Lithium metal composite negative electrode and preparation method and application thereof

By modifying the Li/Li3Sb-LiCl composite electrode in lithium metal batteries, the Li/Li3Sb-LiCl composite electrode is solved, and the growth and volume expansion problems of lithium dendrites are achieved, efficient lithium ion transmission and battery stability are achieved, and production is reduced. Cost, suitable for large-scale applications.

CN119069646APending Publication Date: 2024-12-03HUAZHONG UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411387068.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

During the charging and discharging process of lithium metal batteries, there are problems with lithium dendrites, uncontrollable volume expansion and unstable electrode/electrolyte interface, resulting in low efficiency, poor cycle stability and safety problems. Preparation steps for existing modified materials Complex and costly, it is difficult to achieve large-scale application.

Method used

Using a three-dimensional current collector as a matrix, a Cu2Sb alloy modification layer is formed by placing it in an antimony-containing solution, and alloying reaction in molten lithium forms a Li3Sb alloy and LiCl layer to form a Li/Li3Sb-LiCl composite electrode, and the LiCl layer is used to provide protection. and high ionic conductivity.

Benefits of technology

The high Coulombic efficiency and long cycle stability of lithium metal batteries are achieved. Through uniform lithium ion deposition and rapid ion transmission, the impact of lithium metal volume changes on the electrodes is reduced, and the safety and performance of the battery is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069646A_ABST
    Figure CN119069646A_ABST
Patent Text Reader

Abstract

The invention provides a lithium metal composite negative electrode and a preparation method and application thereof. The lithium metal composite negative electrode comprises a three-dimensional copper current collector and Li / Li3Sb-LiCl arranged in the three-dimensional copper current collector. The preparation method comprises the following steps: placing a three-dimensional copper current collector in a SbCl3 solution, and forming Cu2Sb and CuCl2 on the surface of the three-dimensional copper current collector through a replacement reaction; putting the Cu2Sb and CuCl2 into molten lithium, and enabling the molten lithium to react with the Cu2Sb and the CuCl2 to generate Li3Sb and LiCl in situ; wherein lithium-loving Li3Sb is uniformly distributed in a Li-rich phase, LiCl is spontaneously distributed on the surface of the three-dimensional Li / Li3Sb along with charge and discharge to form a protective layer, and the Li / Li3Sb-LiCl composite electrode with a three-dimensional network structure is obtained. The uniform compounding of Li3Sb and Li helps to realize the rapid transmission of Li < + > in the whole composite electrode, and the LiCl protective layer can enhance the stability of the electrode interface, accelerate the transmission rate of Li < + > and form a stable solid electrolyte interface film; meanwhile, the three-dimensional skeleton provides a space for expansion of metal lithium, the stability and small volume change of the electrode structure are maintained, and the stability and safety of the battery are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium metal batteries, and in particular relates to a lithium metal composite negative electrode and a preparation method and application thereof. Background Art

[0002] Lithium metal has a high theoretical specific capacity (3860 mAh g -1 ) and low redox potential (-3.04V), it is considered to be a highly promising negative electrode material for the next generation of high energy density batteries. However, lithium metal still faces problems such as lithium dendrite growth, uncontrollable volume expansion and unstable electrode / electrolyte interface (SEI) in practical applications. Lithium dendrites will pierce the diaphragm during the battery cycle, causing the battery to short-circuit, and in severe cases, cause safety issues. Due to the host-free structure of lithium metal, it undergoes huge volume changes during the repeated charge and discharge of the battery, which will cause the electrode structure to be destroyed and the cycle life of the battery to decay. In addition, the fragile SEI layer produced by the side reactions between the highly reactive lithium metal and the electrolyte will also be continuously destroyed during the growth of lithium dendrites and huge volume changes. These problems cause lithium metal batteries to exhibit low coulombic efficiency, poor cycle stability, and battery safety issues during the charge and discharge process.

[0003] Based on the uncontrollable volume expansion problem of lithium metal during the charge and discharge process, some three-dimensional skeleton materials (such as copper foam, nickel foam, copper mesh, porous copper current collector, carbon nanofiber) have been introduced into the research of lithium metal negative electrodes. Because the three-dimensional skeleton has a large specific surface area and space, it can not only reduce the local current density and uniform electric field to induce uniform lithium deposition, but also the large and stable spatial structure can withstand the huge volume change of lithium metal to improve the stability of the entire electrode. However, some three-dimensional skeletons such as copper foam have relatively poor lithium wettability, so they need to be modified to obtain three-dimensional skeleton materials with good lithium wettability.

