Battery, battery pack, electronic equipment and energy storage system

By doping inactive metal elements into the positive electrode material of sodium ion batteries and using phosphate coating, the cycle stability and metal element dissolution problems of layered oxide materials are solved, and higher battery stability and safety are achieved , especially in high temperature environments.

CN119069653APending Publication Date: 2024-12-03HUAWEI DIGITAL POWER TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310628555.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-30
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Laminated oxide materials have poor circulation stability in sodium ion batteries, especially in high temperature environments, severe cycle life attenuation, and metal element dissolution problems, affecting battery safety.

Method used

Using a core material doped with the first inactive metal element and a phosphate cladding material, the gradient structure is formed to improve the positive electrode material by gradually increasing the concentration of the active metal element and reducing the concentration of the second inactive metal element in the core material. Structural stability and reduce the risk of metal element dissolution by phosphate coating.

Benefits of technology

It significantly improves the cycle stability, cycle life and voltage of the positive electrode material, enhances the safety of the battery, and performs more significantly in high temperature environments, extending the service life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069653A_ABST
    Figure CN119069653A_ABST
Patent Text Reader

Abstract

The invention provides a battery, a positive electrode plate of the battery comprises a positive electrode active material layer, the positive electrode active material layer comprises a positive electrode material, the positive electrode material comprises a core material and a coating layer material coating the surface of the core material, the core material is a metal oxide, and a first inactive metal element is doped in the core material, and the coating layer is made of phosphate. The invention also provides a battery pack and electronic equipment using the battery, and an energy storage system using the battery pack. The first inactive metal element is doped in the positive electrode material, and the surface of the positive electrode material is coated with the phosphate coating material, so that the positive electrode material has relatively high structural stability, and dissolution of the metal elements is effectively reduced, so that the battery shows relatively good cycle stability, relatively long cycle life and relatively high voltage; and meanwhile, the use safety of the battery is also improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of battery technology, and in particular to a battery, a battery pack and electronic equipment using the battery, and an energy storage system using the battery pack. Background Art

[0002] As a new generation of green energy storage devices, the commonly used positive electrode materials of sodium-ion batteries include layered oxides. Layered oxide materials are considered to be the first materials to be commercialized due to their advantages such as high gram capacity, simple synthesis process and high compaction density.

[0003] However, in practical applications, it is found that the cycle stability of layered oxide materials is poor, especially in high temperature environments, where the cycle life is severely attenuated; in addition, layered oxide materials also have the problem of metal element dissolution, which can pose a hidden danger to battery safety. Summary of the invention

[0004] In view of this, in order to solve at least one of the above defects, an embodiment of the present application provides a battery, the positive electrode plate of the battery can improve the cycle stability and voltage of the battery, extend the cycle life of the battery, and improve the safety of battery use.

[0005] In addition, embodiments of the present application also provide a battery pack and electronic device using the above-mentioned battery, and an energy storage system using the above-mentioned battery pack.

[0006] The first aspect of the embodiment of the present application provides a battery, which includes a positive electrode plate, a negative electrode plate and a separator, wherein the separator is arranged between the positive electrode plate and the negative electrode plate, the positive electrode plate includes a current collector and a positive electrode active material layer arranged on the current collector, and the positive electrode active material layer includes a positive electrode material. Among them, the positive electrode material includes a core material and a coating layer material coated on the surface of the core material, the core material is a metal oxide, the coating layer material is a phosphate, and the core material is doped with a first inactive metal element. Among them, the first inactive metal element is doped into the core material after molding by doping. The core material contains an active metal element and a second inactive metal element, and the concentration of the active metal element gradually increases from the surface of the core material to the core of the core material, and the concentration of the second inactive metal element gradually decreases from the surface of the core material to the core of the core material.

[0007] By doping the first inactive metal element in the core material, the first inactive metal element will not participate in the charge and discharge reaction, and can play an effective structural support role, stabilize the structure of the core material, and then optimize the layered structure of the positive electrode material, effectively inhibit the harmful phase transformation of the positive electrode material during the cycle (especially at high voltage), which is beneficial to improve the stability of the positive electrode material; in addition, by doping the first inactive metal element in the core material, the problem of uneven stress inside the core material during the cycle can also be reduced to reduce the formation of microcracks inside the core material, so as to further improve the stability of the positive electrode material. Therefore, after doping the first inactive metal element in the core material, it is beneficial to improve the cycle stability, cycle life and voltage of the positive electrode sheet, so that the battery has both high cycle stability (especially high voltage cycle stability), long cycle life and high voltage.

[0008] By coating the surface of the core material with a phosphate coating material, not only is the risk of contact between the metal elements in the core material and the electrolyte reduced, the dissolution of the metal elements is reduced, and the safety of the battery is improved, but also the interface side reactions between the positive electrode plate using the positive electrode material and the electrolyte are reduced, and the risk of generating a passivation layer at the interface between the positive electrode plate and the electrolyte is reduced, thereby ensuring smooth ion transmission, so as to improve the cycle stability and cycle life (especially the cycle life in a high temperature environment) of the battery using the positive electrode material; in addition, phosphate contains PO bonds with strong bond energy, is not easy to lose oxygen atoms in the electrolyte, has higher structural stability, and is conducive to further reducing interface side reactions.

