Electrolytic capacitor, manufacturing method thereof and electric drive controller

The electrolytic capacitor design with a preset anode and cathode foil voltage, along with a specific electrolyte, addresses the issue of low ripple current capacity and short service life, achieving enhanced performance and longevity.

CN119069262APending Publication Date: 2024-12-03ZHUHAI GREE XINYUAN ELECTRONICS +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411486872.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-23
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Existing electrolytic capacitors struggle to withstand higher ripple current and have a shorter service life.

Method used

The electrolytic capacitor design includes an anode foil with a preset voltage, a cathode foil with a preset breakdown voltage, and a specific electrolyte composition, such as nano-silicon dioxide, to enhance its performance.

Benefits of technology

The capacitor can withstand higher ripple current and has a significantly longer service life, with an increase in ripple current capacity by over 60% and improved high-temperature stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069262A_ABST
    Figure CN119069262A_ABST
Patent Text Reader

Abstract

The invention relates to an electrolytic capacitor and a manufacturing method thereof, and an electric drive controller, the electrolytic capacitor comprises a shell, a core and an electrolyte, the core is arranged in the shell, and the core is formed by winding a cathode foil, electrolytic paper and an anode foil which are stacked in sequence; the electrolyte is attached to the surfaces of the cathode foil and the anode foil; wherein the formation voltage for forming the anode foil is more than 1.4 times of the working voltage of the electrolytic capacitor, the breakdown voltage of the cathode foil is more than 3V, the working voltage of the electrolytic capacitor is 160V to 250V, the sparking voltage of the electrolyte is 350V to 400V, and the conductivity is 3.8 mS / cm to 4.8 mS / cm. According to the electrolytic capacitor, the electrolytic capacitor is provided with the anode foil with the preset voltage, the cathode foil with the preset breakdown voltage and the specific electrolyte, and under the condition, the electrolytic capacitor can bear high ripple current and has the long service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of electronic components, and in particular, relates to an electrolytic capacitor and a manufacturing method thereof, and an electric drive controller. Background Art

[0002] Electrolytic capacitors are widely used in photovoltaic inverters, new energy vehicles, charging piles, energy storage, consumer electronics and other fields. Taking aluminum electrolytic capacitors as an example, leaded aluminum electrolytic capacitors, as a common device in electronic circuits, play electrical roles such as filtering, bypassing, coupling, decoupling, and phase transfer.

[0003] In the prior art, there are few electrolytic capacitors that can withstand higher ripple current and have a longer service life. Therefore, there is an urgent need to provide an electrolytic capacitor with good ripple current capability. Summary of the invention

[0004] The embodiments of the present application provide an electrolytic capacitor and a manufacturing method thereof, and an electric drive controller, wherein the electrolytic capacitor has an anode foil with a preset voltage and a cathode foil with a preset breakdown voltage. In this case, the electrolytic capacitor can withstand a higher ripple current and has a longer service life.

[0005] According to the first aspect of the present application, an embodiment of the present application provides an electrolytic capacitor, comprising: a shell, a core and an electrolyte, wherein the core is arranged in the shell, and the core is wound by a cathode foil, an electrolytic paper and an anode foil stacked in sequence; the electrolyte is attached to the surface of the cathode foil and the anode foil; wherein the formation voltage for forming the anode foil is more than 1.4 times the working voltage of the electrolytic capacitor, the breakdown voltage of the cathode foil is above 3V, and the working voltage of the electrolytic capacitor is 160V-250V.

[0006] In some embodiments, the thickness of the electrolytic paper is 40 microns to 50 microns; and / or the density of the electrolytic paper is 0.7 g / cm 3 -0.8g / cm 3 ; and / or the electrolytic paper is a double-layer fiber composite electrolytic paper.

[0007] In some embodiments, the electrolytic capacitor further comprises:

[0008] an anode lead connected to the anode foil and protruding from the shell;

[0009] A cathode lead is connected to the cathode foil and protrudes from the casing.

[0010] In some embodiments, the shell has an opening, and the core is placed inside the shell through the opening of the shell;

[0011] The electrolytic capacitor further comprises: a sealing plug comprising butyl rubber, the sealing plug being arranged at the opening of the shell, the sealing plug being used to seal the core in the shell, and the anode lead and the cathode lead being able to pass through the sealing plug and protrude from the shell.

[0012] In some embodiments, the anode foil is a metal foil with a surface subjected to corrosion treatment and then subjected to chemical treatment.

[0013] In some embodiments, the electrolyte is an electrolyte including nano-silicon dioxide, in which the weight proportion of the nano-silicon dioxide is 0.8%-1.2%, the flash voltage of the electrolyte is 350V-400V, and the conductivity is 3.8mS / cm-4.8mS / cm.

[0014] According to a second aspect of the present application, a method for manufacturing an electrolytic capacitor is provided, wherein the method comprises:

[0015] Providing an anode foil, wherein a formation voltage for forming the anode foil is more than 1.4 times the working voltage of the electrolytic capacitor, and the working voltage of the electrolytic capacitor is 160V-250V;

[0016] Providing a cathode foil, wherein the breakdown voltage of the cathode foil is above 3V;

[0017] Providing electrolytic paper, and winding the anode foil, electrolytic paper and cathode foil stacked in sequence into a core;

[0018] The core is dried and immersed in the electrolyte for impregnation;

[0019] The core containing the electrolyte is placed in the housing and sealed.

[0020] In some embodiments, the electrolyte is an electrolyte comprising nano-silicon dioxide.

[0021] In some embodiments, in the electrolyte, the weight proportion of the nano-silicon dioxide is 0.8%-1.2%, wherein the flash voltage of the electrolyte is 350V-400V, and the conductivity is 3.8mS / cm-4.8mS / cm.

[0022] In some embodiments, the thickness of the electrolytic paper is 40 microns to 50 microns; and / or the density of the electrolytic paper is 0.7 g / cm 3 -0.8g / cm 3 ; and / or the electrolytic paper is a double-layer fiber composite electrolytic paper.

[0023] In some embodiments, the impregnation step is performed in an impregnation device, wherein during the impregnation process, the impregnation vacuum degree of the impregnation device is set to be above -0.088MPa, the pressure is set to be above 0.2MPa, and the impregnation time is set to be above 8h.

[0024] In some embodiments, the immersion temperature is 45°C-55°C.