[0004] In order to solve the problem of poor lithium wettability of three-dimensional skeleton materials, researchers have reported many modified materials for modifying three-dimensional skeletons. For example, Chinese invention patent CN114975880A discloses a method and application of modifying the surface of copper foam to construct a composite lithium metal negative electrode. A silver-copper foam substrate is prepared by chemical reaction of a silver-containing solution and copper foam, and metallic lithium is further introduced by electrochemical deposition to obtain a composite lithium metal negative electrode, which can effectively inhibit the growth of lithium dendrites and alleviate the volume change of lithium metal. However, the interface problem of unstable electrode still exists, and the synthesis method is time-consuming, the price of silver element is relatively high, which increases equipment investment and production costs, and is not conducive to practical application. In order to further solve the above problems, as reported in the related reports on the modification of three-dimensional skeletons by alloy elements (the preparation method of three-dimensional conductive skeletons, lithium metal composite negative electrodes and surface protective layers, Chinese invention patent CN113380993A), the lithium-philic alloy elements are modified on the surface of the three-dimensional skeleton by a simple magnetron sputtering method, and lithium is infused by hot melting to construct a three-dimensional lithium alloy composite electrode, and further coated on its surface by atomic layer deposition. A layer of inorganic coating layer is finally successfully prepared to prepare a three-dimensional lithium metal composite negative electrode containing a protective layer. The composite negative electrode can alleviate the volume expansion of lithium and has a stable electrode interface. However, on the one hand, the alloy layer in this work only plays a role in enhancing the wettability of lithium. After the introduction of molten lithium, the alloy layer is covered, and the alloy fails to play a further role in the subsequent battery cycle process. On the other hand, the introduction of the protective layer is a non-in-situ means, and the preparation steps are many, which is not conducive to large-scale application. Therefore, how to obtain a three-dimensional current collector and a lithium metal composite negative electrode with stable electrode structure, stable interface, superior performance, low production cost and easy large-scale production has become a technical problem to be solved. Summary of the invention

[0005] The main purpose of the present invention is to provide a lithium metal composite negative electrode and its preparation method and application in view of the problems and shortcomings of the prior art. The lithium metal composite negative electrode has the advantages of high ion conductivity, stable electrode structure and stable interface.

[0006] The technical solution of the present invention is:

[0007] A lithium metal composite negative electrode comprises a three-dimensional current collector and Li metal and Li3Sb alloy filled in the three-dimensional current collector, and the lithium metal composite negative electrode also comprises a LiCl layer coated on the outer surface of the three-dimensional current collector.

[0008] The method for preparing the lithium metal composite negative electrode comprises the following steps:

[0009] placing the three-dimensional current collector in an antimony-containing solution for reaction to obtain a three-dimensional current collector having an antimony-containing alloy modification layer;

[0010] The three-dimensional current collector having the antimony-containing alloy modification layer is placed in molten lithium metal to obtain the lithium metal composite negative electrode, wherein the antimony-containing alloy modification layer is a Cl-containing Cu2Sb alloy modification layer.

[0011] Preferably, the three-dimensional current collector is any one of foam copper, copper mesh, porous copper, copper nanofiber or foam nickel.

[0012] Preferably, the three-dimensional current collector has a thickness of 0.2 to 1.5 mm and a pore size of 0.1 to 0.5 mm.

[0013] Preferably, the concentration of the antimony-containing solution is 0.02-0.08 mol / L.

[0014] Preferably, the three-dimensional current collector is placed in an antimony-containing solution and reacted at 50-100° C. for 10-60 min.

[0015] Preferably, the antimony-containing solution is prepared by placing an antimony-containing reagent in a solvent and stirring until the antimony-containing reagent is uniformly dissolved to obtain the antimony-containing solution.

[0016] Preferably, the antimony-containing reagent is antimony trichloride or antimony trifluoride, and the solvent is dimethyl sulfoxide solution.

[0017] Preferably, the molten lithium metal is prepared by heating the lithium metal on a heating plate at 180-240° C. under the protection of an argon atmosphere to obtain the molten lithium metal.

