Pre-lithiated Si-M-C composite negative electrode material and preparation method and application thereof
Through the preparation of prelithiated Si-M@C composite materials, the combination of Si and M materials is used to solve the problems of capacity and circulation performance of the negative electrode material of lithium-ion batteries, and high capacity and excellent battery performance are achieved.
Patent Information
- Application Number
- CN202411086094.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The negative electrode materials of existing lithium-ion batteries, especially graphite materials, have poor battery performance, especially poor circulation performance due to capacity limitations and the huge volume expansion of silicon-based materials.
Using prelithiated Si-M@C composite anode material, the Si-M material is combined with the carbon cladding layer as a core, and the high capacity and low expansion characteristics of Si are used, and the low expansion characteristics of M material are prepared. Good material with high first-term efficiency and excellent circulation performance.
It achieves an ultra-high capacity 10 times higher than that of the simple graphite material, and significantly improves the cycling and conductive properties of the battery, overcoming the expansion problem of traditional lithium-ion battery materials.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium batteries, and in particular to a pre-lithiated Si-M@C composite negative electrode material and a preparation method and application thereof. Background Art
[0002] Lithium-ion battery is a high-energy-density, high-efficiency energy storage device, which has been widely used in portable digital devices, electric vehicles and other fields. The lithium-ion battery system is composed of four key materials: positive electrode material, negative electrode material, diaphragm and electrolyte. The properties of the materials are directly related to the performance of lithium-ion batteries.
[0003] In recent years, new energy vehicles have developed rapidly. The mainstream negative electrode material of automotive power lithium-ion batteries is graphite. However, due to its capacity problem, the overall quality or volume energy density of the battery is limited. Silicon-based materials have attracted much attention due to their high capacity. However, silicon-based materials have a huge volume expansion, resulting in poor cycle performance. Summary of the invention
[0004] Based on this, in order to address the problems existing in the current prior art, the purpose of the present invention is to provide a pre-lithiation Si-M@C composite negative electrode material and a preparation method and application thereof. The Si-M material with Si as the core and M material as the shell is pre-lithiation and then carbon-coated. The obtained pre-lithiation Si-M@C negative electrode material has high initial efficiency, high capacity and good cycle performance.
[0005] To achieve the above object, the present invention adopts the following technical solutions:
[0006] The present invention provides a pre-lithiated Si-M@C composite negative electrode material, comprising a pre-lithiated Si-M material and a carbon coating layer coated on the pre-lithiated Si-M material, wherein the Si-M material is a material with Si as a core and M material as an outer shell, and the M material is SiO x , graphite, soft carbon, and hard carbon.
[0007] In the pre-lithiation Si-M@C composite negative electrode material provided by the present invention, the Si-M material has silicon with a high expansion coefficient as the core and M material with a low expansion coefficient as the shell, which can effectively inhibit the expansion of the material. After the pre-lithiation Si-M material is coated with carbon, the material has good conductivity, high initial efficiency and good cycle performance; and because the capacity of silicon is about 10 times that of graphite material, compared with simple graphite material, the pre-lithiation Si-M@C composite negative electrode material of the present invention has an ultra-high capacity.
[0008] As a further improvement of the above solution of the present invention, the M material has a full charge expansion coefficient of 0-100%. The M material with a full charge expansion coefficient of 0-100% is selected. The full charge expansion coefficient of the M material is much smaller than that of silicon, which can effectively inhibit material expansion, thereby improving the cycle performance of the negative electrode material.
[0009] As a further improvement of the above solution of the present invention, when M is SiO x When M is graphite, soft carbon or hard carbon, the Si-M material is prepared by a ball milling method; when M is graphite, soft carbon or hard carbon, the Si-M material is prepared by a solid phase high temperature method. The preparation method is simple.
[0010] The present invention provides a method for preparing the above-mentioned pre-lithiation Si-M@C composite negative electrode material, comprising the following steps:
[0011] S1. The Si-M material is mixed with a lithium source by ball milling, and calcined under an inert atmosphere to obtain a pre-lithiated Si-M material;
[0012] S2. Placing the pre-lithiated Si-M material in a CVD furnace, and reacting in a C2H4 atmosphere to obtain a pre-lithiated Si-M@C composite material.