[0009] Specifically, the general formula of the core material can be: ɑ X γ Y β O2, ɑ is 0.9-1.1, γ+β=1, wherein A can be a sodium ion or a lithium ion, X is an active metal element, and Y is a second inactive metal element.

[0010] In the core material, the active metal element can participate in the electrochemical reaction, which can increase the specific capacity of the positive electrode material to meet the needs of high energy density; and the addition of the second inactive metal element can play a structural support role in the layered metal oxide, which can delay or inhibit the formation of phase change, so that the positive electrode material has higher safety and structural stability. In addition, by gradually increasing the concentration of the active metal element from the surface layer to the core of the core material, the concentration of the second inactive metal element gradually decreases from the surface layer to the core of the core material, that is, the concentration of the active metal element on the surface layer of the core material is low, while the concentration of the second inactive metal element is high, which is conducive to further reducing the risk of dissolution of the active metal element.

[0011] Therefore, the positive electrode material of the embodiment of the present application has high structural stability and can reduce the dissolution of metal elements, so that the battery using the positive electrode material has good cycle stability, long cycle life, high voltage, and high safety in use.

[0012] Furthermore, the active metal element is at least one selected from metal elements such as iron, cobalt, nickel, vanadium, copper and chromium. The second inactive metal element is at least one selected from metal elements such as manganese and niobium.

[0013] Furthermore, in the core material, the molar ratio of the active metal element to the second inactive metal element is 9:1 to 6:4. For example, the molar ratio may be 9:1, 8:2, 7:3 or 6:4.

[0014] In combination with the first aspect, in some possible embodiments, the first inactive metal element is selected from Ca 2+ 、Zn 2+ Mg 2+ 、Ti 3+ 、Al 3+ 、Na + and Li + When the core material is a sodium-containing oxide, the first inactive metal element is not Na + When the core material is a lithium-containing oxide, the first inactive metal element is not Li + .

[0015] By using the first inactive metal element to dope the core material, since the ion radius of this type of inactive metal element is closer to the transport ions in the core material (such as Li + Or Na + ) radius, such as the active metal elements listed above (such as Ni 2+ ) is more likely to occupy the position of the transport ions, and the structural support is stronger, which is more conducive to limiting the transport ions in the core material (such as Li + Or Na + ) and active metal elements (such as Ni 2+ ) to improve the structural stability of the core material.

[0016] In combination with the first aspect, in some possible embodiments, the doping concentration of the first inactive metal element gradually decreases from the surface layer of the core material to the core of the core material.

[0017] By designing the doping concentration of the doping element to gradually decrease from the surface of the core material to the core of the core material, the first inactive metal element is distributed in a non-uniform gradient state, which can ensure that the first inactive metal element optimizes the layered structure of the core material and improves the stability of the core material structure. At the same time, it can effectively reduce the doping amount of the first inactive metal element, improve the purity of the core material, and reduce the impact of the doping of the first inactive metal element on the electrochemical properties of the core material.

[0018] In combination with the first aspect, in some possible embodiments, the molar ratio of the core material to the first inactive metal element is 1:(0.0001-0.04), further 1:(0.0001-0.01), further 1:(0.0001-0.005), further 1:(0.0001-0.001). Exemplarily, the molar ratio of the core material to the first inactive metal element can be 1:0.001, 1:0.005, 1:0.01, etc.

[0019] If the doping amount of the first inactive metal element is too low, it cannot play a good structural support role and has a weak effect on optimizing the layered structure of the core material. If the doping amount of the first inactive metal element is too high, too much of the first inactive metal element will reduce the purity of the core material, affect ion transport, and reduce the specific capacity of the positive electrode material. Therefore, the embodiment of the present application can improve the purity of the core material while achieving the premise of improving the structural stability of the core material, so as to reduce the influence of the doping of the first inactive metal element on the electrochemical performance of the positive electrode material.

[0020] In combination with the first aspect, in some possible embodiments, the phosphate contains at least two phosphate groups and / or at least one pyrophosphate group.

[0021] Phosphates containing at least two phosphate groups and / or at least one pyrophosphate group have a higher PO bond content, and the PO bond energy is relatively strong and it is not easy to lose oxygen atoms, thereby making the structural stability of the coating layer material higher and less likely to react with the electrolyte, which is beneficial to further improve the stability of the positive electrode material.

[0022] In combination with the first aspect, in some possible embodiments, the molecular formula of the phosphate is: x R y (PO4) a (P2O7) b , wherein A is a sodium ion or a lithium ion; R is selected from at least one of the elements Fe, V, Ti, Mn, Co, etc.; the values ​​of x, y, a and b can satisfy the algebraic sum of positive and negative valences in the molecular formula of the phosphate to be zero.

[0023] Phosphate contains sodium or lithium elements, so the coating layer material is a sodium or lithium storage material. This type of coating layer material is used to modify the surface of sodium oxide positive electrode materials or lithium oxide positive electrode materials, which is beneficial to reduce interfacial side reactions while not sacrificing the capacity of the positive electrode material.

[0024] Furthermore, the core material is a sodium oxide, and the phosphate is selected from at least one of Na2FeP2O7, Na3Fe2(PO4)P2O7, Na3V2Fe(PO4)3, Na3VMn2Fe(PO4)3, Na3VTiFe(PO4)3, Na3Fe2Fe(PO4)3 and Na3MnTiFe(PO4)3.