[0018] The lithium metal composite negative electrode is used in a lithium metal battery.

[0019] The principle of the present invention is as follows: a three-dimensional copper current collector is placed in a SbCl3 solution, and Cu2Sb and CuCl2 are formed on the surface of the three-dimensional copper current collector through a replacement reaction; the three-dimensional copper current collector is placed in molten lithium, and the molten lithium reacts with Cu2Sb and CuCl2 to generate Li3Sb and LiCl in situ; wherein, the lithium-philic Li3Sb is uniformly distributed in the Li-rich phase, and LiCl is spontaneously distributed on the surface of the three-dimensional Li / Li3Sb to form a protective layer as the charge and discharge proceed, thereby obtaining a Li / Li3Sb-LiCl composite electrode with a three-dimensional network structure.

[0020] The beneficial effects of the present invention are as follows: the present invention prepares a lithium metal composite negative electrode by a simple synthesis method, modifies a chlorine-containing Cu2Sb alloy layer on the surface of the foamed copper, further introduces molten lithium, and forms a Li3Sb alloy in situ on the surface of its skeleton through a spontaneous alloying reaction between the molten lithium and the Cu2Sb alloy, and the generated LiCl with high ionic conductivity and electrical insulation is coated on the outermost layer, and finally obtains a three-dimensional LiCl-coated lithium-rich / Li3Sb alloy composite negative electrode. In the three-dimensional composite electrode, the uniform dispersion, lithium affinity and high ion diffusion coefficient of the Li3Sb alloy are conducive to guiding the uniform deposition of lithium metal and accelerating the diffusion kinetics of lithium ions; in addition, the presence of the LiCl protective layer can not only enhance the interface stability, but also further enhance the ion transfer rate of the three-dimensional composite electrode, thereby providing a uniform lithium ion transfer channel; the effective use of the three-dimensional skeleton, its stable framework and large space can slow down the volume change of lithium metal, which is conducive to enhancing the stability of the lithium metal battery in the subsequent cycle process. The synergistic effect between the above advantages finally realizes a lithium metal battery with high coulomb efficiency and long cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 It is a schematic diagram of the preparation process of the present invention.

[0022] Figure 2 The SEM morphology images of the current collector Cu2Sb-Cl@Cu foam current collector prepared in Example 1 of the present invention, the Cufoam current collector prepared in Comparative Example 1, and the Cu2Sb@Cu foam current collector prepared in Comparative Example 2;

[0023] (a) SEM image of Cu foam current collector; (b) SEM image of Cu2Sb@Cu foam current collector; (c) SEM image of Cu2Sb-Cl@Cufoam current collector; (d) SEM partial enlargement image of Cu foam current collector; (e) SEM partial enlargement image of Cu2Sb@Cu foam current collector; (f) SEM partial enlargement image of Cu2Sb-Cl@Cu foam current collector; EDS distribution diagram of (g) Cu, (h) Sb and (i) Cl elements of Cu2Sb-Cl@Cu foam current collector.

[0024] Figure 3 A half-cell assembled by matching the current collector Li3Sb-LiCl@Cu foam current collector prepared in Example 1 of the present invention, the Cu foam current collector prepared in Comparative Example 1, and the Li3Sb@Cu foam current collector prepared in Comparative Example 2 with lithium metal, a nucleation overpotential test graph of the first lithium deposition at different current densities and a comparative bar graph thereof;

[0025] (a) Li3Sb-LiCl@Cu foam current collector, Li3Sb@Cu foam current collector and pure Cu foam current collector at 0.5mAcm -2 Nucleation overpotential test under current density; (b) Li3Sb-LiCl@Cu foam current collector, Li3Sb@Cu foam current collector and pure Cu foam current collector at 1.0 mA cm -2 Nucleation overpotential test under current density; (c) Li3Sb-LiCl@Cufoam current collector, Li3Sb@Cu foam current collector and pure Cu foam current collector at 2.0mAcm -2 Nucleation overpotential test under current density; (d) Li3Sb-LiCl@Cu foam current collector, Li3Sb@Cu foam current collector and pure Cu foam current collector at 3.0mAcm -2 Nucleation overpotential test under current density; (e) Li3Sb-LiCl@Cu foam current collector, Li3Sb@Cu foam current collector and pure Cu foam current collector at 5.0mAcm -2 Nucleation overpotential test under current density; (f) Bar chart comparing the nucleation overpotential of Li3Sb-LiCl@Cufoam current collector, Li3Sb@Cu foam current collector and pure Cu foam current collector at different current densities.

