Low-gradient resistor disc for lightning arrester monitor and preparation method of low-gradient resistor disc
By using special low-temperature glass, boric acid and titanium dioxide as sintering promoters in low-gradient resistor sheets, the microstructure of the resistor sheets is optimized, and the problems of high residual lightning waves and low charge transfer performance are solved, and better charge transfer performance is achieved and reduce the residual voltage of lightning waves, improving the protection effect of the lightning arrester.
Patent Information
- Application Number
- CN202411287049.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-13
AI Technical Summary
The existing low-gradient resistor sheets have high residual voltage of lightning waves and low charge transfer performance, resulting in equipment insulation damage and breakdown, affecting system stability and power supply quality.
Special low-temperature glass, boric acid and titanium dioxide are used as sintering accelerators. By adjusting their proportion and bulk density, the microstructure and electrical performance of the resistor sheet are optimized, the residual voltage of the lightning wave is reduced and the charge transfer performance is improved.
It effectively reduces the residual voltage of lightning waves, improves the charge transfer performance, enhances the overall performance of the resistor, and improves the overvoltage protection capability and system reliability of the lightning arrester.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of resistor sheets, and in particular to a low-gradient resistor sheet for a lightning arrester monitor and a preparation method thereof. Background Art
[0002] The resistor for the arrester monitor is an important component used in the arrester monitor. The resistor for the arrester detector can be classified into high-gradient resistors, medium-gradient resistors, and low-gradient resistors according to the gradient. The voltage generated by the low-gradient resistor per unit thickness is relatively low, and it can effectively limit the overvoltage at a lower voltage. Due to its good nonlinear characteristics and high stability, it is widely used in power systems, industrial fields, and rail transportation. However, the low-gradient resistors currently used generally have problems such as large residual voltage of lightning waves, low charge transfer performance, large resistor diameter, and are not conducive to the miniaturization and installation of detectors. The excessive residual voltage of lightning waves will not only cause the protected electrical equipment to withstand excessive voltage, resulting in equipment insulation damage and breakdown, but also affect the system stability, leading to system voltage fluctuations, tripping and other problems, affecting the power supply quality and reliability, and reducing the protection effect of the arrester. The low charge transfer performance means that the resistor cannot quickly transfer the charge generated by the lightning impulse in a short time, resulting in the overvoltage not being released in time, reducing the overvoltage protection capability of the arrester, increasing the risk of equipment damage, and affecting the reliability of the system. Therefore, developing a low-gradient resistor with low lightning wave residual voltage and high charge transfer performance is an urgent problem to be solved. Summary of the invention
[0003] The present invention provides a low-gradient resistor for a lightning arrester monitor and a preparation method thereof, which solves the problems of high residual voltage of lightning waves and low charge transfer performance of low-gradient resistors in related technologies.
[0004] The technical solution of the present invention is as follows: The present invention provides a low-gradient resistor for a lightning arrester monitor, comprising the following component raw materials in parts by weight: 85-90 parts of zinc oxide, 1.2-3.6 parts of a sintering accelerator; The sintering accelerator includes one or more of special low-temperature glass, boric acid, and titanium dioxide.
[0005] As a further technical solution, the bulk density of the special low-temperature glass is 0.61-0.81 g / cm 3 .
[0006] In the present invention, the bulk density is selected to be 0.61~0.81g / cm 3The special low-temperature glass is used as one of the raw materials of the sintering accelerator, which helps to achieve more uniform filling and distribution of the resistor in the production process, ensure the consistency of the resistor's microstructure, optimize the sintering process, make the sintering more complete and uniform, thereby improving the electrical performance of the resistor and obtaining a resistor with low lightning wave residual voltage and high charge transfer performance.
[0007] As a further technical solution, when the sintering accelerator is composed of special low-temperature glass, boric acid, and titanium dioxide, the mass ratio of the special low-temperature glass to boric acid and titanium dioxide is 2~4:1:1.
[0008] In the present invention, by adjusting the ratio between the sintering promoters, the respective advantages of the three substances are fully utilized, so that they produce a synergistic effect in improving the performance of the resistor, effectively reducing the residual voltage of lightning waves, improving the charge transfer performance, and enhancing the overall performance of the resistor.
[0009] As a further technical solution, the mass ratio of the special low-temperature glass, boric acid and titanium dioxide is 3:1:1.
[0010] As a further technical solution, the following component raw materials are also included in weight: 1 to 3 parts of additives, wherein the additives include one or more of cobalt trioxide, manganese carbonate, antimony trioxide, and chromium trioxide.