[0025] In some embodiments, the step of placing the core storing the electrolyte into the housing for sealing comprises:

[0026] The core storing the electrolyte is inserted into the sealing plug and then placed into the shell for sealing.

[0027] In some embodiments, the sealing plug comprises butyl rubber, wherein the weight percentage of the butyl rubber in the sealing plug is not less than 28%.

[0028] In some embodiments, the sealing plug comprising butyl rubber is a sealing plug of mixed butyl rubber formed by EP rubber and butyl rubber; or is a butyl rubber sealing plug.

[0029] In some embodiments, providing an anode foil comprises:

[0030] The metal foil after the corrosion treatment is placed in a forming solution, and a preset forming voltage is applied, wherein the preset forming voltage is more than 1.4 times the working voltage of the electrolytic capacitor.

[0031] According to a third aspect of the present application, an electric drive controller is provided, wherein the electric drive controller includes a controller body and an electrolytic capacitor connected to the controller body, wherein the electrolytic capacitor is the electrolytic capacitor described above or is an electrolytic capacitor manufactured according to the method for manufacturing an electrolytic capacitor described above.

[0032] Compared with the prior art, the embodiments of the present invention have the following beneficial effects:

[0033] The electrolytic capacitor provided in the embodiment of the present application has an anode foil with a preset voltage, a cathode foil with a preset breakdown voltage, and a specific electrolyte. In this case, the electrolytic capacitor can withstand a higher ripple current and has a longer service life.

[0034] It can be understood that the beneficial effects of the second to third aspects mentioned above can be found in the relevant description of the first aspect mentioned above, and will not be repeated here. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0036] Figure 1 A schematic diagram of a process flow of a method for manufacturing an electrolytic capacitor provided for the implementation of the present application;

[0037] Figure 2 A schematic diagram of the structure of an electrolytic capacitor provided in an embodiment of the present application;

[0038] Figure 3 A schematic diagram of the dissected structure of a core of an electrolytic capacitor provided in an embodiment of the present application.

[0039] Explanation of symbols

[0040] 1-shell; 2-core; 21-electrolytic paper; 22-anode foil; 23-cathode foil; 3-sealing plug; 4-cathode lead; 5-anode lead. DETAILED DESCRIPTION

[0041] The following specific embodiments are provided to help the reader obtain a comprehensive understanding of the methods, devices and / or systems described herein. However, after understanding the disclosure of the present application, various changes, modifications and equivalents of the methods, devices and / or systems described herein will be clear. For example, the order of operations described herein is only an example and is not limited to those orders set forth herein, but can be changed as will be clear after understanding the disclosure of the present application, except for operations that must occur in a specific order. In addition, for greater clarity and simplicity, the description of features known in the art may be omitted.

[0042] The features described herein can be implemented in different forms and should not be construed as being limited to the examples described herein. Rather, the examples described herein have been provided to illustrate only some of the many possible ways to implement the methods, devices, and / or systems described herein, which will be clear after understanding the disclosure of the present application.

[0043] As used herein, the term "and / or" includes any one of the associated listed items and any combination of any two or more.

[0044] Although terms such as "first", "second", and "third" may be used herein to describe various members, components, regions, layers, or portions, these members, components, regions, layers, or portions should not be limited by these terms. Instead, these terms are only used to distinguish one member, component, region, layer, or portion from another member, component, region, layer, or portion. Therefore, without departing from the teachings of the examples described herein, the first member, first component, first region, first layer, or first portion referred to in the examples may also be referred to as the second member, second component, second region, second layer, or second portion.

[0045] In the specification, when an element such as a layer, a region or a substrate is described as being "on", "connected to" or "mounted to" another element, the element may be directly "on", "connected to" or "mounted to" another element, or one or more other elements may be present therebetween. Conversely, when an element is described as being "directly on", "directly connected to" or "directly mounted to" another element, there may be no other elements therebetween.

[0046] The terms used herein are only used to describe various examples and are not intended to limit the disclosure. Unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. The terms "comprise", "include" and "have" indicate the presence of the described features, quantities, operations, components, elements and / or combinations thereof, but do not exclude the presence or addition of one or more other features, quantities, operations, components, elements and / or combinations thereof. The term "plurality" represents two and any number greater than two.

[0047] The definitions of directional terms such as "upper", "lower", "top" and "bottom" in this application are all based on the orientation of the product when it is placed upright.

[0048] Unless otherwise defined, all terms used herein, including technical terms and scientific terms, have the same meaning as those generally understood by ordinary technicians in the field to which the present invention belongs after understanding the present invention. Unless explicitly defined as such herein, terms such as those defined in general dictionaries should be interpreted as having a meaning consistent with their meaning in the context of the relevant field and the present invention, and should not be interpreted in an idealized or overly formal way.

[0049] Furthermore, in the description of the examples, when it is deemed that a detailed description of well-known related components or functions will cause vague interpretation of the present invention, such detailed description will be omitted.

[0050] The following will be combined Figure 2 and Figure 3 The electrolytic capacitor provided in the embodiments of the present application is introduced.

[0051] According to a first aspect of the present application, an electrolytic capacitor is provided, specifically a medium voltage aluminum electrolytic capacitor, which is used in an electric drive controller of a vehicle, wherein: Figure 2 and Figure 3 As shown, the electrolytic capacitor includes a shell 1, a core 2 and an electrolyte, wherein the core 2 is arranged in the shell, and the core is wound by stacking a cathode foil 23, an electrolytic paper 21 and an anode foil 22 in sequence; the electrolyte is attached to the surface of the cathode foil 23 and the anode foil 22; wherein the formation voltage of the anode foil is more than 1.4 times the working voltage of the electrolytic capacitor, and the breakdown voltage of the cathode foil is more than 3V, wherein the working voltage of the electrolytic capacitor is 160V-250V, wherein the flash voltage of the electrolyte is 350V-400V, and the conductivity is 3.8mS / cm-4.8mS / cm.

[0052] According to the electrolytic capacitor provided in the embodiment of the present application, it has an anode foil with a preset voltage, a cathode foil with a preset breakdown voltage, and a specific electrolyte. In this case, the electrolytic capacitor can withstand a higher ripple current and have a longer service life. Specifically, the ripple current can be increased from 533mA (105℃120Hz) to 900mA (105℃120Hz), with an increase rate of more than 60%.