[0026] Figure 4 The half-cell assembled by matching the current collector Li3Sb-LiCl@Cu foam current collector prepared in Example 1 of the present invention, the Cu foam current collector prepared in Comparative Example 1 and the Li3Sb@Cu foam current collector prepared in Comparative Example 2 with lithium metal, at 1.0 mA cm -2 Coulombic efficiency test under current density.

[0027] Figure 5 The three-dimensional lithium metal composite negative electrode formed by the current collector Cu2Sb-Cl@Cu foam current collector prepared in Example 1 of the present invention, the Cufoam current collector prepared in Comparative Example 1 and the Cu2Sb@Cu foam current collector prepared in Comparative Example 2 and lithium metal, namely, a symmetrical battery assembled by Li / Li3Sb-LiCl@Cu foam, Li@Cu foam and Li / Li3Sb@Cu foam, has a high conductivity at 1.0 mA cm -2 Cyclic stability test at current density and its corresponding cycle time-polarization potential line graph, as well as EIS curve graph;

[0028] (a) Symmetric cells assembled from Li / Li3Sb-LiCl@Cu foam, Li@Cu foam, and Li / Li3Sb@Cu foam at 1.0 mA cm -2 Cyclic stability test under 5.0 mA cm-1; (b) Polarization potential line graph of symmetrical batteries assembled with Li / Li3Sb-LiCl@Cu foam and Li / Li3Sb@Cu foam at different test times; (c) Symmetric batteries assembled with Li / Li3Sb-LiCl@Cu foam, Li@Cufoam and Li / Li3Sb@Cu foam at 5.0 mA cm-1 -2 Cyclic stability test under 400 nm; (d) Electrochemical impedance spectroscopy of symmetrical batteries assembled with Li / Li3Sb-LiCl@Cu foam, Li@Cu foam and Li / Li3Sb@Cu foam.

[0029] Figure 6 The three-dimensional lithium metal composite negative electrode formed by the current collector Cu2Sb-Cl@Cu foam current collector prepared in Example 1 of the present invention, the Cufoam current collector prepared in Comparative Example 1, and the Cu2Sb@Cu foam current collector prepared in Comparative Example 2 and lithium metal, i.e., full batteries assembled by matching Li / Li3Sb-LiCl@Cu foam, Li@Cu foam and Li / Li3Sb@Cu foam with commercial lithium iron phosphate, cycle stability test and rate performance test at 1C, and EIS curves before and after cycling;

[0030] (a) Li / Li3Sb-LiCl@Cu foam, Li@Cu foam and Li / Li3Sb@Cu foam are matched with lithium iron phosphate to obtain the cycle stability test of the full battery at 1C rate; (b) Li / Li3Sb-LiCl@Cu foam, Li@Cu foam and Li / Li3Sb@Cu foam are matched with lithium iron phosphate to obtain the rate performance test of the full battery at 0.5, 1, 2 and 3C; (c) Li / Li3Sb-LiCl@Cu foam, Li@Cu foam and Li / Li3Sb@Cu foam are matched with lithium iron phosphate to obtain the electrochemical impedance spectroscopy of the full battery before cycling; (d) Li / Li3Sb-LiCl@Cu foam, Li@Cu foam and Li / Li3Sb@Cu foam are matched with lithium iron phosphate to obtain the electrochemical impedance spectroscopy of the full battery after cycling. DETAILED DESCRIPTION

[0031] The principles and features of the present invention are described below in conjunction with examples, which are only used to explain the present invention and are not intended to limit the scope of the present invention. In addition, it is worth noting that the raw materials involved in the present invention are all common commercial products unless otherwise specified.

[0032] Example 1

[0033] like Figure 1 As shown, this embodiment provides a method for preparing a lithium metal composite negative electrode, comprising the following steps:

[0034] (1) The area is 25cm 2 The commercial copper foam was ultrasonically cleaned in anhydrous ethanol, dilute hydrochloric acid and ultrapure water, and dried in a 60℃ forced air oven for later use.