[0011] As a further technical solution, the following component raw materials are also included in weight: 1 to 6 parts of flux, wherein the flux includes one or more of oxalic acid, acetic acid, and citric acid.
[0012] As a further technical solution, the method further includes the following component raw materials in parts by weight: 2 to 8 parts of a uniformity aid, wherein the uniformity aid includes one or more of zinc hydroxide, cobalt hydroxide, and nickel hydroxide.
[0013] As a further technical solution, it also includes the following component raw materials in parts by weight: 7 to 10 parts of bismuth-based low-temperature lead-free glass glaze powder, which is composed of the following raw materials in parts by weight: 4.5 to 5 parts of bismuth oxide, 0.5 to 1 part of silicon dioxide, 0.5 to 0.8 parts of boron trioxide, 0.3 to 0.5 parts of aluminum oxide, 0.6 to 0.8 parts of calcium oxide, 0.5 to 1 part of lithium oxide, and 0.5 to 0.8 parts of potassium oxide.
[0014] As a further technical solution, the preparation method of the bismuth-based low-temperature lead-free glass glaze powder includes the following steps: mixing the raw materials of the bismuth-based low-temperature lead-free glass glaze powder, melting, cooling, and crushing to obtain the bismuth-based low-temperature lead-free glass glaze powder.
[0015] As a further technical solution, the particle size D50 of the bismuth-based low-temperature lead-free glass glaze powder obtained after the pulverization is 1 μm to 3 μm.
[0016] The present invention also provides a method for preparing a low-gradient resistor for a lightning arrester monitor, comprising the following steps: S1, weighing the zinc oxide sintering accelerator in parts by weight, mixing, granulating, and molding to obtain a resistor green body; S2, drying, calcining and debinding the resistor green body to obtain a resistor pre-sintered green body; S3, spraying aluminum on the end surface of the pre-sintered body of the resistor, coating the side with bismuth-based low-temperature lead-free glass glaze, and obtaining a low-gradient resistor after sintering.
[0017] As a further technical solution, the debinding temperature is 300-400°C, the debinding time is 1-3 hours, and the sintering temperature is 1200-1300°C.
[0018] The working principle and beneficial effects of the present invention are: In the present invention, special low-temperature glass, boric acid and titanium dioxide are used as sintering accelerators, which can not only promote the good growth and uniform distribution of zinc oxide grains, form a dense microstructure, adjust the electrical performance parameters of the resistor, so that the resistor as a whole can better withstand lightning impact and reduce the lightning residual voltage value, but also improve the conductive channel inside the resistor, improve the efficiency of charge transfer, avoid local charge accumulation, and improve the response speed and charge transfer performance of the resistor. DETAILED DESCRIPTION
[0019] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0020] Example 1 Bismuth-based low-temperature lead-free glass glaze powder: weigh 4.5 parts of bismuth oxide, 0.5 parts of silicon dioxide, 0.5 parts of boron trioxide, 0.3 parts of aluminum oxide, 0.6 parts of calcium oxide, 0.5 parts of lithium oxide, and 0.5 parts of potassium oxide, mix them evenly, melt them at 800°C, pour them into water and cool them quickly to form glass slag, and obtain bismuth-based low-temperature lead-free glass glaze powder with a particle size D50 of 1 μm after ball milling and screening.
[0021] A method for preparing a low-gradient resistor for a lightning arrester monitor comprises the following steps: S1. Weigh 85 parts of zinc oxide, 1 part of cobalt trioxide, and special low-temperature glass (with a bulk density of 0.57 g / cm 3 , Model D270, melting point 700℃, linear expansion coefficient 90×10 -7, the manufacturer is Anmi Micro-Nano New Materials Co., Ltd.) 1.2 parts, oxalic acid 1 part, zinc hydroxide 2 parts, mixed and dried to granulate, and molded to obtain the resistor green body; S2. After the resistor green body is dried, it is placed in a calcination and debinding chamber, and the temperature is raised to 300°C at a heating rate of 3°C / min. The calcination and debinding are started and the temperature is kept for 1 hour. The resistor green body is cooled to room temperature to obtain a resistor pre-sintered body. S3, use an automatic aluminum spraying machine to spray the end face of the pre-sintered resistor sheet with full electrode, coat the side with bismuth-based low-temperature lead-free glass glaze, and sinter at 1200℃ for 30 minutes to obtain a low-gradient resistor sheet. The gradient of the resistor sheet is 25V / mm, the thickness is 8mm, and the diameter is 60mm.
