Manufacturing method of grain boundary diffusion thick neodymium iron boron magnetic steel
Through the synergistic effect of homogeneous stacking hot pressing composite technology and ion etching sputtering coating, the problem of insufficient diffusion depth of neodymium iron boron magnets is solved, the magnetic performance and heavy rare earth utilization rate are improved, and the cost is reduced. It is suitable for thick Preparation of neodymium iron boron magnetic steel.
Patent Information
- Application Number
- CN202411551017.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-01
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-11-01
AI Technical Summary
In the prior art, when preparing large-thick neodymium iron boron magnets, the grain boundary diffusion depth is insufficient, resulting in waste of heavy rare earth elements and poor magnetic performance, and traditional methods increase costs.
The same-direction stacking hot pressing composite technology is adopted, combining the synergistic effect of ion etching and sputtering plating to enhance the grain boundary diffusion of neodymium iron boron magnets, reduce dependence on alloy powders and binders, and improve magnetic performance.
It significantly improves the coercive force and residual magnetic properties of large-thick neodymium iron boron magnets, improves the utilization rate of heavy rare earths, reduces production costs, and simplifies the production process.
Smart Images

Figure CN119069250A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of preparation of NdFeB magnetic steel, and in particular to a method for manufacturing grain boundary diffusion thick NdFeB magnetic steel. Background Art
[0002] As the third generation of permanent magnets, NdFeB is widely used in electronic information, wind power generation, medical equipment, robots and other fields. After decades of development, the residual magnetization intensity of sintered NdFeB has approached 90% of the theoretical limit, but the coercive force is still far from the theoretical value. In recent years, with the rapid development of new energy vehicles, the market demand for sintered NdFeB magnets, which are key components of electric vehicle motors, is increasing. In addition, the heat generated by the high-speed operation of the motor keeps the magnets at a higher operating temperature, which requires NdFeB magnets to have higher temperature resistance and higher coercive force.
[0003] The grain boundary diffusion technology is used to allow heavy rare earth elements to enter the interior of the magnet and form a heavy rare earth shell with a high anisotropy field on the surface of the NdFeB grains. This is a method that can effectively improve the coercivity of sintered NdFeB magnets. Faced with the soaring price of heavy rare earths, the grain boundary diffusion technology can effectively improve the utilization rate of heavy rare earths compared to the traditional smelting and adding technology, thereby significantly reducing costs. However, for thick NdFeB magnets, the diffusion depth of the grain boundary diffusion technology for NdFeB magnets with a thickness of more than 11mm is far from reaching the design requirement depth.
[0004] In order to increase the interface diffusion depth of NdFeB magnets, for example, the invention patent with patent application number 202410592008.5 specifically discloses a grain boundary diffusion method for thick NdFeB magnets. The first alloy powder and the second alloy powder are used for partition printing on the orientation plane of the NdFeB magnet to obtain the printed magnet, thereby solving the common problems of grain boundary diffusion technology such as insufficient diffusion depth and surface enrichment of heavy rare earths, which lead to waste of heavy rare earths. However, the use of the first alloy powder and the second alloy powder still greatly increases the manufacturing cost.
[0005] In addition, the invention patent with patent application number 201810921550.5 also specifically discloses a method for preparing low-cost large-block NdFeB magnets by grain boundary diffusion, which specifically involves selecting dysprosium, terbium, iron, aluminum, copper, and gallium alloy powders as diffusion sources, coating them on oriented or non-oriented surfaces of 2 to 8 mm, and then selecting an appropriate number of magnets to be stacked and placed in a sintering furnace for diffusion bonding treatment based on the final size of the finished product to obtain large-block high-performance sintered magnets. However, when alloy powders are directly used as diffusion sources for coating, the diffusion depth cannot reach the preset depth when the alloy powders diffuse at the grain boundaries, and there is still a problem of enrichment of diffusion elements, resulting in waste of alloy powders.
[0006] On the other hand, there is also a method of using glue to bond small magnets to produce large magnets, but this method has high requirements on the quality of the glue, and the introduction of expensive glue will inevitably increase production costs.
[0007] Therefore, in order to solve the above problems, it is necessary to develop a method for manufacturing grain boundary diffusion thick NdFeB magnets without using excess binder or alloy powder. Summary of the invention
[0008] In response to the existing technical problems, the present invention aims to provide a method of utilizing the same-direction stacking hot pressing composite technology, in combination with the synergistic effect of ion etching and sputtering coating, to enhance the grain boundary diffusion of NdFeB magnets without adding other reagents and alloy powders, thereby significantly improving the coercive force of thick NdFeB magnets, alleviating the problem of reduced remanence of the magnets caused by the diffusion of heavy rare earth elements, and improving the comprehensive magnetic properties.
[0009] To achieve the above object, the present invention provides the following technical solutions:
[0010] A method for manufacturing grain boundary diffusion thick NdFeB magnetic steel comprises the following steps:
[0011] Step S1, magnet loading, hoisting the magnetic steel sheet to be prepared onto the rotating frame system. During hoisting, the magnetic steel sheet is arranged vertically, and the orientation plane A of the magnetic steel sheet in the magnetic field orientation direction is arranged toward the central axis B of the rotating frame system. After loading is completed, the sealing door of the etching and coating machine is closed;
[0012] Step S2: preheating the etching process, turn on the mechanical pump, Roots pump and molecular pump in the vacuum pump group in turn, so that the vacuum degree of the working chamber of the etching and coating machine reaches 1.0×10 -2 pa~2.0×10 -2 pa, the electric heating system and the ion etching system are respectively turned on to preheat and etch the magnetic steel sheet to remove impurities on the surface of the magnetic steel sheet. During etching, the Ar gas concentration at the columnar target in the working chamber is higher than the Ar gas concentration in the working chamber. Specifically, the gas pressure reflects the Ar gas concentration, and the gas pressure at the columnar target is 5.0×10 -2 pa~8.0×10 -2 pa, and the air pressure in the working chamber is 3.0×10 -2 pa~3.5×10 -2 pa;
[0013] Step S3, sputtering coating, after etching is completed, the ion etching system is turned off, the electric heating system is kept running, Ar gas is input into the working chamber again, the sputtering system is turned on, the columnar target and the pancake target are both Dy metal targets, the columnar target and the pancake target emit Dy plasma, and the Dy plasma is deposited on the surface of the magnetic steel sheet of the turret system for coating;
[0014] Step S4, polishing treatment, taking out the magnetic steel sheet that has completed the coating from the etching and coating machine, polishing and cleaning the magnetic steel sheet to form an edge magnetic steel sheet and an intermediate magnetic steel sheet, wherein the edge magnetic steel sheet is a magnetic steel sheet with polishing treatment on the orientation surface A, and the intermediate magnetic steel sheet is a magnetic steel sheet with polishing treatment on both orientation surfaces, and the polishing treatment is to make the magnetic steel sheets fit better when they are compounded;
[0015] Step S5, stacking, stacking the edge magnetic steel sheets and the middle magnetic steel sheets in the magnetic field orientation direction in a stacking manner of edge magnetic steel sheet-middle magnetic steel sheet-edge magnetic steel sheet to form a magnetic sheet stack. During stacking, the polished surface of the edge magnetic steel sheet is fitted with the polished surface of another edge magnetic steel sheet or the middle magnetic steel sheet, and the number N of the middle magnetic steel sheets is an integer ≥ 0. The stacking thickness of the edge magnetic steel sheets and the middle magnetic steel sheets depends on the designed thickness requirement. After the stacking thickness reaches the designed requirement, the number N of the middle magnetic steel sheets can be 0.
