Vanadium-doped nickel-cobalt-manganese ternary positive electrode material and preparation method and application thereof
By using anhydrous vanadium citrate as the doping carrier of vanadium element and lithium nickel cobalt manganese oxide, the problem of high nickel nickel cobalt manganese positive electrode material is solved, and the performance and energy consumption of the material are improved. The reduction solves the problem of large energy consumption during doping modification.
Patent Information
- Application Number
- CN202411105195.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-12
AI Technical Summary
High-nickel nickel cobalt manganese ternary cathode materials are susceptible to internal stress during charging and discharging, causing microcracks, resulting in attenuation of circulation capacity, and the energy consumption of the doping modification process is large, affecting production costs.
Anhydrous vanadium citrate is used as the doping carrier for vanadium element and lithium nickel cobalt manganese oxide. The vanadium-doped nickel cobalt manganese ternary cathode material is prepared through evaporation crystallization and multiple calcination processes, reducing lithium nickel mixed discharge and improving cations. order and crystal structure stability.
It significantly improves the cycle life and safety performance of the cathode material, reduces production costs, saves energy consumption, and achieves more significant performance improvement effects.
Smart Images

Figure CN119069669A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of battery positive electrode material preparation methods, and specifically to a vanadium-doped nickel-cobalt-manganese ternary positive electrode material and a preparation method and application thereof. Background Art
[0002] Nickel-cobalt-manganese ternary cathode materials (NCM) are widely used in lithium-ion cathode materials. In order to further increase capacity and reduce costs, NCM materials are currently developing towards high nickel. However, due to the sudden change in lattice volume during charging and discharging, high-nickel NCM material particles are susceptible to internal stress and produce microcracks, which extend along the interface between the active material and the electrolyte, accelerating particle pulverization and electrolyte decomposition, resulting in cycle capacity decay. Means for modifying high-nickel NCM materials to solve the above problems include element doping.
[0003] However, doping elements in high-nickel NCM materials will affect the band gap, interlayer spacing, defect concentration and bonding force between atoms of the material to a certain extent. However, the performance improvement effect of the high-nickel NCM material after doping modification still needs to be improved. Moreover, the doping process requires a long calcination time and consumes a lot of energy, which is not conducive to controlling production costs. Summary of the invention
[0004] In view of this, the present application provides a modified high-nickel NCM material to solve at least one of the above technical problems.
[0005] To achieve the above-mentioned purpose, the present application provides a method for preparing a vanadium-doped nickel-cobalt-manganese ternary positive electrode material, comprising: providing a vanadium citrate aqueous solution, evaporating and crystallizing the vanadium citrate aqueous solution and performing a primary calcination to obtain anhydrous vanadium citrate; mixing the anhydrous vanadium citrate with lithium nickel-cobalt-manganese oxide to obtain a mixture, and performing a secondary calcination on the mixture to obtain the vanadium-doped nickel-cobalt-manganese ternary positive electrode material.
[0006] In some possible implementations, providing the vanadium citrate aqueous solution includes mixing vanadium pentoxide with citric acid, and heating the mixture to allow the vanadium pentoxide to react with the citric acid.
[0007] In some possible implementations, the evaporation crystallization is carried out at a temperature of 60° C. to 100° C. and for a time of 2 h to 4 h.
[0008] In some possible implementations, the primary calcination is performed in an oxygen-containing atmosphere, the temperature of the primary calcination is 180° C. to 220° C., and the time is 2 h to 3 h.
[0009] In some possible implementations, the particle size of the anhydrous vanadium citrate is 500 nm to 800 nm.
[0010] In some possible implementations, the mixing rotation speed is 200 r / min to 300 r / min.
[0011] In some possible implementations, the secondary calcination is performed in an oxygen-containing atmosphere, the temperature of the secondary calcination is 400° C. to 730° C., and the time is 3 h to 6 h.
[0012] The present application also provides a vanadium-doped nickel-cobalt-manganese ternary positive electrode material, which is prepared by the preparation method. The molecular formula of the vanadium-doped nickel-cobalt-manganese ternary positive electrode material is LiNi x Co y Mn z V a O2, 0.8≤x≤0.96, 0.02≤y≤0.2, 0.02≤z≤0.2, 0.0013≤a≤0.0043.