[0025] In combination with the first aspect, in some possible embodiments, the average particle size of the particles of the coating layer material is 40nm~90nm, further 50~70. Exemplarily, the average particle size of the particles of the coating layer material can be 40nm, 45nm, 50nm, 55nm, 60nm, 65nm, 70nm, 75nm, 80nm, 85nm, 90nm or a value between any two of the above values.

[0026] By controlling the particle size of the coating layer material, it is advantageous to form a coating layer with uniform thickness and uniform coating on the surface of the core material, so as to fully isolate the core material and the electrolyte.

[0027] In combination with the first aspect, in some possible embodiments, the mass ratio of the coating layer material to the positive electrode material is 1% to 40%, further 5% to 20%. Exemplarily, the mass ratio of the coating layer material to the positive electrode material is 1%, 5%, 10%, 20%, 30% or 40%, etc.

[0028] When the content of the coating material is too much, the coating thickness is too thick, which affects the ion transmission, and also reduces the proportion of the core material, so that the capacity of the positive electrode material is reduced; when the content of the coating material is too little, a uniform and effective coating layer cannot be formed, and the effect on reducing the interface side reaction is not obvious. Therefore, the embodiment of the present application controls the content of the coating material in the positive electrode material within the above range, on the one hand, a positive electrode material with excellent surface morphology can be obtained after coating, and the coating thickness is moderate, which is conducive to reducing the interface side reaction, and has a positive effect on the capacity and ion transmission of the positive electrode material. In addition, the metal element in the core material and the oxygen element in the coating material are bonded to form a chemical bond, and the chemical bond can be an ionic bond, a covalent bond, etc., for example: Mn-O. Since the core material and the coating material are combined together by solid phase grinding and microwave treatment to form a modified positive electrode material, it can promote the bonding reaction between the oxygen element in the coating material and the metal element in the core material, produce chemical bonds such as Mn-O, and then enhance the bonding force between the coating material and the core material.

[0029] The second aspect of the embodiment of the present application provides a battery pack, which includes a plurality of batteries as described above, wherein the plurality of batteries are connected in series or in parallel to a diaphragm. Since the positive electrode plate in the above battery is conducive to improving the cycle stability, overall cycle life, voltage and use safety of the battery, it is conducive to improving the service life and use safety of the battery pack using the above battery.

[0030] The third aspect of the embodiment of the present application provides an electronic device, the electronic device includes a housing and a battery as described above, the battery being installed in the housing. Since the positive electrode sheet in the battery is conducive to improving the battery cycle stability, overall cycle life, voltage and use safety, it is conducive to improving the service life and use safety of the electronic device using the battery.

[0031] The fourth aspect of the embodiment of the present application provides an energy storage system, including a power converter and the above-mentioned battery pack. The power converter is used to perform power conversion on the voltage output by the battery pack, and / or the power converter is used to perform power conversion on the voltage output by an external power source and output it to the battery pack. Since the positive electrode plate in the above-mentioned battery is conducive to improving the battery cycle stability, overall cycle life, voltage and safety of use, it is conducive to improving the service life and safety of use of the energy storage system using the above-mentioned battery pack. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 It is a schematic diagram of the structure of the positive electrode material provided in one embodiment of the present application.

[0033] Figure 2 It is a schematic diagram of the structure of the positive electrode plate provided in one embodiment of the present application.

[0034] Figure 3 It is a schematic diagram of the structure of a battery provided in one embodiment of the present application.

[0035] Figure 4 It is a schematic diagram of the structure of a battery pack provided in one embodiment of the present application.

[0036] Figure 5 It is a schematic diagram of the structure of an electronic device provided in one embodiment of the present application.

[0037] Figure 6 It is a curve graph showing the concentration of Ni, Fe and Mn in the core material of Example 1 as the distance from the center of the core material surface layer changes.

[0038] Fig. 7A It is the cycle performance curve (positive electrode median voltage stability test) of the half-cell prepared by using the positive electrode materials of Example 1 (after improvement) and Comparative Example 1 (before improvement).

[0039] Figure 7B It is the cycle performance curve (cycle stability test) of the half-cell prepared by using the positive electrode materials of Example 1 (after improvement) and Comparative Example 1 (before improvement).

[0040] Figure 8 This is a scanning electron microscope photograph of the positive electrode material of Comparative Example 1.

[0041] Fig. 9 This is a scanning electron microscope photograph of the positive electrode material of Example 1 of the present application.

[0042] Main component symbols

[0043] Positive electrode 100

[0044] Current Collectors 101

[0045] Positive electrode active material layer 102

[0046] Positive electrode material 10

[0047] Core material 1

[0048] Coating material 2

[0049] Battery 200

[0050] Negative electrode 201

[0051] Diaphragm 202

[0052] Electrolyte 203

[0053] Battery Pack 300

[0054] Electronic equipment 400

[0055] Housing 401 DETAILED DESCRIPTION

[0056] The following specific embodiments illustrate the implementation of the present application, and those skilled in the art can easily understand other advantages and effects of the present application from the contents disclosed in this specification. Although the description of the present application will be introduced in conjunction with the embodiments, this does not mean that the features of this application are limited to the implementation. On the contrary, the purpose of introducing the application in conjunction with the implementation is to cover other options or modifications that may be extended based on the claims of the present application. In order to provide a deep understanding of the present application, the following description will include many specific details. The present application can also be implemented without using these details. In addition, in order to avoid confusion or blurring the focus of the present application, some specific details will be omitted in the description. It should be noted that the embodiments in the present application and the features in the embodiments can be combined with each other without conflict.

