then, 0.2 parts of zirconium aluminate coupling agent and 0.2 parts of lauryl phosphate were added and stirred thoroughly to obtain aluminum paste.

[0101] The sample aluminum paste prepared as above was used to form a positive electrode fine grid on the back side of a P-type single crystal silicon wafer with a size of 182mm×182mm by 380 mesh screen printing, and then sintered in a sintering furnace with a peak temperature of 768°C.

[0102] After sintering, the electrical properties tested were: open circuit voltage of 0.722V, short circuit current of 13.885A, fill factor of 83.2, and photoelectric conversion efficiency of 25.17%.

[0103] Example 3

[0104] The difference between Example 3 and Example 2 is that in step (1), 15 parts of Bi2O3, 10 parts of SiO2, 10 parts of Pb2O5, 15 parts of ZnO, 15 parts of Sb2O5, 15 parts of V2O5, 15 parts of TiO2, and 5 parts of BaO are weighed by mass, mixed evenly with a mixer, loaded into a porcelain crucible, placed in a muffle furnace, and kept warm at 950°C for 120 minutes. The melted glass powder particles are quenched with ionized water, ball-milled for 4 hours, and sieved through a 300-mesh sieve to obtain glass powder with a particle size D50 of 1 to 1.6 μm.

[0105] The sample aluminum paste prepared in Example 3 was used to form a positive electrode fine grid on the back side of a P-type single crystal silicon wafer with a size of 182mm×182mm by 360-mesh screen printing, and then sintered in a sintering furnace with a peak temperature of 768°C.

[0106] After sintering, the electrical properties tested were: open circuit voltage of 0.720V, short circuit current of 13.835A, fill factor of 83.25, and photoelectric conversion efficiency of 25.117%.

[0107] Example 4

[0108] The difference between Example 4 and Example 2 is that in step (1), 25 parts of Bi2O3, 6 parts of SiO2, 10 parts of Pb2O5, 5 parts of ZnO, 15 parts of Sb2O5, 15 parts of V2O5, 15 parts of TiO2, and 9 parts of BaO are weighed by mass, mixed evenly with a mixer, loaded into a porcelain crucible, placed in a muffle furnace, and kept warm at 950°C for 120 minutes. The melted glass powder particles are quenched with ionized water, ball-milled for 4 hours, and sieved through a 300-mesh sieve to obtain glass powder with a particle size D50 of 1 to 1.6 μm.

[0109] The sample aluminum paste prepared in Example 4 was used to form a positive electrode fine grid on the back side of a P-type single crystal silicon wafer with a size of 182mm×182mm by 380 mesh screen printing, and then sintered in a sintering furnace with a peak temperature of 768°C.

[0110] After sintering, the electrical properties tested were as follows: open circuit voltage was 0.7205V, short circuit current was 13.832A, fill factor was 83.28, and photoelectric conversion efficiency was 25.139%.

[0111] Example 5

[0112] The difference between Example 5 and Example 2 is that in step (4), 0.1 parts of boron nitride powder, 72 parts of aluminum powder, 0.2 parts of elemental gallium powder, 26.3 parts of organic binder, and 1.2 parts of glass powder are weighed by mass and mixed, and after being evenly mixed using a disperser, they are ground to less than 20 microns using a three-roll grinder, and then 0.1 parts of zirconium aluminate coupling and 0.1 parts of lauryl phosphate are added, and the mixture is fully stirred to obtain aluminum paste.

[0113] The sample aluminum paste prepared in Example 5 was used to form a positive electrode fine grid on the back side of a P-type single crystal silicon wafer with a size of 182mm×182mm by 380 mesh screen printing, and then sintered in a sintering furnace with a peak temperature of 768°C.

[0114] After sintering, the electrical properties tested were: open circuit voltage of 0.7201V, short circuit current of 13.828A, fill factor of 83.31, and photoelectric conversion efficiency of 25.126%.