[0013] The present application also provides a positive electrode plate, comprising a positive electrode current collector and a positive electrode active material layer disposed on at least one surface of the positive electrode current collector, wherein the positive electrode active material layer comprises the vanadium-doped nickel-cobalt-manganese ternary positive electrode material.
[0014] The present application also provides a lithium-ion battery, comprising an electrode assembly, wherein the electrode assembly comprises a separator, a negative electrode sheet and the positive electrode sheet, and the separator is disposed between the positive electrode sheet and the negative electrode sheet.
[0015] The present application uses anhydrous vanadium citrate as a doping carrier for vanadium elements and lithium nickel cobalt manganese oxide, which helps to reduce the degree of lithium nickel mixing and improve the orderliness of cations. It has the function of stabilizing the crystal structure skeleton, stabilizing the lattice oxygen, inhibiting oxygen release, and improving the cycle life and safety performance of the material. Compared with other vanadium-doped carriers, the use of anhydrous vanadium citrate for doping modification can obtain a positive electrode material with a more significant performance improvement effect after modification. The preparation method of the present application is simple in process, and the preparation of vanadium-doped nickel-cobalt-manganese ternary positive electrode materials by using the method is conducive to significantly improving the performance of the positive electrode material, reducing production costs and saving energy consumption. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 (a) is a charge-discharge cycle curve of comparative example 1 of the present application under the conditions of 3-4.5V and 0.2C;
[0017] Figure 1 (b) is a charge-discharge cycle curve diagram of Example 1 of the present application under the conditions of 3-4.5V and 0.2C;
[0018] Figure 1 (c) is the cycle performance test result of Example 1 and Comparative Example 1 of the present application under the conditions of 3-4.5V and 0.2C;
[0019] Figure 1 (d) is the rate performance test result of Example 1 and Comparative Example 1 of the present application;
[0020] Figure 1 (e) is a CV graph of Comparative Example 1 of the present application at 3-4.5V and 0.2mV / s;
[0021] Figure 1 (f) is a CV graph of Example 1 of the present application at 3-4.5V and 0.2mV / s;
[0022] Figure 1 (g) is the EIS graph of Example 1 and Comparative Example 1 of the present application before charge and discharge cycles;
[0023] Figure 1 (h) is the EIS graph of comparative example 1 of the present application after 10 charge and discharge cycles under 3-4.5V and 0.2C conditions.
[0024] Figure 2 (a) is a charge-discharge cycle curve of Comparative Example 2 of the present application under the conditions of 3-4.3V and 0.2C;
[0025] Figure 2 (b) is a charge-discharge cycle curve diagram of Example 2 of the present application under the conditions of 3-4.3V and 0.2C;
[0026] Figure 2 (c) is the cycle performance test result of Example 2 and Comparative Example 2 of the present application under the conditions of 3-4.3V and 0.2C;
[0027] Figure 2 (d) is the cycle performance test result of Example 2 and Comparative Example 2 of the present application under the conditions of 3-4.5V and 0.2C;
[0028] Figure 2 (e) is the CV graph of Comparative Example 2 of the present application under the conditions of 3-4.5V and 0.2mV / s;
[0029] Figure 2 (f) is the CV graph of Example 2 of the present application under the conditions of 3-4.5V and 0.2mV / s;
[0030] Figure 2 (g) is the rate performance test result of Example 2 and Comparative Example 2 of the present application;
[0031] Figure 2 (h) is the EIS graph of Example 2 of the present application and Comparative Example 2 before charge and discharge cycles;
[0032] Figure 2(i) is the EIS graph of Example 2 and Comparative Example 2 of the present application after 10 charge and discharge cycles under 3-4.5V and 0.2C conditions.
[0033] Figure 3 (a) is a charge-discharge cycle curve of comparative example 3 of the present application under the conditions of 3-4.5V and 1C;
[0034] Figure 3 (b) is a charge-discharge cycle curve diagram of Example 3 of the present application under the conditions of 3-4.5V and 1C;
[0035] Figure 3 (c) is the cycle performance test result of Example 3 and Comparative Example 3 of the present application under 3-4.5V, 1C conditions;
[0036] Figure 3 (d) in the figure is the rate performance test result of Example 3 and Comparative Example 3 of the present application.