[0053] According to the present application, the operating voltage of the electrolytic capacitor is 160V-250V, and the operating voltage is the voltage range in which the electrolytic capacitor is used for working. Within this range, the electrolytic capacitor can work stably and exert its performance. The formation voltage of the anode foil is more than 1.4 times the working voltage of the electrolytic capacitor. The formation voltage is the voltage applied during the formation treatment of the anode foil, which can determine the thickness and quality of the oxide film on the surface of the anode foil. In the present application, the formation voltage is high, which means that there is an oxide film of suitable thickness on the surface of the anode foil, and the anode foil has good corrosion resistance, so that the electrolytic capacitor formed by the anode foil can work stably in the medium voltage section (for example, 160V-250V).

[0054] In some embodiments, the working voltage of the electrolytic capacitor is 160V-250V, and the formation voltage of the anode foil is more than 1.4 times the working voltage of the electrolytic capacitor, preferably 1.4 times-2.0 times. That is, the formation voltage of the anode foil can be 224V-500V. Preferably, it is 224V-300V.

[0055] In some embodiments, the anode foil is a metal foil after the surface has been corroded and then subjected to chemical treatment. As an example, the corrosion treatment process of the anode foil generally includes multiple steps such as pre-treatment, pre-stage corrosion, post-stage corrosion and post-treatment. These steps act together on the anode foil to optimize its surface structure and improve its performance. Among them, the pre-treatment is a series of physical and chemical treatments before the bare foil (aluminum foil that has not been corroded) is electro-etched. Its main purpose is to remove oil stains, impurities and natural oxide films on the surface of the aluminum foil, adjust the organizational structure of the aluminum foil, improve its surface state, make its surface uniform and activated, so as to facilitate the formation of uniformly distributed initial holes during subsequent corrosion treatment. Preferably, a compound or mixture containing Zn or Pb can be added to the pre-treatment liquid as an additive. These additives help to form more uniform corrosion pits during the corrosion process, improve the expansion rate and specific volume of the aluminum foil, and maintain its good mechanical strength. Pre-stage corrosion and post-stage corrosion are the core steps of the anode foil corrosion treatment. These two stages usually use different etching solutions and corrosion conditions to form corrosion pits of different depths and shapes on the surface of the aluminum foil. The first stage of corrosion mainly forms the initial corrosion pits, while the second stage of corrosion further deepens and refines these corrosion pits to obtain a higher surface area. Post-treatment is to clean and dry the corroded anode foil to remove residual corrosion liquid and other impurities to ensure the surface cleanliness and stability of the anode foil.

[0056] In these embodiments, the surface corrosion treatment of the anode foil can expand its effective surface area, thereby increasing the electrostatic capacitance (specific capacitance) of the mS / cm area. Through chemical or electrochemical corrosion treatment, high-density and evenly distributed corrosion pits can be formed on the surface of the anode foil, and these corrosion pits can significantly increase the surface area of ​​the aluminum foil, thereby increasing the capacitance of the electrolytic capacitor. In addition, a reasonable corrosion treatment process can make the corrosion pits on the surface of the anode foil more evenly distributed, thereby improving the performance stability of the electrolytic capacitor. In addition, during the corrosion treatment process, by optimizing the process parameters and adding appropriate additives, the surface area of ​​the aluminum foil can be increased while maintaining its good mechanical strength.

[0057] According to the present application, the breakdown voltage of the cathode foil is above 3V, where the breakdown voltage is the maximum voltage value that the electrolytic capacitor can withstand, and the electrolytic capacitor will be damaged if the voltage exceeds this value. In some embodiments, the breakdown voltage of the cathode foil is above 3V, preferably 3V-4V. In this case, the electrolytic capacitor has good ripple current capability, so it can withstand higher ripple current and has a longer service life.

[0058] According to the present application, the electrolyte is a conductive liquid stored in the core, which serves as a conductive medium between the internal electrodes of the electrolytic capacitor. The composition and properties of the electrolyte have an important influence on the performance of the electrolytic capacitor, for example, it affects the ripple life and high temperature performance of the electrolytic capacitor.

[0059] In some embodiments, the electrolyte is an electrolyte including nano-silicon dioxide, the flash voltage of the electrolyte is 350V-400V, and the conductivity is 3.8mS / cm-4.8mS / cm. In this way, the high temperature stability and ripple resistance of the electrolyte can be effectively improved. The nano effect of nano-silicon dioxide can improve the conductive path of the electrolyte, reduce the resistance to ion migration, and at the same time increase the flash voltage of the electrolyte to more than 350V, thereby enhancing the high temperature performance and reliability of the electrolytic capacitor. As an example, in addition to nano-silicon dioxide, the electrolyte also includes phosphoric acid, mannitol, p-nitrobenzoic acid, citric acid, sorbitol and water. Specifically, in terms of the weight percentage of the electrolyte, nano silicon dioxide is 0.8%-1.2%, phosphoric acid is 0.3%-0.5%, mannitol is 1%-5%, p-nitrobenzoic acid is 0.5%-2%, citric acid is 0.1%-0.5%, sorbitol is 1%-3% and the balance is water. Among them, the content of phosphoric acid is controlled between 0.3% and 0.5%, which helps to adjust the acidity of the electrolyte and provide the necessary ionic conductivity. The content of mannitol is controlled between 1% and 5%, which, as a stabilizer, helps to prevent the electrolyte from decomposing or precipitating at high temperatures. The content of p-nitrobenzoic acid is controlled between 0.5% and 2%, which, as a preservative, helps to extend the service life of the electrolyte. The content of citric acid is controlled between 0.1% and 0.5%, which helps to adjust the pH value of the electrolyte and improve the stability of the capacitor. The content of sorbitol is controlled between 1% and 3%. As a thickener, it helps to improve the fluidity and uniformity of the electrolyte. In this way, an electrolyte with the above-mentioned flash voltage and conductivity can be formed, thereby ensuring that the electrolyte has many advantages, such as, but not limited to, directly affecting the ripple current tolerance and life of the capacitor. In addition, according to the present application, the electrolyte pH = 8.0 ± 1.0 can keep the aluminum oxide in the capacitor stable under this condition, which is beneficial to the stability of the capacitor. The moisture content is ≤ 8% to ensure the stability of the electrolyte and the long-term reliability of the capacitor. Under the test temperature of 30 ± 2 ° C, the conductivity is 3.8mS / cm-4.8mS / cm, the conductivity is relatively high, and the product has good conductivity and response speed.