[0013] As a further improvement of the above scheme of the present invention, in step S1, the mixing mass ratio of the Si-M material and the lithium source is 1-100: 1. The purpose of pre-lithium is to allow the material to continuously replenish lithium during the cycle, so as to obtain better first effect and cycle, so the amount of lithium replenished will be reduced relative to the amount of the main material.
[0014] As a further improvement of the above solution of the present invention, in step S1, the lithium source is lithium powder and / or Li2CO3. Si and Si-O can form Li-Si or Li-Si-O alloy with one or more of lithium powder and Li2CO3 at high temperature, thereby achieving a pre-lithium effect.
[0015] As a further improvement of the above scheme of the present invention, in step S1, the calcination temperature is 500-1000°C and the time is 2-12 hours. Under this condition, Si and Si-O can better form Li-Si or Li-Si-O alloy with one or more of lithium powder and Li2CO3 at high temperature, thereby achieving the pre-lithium effect.
[0016] As a further improvement of the above solution of the present invention, in step S2, the reaction temperature is 600-1000°C and the reaction time is 1-12 hours. Under this condition, the surface of the pre-lithiated Si-M material can be effectively carbon-coated, so that the material has better conductivity.
[0017] As a further improvement of the above scheme of the present invention, in step S2, the flow rate of C2H4 is 0.1-10 L / min. Under this condition, the surface of the pre-lithiated Si-M material can be effectively carbon-coated, and the carbon layer is more dense and uniform, so that the material has better conductivity.
[0018] The present invention provides an application of the pre-lithiated Si-M@C composite negative electrode material as described above in a negative electrode active material of a lithium battery.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] In the pre-lithiation Si-M@C composite negative electrode material provided by the present invention, the Si-M material has silicon with a high expansion coefficient as the core and M material with a low expansion coefficient as the shell, which can effectively inhibit the expansion of the material. After the pre-lithiation Si-M material is coated with carbon, the material has good conductivity, high initial efficiency and good cycle performance; and because the capacity of silicon is about 10 times that of graphite material, compared with simple graphite material, the pre-lithiation Si-M@C composite negative electrode material of the present invention has an ultra-high capacity. DETAILED DESCRIPTION
[0021] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively below in conjunction with specific embodiments. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thoroughly understood.
[0022] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
[0023] Example 1
[0024] This embodiment provides a pre-lithiation Si-SiO x @C composite negative electrode material, the preparation method thereof comprises the following steps:
[0025] S1. After the micron silicon material and water are mixed evenly at a mass volume ratio of 1g:10mL, a slurry is obtained, and the slurry is transferred to a sand mill and sand-milled at 100r / min for 0.5h to obtain a sand-milled slurry; 4wt% HF solution is added to the sand-milled slurry, and the volume ratio of the sand-milled slurry to the 4wt% HF solution is 1:3, and after stirring, the slurry is filtered and dried to obtain Si-SiO x Material;
[0026] S2. Lithium powder and Si-SiO xThe materials were mixed by ball milling at a mass ratio of 1:50 and calcined at 950 °C for 8 h in a N2 atmosphere to obtain pre-lithiated Si-SiO x Material;
[0027] S3. Pre-lithiated Si-SiO x The material was placed in a CVD furnace and reacted at 950°C for 6 h in a C2H4 atmosphere (flow rate of 0.5 L / min) to obtain pre-lithiated Si-SiO x @C composite negative electrode material.
[0028] Example 2
[0029] This embodiment provides a pre-lithiation Si-SiO x @C composite negative electrode material, the preparation method thereof comprises the following steps:
[0030] S1. After the micron silicon material and NMP are mixed evenly at a mass volume ratio of 1g:10mL, a slurry is obtained, and the slurry is transferred to a sand mill and sand-milled at 100r / min for 0.5h to obtain a sand-milled slurry; 5wt% HF solution is added to the sand-milled slurry, and the volume ratio of the sand-milled slurry to the 5wt% HF solution is 1:5, and after stirring, the slurry is filtered and dried to obtain Si-SiO x Material;
[0031] S2. Lithium powder, Li2CO3 and Si-SiO x The materials were mixed by ball milling at a mass ratio of 1:0.1:50 and calcined at 800 °C for 8 h in a N2 atmosphere to obtain pre-lithiated Si-SiO x Material;
[0032] S3. Pre-lithiated Si-SiO x The material was placed in a CVD furnace and reacted at 950°C for 6 h in a C2H4 atmosphere (flow rate of 0.5 L / min) to obtain pre-lithiated Si-SiO x @C composite negative electrode material.