[0016] Step S6, composite treatment, applying a pressure of 0.5-12MPa in the magnetic field orientation direction of the magnetic sheet stack, and performing heat treatment at a temperature of 800-1050°C in a vacuum or inert atmosphere for 10-40h, and after heat treatment, performing tempering treatment at a temperature of 440-640°C for 5-15h to obtain a grain boundary diffusion thick NdFeB magnet. The remanence of the grain boundary diffusion thick NdFeB magnet with a thickness of ≥11mm reaches more than 14.12kG, and the coercive force reaches more than 23.75kOe. The sintering composite process is also a process of grain boundary diffusion. Increasing the pressure can, on the one hand, avoid the diffusion depth being limited due to too low pressure, and only a small amount of heavy rare earth elements diffuse into the deeper area of the magnet, and the coercive force is not increased much. On the other hand, it can further promote the mutual bonding between the magnetic steel sheets. At the same time, it is also necessary to avoid excessive pressure causing the heavy rare earth elements to diffuse into the interior of the grains and significantly reduce the remanence.
[0017] As an improvement, the preheat etching comprises the following steps:
[0018] Step T1, preheating, turning on the electric heating system to raise the temperature in the working chamber to 200-250°C;
[0019] Step T2, closing the cylindrical target, starting the sleeve module surrounding the outer side of the cylindrical target, and sealing and isolating the cylindrical target from the working chamber;
[0020] Step T3: Filling Ar gas into the sleeve module and the working chamber respectively, so that the pressure in the sleeve module is 5.0×10 -2 pa~8.0×10 -2 pa, synchronously, the air pressure in the working chamber is 3.0×10 -2 pa~3.5×10 -2 pa;
[0021] Step T4, etching arc initiation, the first arc initiation needle 51 beside the cylindrical target 5 rotates and swings, and instantly touches the cylindrical target, so that the arc initiation power supply on the cylindrical target is short-circuited, and the Ar gas in the sleeve module is discharged to start the arc and emit a glow, forming Ar positive ions and electrons;
[0022] Step T5, the anode ring is opened. Synchronously with step T4, the partition door assembly on the sleeve module is opened, so that a gap is formed on the side of the sleeve module facing away from the turret system, and an anode ring is simultaneously formed at the gap. The anode ring performs a bunching acceleration process on Ar positive ions and electrons, and pulls the Ar positive ions and electrons out of the sleeve module from the gap.
[0023] Step T6, anode pulling, synchronous with step T4, the anode power supply supplies power to the pancake target, the pancake target pulls and accelerates the electrons released in step T4, and collides with the Ar gas in the working chamber to form Ar positive ions, and the working current and voltage of the anode power supply are 30A / 60V;
[0024] Step T7, etching, the bias power supply supplies power to the turntable system, the turntable system pulls Ar positive ions, and the Ar positive ions collide with the surface of the magnetic steel sheet on the turntable system. The working current and voltage of the bias power supply are as follows: the working voltage is 50V~250V, the current is 0.2A~10A, and the working time is 25min~45min.
[0025] Preferably, in step T2, the air pressure in the sleeve module is 6.0×10 -2 pa, the air pressure in the working chamber is 3.2×10 -2 pa.
[0026] Preferably, in step T3, the initial voltage of the arc starting power supply is 150-250V, and the working current and voltage after arc stabilization are 100A / 20V.
[0027] Preferably, in step T6, the current of the anode power supply is gradually increased from 30A to 100A.
[0028] Preferably, in step T7, the voltage of the bias power supply is gradually increased from 50V to 250V.
[0029] As an improvement, the sputtering coating comprises the following steps:
[0030] Step U1, heating and heat preservation, maintaining the operation of the electric heating system, raising the temperature in the working chamber to 550-650° C., and heat preservation;
[0031] Step U2: Filling Ar gas into the working chamber to maintain the vacuum degree in the working chamber at 2.5×10 -1 Pa~4.5×10 -1 Pa;
[0032] Step U3, gap switching, adjusting the partition door assembly on the sleeve module so that the sleeve module forms a gap on the side facing the rotating rack system;
[0033] Step U4, glow sputtering, the first arc starting needle at the cylindrical target rotates and swings to instantly touch the cylindrical target, and the second arc starting needle at the pancake target touches the pancake target, respectively short-circuiting the arc starting power supply and the anode power supply, and emitting glow to the Ar gas discharge arc in the working chamber, and the cylindrical target and the pancake target sputter and overflow Dy plasma;
[0034] Step U5, coating, the bias power supply supplies power to the turret system, the working voltage is 100V, the turret system draws the Dy plasma to adhere to the surface of the magnetic steel sheet on the turret system to form a coating with a thickness of 2.5 to 3 μm, and the working time is 45 to 50 minutes.
[0035] Preferably, in step U2, the vacuum degree in the working chamber is maintained at 3.5×10 -1 Pa.
[0036] Preferably, in step U4, the operating current and voltage of the arc starting power supply and the anode power supply are 180A / 25V.
[0037] Preferably, in step S6, a pressure of 6 MPa is applied to the magnetic field orientation direction of the magnetic sheet stack, and heat treatment is carried out at 950°C in a vacuum or inert atmosphere for 35 hours. After the heat treatment, the magnetic sheet stack is tempered at 550°C for 10 hours to obtain grain boundary diffusion thick NdFeB magnets. The remanence of the grain boundary diffusion thick NdFeB magnets with a thickness ≥11 mm reaches more than 14.12 kG, and the coercive force reaches more than 23.75 kOe.
[0038] The beneficial effects of the present invention are:
[0039] (1) The present invention utilizes the same-direction stacking hot pressing composite technology, in combination with the synergistic effect of ion etching and sputtering coating, to enhance the grain boundary diffusion of NdFeB magnets without adding other reagents and alloy powders, thereby significantly improving the coercive force of thick NdFeB magnets;
[0040] (2) The ion etching of the present invention utilizes reactive gas to react with the material in a plasma or reactive ion etching environment. This etching process etches the surface and near-surface of the material, removes part of the material, and exposes more grain boundaries. After the grain boundaries are exposed, more channels and contact areas are provided for subsequent diffusion, which is beneficial for the diffusion of the material along the grain boundaries. In addition, the bombardment of ions will produce defects in the material, such as vacancies and dislocations. These defects will affect the crystal structure and atomic arrangement of the material, change the atomic structure at the grain boundaries, and increase the activity of the grain boundaries. At the same time, ion etching will also generate stress in the material. The presence of stress will promote the migration and diffusion of atoms, which is beneficial for opening the diffusion channel of the grain boundaries.