[0115] Example 6

[0116] The difference between Example 6 and Example 2 is that in step (4), 0.3 parts of boron nitride powder, 72 parts of aluminum powder, 0.5 parts of elemental gallium powder, 25.6 parts of organic binder, and 1.4 parts of glass powder are weighed by mass and mixed, and after being evenly mixed using a disperser, they are ground to less than 20 microns using a three-roll grinder, and then 0.1 parts of zirconium aluminate coupling and 0.1 parts of lauryl phosphate are added, and the mixture is fully stirred to obtain aluminum paste.

[0117] The sample aluminum paste prepared in Example 6 was used to form a positive electrode fine grid on the back side of a P-type single crystal silicon wafer with a size of 182mm×182mm by 380 mesh screen printing, and then sintered in a sintering furnace with a peak temperature of 768°C.

[0118] After sintering, the electrical properties tested were: open circuit voltage of 0.7205V, short circuit current of 13.831A, fill factor of 83.26, and photoelectric conversion efficiency of 25.131%.

[0119] Comparative Example 1

[0120] (1) Preparation of glass powder: 22 parts of Bi2O3, 6 parts of SiO2, 12 parts of Pb2O5, 10 parts of ZnO, 18 parts of Sb2O5, 7 parts of V2O5, 15 parts of TiO2, and 10 parts of BaO were weighed by mass, mixed evenly with a mixer, loaded into a porcelain crucible, placed in a muffle furnace, and kept at 950°C for 120 minutes. The melted glass powder particles were quenched with deionized water, ball-milled for 4 hours, and sieved through a 300-mesh sieve to obtain glass powder with a particle size D50 of 1 to 1.6 μm;

[0121] (2) Preparation of organic binder: 9 parts of ethyl cellulose-N100 and 91 parts of organic solvent were weighed by weight, mixed and dispersed on a large disperser for 40 to 50 minutes to obtain a transparent and uniform organic binder; wherein, by weight, the organic solvent includes 0.5 parts of phenylmethyl alcohol, 62 parts of butyl carbitol, 32.7 parts of butyl carbitol acetate, 0.3 parts of tributyl citrate, 0.5 parts of Span 85 and 4 parts of alcohol ester dodecahydrate;

[0122] (3) Preparation of aluminum powder: Weigh 92 parts by mass of micron-grade aluminum powder and 8 parts by mass of nano-grade aluminum powder, and mix them to obtain mixed aluminum powder;

[0123] (4) Preparation of aluminum paste: 0.15 parts of boron powder, 77 parts of aluminum powder, 0.4 parts of elemental gallium powder, 20.55 parts of organic binder, and 1.2 parts of glass powder were weighed by mass and mixed. After mixing evenly with a disperser, the mixture was ground to less than 20 μm with a three-roll grinder. Then, 0.2 parts of zirconium aluminate coupling agent and 0.2 parts of lauryl phosphate were added and stirred thoroughly to obtain aluminum paste.

[0124] The sample aluminum paste prepared as above was used to form a positive electrode fine grid on the back side of a P-type single crystal silicon wafer with a size of 182mm×182mm by 380 mesh screen printing, and then sintered in a sintering furnace with a peak temperature of 788°C.

[0125] After sintering, the electrical properties tested were: open circuit voltage of 0.715V, short circuit current of 13.855A, fill factor of 83.52, and photoelectric conversion efficiency of 25.061%.

[0126] Experiments show that the aluminum paste provided in the embodiments of the present invention can increase the battery conversion efficiency by more than 0.08% while reducing the cost.