[0035] (2) Place 1.0 mmol of antimony trichloride reagent in 20 ml of dimethyl sulfoxide solvent and stir at 25°C until the antimony trichloride is uniformly dissolved in the solvent to obtain a concentration of 0.05 mol / L -1 of antimony trichloride solution;

[0036] (3) placing the copper foam obtained in step (1) into the antimony trichloride solution obtained in step (2), reacting at 80° C. for 30 min, and then vacuum drying at 60° C. for 12 h to obtain a Cu2Sb alloy-modified copper foam current collector (Cu2Sb-Cl@Cu foam);

[0037] (4) In a glove box, commercial lithium metal foil is placed in a container and heated on a hot plate at 200° C. to melt it, and the Cu2Sb-Cl@Cu foam current collector obtained in step (3) is placed therein, and the molten lithium reacts with the current collector in situ to form a Li3Sb with a three-dimensional skeleton and a lithium-rich composite negative electrode (Li / Li3Sb-LiCl@Cu foam).

[0038] (5) Assembling a battery with the Li / Li3Sb-LiCl@Cu foam negative electrode obtained in step (4), wherein the counter electrode in the half-cell is a commercial lithium metal foil, the counter electrode in the symmetric cell is a Li / Li3Sb-LiCl@Cu foam negative electrode, and the positive electrode material in the full cell is lithium iron phosphate; in all the battery components, the separator is a commercial PP film, and the concentration of the electrolyte is 1 molL -1 , wherein the lithium salt is LiTFSI and the solvent is DOL / DME solution.

[0039] Example 2

[0040] This example uses the same experimental raw materials and conditions as Example 1, except that the amount of antimony trichloride is changed in step (2), specifically:

[0041] (1) The area is 25cm 2 The commercial copper foam was ultrasonically cleaned in anhydrous ethanol, dilute hydrochloric acid and ultrapure water, and dried in a 60℃ forced air oven for later use.

[0042] (2) Place 0.6 mmol of antimony trichloride reagent in 20 ml of dimethyl sulfoxide solvent and stir at 25°C until the antimony trichloride is uniformly dissolved in it to obtain a concentration of 0.03 mol / L -1 of antimony trichloride solution;

[0043] Steps (3) to (5) are the same as those in Example 1 and will not be repeated here.

[0044] Example 3

[0045] This example uses the same experimental raw materials and conditions as Example 1, except that the amount of antimony trichloride is changed in step (2), specifically:

[0046] (1) The area is 25cm 2 The commercial copper foam was ultrasonically cleaned in anhydrous ethanol, dilute hydrochloric acid and ultrapure water, and dried in a 60℃ forced air oven for later use.

[0047] (2) Place 0.8 mmol of antimony trichloride reagent in 20 ml of dimethyl sulfoxide solvent and stir at 25°C until the antimony trichloride is uniformly dissolved in it to obtain a concentration of 0.04 mol / L -1 of antimony trichloride solution;

[0048] Steps (3) to (5) are the same as those in Example 1 and will not be repeated here.

[0049] Example 4

[0050] This example uses the same experimental raw materials and conditions as Example 1, except that the amount of antimony trichloride is changed in step (2), specifically:

[0051] (1) The area is 25cm 2 The commercial copper foam was ultrasonically cleaned in anhydrous ethanol, dilute hydrochloric acid and ultrapure water, and dried in a 60℃ forced air oven for later use.

[0052] (2) Place 1.2 mmol of antimony trichloride reagent in 20 ml of dimethyl sulfoxide solvent and stir at 25°C until the antimony trichloride is uniformly dissolved in it to obtain a concentration of 0.06 mol / L -1 of antimony trichloride solution;

[0053] Steps (3) to (5) are the same as those in Example 1 and will not be repeated here.

[0054] Example 5

[0055] This example uses the same experimental raw materials and conditions as Example 1, except that the amount of antimony trichloride is changed in step (2), specifically:

[0056] (1) The area is 25cm 2 The commercial copper foam was ultrasonically cleaned in anhydrous ethanol, dilute hydrochloric acid and ultrapure water, and dried in a 60℃ forced air oven for later use.

[0057] (2) Place 1.4 mmol of antimony trichloride reagent in 20 ml of dimethyl sulfoxide solvent and stir at 25°C until the antimony trichloride is uniformly dissolved in it to obtain a concentration of 0.07 mol / L -1 of antimony trichloride solution;

[0058] Steps (3) to (5) are the same as those in Example 1 and will not be repeated here.