[0057] Hereinafter, if used, the terms "first", "second", etc. are used for descriptive purposes only and are not to be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, a feature defined as "first", "second", etc. may explicitly or implicitly include one or more of the feature. In the description of this application, unless otherwise specified, "multiple" means two or more.

[0058] The embodiments of the present application are described below in conjunction with the accompanying drawings in the embodiments of the present application. The data range values ​​recorded in the present application should include the end values ​​unless otherwise specified.

[0059] Layered oxide sodium ion positive electrode materials have poor cycle stability, especially in high temperature environments where the cycle life is severely reduced; in addition, layered oxide materials also have problems with metal element dissolution and electrode degradation, and the dissolution of metal elements will pose a hidden danger to battery safety.

[0060] In view of this, an embodiment of the present application provides a battery, which includes a positive electrode sheet, a negative electrode sheet and a separator, the separator is arranged between the positive electrode sheet and the negative electrode sheet, the positive electrode sheet includes a current collector and a positive electrode active material layer arranged on the current collector, and the positive electrode active material layer includes a positive electrode material. After the positive electrode material is modified, the structural stability is stronger and the metal elements are not easily dissolved. The positive electrode material can be used as an active material of the positive electrode in a sodium ion battery or a lithium ion battery, but is not limited thereto. The battery using the positive electrode material has good cycle stability, a long cycle life, a high voltage, and high safety in use.

[0061] The positive electrode material provided in the embodiment of the present application includes a core material and a coating layer material coated on the surface of the core material, the core material is a metal oxide, and the core material is doped with a first inactive metal element; in addition, the coating layer material is a phosphate.

[0062] in,

[0063] The core material is a layered metal oxide material containing an active metal element and a second inactive metal element. Specifically, the core material may have a general formula of: A ɑ X γ Y β O2, where ɑ ranges from 0.9 to 1.1, γ+β=1, and in order to satisfy the algebraic sum of positive and negative valences in the above molecular formula to be zero, the values ​​of ɑ, γ, and β can satisfy A ɑ X γ Y β It has a valence of -4, A can be a sodium ion or a lithium ion, X is an active metal element, and Y is a second inactive metal element. Further, the active metal element is selected from at least one of iron, cobalt, nickel, vanadium, copper and chromium, and these active metal elements exist in the core material in the form of ions; the second inactive metal element is selected from at least one of manganese (Mn) and niobium (Nb), and these inactive metal elements exist in the core material in the form of ions. For example, the general formula of the core material can be Na ɑ Ni x Fe y Mn β O2, ɑ ranges from 0.9 to 1.1, x+y+β=1. Among them, "active metal elements" refer to metal elements that participate in electrochemical reactions. Such metal elements will change their valence during the charge and discharge process. For example, taking iron as an example, the iron element in the core material is usually Fe 3+ , Fe 3+ It reacts with the electrolyte and easily turns into Fe 4+ , and then dissolved from the core material; "inactive metal elements" refer to: metal elements that do not participate in electrochemical reactions. The valence state of such metal elements will not change during the charge and discharge process. Inactive metal elements mainly play a structural support role. In the core material, the aforementioned active metal elements can participate in electrochemical reactions, which can increase the specific capacity of the positive electrode material to meet the needs of high energy density; and the addition of the second inactive metal element can play a structural support role in the layered metal oxide, which can delay or inhibit the formation of phase change, making the positive electrode material have higher safety and structural stability.

[0064] In some embodiments, the concentration of the active metal element gradually increases from the surface of the core material to the core of the core material, and the concentration of the second inactive metal element gradually decreases from the surface of the core material to the core of the core material. Active metal elements (such as nickel and iron) are active and are prone to valence changes when in contact with the electrolyte, causing the active metal elements to dissolve, resulting in reduced stability of the positive electrode material. The second inactive metal element (such as manganese) can play a role in structural support. The concentration of the active metal element is gradually increased from the surface of the core material to the core, and the concentration of the second inactive metal element is gradually reduced from the surface of the core material to the core, that is, the concentration of the active metal element on the surface of the core material is low, while the concentration of the second inactive metal element is high, which is conducive to further reducing the risk of active metal element dissolution and improving the stability of the positive electrode material.

[0065] In some embodiments, in the core material, the molar ratio of the active metal element to the second inactive metal element is 9:1 to 6:4. For example, the molar ratio may be 9:1, 8:2, 7:3 or 6:4.

[0066] The core material is doped with a first inactive metal element, which does not participate in the charge and discharge reaction and does not change its valence state during the charge and discharge process. The first non-metal element is added to the core material to achieve effective structural support to stabilize the structure of the core material, thereby optimizing the layered structure of the positive electrode material, effectively inhibiting the harmful phase transition of the positive electrode material during the cycle (especially at high voltage), and helping to improve the stability of the positive electrode material. In addition, by doping the core material with the first inactive metal element, the problem of uneven stress inside the core material during the cycle can also be reduced to reduce the formation of microcracks inside the core material, so as to further improve the stability of the positive electrode material. Therefore, after the core material is doped with the first inactive metal element, it is beneficial to improve the cycle stability, cycle life and voltage of the positive electrode material.