[0022] Example 2 Bismuth-based low-temperature lead-free glass glaze powder: weigh 4.8 parts of bismuth oxide, 0.8 parts of silicon dioxide, 0.6 parts of boron trioxide, 0.4 parts of aluminum oxide, 0.7 parts of calcium oxide, 0.8 parts of lithium oxide, and 0.6 parts of potassium oxide, mix them evenly and melt them at 850°C, pour them into water and quickly cool them to form glass slag, and then obtain bismuth-based low-temperature lead-free glass glaze powder with a particle size D50 of 2μm after ball milling and screening.
[0023] A method for preparing a low-gradient resistor for a lightning arrester monitor comprises the following steps: S1. Weigh 88 parts of zinc oxide, 2 parts of manganese carbonate, and special low-temperature glass (with a bulk density of 0.57 g / cm 3 , Model D270, melting point 700℃, linear expansion coefficient 90×10 -7 , the manufacturer is Anmi Micro-Nano New Materials Co., Ltd.) 2.4 parts, acetic acid 3 parts, cobalt hydroxide 5 parts, mixed and dried to granulate, and molded to obtain the resistor green body; S2. After the resistor green body is dried, it is placed in a calcination and debinding chamber, and the temperature is raised to 350°C at a heating rate of 4°C / min. The calcination and debinding are started, and the temperature is kept for 2 hours. The resistor green body is cooled to room temperature to obtain a resistor pre-sintered body. S3. Use an automatic aluminum spraying machine to spray the end face of the pre-sintered resistor sheet with full electrodes, coat the side with bismuth-based low-temperature lead-free glass glaze, and sinter at 1250℃ for 20 minutes to obtain a low-gradient resistor sheet. The gradient of the resistor sheet is 25V / mm, the thickness is 8mm, and the diameter is 60mm.
[0024] Example 3 Bismuth-based low-temperature lead-free glass glaze powder: weigh 5 parts of bismuth oxide, 5 parts of silicon dioxide, 0.8 parts of boron trioxide, 0.5 parts of aluminum oxide, 0.5 parts of calcium oxide, 5 parts of lithium oxide, and 0.8 parts of potassium oxide, mix them evenly, melt them at 900°C, pour them into water and quickly cool them to form glass slag, and obtain bismuth-based low-temperature lead-free glass glaze powder with a particle size D50 of 3μm after ball milling and screening.
[0025] A method for preparing a low-gradient resistor for a lightning arrester monitor comprises the following steps: S1. Weigh 90 parts of zinc oxide, 3 parts of antimony trioxide, and special low-temperature glass (with a bulk density of 0.57 g / cm 3 , Model D270, melting point 700℃, linear expansion coefficient 90×10 -7 , the manufacturer is Anmi Micro-Nano New Materials Co., Ltd.) 3.6 parts, citric acid 6 parts, nickel hydroxide 8 parts, mixed and dried to granulate, and molded to obtain the resistor green body; S2. After the resistor green body is dried, it is placed in a calcination and debinding chamber, and the temperature is raised to 400°C at a heating rate of 5°C / min. The calcination and debinding are started and the temperature is kept for 3 hours. The resistor green body is cooled to room temperature to obtain a resistor green body; S3. Use an automatic aluminum spraying machine to spray the end face of the pre-sintered resistor sheet with full electrodes, coat the side with bismuth-based low-temperature lead-free glass glaze, and sinter at 1300℃ for 10 minutes to obtain a low-gradient resistor sheet. The gradient of the resistor sheet is 25V / mm, the thickness is 8mm, and the diameter is 60mm.
[0026] Example 4 Compared with Example 1, Example 4 is different in that the special low-temperature glass (with a bulk density of 0.57 g / cm 3 , Model D270, melting point 700℃, linear expansion coefficient 90×10 -7 , manufacturer is Anmi Micro-Nano New Materials Co., Ltd.) 1.2 parts are replaced with an equal amount of special low-temperature glass (bucket density is 0.61g / cm 3 , model D255, melting point 550℃, linear expansion coefficient 85×10 -7 , the manufacturer is Anmi Micro-Nano New Materials Co., Ltd.).
[0027] Example 5 Compared with Example 1, Example 5 is different in that the special low-temperature glass (with a bulk density of 0.57 g / cm 3 , Model D270, melting point 700℃, linear expansion coefficient 90×10 -7 , manufacturer is Anmi Micro-Nano New Materials Co., Ltd.) 1.2 parts are replaced with an equal amount of special low-temperature glass (bucket density is 0.75g / cm 3 , Model D245, melting point 450℃, linear expansion coefficient 90×10 -7 , the manufacturer is Anmi Micro-Nano New Materials Co., Ltd.).