[0059] Example 6

[0060] This example uses the same experimental raw materials and conditions as Example 1, except that the type of antimony-containing reagent is changed in step (2), specifically:

[0061] (1) The area is 25cm 2 The commercial copper foam was ultrasonically cleaned in anhydrous ethanol, dilute hydrochloric acid and ultrapure water, and dried in a 60℃ forced air oven for later use.

[0062] (2) Place 1.0 mmol of antimony trifluoride reagent in 20 ml of dimethyl sulfoxide solvent and stir at 25°C until antimony trifluoride is uniformly dissolved in it to obtain a concentration of 0.05 mol / L -1 of antimony trifluoride solution;

[0063] Steps (3) to (5) are the same as those in Example 1 and will not be repeated here.

[0064] Example 7

[0065] This example uses the same experimental materials and conditions as Example 1, except that the heating temperature is changed in step (4), specifically:

[0066] Steps (1) and (3) are the same as those in Example 1 and will not be repeated here;

[0067] (4) In a glove box, commercial lithium metal foil is placed in a container, heated on a hot plate at 180° C. to melt it, and the Cu2Sb-Cl@Cu foam current collector obtained in step (3) is placed therein, and the molten lithium reacts with the current collector in situ to form a Li3Sb with a three-dimensional skeleton and a lithium-rich composite negative electrode (Li / Li3Sb-LiCl@Cu foam);

[0068] (5) The steps are the same as those in Example 1 and will not be repeated here.

[0069] Example 8

[0070] This example uses the same experimental materials and conditions as Example 1, except that the heating temperature is changed in step (4), specifically:

[0071] Steps (1) and (3) are the same as those in Example 1 and will not be repeated here;

[0072] (4) In a glove box, commercial lithium metal foil is placed in a container, heated on a hot plate at 220° C. to melt it, and the Cu2Sb-Cl@Cu foam current collector obtained in step (3) is placed therein, and the molten lithium reacts with the current collector in situ to form a Li3Sb with a three-dimensional skeleton and a lithium-rich composite negative electrode (Li / Li3Sb-LiCl@Cu foam);

[0073] (5) The steps are the same as those in Example 1 and will not be repeated here.

[0074] Example 9

[0075] This example uses the same experimental materials and conditions as Example 1, except that the heating temperature is changed in step (4), specifically:

[0076] Steps (1) and (3) are the same as those in Example 1 and will not be repeated here;

[0077] (4) In a glove box, commercial lithium metal foil is placed in a container, heated on a hot plate at 240° C. to melt it, and the Cu2Sb-Cl@Cu foam current collector obtained in step (3) is placed therein, and the molten lithium reacts with the current collector in situ to form a Li3Sb with a three-dimensional skeleton and a lithium-rich composite negative electrode (Li / Li3Sb-LiCl@Cu foam);

[0078] (5) The steps are the same as those in Example 1 and will not be repeated here.

[0079] In order to compare the excellent functions of the three-dimensional lithium metal composite negative electrode Li / Li3Sb-LiCl@Cu foam of the present invention, such as inhibiting lithium dendrites, the following comparative example is set:

[0080] Comparative Example 1

[0081] The area is 25cm 2 The foamed copper was ultrasonically cleaned in anhydrous ethanol, dilute hydrochloric acid and ultrapure water, and dried in a 60°C blast oven for later use. Since the lithium affinity of the foamed copper is poor, it is difficult for molten lithium to be loaded onto the foamed copper skeleton. Therefore, the lithium metal in this comparative example 1 was introduced by electrodeposition.

[0082] Comparative Example 2

[0083] This comparative example uses the same experimental materials and conditions as Example 1, except that a cleaning step is added in step (3), specifically:

[0084] Steps (1) and (2) are the same as those in Example 1 and will not be repeated here;

[0085] (3) placing the copper foam obtained in step (1) into the antimony trichloride solution obtained in step (2), reacting at 80° C. for 30 min, washing the copper foam after the reaction with dimethyl sulfoxide, and then vacuum drying at 60° C. for 12 h to obtain a Cu2Sb alloy-modified copper foam current collector (Cu2Sb@Cu foam);

[0086] (4) In a glove box, commercial lithium metal foil is placed in a container, heated on a hot plate at 200° C. to melt it, and the Cu2Sb@Cu foam current collector obtained in step (3) is placed therein, and the molten lithium reacts with the current collector in situ to form a Li3Sb with a three-dimensional skeleton and a lithium-rich composite negative electrode (Li / Li3Sb@Cu foam);