[0037] Figure 4 (a) is a charge-discharge cycle curve of comparative example 4 of the present application under the conditions of 3-4.5V and 1C;
[0038] Figure 4 (b) is a charge-discharge cycle curve diagram of Example 4 of the present application under the conditions of 3-4.5V and 1C;
[0039] Figure 4 (c) is the cycle performance test result of Example 4 and Comparative Example 4 of the present application under 3-4.5V, 1C conditions;
[0040] Figure 4 (d) in the figure is the rate performance test result of Example 4 and Comparative Example 4 of the present application. DETAILED DESCRIPTION
[0041] The embodiments of the present application are described in detail below. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present application, and cannot be understood as limiting the present application; it should be noted that, unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by technicians in the technical field of the present application; in the absence of conflict, the embodiments of the present application and the features in the embodiments can be combined with each other; many specific details are elaborated in the following description to facilitate a full understanding of the present application, and the described embodiments are only part of the embodiments of the present application, not all of the embodiments.
[0042] An embodiment of the present application provides a method for preparing a vanadium-doped nickel-cobalt-manganese ternary positive electrode material, comprising:
[0043] The first step is to provide a vanadium citrate aqueous solution, evaporate and crystallize the vanadium citrate aqueous solution and perform a roasting to obtain anhydrous vanadium citrate (C 15 H 14 O9V2).
[0044] The vanadium citrate aqueous solution is subjected to evaporation crystallization to obtain vanadium citrate crystals. The evaporation crystallization method is more conducive to maintaining the stability of the vanadium citrate structure, thereby making it easier to obtain vanadium citrate crystals. In other crystallization methods, such as cooling crystallization, when the temperature drops to about 36°C, citric acid crystals may precipitate in the solution, affecting the output of vanadium citrate, and the required crystallization time is also relatively longer. Therefore, obtaining vanadium citrate crystals by evaporation crystallization is conducive to avoiding the risk of citric acid precipitation in the crystallized product, and is also conducive to reducing the time cost of the preparation process.
[0045] The obtained vanadium citrate crystals are calcined to remove the crystal water and obtain anhydrous vanadium citrate, which can prevent the crystal water from damaging the structure and performance of the ternary positive electrode material during the subsequent mixing process with the ternary positive electrode material.
[0046] In some embodiments, providing the vanadium citrate aqueous solution includes mixing vanadium pentoxide with citric acid, heating, and reacting the vanadium pentoxide with the citric acid. Preferably, the molar ratio of the vanadium pentoxide to the citric acid can be 3:1, and the heating temperature can be 80° C., wherein an oil bath can be selected to improve uniform heating. The reaction can obtain a clear dark blue solution, i.e., a vanadium citrate aqueous solution.
[0047] In some embodiments, the evaporation crystallization temperature is 60° C. to 100° C., and the time is 2 h to 4 h. Controlling the evaporation crystallization temperature within the above range is beneficial to reducing the risk of precipitating crystals with citric acid in the vanadium citrate aqueous solution, and controlling the crystallization time within the above range is beneficial to the full crystallization of vanadium citrate.
[0048] In some embodiments, the primary calcination is performed in an oxygen-containing atmosphere, the primary calcination temperature is 180° C. to 220° C., and the primary calcination time is 2 h to 3 h.
[0049] A single calcination in an oxygen-containing atmosphere helps to fully convert the vanadium element in vanadium citrate into +5-valent vanadium, promoting doping with +5-valent vanadium. 5+ During charging, there is no change in valence state, and thus no change in volume, which can stabilize the framework of the crystal structure. Controlling the temperature and time of the primary calcination within the above range is conducive to fully removing the crystal water in the vanadium citrate crystals.
[0050] The second step: mixing the anhydrous vanadium citrate with lithium nickel cobalt manganese oxide (LiNi x Co yMn z O2) to obtain a mixture, and the mixture is subjected to secondary calcination to obtain the vanadium-doped nickel-cobalt-manganese ternary positive electrode material.