[0060] In some embodiments, the electrolytic capacitor further includes an anode lead and a cathode lead, wherein the anode lead is connected to the anode foil and protrudes from the casing; and the cathode lead is connected to the cathode foil and protrudes from the casing.

[0061] In these embodiments, the anode lead and the cathode lead are connected to the corresponding anode foil and cathode foil in the core and protrude from a position of the shell, so as to facilitate connection with an external circuit.

[0062] In some embodiments, the housing 1 has an opening, and the core 2 is placed inside the housing 1 through the opening of the housing 1, wherein Figure 3 As shown, the electrolytic capacitor further includes a sealing plug 3 , which is disposed at the opening of the housing 1 . The sealing plug 3 is used to seal the core 2 in the housing 1 , and the cathode lead 4 and the anode lead 5 can pass through the sealing plug 3 and protrude out of the housing.

[0063] In these embodiments, the shell 1 of the electrolytic capacitor is provided with an opening so that a core impregnated with an electrolyte can be placed inside the shell 1 through the opening when the electrolytic capacitor is manufactured. After the core is properly placed, a sealing plug is used to close the opening to ensure that the electrolyte in the shell does not leak and to maintain the humidity and pressure inside the core stable. The sealing plug is arranged at the opening of the shell, and the sealing plug not only plays a sealing role, but also needs to provide a channel for the lead-out of the anode lead and the cathode lead. Specifically, the two leads pass through the hole or channel on the sealing plug and protrude from the shell to be connected to the external circuit. The design of the sealing plug needs to ensure that the shell opening can be tightly closed to prevent leakage of the electrolyte, and the leads can pass through smoothly without affecting the normal operation and life of the electrolytic capacitor.

[0064] In some embodiments, the sealing plug includes butyl rubber, wherein the weight percentage of butyl rubber in the sealing plug is not less than 28%. As an example, the sealing plug including butyl rubber is an EPDM+IIR mixed butyl rubber or an IIR butyl rubber sealing plug, specifically, the weight percentage of butyl rubber in the EPDM+IIR mixed butyl rubber sealing plug is not less than 28%-45%. The sealing plugs including butyl rubber as above can meet the actual requirements of the product and have a long service life, thereby improving the ripple current capacity and service life of the electrolytic capacitor. In addition, the service life of the IIR butyl rubber sealing plug is extremely long.

[0065] According to the present application, electrolytic paper, as a key component in an electrolytic capacitor, mainly plays the role of isolation and support. It can effectively separate the anode and cathode of the electrolytic capacitor to prevent short circuit, and at the same time provide certain mechanical support to ensure the structural stability of the capacitor. In the present application, the type of electrolytic paper can improve the ripple current capability of the electrolytic capacitor to a certain extent.

[0066] When selecting electrolytic paper, it is necessary to comprehensively consider multiple factors such as insulation performance, liquid absorption capacity, mechanical strength, ESR, capacity and loss to ensure that the electrolytic capacitor has excellent performance and stable reliability. In some embodiments, the electrolyte is a double-layer fiber composite electrolytic paper, and the double-layer fiber composite electrolytic paper is composited by two or more layers of different fibers or materials. The double-layer fiber composite electrolytic paper can combine the advantages of different materials, so that it can maintain good liquid absorption capacity, insulation performance and low ESR while improving mechanical strength. In this way, it can better adapt to the working environment of large ripple current and reduce the performance degradation caused by internal vibration and deformation of the electrolytic capacitor. Specifically, the double-layer fiber composite electrolytic paper is a double-layer sisal fiber composite electrolytic paper, wherein sisal fiber is used as the material of the electrolytic paper of the present application, and high specific strength, high specific modulus, good air permeability, environmental protection, recyclability, etc. can be obtained. At the same time, the surface of sisal fiber has certain hydroxyl groups, which are easy to copolymerize with high molecular polymers to form composite materials, and have composite advantages that traditional single materials do not have. In addition, sisal fiber has good moisture absorption and heat dissipation properties, which is of great significance for the heat management generated by capacitors during operation.

[0067] like Figure 2 It can be seen that the electrolytic paper adopts a double-layer structure. The inner layer is a sisal fiber paper layer, which is located between the cathode foil and the anode foil and is mainly responsible for adsorbing and retaining the electrolyte; the outer layer is a sisal fiber reinforced electrolytic capacitor paper layer, which is arranged on the outside of the entire core, and can provide the necessary mechanical and electrical strength and prevent charge breakdown.

[0068] In some embodiments, the thickness of the electrolytic paper is 40 μm to 50 μm, and the density is 0.7 g / cm 3 Up to 0.8g / cm 3 . Appropriate thickness and density can well balance the performance of multiple aspects such as insulation performance, liquid absorption capacity, mechanical strength, ESR, capacity and loss. Electrolytic paper with appropriate thickness and density can not only ensure the effective isolation of the positive and negative electrodes inside the electrolytic capacitor, but also provide sufficient mechanical strength to prevent the capacitor from being damaged by vibration or impact during use. At the same time, moderate thickness and density can also maintain a low internal resistance, so that the capacitor can still maintain good performance under high-frequency signals. In addition, appropriate thickness and density also help to maintain a good loss angle of the electrolytic capacitor, that is, when the capacitor works under alternating current, its energy loss remains at a low level. Moreover, appropriate thickness and density can ensure the liquid absorption capacity of the electrolytic paper, that is, the ability to absorb and retain electrolyte, to avoid uneven distribution of electrolyte inside the capacitor due to insufficient liquid absorption capacity, thereby affecting the capacity and stability of the capacitor.

[0069] In the above embodiments, the type of electrolytic paper can comprehensively consider multiple factors such as insulation performance, liquid absorption capacity, mechanical strength, ESR, capacity and loss, and interacts with the electrolyte and electrode foil to ensure that the electrolytic capacitor has excellent performance and stable reliability.

[0070] According to the second aspect of the present application, Figure 1 As shown, a method for manufacturing an electrolytic capacitor is provided, wherein the method comprises:

[0071] Step S101, providing an anode foil, wherein a forming voltage for forming the anode foil is more than 1.4 times the working voltage of the electrolytic capacitor, and the working voltage of the electrolytic capacitor is 160V-250V.