[0087] (5) Assembling a battery with the Li / Li3Sb@Cu foam negative electrode obtained in step (4), wherein the counter electrode in the half-cell is a commercial lithium metal foil, the counter electrode in the symmetric cell is a Li / Li3Sb@Cu foam negative electrode, and the positive electrode material in the full cell is lithium iron phosphate; in all the battery components, the separator is a commercial PP film, and the concentration of the electrolyte is 1 molL -1 , wherein the lithium salt is LiTFSI and the solvent is DOL / DME solution.

[0088] The following is a description of the detection and analysis of the above embodiments and comparative examples:

[0089] The three-dimensional lithium metal composite negative electrode Li / Li3Sb-LiCl@Cu foam prepared in Examples 1-9 of the present invention can control the alloy element content of the Cu2Sb-Cl@Cu foam current collector and the preparation time of the current collector by controlling the amount, type and reaction temperature of the antimony-containing reagent. At the same time, the preparation process is easy to operate, low in cost, highly repeatable and easy to prepare on a large scale.

[0090] The Cu2Sb-Cl@Cu foam current collector prepared in Example 1 of the present invention, the foam Cu current collector prepared in Comparative Example 1 and the Cu2Sb@Cu foam current collector prepared in Comparative Example 2 were subjected to morphological observation and component analysis. The results are as follows: Figure 2As shown, the SEM plan view and the corresponding local enlarged view show that the Cu2Sb-Cl alloy material prepared in Example 1 is distributed on the surface of the foam copper in a granular form, and the modified layer is uniform and dense, indicating that the Cu2Sb-Cl@Cu foam is successfully prepared.

[0091] The Cu2Sb-Cl@Cu foam current collector prepared in Example 1 of the present invention, the foam Cu current collector prepared in Comparative Example 1, and the Cu2Sb@Cu foam current collector prepared in Comparative Example 2 were matched with lithium metal to form a half-cell, and the nucleation overpotential test under different current densities was performed. The results are as follows: Figure 3 As shown, whether it is 0.5, 1.0, 2.0, 3.0 or 5.0mAcm -2 At a current density of , compared with the foam Cu current collector, both Li3Sb@Cu foam and Li3Sb-LiCl@Cu foam current collectors exhibit lower nucleation overpotentials, among which the nucleation overpotential of Li3Sb-LiCl@Cu foam current collector is even lower. On the one hand, this shows that the Cu2Sb modification layer can effectively reduce the nucleation overpotential of lithium metal, which is beneficial to further induce the uniform deposition of lithium ions. On the other hand, the introduction of LiCl further improves the ionic conductivity of the modification layer. Therefore, compared with the pure Cu2Sb modification layer, the Cu2Sb modification layer containing LiCl exhibits the lowest nucleation overpotential.

[0092] The Cu2Sb-Cl@Cu foam current collector prepared in Example 1 of the present invention, the foam Cu current collector prepared in Comparative Example 1, and the Cu2Sb@Cu foam current collector prepared in Comparative Example 2 were matched with lithium metal to form a half-cell, and the coulombic efficiency was tested. The results are as follows: Figure 4 As shown, at 1.0mAcm -2 At the current density, Li3Sb-LiCl@Cu foam current collector exhibits higher Coulombic efficiency and longer cycle stability. Li3Sb alloy has a lower ion diffusion barrier, which helps to reduce the interface impedance and uniform interface electric field and Li + The enhanced electrochemical performance can be attributed to the following aspects: its 3D skeleton has ample space and large surface area, which not only accommodates the volume change of lithium metal, but also helps to reduce the local current density and uniform the electric field distribution. At the same time, the high ionic conductivity of LiCl enables efficient lithium ion transport. In addition, the lithiophilic Li3Sb alloy is conducive to uniform Li deposition and stripping repeatability.