[0051] Anhydrous vanadium citrate is used as a doping carrier of vanadium element and mixed with lithium nickel cobalt manganese oxide, so that the high-valent vanadium (such as +5 valence) in anhydrous vanadium citrate is doped in the lithium nickel cobalt manganese oxide material, which can make the Ni in the material 2+ Converted to Ni 3 + , reducing the degree of lithium-nickel mixing and improving the orderliness of cations. In the related art, during the charging process, nickel ions will undergo Ni 3+ To You 4+ The transformation is accompanied by the shrinkage of volume, which is prone to irreversible phase change and eventually loses electrochemical activity. 5+ Occupy Ni 3+ Bit, V 5+ During charging, there is no change in valence state, and thus no change in volume, which can stabilize the crystal structure skeleton. At the same time, the vanadium atoms and oxygen atoms in anhydrous citric acid form a strong bond. The VO chemical bond strength between vanadium and oxygen is stronger than the MO chemical bond strength between transition metals and oxygen. Therefore, it can stabilize the lattice oxygen in the positive electrode material, inhibit the release of lattice oxygen, reduce the risk of structural collapse caused by the formation of oxygen vacancies, and help maintain the stability of the lattice structure, thereby improving the cycle life and safety performance of the material.
[0052] The present application finds that using vanadium citrate as a doping carrier of vanadium element, compared with other vanadium doping carriers (such as vanadium pentoxide V2O5, ammonium metavanadate NH4VO3), on the basis of using the same size of vanadium doping carrier and obtaining the same vanadium doping amount, can obtain a positive electrode material with more significantly improved performance after doping modification.
[0053] In some embodiments, the anhydrous vanadium citrate (C 15 H 14 The particle size of the anhydrous vanadium citrate (V2) is nanometer-sized. In some embodiments, the particle size of the anhydrous vanadium citrate is 500nm to 800nm. 15 H 14 When the O9V2) is at the nano level, due to the smaller particle size and larger specific surface area, it is helpful to increase the doping amount of vanadium and help improve the uniformity of doping, so that the doping modification effect of lithium nickel cobalt manganese oxide is more significant. In some embodiments, the doping amount of vanadium is 0.13% to 0.43% of the molar amount of lithium nickel cobalt manganese oxide, or 0.3% to 1% of the mass of lithium nickel cobalt manganese oxide, achieving a higher doping amount.
[0054] In some embodiments, the mixing is performed at a low speed, for example, the speed may be 200 r / min to 300 r / min. The present application uses anhydrous vanadium citrate as a doping carrier of vanadium element and lithium nickel cobalt manganese oxide, which can achieve a fully uniform mixing at a relatively low speed, thereby achieving a better doping effect, and the low speed reduces the energy consumption of the preparation process.
[0055] In some embodiments, the secondary calcination is performed in an oxygen-containing atmosphere, the temperature of the secondary calcination is 400°C to 730°C, and the time is 3h to 6h. In an atmosphere containing O2, the temperature and time are controlled within the above range, and the high temperature first promotes the nucleation of the mixture of anhydrous vanadium citrate and lithium nickel cobalt manganese oxide, and then promotes the growth of the nucleated grains of the mixture to form a vanadium-doped nickel-cobalt-manganese ternary positive electrode material. In this process, if there is a lack of O2, it is difficult to convert Ni 2+ Oxidized to Ni 3+ , resulting in a high degree of lithium-nickel mixing, affecting lithium ion transmission. If the temperature is too high or the time is too long, it is easy to generate oxygen-deficient compounds and promote secondary recrystallization. At the same time, the grain size of the material becomes larger and the specific surface area becomes smaller, which is not conducive to the release and embedding of lithium ions in the material. If the temperature is too low or the time is too short, the reaction is incomplete and it is easy to generate amorphous materials. The crystallization performance of the material is poor and it is easy to contain impurities, which has a greater impact on the electrochemical properties of the material.
[0056] In some embodiments, the lithium nickel cobalt manganese oxide LiNi x Co y Mn z In O2, 0.8≤x≤0.96, 0.02≤y≤0.2, 0.02≤z≤0.2.
[0057] An embodiment of the present application provides a vanadium-doped nickel-cobalt-manganese ternary positive electrode material, which is prepared by the preparation method. The molecular formula of the vanadium-doped nickel-cobalt-manganese ternary positive electrode material is LiNi x Co y Mn z V a O2, 0.8≤x≤0.96, 0.02≤y≤0.2, 0.02≤z≤0.2, 0.0013≤a≤0.0043.
[0058] Another embodiment of the present application provides a positive electrode plate, including a positive electrode current collector and a positive electrode active material layer disposed on at least one surface of the positive electrode current collector, wherein the positive electrode active material layer includes the vanadium-doped nickel-cobalt-manganese ternary positive electrode material.