[0072] In the embodiment of the present application, the step of manufacturing an anode foil is included, wherein the formation voltage of the anode foil is more than 1.4 times the working voltage of the electrolytic capacitor. As an example, the formation voltage of the anode foil can be between 224V and 350V, so that the manufactured electrolytic capacitor can be ensured to work safely and stably within the working voltage range of 160V-250V.

[0073] In the embodiment of the present application, the aluminum oxide film on the surface of the anode foil with a high formation voltage is more dense and uniform, which helps to reduce the heat generated by the electrolytic capacitor when it is subjected to ripple current and improve the service life and stability of the electrolytic capacitor.

[0074] Step S102, providing a cathode foil, wherein the breakdown voltage of the cathode foil is above 3V.

[0075] In the embodiment of the present application, the step of manufacturing a cathode foil is included, wherein the breakdown voltage of the cathode foil is above 3 V. The breakdown voltage is the voltage value when a material undergoes electrical breakdown under the action of an electric field. A cathode foil with a high breakdown voltage can ensure that the electrolytic capacitor will not undergo electrical breakdown under normal working conditions, thereby improving the reliability and safety of the electrolytic capacitor during operation.

[0076] Step S103, providing electrolytic paper, and winding the anode foil, electrolytic paper and cathode foil stacked in sequence into a core.

[0077] In the embodiment of the present application, electrolytic paper is used as an isolation layer to separate the anode foil and the cathode foil, and they are tightly combined with the electrolytic paper by winding to form the core of the electrolytic capacitor.

[0078] In the embodiment of the present application, the electrolytic paper not only serves to isolate the anode and cathode, but also participates in the absorption and retention of the electrolyte, which has an important influence on the performance of the electrolytic capacitor. In addition, the structure of winding into a core is conducive to reducing the volume of the electrolytic capacitor and improving space utilization.

[0079] Step S104, drying the core and immersing it in an electrolyte.

[0080] In an embodiment of the present application, before the core is immersed in the electrolyte, it is first necessary to perform a drying treatment. The purpose of drying is to remove any moisture or solvent residue that may exist in the core, to ensure that the electrolyte can evenly penetrate into the core and fully contact the anode foil and cathode foil. Drying is usually carried out in a specific oven or drying equipment, and the temperature and time need to be adjusted according to the material and size of the core to ensure the drying effect. As an example, the temperature can be 80°C-90°C, and the time can be 2h-3h.

[0081] In the embodiment of the present application, after drying, the core is immersed in an electrolyte. The electrolyte is an important component of the electrolytic capacitor, which provides an ion conductive channel so that the capacitor can store and release charge. The type and concentration of the electrolyte have a great influence on the performance of the capacitor. As an example, the electrolyte includes nano-silicon dioxide, and the flash voltage is 350V-400V, and the conductivity is 3.8mS / cm-4.8mS / cm. The flash voltage of the electrolyte is within a suitable range, and the electrolyte can withstand higher voltages without electrical breakdown, which can improve the safety and reliability of the electrolytic capacitor. The conductivity of the electrolyte is within a suitable range, and it can be understood that the ion transmission speed in the electrolyte is faster, which helps to reduce the internal resistance of the electrolytic capacitor and improve its response speed.

[0082] In the embodiment of the present application, during the impregnation process, it is necessary to ensure that the electrolyte can fully penetrate into the core and tightly bond with the aluminum oxide film formed on the surface of the anode foil and the cathode foil, which helps to increase the capacity of the capacitor and reduce leakage current and loss.

[0083] Step S105, placing the core containing the electrolyte into a shell and sealing it.

[0084] In the embodiment of the present application, the core storing the electrolyte is placed in the shell of the electrolytic capacitor and sealed. The shell is an external barrier to protect the internal structure of the electrolytic capacitor, and the sealing process can prevent the electrolyte from leaking and the influence of the external environment on the electrolytic capacitor.

[0085] In the embodiments of the present application, the packaging and sealing process can ensure the integrity and reliability of the electrolytic capacitor. Through packaging and sealing, the electrolytic capacitor can be safely used in various electronic devices.

[0086] According to the method for manufacturing an electrolytic capacitor of the present application, an anode foil with a preset voltage and a cathode foil with a preset breakdown voltage are used to manufacture an electrolytic capacitor, and the manufactured electrolytic capacitor can withstand a higher ripple current and has a longer service life.

[0087] According to the present application, the electrolyte has a crucial influence on the performance of the electrolytic capacitor. In some embodiments, the electrolyte contains nano-silicon dioxide and has a specific flash voltage and conductivity. The addition of a preset amount of nano-silicon dioxide can significantly increase the flash voltage of the electrolyte of the present application. Specifically, due to its high specific surface area and excellent physical and chemical properties, nano-silicon dioxide can form a stable dispersion system in the electrolyte, thereby improving the insulation performance and withstand voltage of the electrolyte. This improvement enables the electrolyte containing nano-silicon dioxide to withstand a higher voltage without flashing under the same conditions, that is, the flash voltage of the electrolyte is increased. In addition, the addition of nano-silicon dioxide will also increase the conductivity of the electrolyte. This is because, on the one hand, there are a large number of hydroxyl groups and other active groups on the surface of nano-silicon dioxide particles, which can interact with ions in the electrolyte to form ion transmission channels, thereby improving the ionic conductivity of the electrolyte. On the other hand, the uniform dispersion of nano-silicon dioxide particles in the electrolyte can also increase the ion migration path of the electrolyte, further promoting the transmission of ions. Therefore, the conductivity of the electrolyte can also be improved.

[0088] In some embodiments, in the electrolyte, the weight proportion of nano-silicon dioxide is 0.8%-1.2%, and the remainder is additives. As an example, the additives include ethylene glycol, ammonium sebaceous acid / ammonium, diethylene glycol, ammonium adipate and other additives. Among them, the weight of each component of ethylene glycol, ammonium sebaceous acid / ammonium, diethylene glycol, and ammonium adipate can be set according to actual conditions. In this way, an electrolyte with the above-mentioned flash voltage and conductivity can be formed, so that the electrolyte can be ensured to have many advantages, for example, but not limited to, the electrolyte includes improved flash voltage, conductivity, stability, etc. In addition, the uniform distribution of nanoparticles can also effectively prevent the accumulation of impurities in the electrolyte and extend the service life of the capacitor.