[0041] (3) The present invention combines ion etching with sputtering coating, so that the etching and sputtering coating of the magnetic steel sheet are carried out in the same working chamber. The magnetic steel sheet does not need to switch the working chamber, thereby maintaining the working temperature of the magnetic steel sheet. There is no need to cool down and transfer the etched magnetic steel sheet, thereby ensuring the cleanliness of the surface of the magnetic steel sheet after etching. In addition, during the etching process, in order to expose more grain boundaries, the Ar gas concentration in the working chamber is adjusted to form partitions, so that the Ar gas concentration at the columnar target is much higher than the Ar gas concentration in the working chamber. Therefore, during etching, the number of Ar positive ions generated by the excitation is guaranteed, and the blocking of Ar atoms to the magnetic steel sheet is reduced, so that the Ar positive ions can better impact the surface of the magnetic steel sheet and expose the grain boundaries.
[0042] (4) During the sputtering coating process of the present invention, the bombardment of high-energy particles will cause changes in the structure of the substrate surface, such as generating roughness and forming nanoscale pores. These changes in the surface structure will increase the contact area between the grain boundary and the outside world, providing more entry channels for diffusing substances. In addition, the deposition coating is performed by plasma deposition of the heavy rare earth element Dy, which can form a high coercive force shell at the grain boundary, thereby improving the magnetic properties of the material.
[0043] (5) When the present invention utilizes the same-direction stacking hot-pressing composite technology to pressurize and composite the edge magnetic steel sheets and the middle magnetic steel sheets of the stack, no adhesive is required, thus saving production costs. In addition, the pressurization treatment is performed during the grain boundary diffusion process, which is beneficial to improving the diffusion depth and post-diffusion performance, thereby increasing the utilization rate of heavy rare earths. The grain boundary diffusion process and the magnet assembly splicing process are performed simultaneously, which can effectively simplify the production process.
[0044] In summary, the coercive force of the grain boundary diffusion thick NdFeB magnet prepared by the present invention is significantly improved, the problem of reduced remanence of the magnet caused by the diffusion of heavy rare earth elements is overcome, and the comprehensive magnetic properties are significantly improved. It is particularly suitable for the field of paint technology for the preparation of grain boundary diffusion thick NdFeB magnets. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 It is a schematic diagram of the manufacturing method of the present invention;
[0046] Figure 2 This is a schematic diagram of the edge magnetic steel sheet of the present invention;
[0047] Figure 3 This is a schematic diagram of the middle magnetic steel sheet of the present invention;
[0048] Figure 4 A schematic diagram of a magnetic sheet stack according to the present invention;
[0049] Figure 5 A top view of the rotating rack system of the present invention;
[0050] Figure 6 It is a schematic diagram of the three-dimensional structure of the etching and coating integrated machine of the present invention;
[0051] Figure 7 This is a schematic diagram of the top view of the structure of the etching and coating integrated machine of the present invention;
[0052] Figure 8 This is a schematic diagram of the power connection of the etching and coating integrated machine of the present invention;
[0053] Fig. 9 This is a schematic diagram of the power supply connection of the cylindrical target of the present invention;
[0054] Fig.10 This is a schematic diagram of the cross-sectional structure of the etching and coating integrated machine of the present invention;
[0055] Fig.11 It is a schematic diagram of the three-dimensional structure of the columnar target material of the present invention;
[0056] Fig.12 It is a schematic diagram of the front view structure of the cylindrical target material of the present invention;
[0057] Fig.13 It is a schematic diagram of the top view structure of the column target material of the present invention;
[0058] Fig.14 It is a schematic diagram of the anode ring structure of the present invention.
[0059] The reference numerals in the figure are: 10, magnetic steel sheet, 101, edge magnetic steel sheet, 102, middle magnetic steel sheet, 103, magnetic sheet stack, 1, rotating frame system, 11, bias power supply, 2, etching and coating integrated machine, 20, working chamber, 21, sealing door, 3, vacuum pump group, 4, electric heating system, 5, cylindrical target, 51, first arc starting needle, 52, arc starting power supply, 6, pancake target, 61, anode power supply, 62, second arc starting needle, 7, sleeve module, 70, sleeve, 701, opening, 71, partition door assembly, 711, partition door, 712, gear, 72, notch, 73, drive unit, 731, drive motor, 732, drive gear, 8, anode ring, 81, anode strip, 82, anode connecting strip. DETAILED DESCRIPTION
[0060] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0061] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention.
[0062] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0063] Example:
[0064] like Figure 1 As shown, a method for manufacturing a grain boundary diffused thick NdFeB magnetic steel comprises the following steps:
[0065] Step S1, magnet loading, hoisting the magnetic steel sheet 10 to be prepared onto the rotating frame system 1, during hoisting, the magnetic steel sheet 10 is vertically arranged, and the orientation plane A of the magnetic steel sheet 10 in the magnetic field orientation direction is arranged toward the central axis B of the rotating frame system 1, after loading is completed, closing the sealing door 21 of the etching and coating machine 2;
[0066] Step S2: preheating the etching process, turn on the mechanical pump, Roots pump and molecular pump in the vacuum pump group 3 in sequence, and make the vacuum degree of the working chamber 20 of the etching and coating machine 2 reach 1.0×10 -2 pa~2.0×10 -2 pa, the electric heating system 4 and the ion etching system are respectively turned on to preheat and etch the magnetic steel sheet 10 to remove impurities on the surface of the magnetic steel sheet 10. During etching, the Ar gas concentration at the columnar target 5 in the working chamber 20 is higher than the Ar gas concentration at the rest of the working chamber 20. Specifically, the gas pressure reflects the Ar gas concentration, and the gas pressure at the columnar target 5 is 5.0×10 -2 pa~8.0×10 -2 pa, while the pressure in the rest of the working chamber 20 is 3.0×10 -2 pa~3.5×10 -2 pa;
[0067] Step S3, sputtering coating. After etching is completed, the ion etching system is turned off, the electric heating system 4 is kept running, Ar gas is input into the working chamber 20 again, and the sputtering system is turned on. The columnar target 5 and the pancake target 6 are both Dy metal targets. The columnar target 5 and the pancake target 6 are excited to emit Dy plasma, and the Dy plasma is deposited on the surface of the magnetic steel sheet 10 of the turret system 1 for coating;
[0068] Step S4, polishing treatment, taking out the magnetic steel sheet 10 that has completed the coating from the etching and coating machine 2, polishing and cleaning the magnetic steel sheet 10 to form an edge magnetic steel sheet 101 and an intermediate magnetic steel sheet 102, wherein the edge magnetic steel sheet 101 is a magnetic steel sheet with an orientation surface A polished, and the intermediate magnetic steel sheet 102 is a magnetic steel sheet with an orientation surface polished. The polishing treatment is to make the magnetic steel sheets fit better when they are compounded. Although the polished surfaces of the edge magnetic steel sheet 101 and the intermediate magnetic steel sheet 102 are polished, there is still a Dy metal coating on the polished surface, and the inside of the polished surface has also been deposited and infiltrated with Dy metal elements during the coating process;
[0069] Step S5, stacking, stacking the edge magnetic steel sheets 101 and the middle magnetic steel sheets 102 in the magnetic field orientation direction in a stacking manner of edge magnetic steel sheets-middle magnetic steel sheets-edge magnetic steel sheets to form a magnetic sheet stack 103. During stacking, the polished surface of the edge magnetic steel sheet 101 is fitted with the polished surface of another edge magnetic steel sheet 101 or the middle magnetic steel sheet 102, and the number N of the middle magnetic steel sheets 102 is an integer ≥ 0. The stacking thickness of the edge magnetic steel sheets 101 and the middle magnetic steel sheets 102 depends on the designed thickness requirement. After the stacking thickness reaches the designed requirement, the number N of the middle magnetic steel sheets can be 0.