[0067] In some embodiments, the content of the first inactive metal element in the core material can be uniformly distributed or non-uniformly distributed. Specifically, in the embodiment of the present application, the doping concentration of the first inactive metal element gradually decreases from the surface of the core material to the core of the core material to form a non-uniform gradient distribution morphology. And this non-uniform gradient distribution morphology mainly depends on the doping method of the first inactive metal element. In the embodiment of the present application, the first inactive metal element is directly mixed with the prepared core material. At this time, the first inactive metal element will be preferentially doped into the interlayer of the core material that has formed a fixed structure. Moreover, the usual layered metal oxide core material is a spherical particle with a certain particle size. The amount of the first inactive metal element doped into the positive electrode material will gradually decrease with the increase of the doping depth, thereby forming a non-uniform gradient distribution state. By designing the doping concentration of the doping element to gradually decrease from the surface of the core material to the core of the core material, the first inactive metal element is distributed in a non-uniform gradient state, which can ensure that the first inactive metal element optimizes the layered structure of the core material and improves the stability of the core material structure. At the same time, it can effectively reduce the doping amount of the first inactive metal element, improve the purity of the core material, and reduce the impact of the doping of the first inactive metal element on the electrochemical properties of the core material.

[0068] In some embodiments, the first inactive metal element doped may be selected from Ca 2+ 、Zn 2+ Mg 2+ 、Ti 3+ 、Al 3+ 、Na + and Li + When the core material is a sodium-containing oxide (i.e., the battery is a sodium ion battery and the transported ions are sodium ions), the first inactive metal element is not Na + When the core material is a lithium-containing oxide (i.e., the battery is a lithium-ion battery and the transported ions are lithium ions), the first inactive metal element is not Li + By doping the core material with the first inactive metal element, since the ion radius of this type of inactive metal element is closer to the transport ions in the core material (such as Li + Or Na + ) radius, such as the active metal elements listed above (such as Ni 2+ ) is more likely to occupy the position of the transport ions, and the structural support is stronger, which is more conducive to limiting the transport ions in the core material (such as Li + Or Na + ) and active metal elements (such as Ni 2+) to improve the structural stability of the core material.

[0069] In some embodiments, the core material is first prepared, and then the first inactive metal element is doped into the core material by doping, wherein the active metal element and the second inactive metal element are the main elements of the core material, and the amount of the doped first inactive metal element is much lower than that of the first inactive metal element. Specifically, in the core material, the molar ratio of the core material to the first inactive metal element is 1:(0.0001-0.04), further 1:(0.0001-0.01), further 1:(0.0001-0.005), further 1:(0.0001-0.001). Exemplarily, the molar ratio of the core material to the first inactive metal element can be 1:0.001, 1:0.005, 1:0.01, etc. If the doping amount of the first inactive metal element is too low, it cannot play a good structural support role and has a weak effect on optimizing the layered structure of the core material. If the doping amount of the first inactive metal element is too high, too much of the first inactive metal element will reduce the purity of the core material, affect ion transmission, and reduce the specific capacity of the positive electrode material. Therefore, how to reduce the doping amount of the first inactive metal element under the premise of ensuring that the core material has an excellent layered structure and improving the structural stability of the core material has become a research focus of the embodiment of the present application. To this end, the embodiment of the present application can effectively reduce the doping amount of the first inactive metal element by doping the first inactive metal element after the core material is synthesized and forming a non-uniform gradient distribution state, and control the molar ratio of the core material to the first inactive metal element within a low content range of 1: (0.0001-0.04), especially 1: (0.001-0.01), so that the purity of the core material can be improved while achieving the premise of improving the structural stability of the core material, so as to reduce the influence of the doping of the first inactive metal element on the electrochemical properties of the positive electrode material.

[0070] In order to reduce the interface side reaction between the positive electrode plate and the electrolyte, and further reduce the dissolution of metal elements on the surface of the core material, the layered oxide core material is coated with a phosphate coating material. The coating layer material not only reduces the risk of contact between the metal elements in the core material and the electrolyte, reduces the dissolution of metal elements, and improves the safety of battery use, but also reduces the interface side reaction between the positive electrode plate and the electrolyte using the positive electrode material, and reduces the risk of generating a passivation layer at the interface between the positive electrode plate and the electrolyte, thereby ensuring smooth ion transmission, so as to improve the cycle stability and cycle life (especially the cycle life in high temperature environment) of the battery using the positive electrode material; in addition, phosphate contains PO bonds, which have strong bond energy, are not easy to lose oxygen atoms in the electrolyte, and have higher structural stability, which is conducive to further reducing interface side reactions.

[0071] In some embodiments, the phosphate contains at least two phosphates and / or at least one pyrophosphate. The phosphate containing at least two phosphates and / or at least one pyrophosphate has a high content of PO bonds, and the PO bond energy is relatively strong, and it is not easy to lose oxygen atoms, so that the structural stability of the coating material is higher, and it is less likely to have side reactions with the electrolyte, which is conducive to further improving the stability of the positive electrode material.

[0072] Specifically, the molecular formula of phosphate can be: x R y (PO4) a (P2O7) b , wherein A is a sodium ion or a lithium ion; R is selected from at least one of Fe, V, Ti, Mn, Co and other elements; and the values ​​of x, y, a and b can satisfy the algebraic sum of positive and negative valences in the molecular formula of phosphate to be zero. Phosphates contain sodium or lithium elements, so the coating layer material is a sodium or lithium storage material. The use of such coating layer materials to modify the surface of sodium oxide positive electrode materials or lithium oxide positive electrode materials is beneficial to reduce interface side reactions while not sacrificing the capacity of the positive electrode material.