[0089] In some embodiments, the thickness of the electrolytic paper is 40 microns to 50 microns; and / or the density of the electrolytic paper is 0.7 g / cm 3 -0.8g / cm 3 ; and / or the electrolytic paper is a double-layer fiber composite electrolytic paper.

[0090] According to the present application, the impregnation step is carried out in a specific impregnation device, and the parameters of the impregnation device include impregnation vacuum, pressure and impregnation time. Among them, the impregnation vacuum is set to be above -0.088MPa, specifically -0.08MPa to -0.12MPa. The setting of the vacuum helps to remove air and bubbles in the electrolytic paper during the impregnation process, so that the electrolyte can more fully penetrate into the pores and fibers of the electrolytic paper, and improve the penetration efficiency of the electrolyte. At the same time, the pressure during the impregnation process is set to be above 0.2MPa, specifically 0.2MPa to 0.6MPa. The increased pressure can further promote the penetration of the electrolyte into the interior of the electrolytic paper, especially under high vacuum, the effect of pressure is more obvious. Appropriate pressure can ensure that the electrolyte can be evenly distributed in various parts of the electrolytic paper, improving the uniformity and effect of the impregnation. The impregnation time is set to be more than 8 hours, specifically 8h-9h. The length of the impregnation time directly affects the penetration depth and penetration amount of the electrolyte in the material. The appropriate impregnation time can ensure that the electrolyte fully penetrates into the deep structure of the electrolytic paper and achieves a better impregnation effect.

[0091] In these embodiments, by properly adjusting these parameters, it is possible to ensure that the impregnation process is carried out efficiently, evenly and fully, thereby satisfying the requirements of the core for the impregnation effect.

[0092] According to the present application, during the impregnation process, the temperature will directly affect the penetration speed, penetration depth and impregnation effect of the electrolyte in the electrolytic paper. In some embodiments, the impregnation temperature is set to 45°C-55°C. Within this temperature range, the electrolyte molecules and the air molecules in the pores of the electrolytic paper will become more active. Higher temperatures help reduce the viscosity of the electrolyte, making it easier to flow and penetrate into the tiny pores of the electrolytic paper. At the same time, the increase in temperature also helps to reduce the surface tension of the electrolytic paper, further promoting the penetration of the electrolyte.

[0093] In these embodiments, impregnation within this temperature range can not only promote the penetration and diffusion of the electrolyte, but also avoid the adverse effects of overheating, while ensuring the quality of the product. For example, it can ensure that the electrolyte evenly penetrates into all parts of the electrolytic paper to form a stable bonding layer.

[0094] According to the present application, placing the core storing the electrolyte into the shell for sealing includes: inserting the core storing the electrolyte into the sealing plug, and then placing it into the shell for sealing. In some embodiments, the step of inserting the impregnated core into the sealing plug and then placing it into the shell needs to be completed within 4 hours. Inserting the impregnated core into the sealing plug and placing it into the shell as soon as possible helps to reduce adverse changes such as deterioration and introduction of foreign matter, and maintain the impregnation effect.

[0095] In the prior art, the electrolytic capacitor contains liquid electrolyte, and its sealing performance is crucial to prevent electrolyte leakage. The material of the sealing plug directly affects the tightness of its sealing with the electrolytic capacitor housing. If the material is not good, it may lead to poor sealing, which in turn causes electrolyte leakage, affecting the performance and life of the electrolytic capacitor. The leaked electrolyte may change the internal environment of the electrolytic capacitor, increase the resistance of the electrolyte, and thus affect the ripple current. In addition, when the electrolytic capacitor is working, the electrolyte will vaporize and generate vapor pressure. The material and sealing performance of the sealing plug will affect the management of vapor pressure. If the sealing performance is poor, the vapor pressure may not be effectively controlled within a safe range, resulting in an increase in the internal pressure of the electrolytic capacitor, which in turn affects the stability of the ripple current and the life of the electrolytic capacitor.

[0096] According to the present application, the sealing plug includes butyl rubber, wherein the weight percentage of butyl rubber in the sealing plug is not less than 28%. As an example, the sealing plug including butyl rubber is a sealing plug of a mixed butyl rubber (EPDM+IIR mixed butyl rubber) formed by ethylene propylene rubber and butyl rubber; or a butyl rubber (IIR butyl rubber) sealing plug. Among them, the weight percentage of butyl rubber in the mixed butyl rubber is not less than 28%-45%. The sealing plugs including butyl rubber as above can meet the requirements of sealing performance, aging resistance, etc., and have a long service life, so they can indirectly improve the ripple current capacity and service life of the electrolytic capacitor. In addition, the service life of the IIR butyl rubber sealing plug is extremely long.

[0097] In some embodiments, step S101, providing an anode foil, includes:

[0098] Step S1011, placing the metal foil after corrosion treatment in a forming solution, and applying a preset forming voltage, wherein the preset forming voltage is more than 1.4 times the working voltage of the electrolytic capacitor. Here, the metal foil is usually aluminum foil, because aluminum has good electrochemical properties and cost-effectiveness. The metal foil is subjected to corrosion treatment. The purpose of the corrosion treatment is to form a porous, high-specific surface area oxide layer on the surface of the metal foil, which helps to increase the capacitance value of the electrolytic capacitor. Subsequently, the treated metal foil is placed in a forming solution. The forming solution can be an aqueous solution containing an electrolyte. While the metal foil is placed in the forming solution, a preset forming voltage needs to be applied. This voltage is a key parameter of the working voltage of the electrolytic capacitor, which determines the growth rate and quality of the oxide layer during the forming process. The preset forming voltage is more than "1.4 times" the working voltage of the electrolytic capacitor. This setting is to ensure that during the forming process, the oxide layer can be fully and evenly formed, and has a certain thickness and stability to withstand the voltage required by the electrolytic capacitor when it is working. Higher formation voltages help form a denser and more stable oxide layer, thereby improving the performance and life of electrolytic capacitors.

[0099] According to a third aspect of the present application, another method for manufacturing an electrolytic capacitor is provided, the method comprising:

[0100] Raw material cutting: cutting anode aluminum foil, cathode aluminum foil and electrolytic paper to the required width to ensure the tightness and consistency of subsequent winding.

[0101] In this step, the formation voltage of the anode aluminum foil should be ≥1.4 times the working voltage of the electrolytic capacitor to improve the stability of the capacitor. Specifically, a mixed acid etching process is used to obtain an etching foil with a desired specific capacitance, and an oxide film is grown through a formation process to form an anode aluminum foil with a desired formation voltage.