[0070] Step S6, composite treatment, after stacking, the magnetic sheet stack 103 is placed in a sintering furnace, a pressure of 0.5 to 12 MPa is applied in the magnetic field orientation direction of the magnetic sheet stack, and a heat treatment is performed at a temperature of 800 to 1050°C in a vacuum or inert atmosphere for 10 to 40 hours. After the heat treatment, the magnetic sheet stack is tempered at a temperature of 440 to 640°C for 5 to 15 hours to obtain a grain boundary diffusion thick NdFeB magnet. The grain boundary diffusion thick NdFeB magnet with a thickness of ≥11mm has a remanence of more than 14.12 kG and a coercive force of more than 23.75 kOe. The sintering composite process is also a process of grain boundary diffusion. Increasing the pressure can, on the one hand, avoid the diffusion depth being limited due to too low pressure, and only a small amount of heavy rare earth elements diffuse into the deeper area of the magnet, and the coercive force is not increased much. On the other hand, it can further promote the mutual bonding between the magnetic steel sheets. At the same time, it is also necessary to avoid excessive pressure causing the heavy rare earth elements to diffuse into the interior of the grains, which significantly reduces the remanence.
[0071] Preferably, in step S6, a pressure of 6 MPa is applied to the magnetic field orientation direction of the magnetic sheet stack, and heat treatment is performed at 950°C in a vacuum or inert atmosphere for 35 hours. After the heat treatment, the magnetic sheet stack is tempered at 550°C for 10 hours.
[0072] First of all, it should be noted that the columnar target 5 and the pancake target 6 in the present application are both Dy metal targets or Dy alloy targets, and in the ion etching system, the columnar target 5 is used as a cathode, and the pancake target 6 is used as an anode. The columnar target 5, the pancake target 6 and the turntable system 1 are combined to form an ion etching system.
[0073] Furthermore, the pressure applied in the magnetic field orientation direction of the magnetic sheet stack cannot be too large, because the sintered NdFeB magnet is a material with high hardness and brittleness, and it is very easy to be damaged due to uneven force during processing. Therefore, it is necessary to ensure that the magnetic sheet stack is not crushed while ensuring that the pressure on the magnetic sheet stack is uniform, and to avoid excessive pressure that causes the Dy element to diffuse into the interior of the grains and reduce the residual magnetism.
[0074] In addition, the temperature of the diffusion heat treatment is controlled to be carried out under low temperature conditions, that is, the temperature is 950°C. On the one hand, it can avoid the temperature being too high, which will lead to more Dy elements diffusing in the lattice and enriching the Dy elements on the surface of the magnet, affecting the grain boundary diffusion depth of Dy, reducing the saturation magnetization intensity of the magnet and the content of Dy elements diffused into the interior of the magnet, avoiding the final decrease in the remanence of the magnet and the low increase in coercive force. On the other hand, it can avoid the temperature being too low, which will lead to a slow diffusion rate and avoid only a small amount of Dy elements diffusing into the magnet.
[0075] It should be emphasized that the heavy rare earth elements used for grain boundary diffusion in the present application are not limited to Dy elements. All heavy rare earth elements that meet the requirements of the present application are within the protection scope of the present application, such as the heavy rare earth element terbium (Tb).
[0076] In the present invention, the thickness of the grain boundary diffusion thick NdFeB magnet is ≥11mm, for example, it can be 11mm, 12mm, 13mm, 14mm, 15mm, 16mm, 17mm, 18mm, 19 or 20mm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0077] like Figures 1 to 14 As shown, the preheat etching comprises the following steps:
[0078] Step T1, preheating, turning on the electric heating system 4 so that the temperature in the working chamber 20 rises to 200-250° C.;
[0079] Step T2, closing the cylindrical target, starting the sleeve module 7 surrounding the outer side of the cylindrical target material 5, and sealing and isolating the cylindrical target material 5 from the working chamber 20;
[0080] Step T3: Filling Ar gas into the sleeve module 7 and the working chamber 20 respectively, so that the gas pressure in the sleeve module 7 is 5.0×10 -2 pa~8.0×10 -2 pa, synchronously, the air pressure in the working chamber 20 is 3.0×10 -2 pa~3.5×10 -2 pa;
[0081] Step T4, etching arc starting, the first arc starting needle 51 beside the cylindrical target 5 rotates and swings, and instantly touches the cylindrical target 5, so that the arc starting power supply 52 on the cylindrical target 5 is short-circuited, and the Ar gas in the sleeve module 7 is discharged to start the arc and emit a glow, forming Ar positive ions and electrons;
[0082] Step T5, the anode ring is opened. Synchronously with step T4, the partition door assembly 71 on the sleeve module 7 is opened, so that a gap 72 is formed on the side of the sleeve module 7 facing away from the turret system 1, and an anode ring 8 is simultaneously formed at the gap 72. The anode ring 8 performs a bunching acceleration process on the Ar positive ions and electrons, and pulls the Ar positive ions and electrons out of the sleeve module 7 from the gap 72;
[0083] Step T6, anode pulling, synchronous with step T4, the anode power supply 61 supplies power to the pancake target 6, the pancake target 6 pulls and accelerates the electrons released in step T4, and collides with the Ar gas in the working chamber 20 to form Ar positive ions, and the working current and voltage of the anode power supply 61 are 30A / 60V;
[0084] Step T7, etching, the bias power supply 11 supplies power to the turntable system 1, the turntable system 1 pulls Ar positive ions, and the Ar positive ions collide with the surface of the magnetic steel sheet 10 on the turntable system 1. The working current and voltage of the bias power supply 11 are as follows: the working voltage is 50V~250V, the current is 0.2A~10A, and the working time is 25min~45min.
[0085] Furthermore, in step T2, the air pressure in the sleeve module 7 is 6.0×10 -2 pa, the air pressure in the working chamber is 3.2×10 -2 pa.
