Method for secondary granulation in homogenizing process of sodium ion battery positive electrode material

By using a planetary defoaming mixer to perform multiple stirring treatments during the homogenization of the positive electrode material of sodium ion battery, the electrochemical performance reduction and production difficulties caused by the size of Prussian blue particles in traditional technology are solved, and cost-effective electrochemistry is achieved Performance improvement and simplify production processes.

CN119069651AInactive Publication Date: 2024-12-03WENZHOU NATECH NEW ENERGY TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411549775.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-01
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the homogenization technology of the positive electrode material of traditional sodium ion battery, Prussian blue particles with larger particle sizes lead to reduced electrochemical performance and difficulty in production, and the preparation process of single crystal Prussian blue is complex and costly, which limits its industrial application.

Method used

The secondary granulation method is adopted during the homogenization process. By adding positive electrode material, binder, zirconium beads and conductive agents to the planetary defoaming mixer, performing multiple stirring treatments, significantly reducing the particle size and increasing electricity. Chemical properties.

Benefits of technology

It significantly improves the homogenization effect and electrochemical performance of the positive electrode material, simplifies the production process, reduces costs, and is suitable for large-scale production and application of sodium ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069651A_ABST
    Figure CN119069651A_ABST
Patent Text Reader

Abstract

The invention provides a secondary granulation method in a sodium-ion battery positive electrode material homogenizing process, which comprises the following steps: S1, adding a positive electrode material and a binder into a planetary defoaming stirrer according to a certain proportion, then adding zirconium beads with different diameters or different numbers, and stirring for the first time to finish primary granulation; s2, adding a conductive agent and deionized water into the powder obtained in the step S1 to regulate and control the solid content of the slurry, and changing the particle size of the material by using a mechanochemical method; and S3, adding glycerol into the mixed slurry obtained in the step S2, and continuously mechanically stirring for 10-20 minutes by using the planetary defoaming stirrer to finish secondary granulation. Compared with the prior art, the secondary granulation method in the anode material homogenizing process has the advantages that the zirconium beads are added and stirred for multiple times in the homogenizing process, so that the homogenizing effect of the anode material is remarkably improved, the particle size of the material is reduced through secondary granulation, and the rate capability and the cycle performance are effectively improved. In addition, according to the homogenizing method, the production process is simplified, the production cost is reduced, and large-scale production and application of the sodium ion battery are facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of sodium ion batteries, and in particular relates to a method for secondary granulation in a sodium ion battery positive electrode material homogenization process. Background Art

[0002] As a sustainable energy storage solution, sodium-ion batteries have attracted much attention due to their wide range of raw materials and low cost. Although sodium-ion batteries have the potential for wide application in theory, they still face many technical challenges in the actual production process. Electrode materials are an important component of the performance of sodium-ion batteries and also their largest source of cost. Therefore, the development of cost-effective electrode materials is crucial for the large-scale commercial application of sodium-ion batteries. As one of the effective positive electrode materials for sodium-ion batteries, the control of Prussian blue particle size during the homogenization process is particularly critical.

[0003] In the traditional sodium-ion battery positive electrode material homogenization technology, larger Prussian blue particles will extend the migration path of sodium ions and electrons, thereby reducing its charge and discharge rate. In addition, in the traditional wet pulping process, larger Prussian blue particles are easily affected by the environment after drying, and the particles are easy to absorb water and moisture, which increases the viscosity of the slurry, making it difficult to coat, affecting the uniformity of the electrode surface density and the consistency of battery performance.

[0004] Although existing technologies attempt to solve these problems by regulating the morphology and particle size of Prussian blue during the synthesis process, such as controlling the crystal size and morphology to reduce cracks and fractures between particles, these methods are often complicated to operate, costly, and difficult to implement on a large scale. In particular, the preparation of single-crystal Prussian blue can improve the cycle life and stability of batteries, but the complexity and high cost of its production process limit its application in industrial production. Summary of the invention

[0005] Based on this, in order to address the above problems, the present application provides a method for secondary granulation during the homogenization process, which can not only significantly reduce the particle size, but also effectively solve the problems of reduced electrochemical performance and production difficulties caused by particle size through improved homogenization technology.

[0006] In order to achieve the above-mentioned purpose of the present invention, the following technical scheme is adopted: S1: Add the positive electrode material, binder and zirconium beads into a planetary degassing mixer and mix them preliminarily; S2: adding a conductive agent and deionized water to the powder obtained in step S1, and preliminarily mixing the powder and the conductive agent using a planetary deaerator; S3: Adjust the speed of the planetary deaerator to make the slurry evenly stirred; S4: After adding glycerol to the slurry obtained in S3, stirring using a planetary deaerator; S5: Adjust the rotation speed of the planetary deaerator to deaerate the slurry.