[0102] In this step, the cathode aluminum foil is selected with a voltage of ≥3V, and the corrosion foil with the required specific capacity is obtained through the corrosion process, and the oxide film is grown. The length of the cathode aluminum foil needs to be slightly longer than the anode foil to ensure that the cathode foil can completely wrap the anode foil when winding, reduce the capacity attenuation ratio during high temperature durability life, and improve product stability.

[0103] In this step, the electrolytic paper is a double-layer sisal fiber composite electrolytic paper with a thickness of 40 μm and a density of 0.7-0.8 g / cm 3 The double-layer structure helps to reduce the loss angle and ESR value of the electrolytic capacitor and improve the overall performance.

[0104] Riveting and Winding: Use a rivet winding machine to rivet the anode guide pin and cathode guide pin to the anode aluminum foil and cathode aluminum foil respectively to ensure a firm connection.

[0105] Insert electrolytic paper between the anode aluminum foil and the cathode aluminum foil, and form a cylindrical core by winding. Pay attention to controlling the winding tension and tightness to avoid affecting the performance of the capacitor.

[0106] Baking and dehumidification: Bake the wound cylindrical core in an environment of 80-90℃ for 1.5 hours to remove excess moisture in the core, which helps to improve the stability and reliability of the capacitor.

[0107] Electrolyte impregnation: The vacuum degree in the impregnation equipment is set to ≤-0.08MPa to ensure that the electrolyte can fully penetrate into the core and reduce the generation of bubbles. The pressurized pressure is set to ≥0.2MPa to enhance the penetration effect of the electrolyte. The impregnation time is not less than 480 minutes to ensure that the core fully absorbs the electrolyte. The upper limit of the impregnation time can be adjusted according to actual conditions, but it should be avoided that the electrolyte overflows or the core is deformed due to excessive time. The impregnation temperature is controlled at 50±10℃ to optimize the penetration rate of the electrolyte and the absorption effect of the core. Among them, nano-silicon dioxide with a mass ratio of 0.8-1.2% is added to the electrolyte to increase the conductivity and flash voltage of the electrolyte (to more than 350V), thereby improving the high temperature stability and reliability of the capacitor. The particle size and dispersibility of nano-silicon dioxide need to be strictly controlled to ensure the stability of the electrolyte performance.

[0108] Sealing assembly: The impregnated core is quickly loaded into the aluminum shell and sealed with a sealing plug. The whole process must be completed within 4 hours to prevent the electrolyte from absorbing moisture in the air. EPDM+IIR composite material is selected as the sealing plug, where the IIR ratio is ≥28%. This material combination has good sealing, aging resistance and mechanical strength, which helps to improve the reliability and service life of the capacitor. In addition, the sealing performance of the sealing plug has an important influence on the overall performance and ripple current bearing capacity of the capacitor.

[0109] Casing identification: A casing is put on the outside of the capacitor, for example, the shell, for identification (such as trademark, capacity, voltage, model, temperature, polarity, etc.) and insulation (to prevent short circuit and static electricity between the pole shell) to improve the safety and recognition of the product.

[0110] High temperature and pressure aging: The sealed capacitors are subjected to high temperature and pressure aging treatment to simulate the harsh environment in actual use and further stabilize the performance of the capacitors.

[0111] In a specific embodiment, the present application provides an aluminum electrolytic capacitor with an operating voltage of 160V, wherein the formation voltage of the anode foil of the aluminum electrolytic capacitor is 224V, and the breakdown voltage of the cathode foil is 3V.

[0112] Example 1: When other materials are the same, aluminum electrolytic capacitors are manufactured using anode aluminum foils with formation voltages of 1.3 times, 1.4 times, and 1.5 times, respectively. The life test comparison of each aluminum electrolytic capacitor after working at the working voltage is shown. The life test parameters are 105°C for 5000 hours. The parameters are shown in Table 1 below:

[0113] Table 1 Capacitance changes of various aluminum electrolytic capacitors

[0114] Aluminum foil forming voltage Capacity change rate (%) 1.3 times the operating voltage -12.41% 1.4 times the operating voltage -2.65% 1.5 times the operating voltage -1.85%

[0115] It can be seen from the experimental results in Table 1 that insufficient formation voltage of the anode foil will lead to a significant capacity decay after the product life test. Therefore, for medium-voltage electrolytic capacitors, aluminum foil with a working voltage of more than 1.4 times that of the electrolytic capacitor can be selected.

[0116] Example 2: When other materials are the same, cathode aluminum foils with different breakdown voltages are selected to manufacture aluminum electrolytic capacitors, and the life test comparison of each aluminum electrolytic capacitor after working at the working voltage is shown. The life test parameters are 105°C, and the parameters are shown in Table 2 below:

[0117] Table 2 Capacity change rate and service life of various aluminum electrolytic capacitors

[0118] Cathode foil breakdown voltage 5000 hours capacity change rate Maximum life span ≥3V -2.43% 7000 hours ≥1V -8.68% 4000 hours 0V -10.41% 3000 hours

[0119] From the experimental results in Table 2, it can be roughly seen that the life of the electrolytic capacitor manufactured with cathode aluminum foil with a voltage of ≥3V can meet the life of 5000 hours, and the capacity change rate can be maintained at about -3%, which is a small change rate.

[0120] Example 3: When other materials are the same, aluminum electrolytic capacitors are manufactured using EPDM+IIR mixed butyl rubber, EPDM ethylene propylene diene monomer rubber, and IIR butyl rubber as sealing plugs, and the life test comparison of each aluminum electrolytic capacitor after working at the working voltage is shown. The life test parameters are 105°C, and the parameters are shown in Table 3 below:

[0121] Table 3 Service life of various aluminum electrolytic capacitors

[0122] Butyl rubber type Life test results IIR Butyl Rubber After 10,000 hours of testing, the rubber plug showed no abnormality EPDM+IIR mixed butyl rubber After 6000 hours of testing, the rubber plug has no abnormality EPDM After 5000 hours, the rubber plug bulged and cracked

[0123] From the experimental results in Table 3, it can be roughly seen that EPDM+IIR mixed butyl rubber and IIR butyl rubber can meet the product design requirements.