[0028] Example 6 Compared with Example 1, Example 6 is different in that the special low-temperature glass (with a bulk density of 0.57 g / cm 3, Model D270, melting point 700℃, linear expansion coefficient 90×10 -7 , manufacturer is Anmi Micro-Nano New Materials Co., Ltd.) 1.2 parts are replaced with an equal amount of special low-temperature glass (bucket density is 0.81g / cm 3 , Model D250, melting point 500℃, linear expansion coefficient 80×10 -7 , the manufacturer is Anmi Micro-Nano New Materials Co., Ltd.).
[0029] Example 7 Compared with Example 1, Example 7 is different in that the special low-temperature glass (with a bulk density of 0.57 g / cm 3 , Model D270, melting point 700℃, linear expansion coefficient 90×10 -7 , manufacturer is Anmi Micro-Nano New Materials Co., Ltd.) 1.2 parts are replaced with an equal amount of special low-temperature glass (bulk density is 1.23g / cm 3 , Model D240, melting point 400℃, linear expansion coefficient 85×10 -7 , the manufacturer is Anmi Micro-Nano New Materials Co., Ltd.).
[0030] Example 8 Compared with Example 5, the difference of Example 8 is that 1.2 parts of special low-temperature glass are replaced by 0.6 parts of titanium dioxide and 0.6 parts of boric acid.
[0031] Example 9 Compared with Example 5, the difference of Example 9 is that 1.2 parts of special low-temperature glass are replaced by 0.4 parts of special low-temperature glass, 0.4 parts of boric acid, and 0.4 parts of titanium dioxide.
[0032] Example 10 Compared with Example 5, the difference of Example 10 is that 1.2 parts of special low-temperature glass are replaced by 0.6 parts of special low-temperature glass, 0.3 parts of boric acid, and 0.3 parts of titanium dioxide.
[0033] Embodiment 11 Compared with Example 5, Example 11 is different in that 1.2 parts of special low-temperature glass are replaced by 0.72 parts of special low-temperature glass, 0.24 parts of boric acid, and 0.24 parts of titanium dioxide.
[0034] Example 12 Compared with Example 5, the difference of Example 12 is that 1.2 parts of special low-temperature glass are replaced by 0.8 parts of special low-temperature glass, 0.2 parts of boric acid, and 0.2 parts of titanium dioxide.
[0035] Embodiment 13 Compared with Example 5, the difference of Example 13 is that 1.2 parts of special low-temperature glass are replaced by 0.9 parts of special low-temperature glass, 0.15 parts of boric acid, and 0.15 parts of titanium dioxide.
[0036] Comparative Example 1 Compared with Example 1, Comparative Example 1 is different in that no special low-temperature glass is added.
[0037] The low-gradient resistor sheet for a lightning arrester monitor prepared in Examples 1 to 13 and Comparative Example 1 was tested according to the following method: 1. Residual voltage: According to the test method specified in JB / T 10492-2011 "Detection device for metal oxide arresters", the residual voltage of the test sample is tested. The test conditions are: two pieces in parallel, 20kA.
[0038] 2. Charge transfer performance improvement rate: According to the test method for rated repetitive transfer charge specified in GB / T 11032-2020 "AC Gapless Metal Oxide Arrester", the charge transfer performance improvement rate of the test sample is tested. The test time is 2ms. The charge transfer performance improvement rate = [(charge transferred after improvement - charge transferred before improvement) / charge transferred before improvement] × 100%.
[0039] The test results are shown in the following table: Table 1 Performance test results of low gradient resistors for arrester monitors prepared in Examples 1 to 13 and Comparative Example 1
[0040] Compared with Comparative Example 1, Example 1 adds special low-temperature glass, and Example 8 adds boric acid and titanium dioxide. As a result, the residual voltages of Examples 1 and 8 are lower than those of Comparative Example 1, and the charge transfer performance improvement rate is higher than that of Comparative Example 1, indicating that the addition of special low-temperature glass or boric acid and titanium dioxide can reduce the residual voltage of the resistor and improve the charge transfer performance of the resistor.
[0041] Compared with Example 1, Examples 4 to 7 add special low-temperature glasses with different stacking densities. As a result, the residual pressure of Examples 4 to 6 is lower than that of Examples 1 and 7, and the charge transfer performance improvement rate is higher than that of Examples 1 and 7, indicating that when the stacking density of the special low-temperature glass is 0.61-0.81 g / cm 3 When, and preferably the bulk density is 0.75g / cm 3 When the residual voltage of the resistor is small, the charge transfer performance is better.