[0033] Example 3
[0034] This embodiment provides a pre-lithiation Si-SiO x @C composite negative electrode material, the preparation method thereof comprises the following steps:
[0035] S1. After the micron silicon material and NMP are mixed evenly at a mass volume ratio of 1g:10mL, a slurry is obtained, and the slurry is transferred to a sand mill and sand-milled at 1000r / min for 2h to obtain a sand-milled slurry; 2wt% HF solution is added to the sand-milled slurry, and the volume ratio of the sand-milled slurry to the 2wt% HF solution is 1:2, and after stirring, the slurry is filtered and dried to obtain Si-SiO x Material;
[0036] S2. Lithium powder, Li2CO3 and Si-SiO x The materials were mixed by ball milling at a mass ratio of 1:0.1:80 and calcined at 700 °C for 8 h in a N2 atmosphere to obtain pre-lithiated Si-SiO x Material;
[0037] S3. Pre-lithiated Si-SiO x The material was placed in a CVD furnace and reacted at 750 °C for 8 h in a C2H4 atmosphere (flow rate of 0.5 L / min) to obtain pre-lithiated Si-SiO x @C composite negative electrode material.
[0038] Example 4
[0039] This embodiment provides a pre-lithiation Si-SiO x @C composite negative electrode material, the preparation method thereof comprises the following steps:
[0040] S1. Mix the micron silicon material and water in a mass volume ratio of 1g:10mL to obtain a slurry, transfer the slurry to a sand mill and sand grind it at 500r / min for 2h to obtain a sand mill slurry; add 1wt% HF solution to the sand mill slurry, the volume ratio of the sand mill slurry to the 1wt% HF solution is 1:1, stir, filter, and dry to obtain Si-SiO x Material;
[0041] S2. Lithium powder and Si-SiO x The materials were mixed by ball milling at a mass ratio of 1:80 and calcined at 950 °C for 8 h in a N2 atmosphere to obtain pre-lithiated Si-SiO x Material;
[0042] S3. Pre-lithiated Si-SiO x The material was placed in a CVD furnace and reacted at 900 °C for 7 h in a C2H4 atmosphere (flow rate of 0.5 L / min) to obtain pre-lithiated Si-SiO x @C composite negative electrode material.
[0043] Example 5
[0044] This embodiment provides a pre-lithiated Si-graphite@C composite negative electrode material, and the preparation method thereof comprises the following steps:
[0045] S1. The micron silicon material and the graphitized carbon source were mixed uniformly in a mass ratio of 4:1, and then graphitized at 2500°C for 24 hours to obtain a Si-graphite material;
[0046] S2. The lithium powder and Si-graphite material were ball-milled in a mass ratio of 1:80, and then calcined at 950°C for 8h in a N2 atmosphere to obtain a pre-lithiated Si-graphite material;
[0047] S3. The pre-lithiated Si-graphite material was placed in a CVD furnace and reacted at 900°C for 7h in a C2H4 atmosphere (flow rate of 0.5L / min) to obtain a pre-lithiated Si-graphite@C composite negative electrode material.
[0048] Example 6
[0049] This embodiment provides a pre-lithiated Si-soft carbon@C composite negative electrode material, and the preparation method thereof comprises the following steps:
[0050] S1. The micron silicon material and the non-graphitized carbon source were mixed uniformly in a mass ratio of 4:1, and then graphitized at 650°C for 12 hours to obtain a Si-soft carbon material;
[0051] S2. The lithium powder and the Si-soft carbon material were ball-milled in a mass ratio of 1:80, and then calcined at 950°C for 8h in a N2 atmosphere to obtain a pre-lithiated Si-soft carbon material;
[0052] S3. The pre-lithiated Si-soft carbon material was placed in a CVD furnace and reacted at 900°C for 7h in a C2H4 atmosphere (flow rate of 0.5L / min) to obtain a pre-lithiated Si-soft carbon@C composite negative electrode material.