[0007] In step S1, the mixing includes stirring.

[0008] Preferably, the rotation speed of the stirring process is 1000-2000 rpm, the rotation speed is 900-1800 rpm, and the stirring process time is 60-180s.

[0009] Further, step S1 includes at least one of the following features (1)-(3); (1) The binder includes but is not limited to polyacrylic acid; (2) The mass of the zirconium beads is 1-10 g; (3) The number of the zirconium beads is 1-10.

[0010] In step S2, the rotation speed of the stirring process is 500-1000 rpm, the rotation speed is 450-900 rpm, and the stirring time is 10-100 s.

[0011] Further, step S2 includes at least one of the following features (1)-(3); (1) The conductive agent includes any one of carbon nanotubes, graphene, Ketjen black, Super-P (SP), acetylene black (AB), or a combination of at least two thereof; (2) The deionization process adjusts the solid content of the slurry to 30%-45%.

[0012] In step S3, the rotation speed of the stirring process is 1200-1700 rpm, the rotation speed is 600-1000 rpm, and the stirring process time is 240 s.

[0013] In step S4, the mass of the glycerol is 10-100 mg.

[0014] Preferably, the rotation speed of the stirring treatment is 1200-1700 rpm, the rotation speed is 1200-1500 rpm, and the stirring treatment time is 200-400 s.

[0015] In step S5, the rotation speed of the degassing treatment is 1200-1700 rpm, the rotation speed is 0-100 rpm, and the degassing treatment time is 100-200 s.

[0016] The present invention is beneficial in that: The method for secondary granulation during the homogenization of the positive electrode material provided by the present invention not only significantly improves the homogenization effect of the positive electrode material by adding zirconium beads and stirring multiple times during the homogenization process, but also reduces the particle size of the material by secondary granulation, thereby effectively improving the rate performance and cycle performance. In addition, the homogenization method of the present invention simplifies the production process, reduces the production cost, and is conducive to the large-scale production and application of sodium ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 This is a comparison chart of the cycle performance test of sodium ion batteries prepared by using the positive electrode slurry of the embodiment and the comparative example of the present invention; Figure 2 This is a comparison chart of the rate performance test of sodium ion batteries prepared by using the positive electrode slurries of the embodiment and the comparative example of the present invention; Figure 3 The SEM images of the positive electrode slurries of Example 1 and Comparative Example 1 of the present invention are shown; Figure 4 The SEM images of the positive electrode sheets coated with the positive electrode slurries of Example 1 and Comparative Example 1 of the present invention are shown; Figure 5 The SEM images of the positive electrode slurries of Example 2 and Comparative Example 2 of the present invention are shown; Figure 6 This is a SEM image of the positive electrode sheet after coating with the positive electrode slurry of Example 2 and Comparative Example 2 of the present invention. DETAILED DESCRIPTION

[0018] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.

[0019] Example 1 S1: The raw material ratio of the positive electrode slurry is: iron-manganese-based Prussian blue A, graphene, carbon nanotubes, and polyacrylic acid in a weight percentage of 91.5:5:1:2.5; S2: Prussian blue, polyacrylic acid and zirconium beads were added into a planetary degassing mixer and mixed evenly. The rotation speed was 1594 rpm, the rotation speed was 1434.6 rpm, and the stirring time was 120 s. S3: adding graphene, carbon nanotubes and deionized water to the powder obtained in S2, and preliminarily stirring in a planetary deaerator, with a rotational speed of 852 rpm, a rotational speed of 766.8 rpm, and a stirring time of 30 s; S4: Adjust the speed of the planetary deaerator to make the slurry evenly stirred, the rotational speed is 1594 rpm, the rotational speed is 797 rpm, and the stirring time is 240 s; S5: adding glycerol to the slurry obtained in S3, stirring in a planetary deaerator, with a rotation speed of 1594 rpm, a rotation speed of 1434.6 rpm, and a stirring time of 360 s; S6: Adjust the rotation speed of the planetary deaerator to deaerate the slurry. The rotation speed is 1594 rpm, the rotation speed is 0 rpm, and the deaeration time is 120 s.

[0020] Example 2 The only difference between this embodiment and embodiment 1 is that the formula of Prussian blue is different, hereinafter referred to as iron-manganese-based Prussian blue B, and the other conditions and parameters are exactly the same as those in embodiment 1.