[0059] Another embodiment of the present application further provides a lithium-ion battery, including an electrode assembly, wherein the electrode assembly includes a separator, a negative electrode sheet and the positive electrode sheet, and the separator is disposed between the positive electrode sheet and the negative electrode sheet.
[0060] The present application uses anhydrous vanadium citrate as a doping carrier for vanadium elements and lithium nickel cobalt manganese oxide, which helps to reduce the degree of lithium nickel mixing and improve the orderliness of cations. It has the function of stabilizing the crystal structure skeleton, stabilizing lattice oxygen, inhibiting oxygen release, and improving the cycle life and safety performance of lithium-ion batteries. Compared with other vanadium-doped carriers, the use of anhydrous vanadium citrate for doping modification can obtain a positive electrode material with more significant performance improvement after modification. The preparation method of the present application is simple in process, and the preparation of vanadium-doped nickel-cobalt-manganese ternary positive electrode materials by using it is conducive to reducing production costs and saving energy consumption.
[0061] The scheme of the present application will be explained below in conjunction with the embodiments. Those skilled in the art will understand that the following examples are only used to explain the present application and cannot be construed as limiting the present application. Unless otherwise stated, the reagents, software and instruments not specifically stated in the following embodiments are all conventional commercial products or open source.
[0062] Embodiment 1:
[0063] A vanadium-doped nickel-cobalt-manganese lithium-ion battery positive electrode material, the preparation method of which comprises:
[0064] Step 1, respectively weighing citric acid monohydrate (C6H8O7·H2O) and vanadium pentoxide (V2O5), wherein the molar ratio of C6H8O7·H2O to V2O5 is 3:1, dissolving the weighed C6H8O7·H2O and V2O5 in deionized water, and stirring at a constant speed for 1 hour in an 80° C. oil bath to obtain a vanadium citrate aqueous solution, and evaporating the solution in a 60° C. forced air oven for 4 hours to obtain vanadium citrate crystals.
[0065] Step 2, calcining the crystals of step 1 in a tube furnace for 3 hours, passing oxygen, and calcining at a temperature of 200° C. to obtain anhydrous vanadium citrate (C 15 H 14 O9V2), the particle size of the obtained anhydrous vanadium citrate is 5-10μm.
[0066] Step 3, weigh 400 mg of single crystal LiNi 0.8 Co 0.1 Mn 0.1 O2 lithium nickel cobalt manganese oxide, 1.2 mg of anhydrous vanadium citrate (C 15 H 14 O9V2), that is, the amount of anhydrous vanadium citrate doped is single crystal LiNi 0.8 Co 0.1 Mn 0.1The mixture is prepared by mixing vanadium-doped nickel-cobalt-manganese lithium-ion battery positive electrode material with oxygen passing therethrough at 400°C for 3h and 710°C for 3h.
[0067] Embodiment 2:
[0068] The difference from Example 1 is that in step 1, the evaporation is adjusted to be carried out in an oil bath at 100° C. with uniform stirring for 2 h; in step 2, the obtained anhydrous vanadium citrate (C 15 H 14 O9V2) is ground to obtain nano-scale anhydrous vanadium citrate with a particle size of 500-800nm; in step 3, lithium nickel cobalt manganese oxide is adjusted to polycrystalline LiNi 0.96 Co 0.02 Mn 0.02 O2; in step 3, calcined at 400°C for 3h, and calcined at 730°C for 3h.
[0069] Embodiment 3:
[0070] The difference from Example 1 is that in step 3, the lithium nickel cobalt manganese oxide is adjusted to single crystal LiNi 0.8 Mn 0.2 O2; in step 2, the obtained anhydrous vanadium citrate (C 15 H 14 O9V2) is ground to obtain nano-scale anhydrous vanadium citrate with a particle size of 500-800nm; in step 3, 400mg single crystal LiNi 0.8 Mn 0.2 O2, 4 mg anhydrous vanadium citrate (C 15 H 14 O9V2).
[0071] Embodiment 4:
[0072] The difference from Example 1 is that in step 3, the lithium nickel cobalt manganese oxide is adjusted to single crystal LiNi 0.8 Co 0.2 O2; in step 2, the obtained anhydrous vanadium citrate (C 15 H 14 O9V2) is ground to obtain nano-scale anhydrous vanadium citrate with a particle size of 500-800nm; in step 3, 400mg single crystal LiNi 0.8 Mn 0.2 O2, 2 mg anhydrous vanadium citrate (C 15 H 14 O9V2).