[0073] In some embodiments, when the core material is a sodium-containing oxide, the phosphate can be selected from at least one of Na2FeP2O7, Na3Fe2(PO4)P2O7, Na3V2Fe(PO4)3, Na3VMn2Fe(PO4)3, Na3VTiFe(PO4)3, Na3Fe2Fe(PO4)3 and Na3MnTiFe(PO4)3. The above phosphates have a large number of PO bonds and strong bond energy, which can make the phosphate coating layer more stable. The coating layer material is a sodium storage material containing sodium ions, which modifies the surface of the positive electrode material containing sodium ions, which is beneficial to reduce the interface side reactions while not sacrificing the capacity of the positive electrode material.

[0074] In some embodiments, the average particle size of the coating material is 40nm to 90nm, further 50 to 70. Exemplarily, the average particle size of the coating material can be 40nm, 45nm, 50nm, 55nm, 60nm, 65nm, 70nm, 75nm, 80nm, 85nm, 90nm or any two values ​​above. By controlling the particle size of the phosphate, it is beneficial to form a coating layer with uniform thickness and uniform coating on the surface of the core material to fully isolate the core material and the electrolyte.

[0075] In some embodiments, the mass ratio of the coating material to the positive electrode material is 1% to 40%, and further 5% to 20%. Exemplarily, the mass ratio of the coating material to the positive electrode material is 1%, 5%, 10%, 20%, 30% or 40%, etc. When the content of the coating material is too much, the coating thickness is too thick, which affects the ion transmission, and also reduces the proportion of the core material, so that the capacity of the positive electrode material is reduced; when the content of the coating material is too little, a uniform and effective coating layer cannot be formed, and the effect of reducing the interface side reaction is not obvious. Therefore, the embodiment of the present application controls the content of the coating material in the positive electrode material within the above range. On the one hand, a positive electrode material with excellent surface morphology can be obtained after coating, and the coating thickness is moderate, which is conducive to reducing the interface side reaction, and has a positive effect on the capacity and ion transmission of the positive electrode material.

[0076] In some embodiments, after the core material is formed, the coating material is coated on the surface of the core material by solid phase grinding and microwave treatment. The coating of the coating material on the surface of the core material can be made more uniform by solid phase grinding. Microwave treatment can also form chemical bonds (such as ionic bonds, covalent bonds, etc.) between the metal elements (such as manganese) in the core material and the oxygen elements in the coating material, such as Mn-O, so that in addition to hydrogen bonds and intermolecular forces between the coating material and the core material, the above chemical bonds are also included, and the binding force of the coating material on the surface of the core material is stronger and is not easy to fall off into the electrolyte.

[0077] By making the concentration of active metal elements in the core material distributed in a gradient, doping magnesium and calcium elements in the core material, and coating the surface of the core material with a phosphate coating material, the positive electrode material can have a higher structural stability, thereby showing better cycle stability and longer cycle life, while reducing the dissolution of metal elements in the positive electrode material and increasing the voltage of the positive electrode material. The battery using this positive electrode material has a cycle life of more than 30% in a high temperature environment, and can effectively inhibit the dissolution of transition metal elements.

[0078] Taking the nickel-iron-manganese ternary positive electrode material required for sodium ion batteries as an example, the preparation method of the positive electrode material is specifically introduced, and the method comprises the following steps:

[0079] In the first step, nickel source, iron source and manganese source are co-precipitated to prepare a precursor with a concentration gradient.

[0080] Wherein: the nickel source is nickel sulfate, the iron source is ferrous sulfate or hydrated ferrous sulfate, and the manganese source is manganese sulfate or hydrated manganese sulfate. The molar ratio of the nickel source, the iron source, and the manganese source is 1:1:1. Among them, Ni, Fe, and Mn have a concentration gradient from the surface of the material to the core of the grain.

[0081] In the second step, the precursor obtained in the first step is dried, and then the sodium source and the doping element are added, ball-milled and mixed evenly, and then solid-phase sintered into single crystal particles to obtain the core material.

[0082] After the precursor material is dried, the sodium source and the precursor are mixed in a molar ratio of (0.9-1.2):1, and then 1000-10000ppm of doping elements are added, ball milled and mixed evenly, and solid phase sintered into single crystal particles. Wherein: the sodium source is sodium carbonate or hydrated sodium carbonate.

[0083] In the third step, phosphate is used as a coating layer, which is quickly ball-milled and mixed with the single crystal core material obtained in the second step, and then subjected to microwave treatment to obtain a phosphate-coated single crystal layered oxide positive electrode material.

[0084] Among them, ball milling parameters: 1000-5000 r / min, ball milling n0.5-2h, microwave heating parameters: temperature 150-500°C, heating time: 3-10min.

[0085] See also Figure 1 , is a schematic diagram of a positive electrode material provided in an embodiment of the present application, wherein the positive electrode material 10 comprises a core material 1 and a coating material 2 uniformly coated on the surface of the core material. The core material 1 is the aforementioned core material, and the coating material 2 is the aforementioned coating material.