[0021] Comparative Example 1: (Compared with the present invention, the addition of zirconium beads is less) S1: The raw material ratio of the positive electrode slurry is: iron-manganese-based Prussian blue A, graphene, carbon nanotubes, and polyacrylic acid in a weight percentage of 91.5:5:1:2.5; S2: Prussian blue and polyacrylic acid were added into a planetary degassing mixer and mixed evenly. The rotation speed was 1594 rpm, the rotation speed was 1434.6 rpm, and the stirring time was 120 s. S3: adding graphene, carbon nanotubes and deionized water to the powder obtained in S2, and preliminarily stirring in a planetary deaerator, with a rotational speed of 852 rpm, a rotational speed of 766.8 rpm, and a stirring time of 30 s; S4: Adjust the speed of the planetary deaerator to make the slurry evenly stirred, the rotational speed is 1594 rpm, the rotational speed is 797 rpm, and the stirring time is 240 s; S5: adding glycerol to the slurry obtained in S3, stirring in a planetary deaerator, with a rotation speed of 1594 rpm, a rotation speed of 1434.6 rpm, and a stirring time of 360 s; S6: Adjust the rotation speed of the planetary deaerator to deaerate the slurry. The rotation speed is 1594 rpm, the rotation speed is 0 rpm, and the deaeration time is 120 s.

[0022] Comparative Example 2 The difference between this comparative example and comparative example 1 is that the formula of Prussian blue is different. This comparative example uses iron-manganese-based Prussian blue B, and the other conditions and parameters are exactly the same as those of comparative example 1.

[0023] Performance Test: The positive electrode slurries prepared in Example 1-2 and Comparative Example 1-2 were assembled into sodium ion batteries for performance testing. The experimental data are as follows: (1) Cycle performance of sodium ion batteries The sodium batteries prepared with the positive electrode slurries of Examples 1 and 2 and Comparative Examples 1 and 2 were subjected to cycle charge and discharge tests. The test results are as follows: Figure 1 shown.

[0024] from Figure 1 It can be seen that the cyclic discharge curve of the sodium ion battery prepared with the positive electrode slurry of Examples 1 and 2 of the present invention is flatter than that of the sodium ion battery prepared with the positive electrode slurry of Comparative Examples 1 and 2, and descends more slowly from right to left, has a higher capacity retention rate, and has a long cycle life, indicating that the cyclic discharge performance of the sodium ion battery prepared with the positive electrode slurry of the embodiment of the present invention is improved compared with the comparative example.

[0025] (2) Rate performance of sodium ion batteries The sodium batteries prepared with the positive electrode slurries of Examples 1 and 2 and Comparative Examples 1 and 2 were subjected to rate discharge tests. The test results are as follows: Figure 2 shown.

[0026] from Figure 2 It can be seen that the various rate discharge capacities of Examples 1 and 2 of the present invention are higher than those of Comparative Examples 1 and 2, indicating that the rate performance of the sodium ion battery prepared by the positive electrode slurry obtained by the secondary granulation method of the present invention is significantly improved.

[0027] The above disclosure is only the preferred embodiment of the present invention, which certainly cannot be used to limit the scope of the present invention. Therefore, equivalent changes made according to the claims of the present invention are still within the scope of the present invention.

Claims

1. A method for secondary granulation during the homogenization process of a positive electrode material for a sodium ion battery, characterized in that: The method comprises the following steps: S1, adding positive electrode material and binder into a planetary degassing mixer, and then adding zirconium beads of different diameters or different quantities for first stirring to complete primary granulation; S2, adding a conductive agent and deionized water to the powder obtained in step S1 to adjust the solid content of the slurry, and using a mechanochemical method to change the particle size of the material; S3, adding glycerol into the mixed slurry obtained in step S2, and continuing mechanical stirring for 10-20 minutes using a planetary degassing mixer to complete secondary granulation.

2. The method for secondary granulation in the homogenization process of the positive electrode material of a sodium ion battery according to claim 1, characterized in that: The mass of the zirconium beads is 1-10 g; the number of the zirconium beads is 1-10.

3. The method for secondary granulation in the homogenization process of the positive electrode material of a sodium ion battery according to claim 1, characterized in that: The conductive agent includes any one of carbon nanotubes, graphene, Ketjen black, Super-P (SP), and acetylene black (AB), or a combination of at least two of them.

4. The method for secondary granulation in the homogenization process of the positive electrode material of a sodium ion battery according to claim 1, characterized in that: Deionized water is used to adjust the solid content of the slurry to 30%-45%.

5. The method for secondary granulation in the homogenization process of the positive electrode material of a sodium ion battery according to claim 1, characterized in that: The added mass percentage of glycerol is 0.1%-2%.

Citation Information

Patent Citations

  • Preparation method of lithium iron phosphate electrode

    CN103400964A

  • Preparation method of three-dimensional porous composite pole piece for flexible lithium ion battery

    CN107742695A

  • Positive electrode slurry, preparation method thereof and lithium ion battery

    CN115050949A

  • Positive electrode slurry of sodium ion battery and preparation method of positive electrode slurry

    CN118073523A

  • Aqueous homogenization process for positive electrode system of lithium-ion battery, slurry and lithium-ion battery

    WO2024120497A1