[0053] Example 7
[0054] This embodiment provides a pre-lithiated Si-hard carbon@C composite negative electrode material, and the preparation method thereof comprises the following steps:
[0055] S1. The micron silicon material and the non-graphitizable carbon source were mixed uniformly in a mass ratio of 4:1, and then graphitized at 1000°C for 24h to obtain a Si-hard carbon material;
[0056] S2. The lithium powder and Si-hard carbon material were mixed by ball milling at a mass ratio of 1:80, and then calcined at 950°C for 8h in a N2 atmosphere to obtain a pre-lithiated Si-hard carbon material;
[0057] S3. The pre-lithiated Si-hard carbon material was placed in a CVD furnace and reacted at 900°C for 7h in a C2H4 atmosphere (flow rate of 0.5L / min) to obtain a pre-lithiated Si-hard carbon@C composite negative electrode material.
[0058] Comparative Example 1
[0059] This comparative example provides a pre-lithiation Si@C composite negative electrode material, and the preparation method thereof comprises the following steps:
[0060] S1. The lithium powder and the micronized silicon material were mixed by ball milling at a mass ratio of 1:50, and then calcined at 800°C for 6h in a N2 atmosphere to obtain a pre-lithiated Si material;
[0061] S2. The pre-lithiated Si material was placed in a CVD furnace and reacted at 900°C for 7h in a C2H4 atmosphere (flow rate of 0.5L / min) to obtain a pre-lithiated Si@C composite negative electrode material.
[0062] Comparative Example 2
[0063] This comparative example provides a pre-lithiation Si@C composite negative electrode material, and the preparation method thereof comprises the following steps:
[0064] S1. After mixing lithium powder, Li2CO3 and micron silicon material in a mass ratio of 1:0.1:50 by ball milling, calcining at 800°C for 6h in a N2 atmosphere to obtain a pre-lithiated Si material;
[0065] S2. The pre-lithiated Si material was placed in a CVD furnace and reacted at 900°C for 7h in a C2H4 atmosphere (flow rate of 0.5L / min) to obtain a pre-lithiated Si@C composite negative electrode material.
[0066] Comparative Example 3
[0067] This comparative example provides a Si@C composite negative electrode material, and the preparation method thereof comprises the following steps:
[0068] S1. Place the micron silicon material in a CVD furnace and react at 900°C for 7h in a C2H4 atmosphere (flow rate is 0.5L / min) to obtain a Si@C composite negative electrode material.
[0069] Test Case
[0070] The composite negative electrode material prepared in the above embodiments and comparative examples is used to prepare a negative electrode plate for a lithium battery. The preparation method is as follows: 80 parts by weight of the composite negative electrode material and 10 parts by weight of a conductive agent are mixed and ground to obtain a negative electrode active material powder; 10 parts by weight of a binder and an NMP solvent are added and stirred to obtain a negative electrode mixture slurry; a layer of the negative electrode mixture slurry with a thickness of 10-500 μm is coated on a metal current collector, and then vacuum dried in an oven at 80°C for 12-24 hours to remove the solvent to obtain a negative electrode plate.
[0071] The above-prepared negative electrode sheet is then used to prepare a lithium battery. The preparation method is as follows: the above-prepared negative electrode sheet, positive electrode sheet (using a 1 mm thick lithium metal sheet), separator, and electrolyte are assembled into a lithium battery, wherein the positive electrode sheet uses a 1 mm thick lithium metal sheet, the separator is Celgard2400, and the electrolyte is EC / DMC / FEC+1M LiPF6. Of course, the selection of positive electrode sheet, separator, and electrolyte, in addition to those specified in this test example, other commonly used materials in the field can be used.
[0072] The gram capacity of the composite negative electrode materials prepared in Examples 1-6 and Comparative Examples 1-3 was tested, and the cycle performance of the lithium battery prepared using the composite negative electrode materials prepared in Examples 1-6 and Comparative Examples 1-3 was tested. The test results are shown in Table 1.