[0086] See also Figure 2 , is a schematic diagram of a positive electrode plate provided in an embodiment of the present application, and the positive electrode plate 100 includes the positive electrode material as described above.

[0087] The positive electrode sheet 100 of the embodiment of the present application includes a current collector 101 and a positive electrode active material layer 102 disposed on the current collector 101 , and the positive electrode active material layer 102 includes the aforementioned positive electrode material.

[0088] See also Figure 3 , is a schematic diagram of a battery provided in an embodiment of the present application, wherein the battery 200 comprises a positive electrode sheet 100, a negative electrode sheet 201, a separator 202 and an electrolyte 203, wherein the separator 202 is disposed between the positive electrode sheet 100 and the negative electrode sheet 201. The battery 200 may be a sodium ion battery, and the shape is not limited to a cylindrical, soft-pack, square shell, etc.

[0089] Based on the same technical concept, an embodiment of the present application also provides a battery pack comprising a plurality of the aforementioned batteries, wherein the plurality of batteries in the battery pack may be connected in series or in parallel.

[0090] See also Figure 4The battery pack 300 includes a plurality of the aforementioned batteries 200, and any two batteries 200 are connected in series or in parallel. The battery pack 300 can be applied to an energy storage system, which also includes a power converter. The power converter is electrically connected to the battery pack, and the power converter is used to convert the voltage output by the battery pack to a power grid or a load, and / or to convert the voltage output by an external power source to a power output by the battery pack. The energy storage battery pack can be used in the fields of UPS backup power supply, site energy storage, smart photovoltaics, data center batteries, and power batteries.

[0091] The use of the above-mentioned positive electrode material is beneficial to improving the overall cycle stability, cycle life and voltage of the battery, while also improving the safety of the battery.

[0092] Based on the same technical concept, the embodiment of the present application also provides an electronic device, which includes a housing and the aforementioned battery installed in the housing. The electronic device can be, for example, a consumer electronic product, such as a mobile phone, a tablet computer, a mobile power supply, a portable computer, a notebook computer, and other wearable or movable electronic devices, or a vehicle, an energy storage device, a base station, and other devices, but is not limited thereto.

[0093] See also Figure 5 , the electronic device 400 of the embodiment of the present application includes a housing 401 and the aforementioned battery 200 (300) installed in the housing 401.

[0094] In this embodiment, the electronic device 400 may be a mobile phone. The use of the aforementioned battery 200 can effectively increase the standby time and service life of this type of consumer electronic device 400, while also improving the safety of use.

[0095] In other embodiments, the electronic device 400 may be an electric car. The use of the battery 300 can effectively improve the cruising range and service life of the electronic device 300 such as an electric car, while improving the safety of use.

[0096] The technical solution of the embodiment of the present application is further explained below through specific examples.

[0097] Example 1

[0098] Positive electrode material 1: The molecular formula of the core material is: NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 The O2 doping elements are: Ga, Zn, the coating layer material is: Na3Fe2(PO4)P2O7, and the average particle size of the coating layer material is: 50nm.

[0099] like Figure 6As shown, in Example 1, Ni, Fe, and Mn have a concentration gradient from the surface to the core of the core material.

[0100] Example 2

[0101] Cathode material 2: The molecular formula of the core material is: NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2, doping elements are: Ti, Zn, coating material is: Na3V2Fe(PO4)3, and the average particle size of the coating material is: 40nm.

[0102] Example 3

[0103] Positive electrode material 3: The molecular formula of the core material is: NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2, the doping elements are: Ga, Mg, Zn, the coating material is: Na2FeP2O7, and the average particle size of the coating material is: 80nm.

[0104] Comparative Example 1

[0105] Cathode MaterialNaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2, Ni, Fe, Mn have no concentration gradient design, no doping elements and coating materials.

[0106] Comparative Example 2

[0107] Cathode MaterialNaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2, Ni, Fe, Mn have no concentration gradient design, doping elements are: Ga, Mg, Zn, and there is no coating layer material.

[0108] Comparative Example 3

[0109] Cathode MaterialNaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2, Ni, Fe, Mn have no concentration gradient design, no doping elements, coating material Na3Fe2(PO4)P2O7, and the average particle size of the coating layer material is 50nm.

[0110] Preparation of half-cell:

[0111] The positive electrode material (active material) prepared in Example 1, carbon black (Super-P, conductive agent) and a binder (polyvinylidene fluoride and 1-methyl-2-pyrrolidone gel in a mass ratio of 1:9) were mixed, and then N-methylpyrrolidone was added and ball-milled to obtain a mixed slurry.

[0112] The mixed slurry is evenly coated on the carbon-coated aluminum foil by using an automatic coating machine, the coated aluminum foil is placed in a forced air drying oven for drying, and then transferred to a vacuum drying oven for vacuum drying and then taken out to obtain a positive electrode sheet.

[0113] After the positive electrode sheet is rolled by a roller press, it is cut into a sheet with a diameter of 12 mm for standby use. The prepared positive electrode sheet is transferred to a glove box to prepare a half-cell. First, the positive electrode sheet is placed in a CR2025 button-type positive electrode shell, covered with a cut Celgard diaphragm, a lithium sheet with a thickness of 2 mm is added, 4 to 6 drops of electrolyte are added, FEC is added as an additive, and finally the negative electrode shell is buckled and compacted to obtain a half-cell.