[0086] Furthermore, in step T3, the initial voltage of the arc starting power supply 52 is 150-250V, and the working current and voltage after arc stabilization are 100A / 20V.
[0087] Furthermore, in step T6, the current of the anode power supply 61 is gradually increased from 30A to 100A.
[0088] In addition, in step T7, the voltage of the bias power supply 11 is gradually increased from 50V to 250V.
[0089] It should be noted that the Ar gas concentration in the sleeve module 7 is high, while the Ar gas concentration in the working chamber 20 is low. This is because the Ar gas concentration in the working chamber 20 is too high. When Ar atoms are not hit by electrons to form Ar positive ions, they will hinder the migration of the already formed Ar positive ions, especially the Ar atoms at the turntable system 1, which directly affects the etching and cleaning effect of the magnetic steel sheet. Conventional ion etching systems have this problem, and the magnetic steel sheet cannot be fully hit by Ar positive ions, exposing the grain boundaries, which affects the subsequent Dy plasma precipitation penetration.
[0090] It is further explained that in the invention patent with patent application number 201810885211.6, an ion source multi-arc column arc composite PVD coating system and method are disclosed, which is similar to the present invention. Ar gas is ionized by arcing of a columnar target to form Ar positive ions, and then pulled by the anode of the pancake target to make the Ar positive ions and electrons transition. Finally, relying on the bias power supply, the Ar positive ions impact the workpiece to form etching. However, since the present application requires sufficient impact on the magnetic steel sheet to expose the grain boundary, and the above-mentioned ion source multi-arc column arc composite PVD coating system is provided with a protective cover at the columnar target after arcing, it is difficult for the Ar positive ions and electrons to leave the area of the protective cover when they are pulled by the anode, resulting in difficulty in the transition of the Ar positive ions and electrons. At the same time, the Ar gas concentration in the entire vacuum chamber is consistent, and it is difficult to form a high concentration of Ar positive ions when the columnar target is etched and arced, and the remaining Ar atoms in the vacuum chamber will still hinder the Ar positive ions.
[0091] The present application fully considers the barrier effect of the protective cover on Ar positive ions and electrons, while retaining the function of the protective cover to avoid contamination of the columnar target by impurities generated during the etching process.
[0092] Specifically, the present application first uses the sleeve module 7 to seal and isolate the cylindrical target 5 after the etching and coating integrated machine completes vacuuming and heating. Then, when the external gas supply device is filled with Ar gas, two Ar gas environments with different concentrations are formed inside and outside the sleeve module 7. Then, when the cylindrical target starts arcing and discharging, the sleeve module 7 forms a gap 72 to connect to the working chamber 20, and at the same time, an anode ring 8 is formed at the gap 72. The anode ring 8 pulls the Ar positive ions and electrons in the sleeve module 7 before the pancake target. At the same time, since there are a large number of Ar positive ions and electrons in the sleeve module 7, the anode ring 8 bunches them. The Ar positive ions and electrons are led out of the sleeve module 7, and then pulled by the anode of the pancake target 6 to make a transition. Since the Ar positive ions and electrons have separated from the sleeve module 7, the path of being pulled by the anode will no longer be blocked. In addition, a large number of Ar positive ions and electrons are formed at the moment of arc discharge of the cylindrical target. The concentration of the remaining Ar atoms in the working chamber 20 has no effect of blocking the Ar positive ions while playing the role of inert gas protection. The Ar positive ions can quickly and fully transition to the rotating rack system 1, impact-etch and clean the magnetic steel sheet, and completely expose the grain boundary.
[0093] In addition, due to the blocking and restriction of the sleeve module 7, the arc discharge in a small space has a better ionization effect on the Ar gas. At the same time, it can also prevent the current of the cylindrical target from igniting the magnetic steel sheet at the moment of arc discharge, thereby avoiding burning of the magnetic steel sheet.
[0094] Specifically, the sputtering coating comprises the following steps:
[0095] Step U1, heating and heat preservation, maintaining the operation of the electric heating system, raising the temperature in the working chamber to 550-650° C., and heat preservation;
[0096] Step U2: Filling Ar gas into the working chamber to maintain the vacuum degree in the working chamber at 2.5×10 -1 Pa~4.5×10 -1 Pa;
[0097] Step U3, gap switching, adjusting the partition door assembly on the sleeve module so that the sleeve module forms a gap on the side facing the rotating rack system;
[0098] Step U4, glow sputtering, the first arc starting needle 51 at the cylindrical target 5 rotates and swings to instantly touch the cylindrical target, and the second arc starting needle 62 at the pancake target 6 touches the pancake target, respectively short-circuiting the arc starting power supply and the anode power supply, and emitting glow to the Ar gas discharge arc in the working chamber, and the cylindrical target and the pancake target sputter and overflow Dy plasma;
[0099] Step U5, coating, the bias power supply 11 supplies power to the turret system 1, the working voltage is 100V, the turret system draws the Dy plasma to adhere to the surface of the magnetic steel sheet on the turret system to form a coating with a thickness of 2.5 to 3 μm, and the working time is 45 to 50 minutes.
[0100] Preferably, in step U2, the vacuum degree in the working chamber is maintained at 3.5×10 -1 Pa.
[0101] Preferably, in step U4, the operating current and voltage of the arc starting power supply and the anode power supply are 180A / 25V.
[0102] It should be noted that when sputtering coating is performed, the cylindrical target 5 and the pancake target 6 discharge and strike an arc at the same time, and a plurality of arc spots are formed on the surface of the cylindrical target 5 and the pancake target 6 by using the electric arc, so that the Dy element of the cylindrical target 5 and the pancake target 6 escapes directly in the form of plasma, forming an evaporation ion source, and the magnetic steel sheet on the turntable system 1 is sputtered and coated by using the evaporation ion source.
[0103] It is further explained that when the magnetic steel sheet is sputter-coated using the cylindrical target material 5 as an evaporation ion source, a notch is formed on the side of the sleeve module 7 facing the turntable system 1, and the Dy plasma can directly jump to the turntable system 1 through the notch without any interference, and the Dy plasma can quickly penetrate into the interior of the magnetic steel sheet.
[0104] Specifically, the sleeve module 7 includes a sleeve 70, a partition door assembly 71 and a driving unit 73;
[0105] The sleeve 70 is coaxially sleeved on the outer side of the cylindrical target 5, and the sleeve 70 is provided with openings 701 on the side opposite to the turret system 1 and the side opposite to the turret system 1;
[0106] The partition door assembly 71 is symmetrically arranged, and the partition door assembly 71 is provided with two groups. The two groups of the partition door assembly 71 are respectively arranged at the corresponding openings 701. The two groups of partition doors 711 in the partition door assembly 71 are arranged to rotate around the inner ring of the sleeve 71, and the lower ends of the partition doors 711 in the same group are arranged to be meshed through gears 712;
[0107] The driving unit 73 includes a driving motor 731 and a driving gear 732 . The driving motor 731 is configured to cooperate with the gear 712 via the driving gear 732 . The driving gear 732 is a toothless gear. The driving unit 73 switches forward and reverse to drive the partition door assembly 71 to open the corresponding gap 72 .