[0127] In summary, in the embodiment of the present invention, the aluminum paste for the positive grid line of an IBC battery provided comprises an organic additive, boron nitride powder, aluminum powder, gallium powder, an organic adhesive and glass powder. Because boron carbide has the characteristic of containing boron elements, and gallium and aluminum are both third main group elements, and have similar chemical properties to aluminum, and gallium has superconductivity and permeability, adding boron nitride and gallium powder to the aluminum paste can not only form a good aluminum-silicon alloy layer and P+ layer doping with silicon, but also penetrate into the aluminum grains, improve the material structure, and improve the conductivity of the battery, thereby improving the efficiency of the battery, thereby solving the problem that the existing aluminum paste for the positive grid line of an IBC battery cannot effectively improve the photoelectric conversion efficiency of the battery.

[0128] Although the preferred embodiments of the present invention have been described, those skilled in the art may make additional changes and modifications to these embodiments once they are aware of the basic creative concept. Therefore, the claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the embodiments of the present invention.

[0129] The above is a detailed introduction to an IBC battery positive grid line aluminum paste and an IBC battery provided by the present invention. Specific examples are used in this article to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core idea; at the same time, for general technicians in this field, according to the ideas of the present invention, there will be changes in the specific implementation methods and application scopes. In summary, the content of this specification should not be understood as a limitation on the present invention.

Claims

1. A kind of IBC battery positive electrode grid line aluminum paste, It is characterized in that The components constituting the aluminum paste include organic additives, boron nitride powder, aluminum powder, gallium powder, organic binder and glass powder.

2. The aluminum paste according to claim 1, It is characterized in that In the aluminum paste, the mass fractions of the organic additive, boron nitride powder, aluminum powder, gallium powder, organic binder and glass powder are 0.2-0.4%, 0.1-0.4%, 72-78%, 0.2-0.5%, 19.4-26.3% and 1.2-1.4% respectively.

3. The aluminum paste according to claim 1 or 2, It is characterized in that The organic auxiliary agent includes one or more of fatty alcohol ether phosphate, aluminate coupling agent, silane coupling agent, zirconium aluminate coupling agent, and laurel phosphate.

4. The aluminum paste according to claim 1, It is characterized in that The gallium powder is micron-sized single-element gallium.

5. The aluminum paste according to claim 1, It is characterized in that The aluminum powder includes micron-sized spherical aluminum powder and nanometer-sized spherical aluminum powder.

6. The aluminum paste according to claim 1, It is characterized in that The aluminum powder includes 88 to 95 parts by mass of micron-sized spherical aluminum powder and 5 to 12 parts by mass of nano-sized spherical aluminum powder.

7. The aluminum paste according to claim 1, It is characterized in that The organic binder includes a high molecular polymer resin and an organic solvent; The mass fraction of the high molecular weight polymer in the organic binder is 6 to 8%; The mass fraction of the organic solvent in the organic binder is 92-94%.

8. The aluminum paste according to claim 7, It is characterized in that The high molecular polymer is ethyl cellulose-N100; The organic solvent includes at least four of benzyl alcohol, diethyl phthalate, terpineol, butyl carbitol, butyl carbitol acetate, tributyl citrate, Span 85 and alcohol ester twelve.

9. The aluminum paste according to claim 1, It is characterized in that The glass powder includes Bi with a mass fraction of 15 to 25%. 2 O 3 , SiO with a mass fraction of 6 to 10% 2 , Pb with a mass fraction of 10-15% 2 O 5 , 5-15% by mass ZnO, 15-25% by mass Sb 2 O 5 , V with a mass fraction of 5 to 15% 2 O 5 , TiO with a content of 15-22% 2 , BaO with a mass fraction of 5 to 15%.

10. An IBC battery, It is characterized in that A positive electrode grid line is attached to the back of the IBC battery, and the positive electrode grid line is prepared from the aluminum paste described in any one of claims 1 to 9.

Citation Information

Patent Citations

  • Aluminum conductive paste for silicon solar cell back surface field and preparation method thereof

    CN101621082A

  • Aluminum conductive paste for crystalline silicon solar cell and preparation method and application thereof

    CN105469855A

  • Solar cell aluminum paste adopting modified boron nitride to replace elementary boron for doping, and preparation method thereof

    CN108447623A