[0124] Taking 160V electrolytic capacitors as an example, the following Table 4 shows the capacity change rate of each electrolytic capacitor after the ripple test endurance test:

[0125] Table 4 Capacity change rate record

[0126]

[0127] Generally, the standard requirement for capacity change rate is within ±20%, wherein the smaller the absolute value of the capacity change rate, the better the product stability.

[0128] It can be seen from the above record table that after the ripple test and the endurance test, the capacity change rate of the electrolytic capacitor of the present application is maintained at about -3%, and the absolute value of the capacity change rate is small, indicating that the product has good stability performance.

[0129] In summary, the medium voltage 160V aluminum electrolytic capacitor used in the automotive electric drive controller of the present application has a durability life of 2.5 times increased from 2000 hours to 5000 hours at 105°C, and the ripple current has increased from 533mA (105°C 120Hz) to 900mA (105°C 120Hz), an increase of more than 60%, so as to improve the reliability of the electrolytic capacitor and thus increase the service life of the electric drive controller. In addition, according to the aluminum electrolytic capacitor of the present application, the temperature range can be -40°C to +105°C, and the temperature stability is relatively high.

[0130] According to a fourth aspect of the present application, an electric drive controller is provided, wherein the electric drive controller includes a controller body and an electrolytic capacitor connected to the controller body, wherein the electrolytic capacitor is an electrolytic capacitor provided according to the above-mentioned embodiment or an electrolytic capacitor manufactured according to the method for manufacturing an electrolytic capacitor provided according to the above-mentioned embodiment.

[0131] In the above embodiments, the description of each embodiment has its own emphasis. For parts that are not described or recorded in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.

[0132] The embodiments described above are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, a person skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present application, and should all be included in the protection scope of the present application.

Claims

1. An electrolytic capacitor, characterized in that: The electrolytic capacitor comprises: case; A core is arranged in the shell, wherein the core is formed by winding cathode foil, electrolytic paper and anode foil stacked in sequence; An electrolyte is attached to the surfaces of the cathode foil and the anode foil; The formation voltage of the anode foil is more than 1.4 times the working voltage of the electrolytic capacitor, and the breakdown voltage of the cathode foil is more than 3V. The working voltage of the electrolytic capacitor is 160V-250V.

2. The electrolytic capacitor according to claim 1, characterized in that: The thickness of the electrolytic paper is 40 microns to 50 microns; and / or the density of the electrolytic paper is 0.7 g / cm 3 -0.8g / cm 3 ; and / or the electrolytic paper is a double-layer fiber composite electrolytic paper.

3. The electrolytic capacitor according to claim 1, characterized in that: The electrolytic capacitor further comprises: an anode lead connected to the anode foil and protruding from the shell; A cathode lead is connected to the cathode foil and protrudes from the casing.

4. The electrolytic capacitor according to claim 3, characterized in that: The shell has an opening, and the core is placed inside the shell through the opening of the shell; The electrolytic capacitor further comprises: a sealing plug comprising butyl rubber, the sealing plug being arranged at the opening of the shell, the sealing plug being used to seal the core in the shell, and the anode lead and the cathode lead being able to pass through the sealing plug and protrude from the shell.

5. The electrolytic capacitor according to claim 1, characterized in that: The anode foil is obtained by subjecting the metal foil with the surface subjected to corrosion treatment to chemical treatment.

6. The electrolytic capacitor according to any one of claims 1 to 5, characterized in that: The electrolyte is an electrolyte including nano-silicon dioxide; in the electrolyte, the weight proportion of the nano-silicon dioxide is 0.8%-1.2%, the flash voltage of the electrolyte is 350V-400V, and the conductivity is 3.8mS / cm-4.8mS / cm.

7. A method for manufacturing an electrolytic capacitor, characterized in that: The method comprises: Providing an anode foil, wherein a formation voltage for forming the anode foil is more than 1.4 times the working voltage of the electrolytic capacitor, and the working voltage of the electrolytic capacitor is 160V-250V; Providing a cathode foil, wherein the breakdown voltage of the cathode foil is above 3V; Providing electrolytic paper, and winding the anode foil, electrolytic paper and cathode foil stacked in sequence into a core; The core is dried and immersed in the electrolyte for impregnation; The core containing the electrolyte is placed in the housing and sealed.

8. The method according to claim 7, characterized in that The electrolyte is an electrolyte including nano-silicon dioxide, wherein the flash voltage of the electrolyte is 350V-400V, and the conductivity is 3.8mS / cm-4.8mS / cm.

9. The method according to claim 8, characterized in that In the electrolyte, the weight proportion of the nano silicon dioxide is 0.8%-1.2%.

10. The method according to claim 7, characterized in that The thickness of the electrolytic paper is 40 microns to 50 microns; and / or the density of the electrolytic paper is 0.7 g / cm 3 -0.8g / cm 3 ; and / or the electrolytic paper is a double-layer fiber composite electrolytic paper.

11. The method according to claim 7, characterized in that The impregnation step is carried out in an impregnation device, wherein during the impregnation process, the impregnation vacuum degree of the impregnation device is set to be above -0.088MPa, the pressure is set to be above 0.2MPa, and the impregnation time is set to be above 8h.

12. The method according to claim 7, characterized in that The immersion temperature is 45°C-55°C.

13. The method according to claim 7, characterized in that The step of placing the core storing the electrolyte into the housing for sealing comprises: The core storing the electrolyte is inserted into the sealing plug and then placed into the shell for sealing.

14. The method according to claim 13, characterized in that The sealing plug comprises butyl rubber, wherein the weight percentage of the butyl rubber in the sealing plug is not less than 28%.

15. The method according to claim 13, characterized in that The sealing plug comprising butyl rubber is a sealing plug of mixed butyl rubber formed by EPDM rubber and butyl rubber; or is a butyl rubber sealing plug.

16. The method according to any one of claims 7 to 15, characterized in that The anode foil is provided, comprising: The metal foil after the corrosion treatment is placed in a forming solution, and a preset forming voltage is applied, wherein the preset forming voltage is more than 1.4 times the working voltage of the electrolytic capacitor.

17. An electric drive controller, characterized in that: The electric drive controller includes a controller body and an electrolytic capacitor connected to the controller body, wherein the electrolytic capacitor is an electrolytic capacitor according to any one of claims 1 to 6 or an electrolytic capacitor manufactured by the method for manufacturing an electrolytic capacitor according to any one of claims 7 to 16.