[0093] The three-dimensional lithium metal composite negative electrode Li / Li3Sb-LiCl@Cu foam prepared in Example 1 of the present invention, the Li@Cu foam prepared in Comparative Example 1 and the Li / Li3Sb@Cu foam prepared in Comparative Example 2 were matched with themselves to assemble into Li / Li3Sb-LiCl@Cufoam||Li / Li3Sb-LiCl@Cu foam, Li@Cu foam||Li@Cu foam and Li / Li3Sb@Cu foam||Li / Li3Sb@Cu foam symmetrical batteries, and the cycle stability, polarization potential and electrochemical impedance tests were carried out. The results are as follows Figure 5 As shown, at 1.0mAcm -2 Under the current density, the three-dimensional lithium metal composite negative electrode Li / Li3Sb-LiCl@Cu foam showed longer cycle stability, lower polarization potential, and lower impedance. LiCl coated on the surface of the composite electrode has high ionic conductivity and electrical insulation properties, which can enhance the interface stability and make Li + The diffusion impedance is low, which is beneficial to Li + Rapid spreading and uniform deposition.

[0094] The three-dimensional lithium metal composite negative electrode Li / Li3Sb-LiCl@Cu foam prepared in Example 1 of the present invention, the Li@Cu foam prepared in Comparative Example 1 and the Li / Li3Sb@Cu foam prepared in Comparative Example 2 were matched with commercial lithium iron phosphate to form LFP||Li / Li3Sb-LiCl@Cu foam, LFP||Li@Cu foam and LFP||Li / Li3Sb@Cu foam full batteries, and cycle stability tests, rate performance tests at different current densities and electrochemical impedance tests before and after cycling were performed on them. The results are as follows: Figure 6 As shown, it can be seen that LFP||Li / Li3Sb-LiCl@Cu foam achieves higher discharge specific capacity, better rate performance and lower electrochemical impedance. The three-dimensional lithium composite electrode has abundant contact interfaces between Li3Sb alloy and lithium, which helps to achieve rapid transmission of lithium ions in the entire composite electrode, greatly improving the lithium ion transmission rate, thereby improving the rate performance of the battery; at the same time, LiCl is coated on the surface of the three-dimensional composite electrode, which greatly enhances the interface stability, and the high mechanical strength of the three-dimensional skeleton itself. The stable framework and large space can withstand the volume change of lithium metal, maintain the stability of the electrode structure, and thus make the battery show better electrochemical performance.

[0095] It should be noted that, for those skilled in the art, several modifications and improvements can be made without departing from the concept of the present invention, and these modifications and improvements all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A lithium metal composite negative electrode, characterized in that: The lithium metal composite negative electrode comprises a three-dimensional current collector and Li metal and Li3Sb alloy filled in the three-dimensional current collector, and the lithium metal composite negative electrode further comprises a LiCl layer coated on the outer surface of the three-dimensional current collector.

2. The method for preparing a lithium metal composite negative electrode according to claim 1, characterized in that: The following steps are involved: placing the three-dimensional current collector in an antimony-containing solution for reaction to obtain a three-dimensional current collector having an antimony-containing alloy modification layer; The three-dimensional current collector having the antimony-containing alloy modification layer is placed in molten lithium metal to obtain the lithium metal composite negative electrode, wherein the antimony-containing alloy modification layer is a Cl-containing Cu2Sb alloy modification layer.

3. The preparation method according to claim 2, characterized in that: The three-dimensional current collector is any one of foam copper, copper mesh, porous copper, copper nanofiber or foam nickel.

4. The preparation method according to claim 2, characterized in that: The three-dimensional current collector has a thickness of 0.2 to 1.5 mm and a pore size of 0.1 to 0.5 mm.

5. The preparation method according to claim 2, characterized in that: The concentration of the antimony-containing solution is 0.02-0.08 mol / L.

6. The preparation method according to claim 2, characterized in that: The three-dimensional current collector is placed in an antimony-containing solution at 50-100° C. for a reaction of 10-60 minutes.

7. The preparation method according to claim 2, characterized in that: The antimony-containing solution is prepared by placing an antimony-containing reagent in a solvent and stirring until the antimony-containing reagent is uniformly dissolved to obtain the antimony-containing solution.

8. The preparation method according to claim 7, characterized in that: The antimony-containing reagent is antimony trichloride or antimony trifluoride, and the solvent is dimethyl sulfoxide solution.

9. The preparation method according to claim 2, characterized in that: The molten lithium metal is prepared by heating the lithium metal on a heating plate at 180-240° C. under the protection of an argon atmosphere to obtain the molten lithium metal.

10. Use of the lithium metal composite negative electrode as claimed in claim 1 in a lithium metal battery.