[0108] Furthermore, anode bars 81 are arranged in parallel at the upper and lower edges of the opening 701 on one side of the sleeve 70 facing away from the turret system 1, and anode connecting bars 82 are respectively arranged at the edges of the two groups of partition doors 711 facing the resin, and the upper and lower ends of the anode connecting bar 82 are respectively slidably arranged on the anode bar 81, and the anode connecting bar 82 and the anode bar 81 are conductively arranged in contact with each other. When the partition door 711 is opened, the anode bar 81 and the anode connecting bar 82 are combined to form an anode ring 8, and the middle part of the anode bar 81 is connected to the arc starting power supply 52, and the current of the arc starting power supply 52 flows through the anode ring 8, forming a voltage / current at the anode ring 8 that is higher than that at the cylindrical target 5.
[0109] It should also be noted that when the cylindrical target 5 is used as an ion etching cathode to discharge and start an arc, the partition door 711 is gradually opened to form a gap 72, and the synchronous anode connecting bar 82 moves on the anode bar 81 to form an anode ring 8. Since the opening of the anode ring 8 is gradually formed from small to large, during the process of the anode ring 8 pulling the Ar positive ions and electrons, the pulling and bunching effect also changes from strong to weak, which is just inversely proportional to the density of Ar positive ions and electrons in the sleeve module 7. The pulling effect of the anode ring 8 on the Ar positive ions and electrons is just the same as the anode pulling at the pancake-shaped target 6 (the current of the anode power supply 61 is gradually increased from 30A to 100A, and the anode pulling effect becomes stronger and stronger), forming a complementary effect.
[0110] In addition, the structure of the etching and coating integrated machine of the present invention can refer to the structure of an ion source multi-arc column arc composite PVD coating system disclosed in the invention patent 201810885211.6, which will not be elaborated here.
[0111] Embodiment 1-4:
[0112] The method for manufacturing the grain boundary diffusion thick NdFeB magnets of Examples 1-4 is the same as that of Example 1. The specific parameters of the manufacturing method are shown in Table 1 below:
[0113] Table 1
[0114] Parameter name Example 1 Example 2 Example 3 Example 4 Vacuum degree <![CDATA[1.0×10 -2 so]]> <![CDATA[1.5×10 -2 so]]> <![CDATA[1.5×10 -2 so]]> <![CDATA[2.0×10 -2 so]]> Preheating temperature 200℃ 225℃ 225℃ 250℃ Air pressure in sleeve module <![CDATA[5.0×10 -2 so]]> <![CDATA[5.5×10 -2 so]]> <![CDATA[6.0×10 -2 so]]> <![CDATA[8.0×10 -2 so]]> Air pressure in the working chamber <![CDATA[3.0×10 -2 so]]> <![CDATA[3.2×10 -2 so]]> <![CDATA[3.2×10 -2 so]]> <![CDATA[3.5×10 -2 so]]> Arc starting voltage of arc starting power supply 150V 200V 200V 250V Arc starting power supply arc stabilization voltage / current 100A / 20V 100A / 20V 100A / 20V 100A / 20V Anode power supply etching working current / voltage 30A / 60V 30A / 60V 30A / 60V 30A / 60V Bias power supply etching working current / voltage 50V / 0.2A~250V / 10A 50V / 0.2A~250V / 10A 50V / 0.2A~250V / 10A 50V / 0.2A~250V / 10A Etching working time 25min 30min 30min 45min Sputtering operating temperature 550℃ 600℃ 600℃ 650℃ Sputtering vacuum <![CDATA[2.5×10 -1 Well]]> <![CDATA[3.5×10 -1 Well]]> <![CDATA[3.5×10 -1 Well]]> <![CDATA[4.5×10 -1 Well]]> Arc starting power supply, anode power supply sputtering working current / voltage 180A / 25V 180A / 25V 180A / 25V 180A / 25V Bias power sputtering operating voltage 100V 100V 100V 100V Coating thickness 2.5μm 2.8μm 2.8μm 3μm Sputtering time 45min 48min 48min 50min Magnetic field orientation pressure 0.5MPa 6MPa 6MPa 12MPa Heat treatment temperature 800℃ 900℃ 950℃ 1050℃ Heat treatment time 10h 20h 20h 40h Tempering temperature 440℃ 500℃ 580℃ 640℃ Tempering time 5h 8h 8h 15h
[0115] Embodiment 5:
[0116] Example 5 is the same as Example 3, except that the magnetic field orientation pressure is 4 MPa.
[0117] Embodiment 6:
[0118] Example 6 is the same as Example 3, except that the heat treatment temperature is 800°C.
[0119] Embodiment 7:
[0120] Example 7 is the same as Example 3, except that during ion etching, no anode ring is provided at the columnar target.
[0121] Comparative Examples 1-4:
[0122] The specific parameters of the NdFeB magnet manufacturing method of Comparative Examples 1-4 are shown in Table 2 below:
[0123] Table 2
[0124] Parameter name Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Vacuum degree <![CDATA[1.0×10 -2 so]]> <![CDATA[1.5×10 -2 so]]> <![CDATA[1.5×10 -2 so]]> <![CDATA[2.0×10 -2 so]]> Preheating temperature 200℃ 225℃ 225℃ 250℃ Air pressure in sleeve module <![CDATA[4.0×10 -2 so]]> <![CDATA[5.5×10 -2 so]]> 0 <![CDATA[9.0×10 -2 so]]> Air pressure in the working chamber <![CDATA[3.0×10 -2 so]]> <![CDATA[3.2×10 -2 so]]> <![CDATA[3.2×10 -2 so]]> <![CDATA[3.5×10 -2 so]]> Arc starting voltage of arc starting power supply 150V 200V 200V 250V Arc starting power supply arc stabilization voltage / current 100A / 20V 100A / 20V 100A / 20V 100A / 20V Anode power supply etching working current / voltage 30A / 60V 30A / 60V 30A / 60V 30A / 60V Bias power supply etching working current / voltage 50V / 0.2A~250V / 10A 50V / 0.2A~250V / 10A 50V / 0.2A~250V / 10A 50V / 0.2A~250V / 10A Etching working time 25min 30min 30min 45min Sputtering operating temperature 550℃ 600℃ 600℃ 650℃ Sputtering vacuum <![CDATA[2.5×10 -1 Well]]> <![CDATA[3.5×10 -1 Well]]> <![CDATA[3.5×10 -1 Well]]> <![CDATA[4.5×10 -1 Well]]> Arc starting power supply, anode power supply sputtering working current / voltage 180A / 25V 180A / 25V 180A / 25V 180A / 25V Bias power sputtering operating voltage 100V 100V 100V 100V Coating thickness 2.5μm 2.8μm 2.8μm 3μm Sputtering time 45min 48min 48min 50min Magnetic field orientation pressure 0.5MPa 0MPa 6MPa 12MPa Heat treatment temperature 700℃ 900℃ 950℃ 1150℃ Heat treatment time 10h 20h 20h 40h Tempering temperature 440℃ 500℃ 580℃ 640℃ Tempering time 5h 8h 8h 15h
[0125] The coercive force Hcj (kOe) and remanence Br (kG) of the diffused NdFeB magnets obtained in Examples 1-6 and Comparative Examples 1-4 were measured using a TD8330 permanent magnet material testing system. The test results are shown in Table 3:
[0126] Table 3
[0127] Coercivity remanence Original magnet 14.35 16.02 Example 1 14.12 23.75 Example 2 14.19 25.01 Example 3 14.20 25.07 Example 4 14.13 23.93 Example 5 14.17 24.93 Example 6 14.18 24.95 Example 7 14.13 23.78 Comparative Example 1 14.09 22.78 Comparative Example 2 14.07 21.45 Comparative Example 3 14.15 23.96 Comparative Example 4 14.11 22.96
[0128] It can be seen from Table 3 that by comparing the coercive force and remanent magnetization data of Examples 1-6 with the coercive force and remanent magnetization data of the original magnet, it can be seen that the grain boundary diffusion thick NdFeB magnet manufacturing method provided by the present invention can make the coercive force of NdFeB magnet (thickness ≥ 11mm) reach above 23.75kOe. In the best embodiment, the coercive force reaches 25.07kOe, which can increase the coercive force by 9.05kG compared with the coercive force of the original magnet, and the remanent magnetism can reach above 14.12kG. In the best embodiment, the remanent magnetism can reach 14.20kG, which can control the reduction of remanent magnetism to 0.15kG compared with the remanent magnetism of the original magnet.