[0073] Table 1 Performance test results
[0074] serial number First effect Gram capacity Cycle performance Example 1 91.5% 1589.6mAh / g 99.12% / 100cycle Example 2 91.8% 1580.3mAh / g 99.15% / 100cycle Example 3 91.1% 1416.7mAh / g 99.10% / 100cycle Example 4 90.7% 1468.2mAh / g 99.05% / 100cycle Example 5 92.0% 1385.9mAh / g 97.14% / 100cycle Example 6 92.1% 1402.7mAh / g 98.11% / 100cycle Example 7 91.6% 1398.4mAh / g 97.21% / 100cycle Comparative Example 1 92.5% 2201.5mAh / g 85.51% / 100cycle Comparative Example 2 92.1% 2156.1mAh / g 86.41% / 100cycle Comparative Example 3 75.1% 1900.4mAh / g 78.65% / 100cycle graphite 92.8% 356.5mAh / g 99.23% / 100cycle
[0075] It can be seen from the results in Table 1 that the capacity of the pre-lithiated Si-M@C composite negative electrode material of the present invention is higher than that of conventional graphite material, and its cycle performance and first efficiency are also very close to those of conventional graphite material; although the capacity of the pre-lithiated Si-M@C composite negative electrode material of the present invention is lower than that of the pre-lithiated Si@C composite material and Si@C composite material, its cycle performance is superior to that of the pre-lithiated Si@C composite material and Si@C composite material.
[0076] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0077] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A pre-lithiation Si-M@C composite negative electrode material, characterized in that: The invention comprises a pre-lithiated Si-M material and a carbon coating layer coated on the pre-lithiated Si-M material, wherein the Si-M material is a material with Si as a core and M material as an outer shell, and the M material is SiO x , graphite, soft carbon, and hard carbon.
2. The pre-lithiation Si-M@C composite negative electrode material according to claim 1, characterized in that: The full-charge expansion coefficient of the M material is 0-100%.
3. The pre-lithiation Si-M@C composite negative electrode material according to claim 2, characterized in that: When M is SiO x When M is graphite, soft carbon or hard carbon, the Si-M material is prepared by a solid phase high temperature method.
4. A method for preparing a pre-lithiated Si-M@C composite negative electrode material as claimed in any one of claims 1 to 3, characterized in that: The following steps are involved: S1. The Si-M material is mixed with a lithium source by ball milling, and calcined under an inert atmosphere to obtain a pre-lithiated Si-M material; S2. Placing the pre-lithiated Si-M material in a CVD furnace, and reacting in a C2H4 atmosphere to obtain a pre-lithiated Si-M@C composite material.
5. The method for preparing the pre-lithiated Si-M@C composite negative electrode material according to claim 4, characterized in that: In step S1, the mixing mass ratio of the Si-M material and the lithium source is 1-100:
1.
6. The method for preparing the pre-lithiated Si-M@C composite negative electrode material according to claim 4, characterized in that: In step S1, the lithium source is lithium powder and / or Li2CO3.
7. The method for preparing the pre-lithiated Si-M@C composite negative electrode material according to claim 4, characterized in that: In step S1, the calcination temperature is 500-1000°C and the time is 2-12 hours.
8. The method for preparing the pre-lithiated Si-M@C composite negative electrode material according to claim 4, characterized in that: In step S2, the reaction temperature is 600-1000° C. and the reaction time is 1-12 h.
9. The method for preparing the pre-lithiated Si-M@C composite negative electrode material according to claim 4, characterized in that: In step S2, the flow rate of C2H4 is 0.1-10 L / min.
10. Use of the pre-lithiated Si-M@C composite negative electrode material as claimed in any one of claims 1 to 3 in a negative electrode active material for a lithium battery.
Citation Information
Patent Citations
Composite silicon based electrode material, preparation method and application thereof
CN107394161A
Silicon-based negative electrode material and preparation method thereof and lithium ion battery
CN112382742A
Si-SiOx (at) C / graphite negative electrode material and preparation method thereof
CN115621457A
Preparation method and application of simple pre-lithiated nano-microstructure silicon-oxygen-carbon composite material
CN117558894A
Pre-lithiated silicon-based composite material and preparation method thereof, negative electrode and lithium-containing battery
CN117747763A