[0114] The method for preparing a half-cell using the positive electrode materials of Examples 2 to 3 and Comparative Examples 1 to 3 is the same as the above method, and will not be described in detail here.

[0115] The obtained half-cell was subjected to cycle performance and metal element dissolution tests.

[0116] The cycle performance test conditions are: test temperature 25°C, current density 10mA·g -1 , the voltage range is 2~4V. The test results are as follows Fig. 7A and Figure 7B As shown, the sodium ion battery positive electrode material prepared in Example 1 has better cycle stability and higher median voltage than that prepared in Comparative Example 1.

[0117] The metal element dissolution test conditions are as follows: scrape off the disassembled negative electrode material, digest it with aqua regia, and then use an ICP instrument to test the metal element content. The test results are shown in Table 1.

[0118] Table 1

[0119]

[0120] It can be seen from Table 1 that the dissolution of metal elements in the positive electrode materials of Examples 1 to 3 of the present application is significantly reduced compared with Comparative Examples 1 to 3.

[0121] The positive electrode materials of Example 1 and Comparative Example 1 were subjected to scanning electron microscopy (SEM) testing, wherein Figure 8 is the SEM image of the positive electrode material of Comparative Example 1, Fig. 9 is a SEM image of the positive electrode material of Example 1; Figure 8 and Fig. 9 It can be seen that the surface of the positive electrode material of Example 1 is uniformly coated with phosphate.

[0122] It should be noted that the above are only specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any technician familiar with the technical field can easily think of changes or substitutions within the technical scope disclosed in the present application, which should be included in the protection scope of the present application; the implementation methods of the present application and the features in the implementation methods can be combined with each other without conflict. Therefore, the protection scope of the present application shall be based on the protection scope of the claims.

Claims

1. A battery, characterized in that: It includes a positive electrode sheet, a negative electrode sheet and a separator, wherein the separator is arranged between the positive electrode sheet and the negative electrode sheet, the positive electrode sheet includes a current collector and a positive electrode active material layer arranged on the current collector, and the positive electrode active material layer includes a positive electrode material; The positive electrode material comprises a core material and a coating layer material coated on the surface of the core material, the core material is a metal oxide, the coating layer material is a phosphate, and the core material is doped with a first inactive metal element; The core material contains an active metal element and a second inactive metal element, wherein the concentration of the active metal element gradually increases from the surface of the core material to the core of the core material, and the concentration of the second inactive metal element gradually decreases from the surface of the core material to the core of the core material.

2. The battery according to claim 1, characterized in that The active metal element is selected from at least one of iron, cobalt, nickel, vanadium, copper and chromium; The second inactive metal element is selected from at least one of manganese and niobium.

3. The battery according to claim 1 or 2, characterized in that: In the core material, a molar ratio of the active metal element to the second inactive metal element is 9:1 to 6:

4.

4. The battery according to any one of claims 1 to 3, characterized in that The first inactive metal element is selected from Ca 2+ 、Zn 2+ Mg 2+ 、Ti 3+ 、Al 3+ 、Na + and Li + At least one of; When the core material is a sodium-containing oxide, the first inactive metal element is not Na + ; When the core material is a lithium-containing oxide, the first inactive metal element is not Li + .

5. The battery according to any one of claims 1 to 4, characterized in that: The doping concentration of the first inactive metal element gradually decreases from the surface layer of the core material to the core of the core material.

6. The battery according to any one of claims 1 to 5, characterized in that: The molar ratio of the core material to the first inactive metal element is 1:(0.0001-0.04).

7. The battery according to any one of claims 1 to 6, characterized in that The phosphate contains at least two phosphate groups and / or at least one pyrophosphate group.

8. The battery according to claim 7, characterized in that The molecular formula of the phosphate is: x R y (PO4) a (P2O7) b , wherein A is a sodium ion or a lithium ion; R is selected from at least one of iron, vanadium, titanium, manganese and cobalt; The values ​​of x, y, a and b can satisfy that the algebraic sum of positive and negative valences in the molecular formula of the phosphate is zero.

9. The battery according to claim 8, characterized in that The core material is a sodium-containing oxide, and the phosphate is selected from at least one of Na2FeP2O7, Na3Fe2(PO4)P2O7, Na3V2Fe(PO4)3, Na3VMn2Fe(PO4)3, Na3VTiFe(PO4)3, Na3Fe2Fe(PO4)3 and Na3MnTiFe(PO4)3.

10. The battery according to any one of claims 1 to 9, characterized in that The average particle size of the coating layer material is 40nm to 90nm.

11. The battery according to any one of claims 1 to 10, characterized in that The mass ratio of the coating layer material to the positive electrode material is 1% to 40%.

12. A battery pack, characterized in that: The method comprises a plurality of batteries according to any one of claims 1 to 11, wherein the plurality of batteries are connected in series or in parallel.

13. An electronic device, characterized in that: The invention comprises a housing and a battery according to any one of claims 1 to 11 located in the housing.

14. An energy storage system, characterized in that: It comprises a battery pack and a power converter as described in claim 12, wherein the power converter is used to perform power conversion on the voltage output by the battery pack, and / or the power converter is used to perform power conversion on the voltage output by an external power source and output it to the battery pack.

Citation Information

Cited By

  • Modified lithium-rich manganese-based positive electrode material and preparation method thereof

    CN121355240A