[0129] Through the lateral comparison of Examples 1-4, the separate comparison of Example 2 and Example 3, the separate comparison of Example 3 and Example 5, and the comparison of Example 3 and Example 6, it can be seen that appropriately increasing the Ar gas concentration in the sleeve module during etching, the magnetic field orientation pressure during composite treatment and the heat treatment temperature can further improve the comprehensive magnetic properties of the diffused NdFeB magnet.
[0130] By comparing Example 1, Example 3 with Example 4, comparing Comparative Example 1 with Example 1, and comparing Comparative Example 4 with Example 4, it can be known that when the Ar gas concentration in the sleeve module and the working chamber is too high, the Ar positive ions in the etching process will be blocked by Ar atoms when exposing the grain boundaries of the magnetic steel sheet, thereby reducing the exposure of the grain boundaries of the magnetic steel sheet and weakening the ability to open the grain boundary diffusion channel during the later grain boundary diffusion. When the Ar gas concentration in the sleeve module and the working chamber is too low, the ionization rate of the Ar positive ions in the etching process is too low, and too few Ar positive ions are formed, which will also reduce the exposure of the grain boundaries of the magnetic steel sheet and weaken the ability to open the grain boundary diffusion channel during the later grain boundary diffusion.
[0131] At the same time, excessive magnetic field orientation pressure and heat treatment temperature will cause more Dy elements to diffuse into the lattice and enrich Dy elements on the surface of the magnet, affecting the grain boundary diffusion depth of Dy, reducing the saturation magnetization intensity of the magnet and the content of Dy elements diffused into the interior of the magnet, and ultimately causing the remanence of the magnet to decrease, and the coercive force to increase slightly. Excessively low magnetic field orientation pressure and heat treatment temperature will lead to a slower diffusion rate, with only a small amount of Dy elements diffusing into the magnet, and the grain boundary diffusion effect is poor.
[0132] By comparing Example 2 with Comparative Example 2, it can be seen that when the magnetic field orientation pressure is cancelled, the grain boundary diffusion depth of Dy will be reduced, the saturation magnetization intensity of the magnet and the content of Dy elements diffused into the interior of the magnet will be reduced, and ultimately the remanence of the magnet will decrease, and the coercive force will not be increased much.
[0133] By comparing Example 3 with Comparative Example 3, it can be seen that during ion etching, when the Ar gas concentration is not zoned, the Ar gas concentration at the columnar target is too low, and the rate of Ar positive ions generated is too low, which will affect the grain boundary exposure rate of the magnetic steel sheet. If the Ar gas concentration at the columnar target is too high, the generated Ar positive ions will be hindered by the Ar atoms in the working chamber, which will also affect the grain boundary exposure rate of the magnetic steel sheet.
[0134] By comparing Example 3 with Example 7, it can be seen that during ion etching, if an anode ring is not provided to accelerate, bunch, guide and pull the Ar positive ions and electrons generated at the columnar target, the Ar positive ion overflow rate at the columnar target will be relatively low, and the grain boundary exposure rate of the magnetic steel sheet will be reduced, affecting the grain boundary diffusion of thick NdFeB magnets.
[0135] In summary, the ion etching of the present invention adopts Ar concentration zoning setting, and cooperates with the synergistic effect of co-directional stacking hot pressing and compounding, which can effectively improve the grain boundary exposure rate of the magnetic steel sheet and promote the opening of the grain boundary channel of the magnetic steel sheet during diffusion. At the same time, it can also enable more Dy elements to diffuse in the lattice. The grain boundary diffusion depth of Dy is deeper than that of the prior art, and is more suitable for the grain boundary diffusion of thick NdFeB magnets, thereby improving the saturation magnetization intensity of the magnet and the content of Dy elements diffused into the interior of the magnet, and improving the comprehensive magnetic properties of thick NdFeB magnets such as remanence and coercive force.