[0042] Compared with Examples 5 and 8, Examples 9 to 13 simultaneously added special low-temperature glass, boric acid, and titanium dioxide. As a result, the residual voltage of Examples 9 to 13 was lower than that of Examples 5 and 8, and the charge transfer performance improvement rate was higher than that of Examples 5 and 8, indicating that the special low-temperature glass, boric acid, and titanium dioxide played a synergistic role, which could reduce the residual voltage of the resistor and improve the charge transfer performance of the resistor. Among Examples 9 to 13, the residual voltage of Examples 10 to 12 was lower than that of Examples 9 and 13, and the charge transfer performance improvement rate was higher than that of Examples 9 and 13, indicating that when the mass ratio of special low-temperature glass, boric acid, and titanium dioxide was 2 to 4:1:1, and the preferred ratio was 3:1:1, the residual voltage of the resistor obtained was the smallest and the charge transfer performance was the best.
[0043] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A low gradient resistor for a lightning arrester monitor, It is characterized in that The composition comprises the following raw materials in parts by weight: 85-90 parts of zinc oxide and 1.2-3.6 parts of sintering accelerator; the sintering accelerator includes one or more of special low-temperature glass, boric acid, and titanium dioxide.
2. A low gradient resistor for a lightning arrester monitor according to claim 1, It is characterized in that The bulk density of the special low-temperature glass is 0.61-0.81 g / cm 3 .
3. The low-gradient resistor for a lightning arrester monitor according to claim 1, It is characterized in that When the sintering accelerator is composed of special low-temperature glass, boric acid and titanium dioxide, the mass ratio of the special low-temperature glass to boric acid and titanium dioxide is 2-4:1:
1.
4. The low-gradient resistor for a lightning arrester monitor according to claim 1, It is characterized in that The invention also includes the following raw materials in parts by weight: 1 to 3 parts of additives, wherein the additives include one or more of cobalt trioxide, manganese carbonate, antimony trioxide, and chromium trioxide.
5. The low gradient resistor for a lightning arrester monitor according to claim 1, It is characterized in that The invention also includes the following raw materials in parts by weight: 1 to 6 parts of flux, wherein the flux includes one or more of oxalic acid, acetic acid, and citric acid.
6. The low-gradient resistor for a lightning arrester monitor according to claim 1, It is characterized in that The invention also includes the following raw materials in parts by weight: 2 to 8 parts of a uniformity aid, wherein the uniformity aid includes one or more of zinc hydroxide, cobalt hydroxide, and nickel hydroxide.
7. The low-gradient resistor for a lightning arrester monitor according to claim 1, It is characterized in that It also includes the following component raw materials in parts by weight: 7 to 10 parts of bismuth-based low-temperature lead-free glass glaze powder, which is composed of the following raw materials in parts by weight: 4.5 to 5 parts of bismuth oxide, 0.5 to 1 part of silicon dioxide, 0.5 to 0.8 parts of boron trioxide, 0.3 to 0.5 parts of aluminum oxide, 0.6 to 0.8 parts of calcium oxide, 0.5 to 1 part of lithium oxide, and 0.5 to 0.8 parts of potassium oxide.
8. The low-gradient resistor for a lightning arrester monitor according to claim 7, It is characterized in that The method for preparing the bismuth-based low-temperature lead-free glass glaze powder comprises the following steps: mixing the raw materials of the bismuth-based low-temperature lead-free glass glaze powder, melting, cooling, and crushing to obtain the bismuth-based low-temperature lead-free glass glaze powder.
9. A method for preparing a low-gradient resistor for a lightning arrester monitor according to any one of claims 1 to 8, It is characterized in that The following steps are involved: S1, weighing the zinc oxide sintering accelerator in parts by weight, mixing, granulating, and molding to obtain a resistor green body; S2, drying, calcining and debinding the resistor green body to obtain a resistor pre-sintered green body; S3, spraying aluminum on the end surface of the pre-sintered body of the resistor, coating the side with bismuth-based low-temperature lead-free glass glaze, and obtaining a low-gradient resistor after sintering.
10. The method for preparing a low-gradient resistor for a lightning arrester monitor according to claim 9, It is characterized in that The debinding temperature is 300-400°C, the debinding time is 1-3h, and the sintering temperature is 1200-1300°C.
Citation Information
Patent Citations
Zinc oxide piezoresistor material with low electric potential gradient and preparation method thereof
CN101759431A
Manufacturing method of low-voltage and high-energy zinc oxide resistor disc
CN103400676A
Zinc oxide resistor disc and preparation method and application thereof
CN111606703A
Resistor disc material with low gradient and large through-flow impact stability and preparation method thereof
CN113716952A
Nanometer doped composite low-voltage zinc oxide pressure sensitive resistor and its manufacture