[0136] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for manufacturing grain boundary diffusion thick NdFeB magnetic steel, It is characterized in that The following steps are involved: Step S1, magnet loading, hoisting the magnetic steel sheet to be prepared onto the rotating frame system. During hoisting, the magnetic steel sheet is arranged vertically, and the orientation plane A of the magnetic steel sheet in the magnetic field orientation direction is arranged toward the central axis B of the rotating frame system. After loading is completed, the sealing door of the etching and coating machine is closed; Step S2: preheating the etching process, turn on the mechanical pump, Roots pump and molecular pump in the vacuum pump group in turn, so that the vacuum degree of the working chamber of the etching and coating machine reaches 1.0×10 -2 pa~2.0×10 -2 After pa, the electric heating system and the ion etching system are respectively turned on to preheat and etch the magnetic steel sheet to remove impurities on the surface of the magnetic steel sheet, wherein during etching, the Ar gas concentration at the cylindrical target in the working chamber is higher than the Ar gas concentration in the working chamber; Step S3, sputtering coating, after etching is completed, the ion etching system is turned off, the electric heating system is kept running, Ar gas is input into the working chamber again, the sputtering system is turned on, and the columnar target and the pancake target emit Dy plasma, which is deposited on the magnetic steel sheet of the turret system for coating; Step S4, polishing treatment, taking out the magnetic steel sheet after coating from the etching and coating machine, polishing and cleaning the magnetic steel sheet to form edge magnetic steel sheet and middle magnetic steel sheet, wherein the edge magnetic steel sheet is the magnetic steel sheet with the orientation surface A polished, and the middle magnetic steel sheet is the magnetic steel sheet with the orientation surface polished; Step S5, stacking, stacking the edge magnetic steel sheets and the middle magnetic steel sheets in the magnetic field orientation direction in a stacking manner of edge magnetic steel sheet-middle magnetic steel sheet-edge magnetic steel sheet to form a magnetic sheet stack. During stacking, the polished surface of the edge magnetic steel sheet is arranged in contact with the polished surface of another edge magnetic steel sheet or the middle magnetic steel sheet, and the number N of the middle magnetic steel sheets is an integer ≥ 0; Step S6, composite treatment, applying a pressure of 0.5 to 12 MPa in the magnetic field orientation direction of the magnetic sheet stack, and performing heat treatment at a temperature of 800 to 1050°C in a vacuum or inert atmosphere for 10 to 40 hours. After the heat treatment, the magnetic sheet stack is tempered at a temperature of 440 to 640°C for 5 to 15 hours to obtain grain boundary diffusion thick NdFeB magnets. The remanence of the grain boundary diffusion thick NdFeB magnets with a thickness of ≥11 mm reaches more than 14.28 kG, and the coercive force reaches more than 22.87 kOe.
2. A method for manufacturing a grain boundary diffused thick NdFeB magnetic steel according to claim 1, It is characterized in that The preheat etching comprises the following steps: Step T1, preheating, turning on the electric heating system to raise the temperature in the working chamber to 200-250°C; Step T2, closing the cylindrical target, starting the sleeve module surrounding the outer side of the cylindrical target, and sealing and isolating the cylindrical target from the working chamber; Step T3: Filling Ar gas into the sleeve module and the working chamber respectively, so that the pressure in the sleeve module is 5.0×10 -2 pa~8.0×10 -2 pa, synchronously, the air pressure in the working chamber is 3.0×10 -2 pa~3.5×10 - 2 pa; Step T4, etching arc initiation, the first arc initiation needle beside the cylindrical target rotates and swings, and instantly touches the cylindrical target, so that the arc initiation power supply on the cylindrical target is short-circuited, and the Ar gas in the sleeve module is discharged to start the arc and emit a glow, forming Ar positive ions and electrons; Step T5, the anode ring is opened. Synchronously with step T4, the partition door assembly on the sleeve module is opened, so that a gap is formed on the side of the sleeve module facing away from the turret system, and an anode ring is simultaneously formed at the gap. The anode ring performs a bunching acceleration process on Ar positive ions and electrons, and pulls the Ar positive ions and electrons out of the sleeve module from the gap. Step T6, anode pulling, synchronous with step T4, the anode power supply supplies power to the pancake target, the pancake target pulls and accelerates the electrons released in step T4, and collides with the Ar gas in the working chamber to form Ar positive ions, and the working current and voltage of the anode power supply are 30A / 60V; Step T7, etching, the bias power supply supplies power to the turntable system, the turntable system pulls Ar positive ions, and the Ar positive ions collide with the surface of the magnetic steel sheet on the turntable system. The working current and voltage of the bias power supply are as follows: the working voltage is 50V~250V, the current is 0.2A~10A, and the working time is 25min~45min.
3. A method for manufacturing a grain boundary diffused thick NdFeB magnetic steel according to claim 2, Features: In step T2, the air pressure in the sleeve module is 6.0×10 -2 pa, the air pressure in the working chamber is 3.2×10 -2 pa.
4. The method for manufacturing a grain boundary diffused thick NdFeB magnetic steel according to claim 2, Features: In step T3, the initial voltage of the arc starting power supply is 150-250V, and the working current and voltage after arc stabilization are 100A / 20V.
5. The method for manufacturing a grain boundary diffusion thick NdFeB magnetic steel according to claim 2, Features: In step T6, the current of the anode power supply is gradually increased from 30A to 100A.
6. The method for manufacturing a grain boundary diffusion thick NdFeB magnetic steel according to claim 2, Features: In step T7, the voltage of the bias power supply is gradually increased from 50V to 250V.
7. The method for manufacturing a grain boundary diffusion thick NdFeB magnetic steel according to claim 1, It is characterized in that The sputtering coating comprises the following steps: Step U1, heating and heat preservation, maintaining the operation of the electric heating system, raising the temperature in the working chamber to 550-650° C., and heat preservation; Step U2: Filling Ar gas into the working chamber to maintain the vacuum degree in the working chamber at 2.5×10 -1 Pa~4.5×10 -1 Pa; Step U3, gap switching, adjusting the partition door assembly on the sleeve module so that the sleeve module forms a gap on the side facing the rotating rack system; Step U4, glow sputtering, the first arc starting needle at the cylindrical target rotates and swings to instantly touch the cylindrical target, and the second arc starting needle at the pancake target touches the pancake target, respectively short-circuiting the arc starting power supply and the anode power supply, and emitting glow to the Ar gas discharge arc in the working chamber, and the cylindrical target and the pancake target sputter and overflow Dy plasma; Step U5, coating, the bias power supply supplies power to the turret system, the working voltage is 100V, the turret system draws the Dy plasma to adhere to the surface of the magnetic steel sheet on the turret system to form a coating with a thickness of 2.5 to 3 μm, and the working time is 45 to 50 minutes.
8. A method for manufacturing a grain boundary diffused thick NdFeB magnetic steel according to claim 7, Features: In step U2, the vacuum degree in the working chamber is maintained at 3.5×10 -1 Pa.
9. The method for manufacturing a grain boundary diffused thick NdFeB magnetic steel according to claim 7, Features: In step U4, the operating current and voltage of the arc starting power supply and the anode power supply are 180A / 25V.
10. The method for manufacturing a grain boundary diffused thick NdFeB magnetic steel according to claim 1, Features: In the step S6, a pressure of 6MPa is applied to the magnetic field orientation direction of the magnetic sheet stack, and a heat treatment is performed at a temperature of 950°C in a vacuum or inert atmosphere for 35 hours. After the heat treatment, the magnetic sheet stack is tempered at a temperature of 550°C for 10 hours to obtain a grain boundary diffused thick NdFeB magnet. The remanence of the grain boundary diffused thick NdFeB magnet with a thickness of ≥11mm reaches more than 14.12kG, and the coercive force reaches more than 23.75kOe.
Citation Information
Patent Citations
Electrochemical apparatus and barrier layer protected substrate
CN101243563A
Large low-voltage, high-efficiency and high-beam direct current hollow negative electrode source
CN108770176A
Ion source multi-arc column-arc composite PVD coating system and coating method
CN108774728A
W-N nano composite-structured coating for miniature end milling cutters and preparation method thereof
CN109267005A
Physical vapor deposition method for surface protection of neodymium iron boron
CN109402556A