[0073] Comparative Example 1:
[0074] The difference from Example 1 is that no doping modification is performed, that is, single crystal LiNi 0.8 Co 0.1 Mn 0.1 O2 is used as the positive electrode material of the battery.
[0075] Comparative Example 2:
[0076] The difference from Example 2 is that no doping modification is performed, that is, polycrystalline LiNi 0.96 Co 0.02 Mn 0.02 O2 is used as the positive electrode material of the battery.
[0077] Comparative Example 3:
[0078] The difference from Example 3 is that no doping modification is performed, that is, single crystal LiNi 0.8 Mn 0.2 O2 is used as the positive electrode material of the battery.
[0079] Comparative Example 4:
[0080] The difference from Example 4 is that no doping modification is performed, that is, single crystal LiNi 0.8 Co 0.2 O2 is used as the positive electrode material of the battery.
[0081] Comparative Example 5:
[0082] The difference from Example 1 is that there are no steps 1 and 2, and in step 3, vanadium pentoxide (V2O5) is used to replace anhydrous vanadium citrate, and the particle size of the vanadium pentoxide (V2O5) used is 5-10 μm.
[0083] Comparative Example 6:
[0084] The difference from Example 1 is that there are no steps 1 and 2, and in step 3, ammonium metavanadate (NH4VO3) is used to replace anhydrous vanadium citrate, and the particle size of the ammonium metavanadate (NH4VO3) used is 5-10 μm.
[0085] Comparative Example 7:
[0086] The difference from Example 1 is that there are no steps 1 and 2. In step 3, vanadium pentoxide (V2O5) is used to replace anhydrous vanadium citrate, and the calcination temperature and time are adjusted so that the vanadium doping amount in the obtained vanadium-doped nickel-cobalt-manganese lithium-ion battery positive electrode material is similar to that in Example 1.
[0087] Comparative Example 8:
[0088] The difference from Example 1 is that there are no steps 1 and 2. In step 3, ammonium metavanadate (NH4VO3) is used to replace anhydrous vanadium citrate, and the calcination temperature and time are adjusted so that the vanadium doping amount in the obtained vanadium-doped nickel-cobalt-manganese lithium-ion battery positive electrode material is similar to that in Example 1.
[0089] In the present application, the vanadium-doped nickel-cobalt-manganese lithium-ion battery positive electrode materials obtained in Examples 1-4 and the materials in Comparative Examples 1-6 are prepared into lithium-ion batteries, and these lithium-ion batteries are subjected to charge and discharge cycles under set voltage and rate conditions, and the first discharge specific capacity, coulombic efficiency, capacity retention rate and impedance, etc. are tested. Please refer to Table 1 for the test results.
[0090] The present application also carried out ICP testing on the vanadium-doped nickel-cobalt-manganese lithium-ion battery positive electrode materials obtained in Example 1 and Comparative Examples 7-8 to detect the vanadium doping amount therein. The test results and the calcination conditions required to achieve the vanadium doping amount are shown in Table 2.
[0091] Table 1. Test results of first discharge specific capacity and cycle capacity retention rate of Example 1 and Comparative Examples 5-6 of the present application
[0092] First discharge specific capacity (mAh / g) Capacity retention after 100 cycles Example 1 203 85% Comparative Example 5 200 81% Comparative Example 6 199 79%
[0093] Please refer to Table 1. Compared with Comparative Examples 5 and 6, Example 1 has a relatively higher first discharge specific capacity and cycle capacity retention rate when using a vanadium source of the same particle size grade and the same preparation conditions, indicating that compared with vanadium pentoxide or ammonium metavanadate, anhydrous vanadium citrate is used as a vanadium doping carrier, and the preparation method of the present application can obtain a positive electrode material with better doping modification effect.
[0094] Table 2. Vanadium doping amount and calcination conditions of Example 1 and Comparative Examples 7-8 of the present application
[0095] Vanadium doping amount Step 3 Calcination temperature (°C) Step 3 Calcination time (h) Example 1 0.13% 400+710 3+3 Comparative Example 7 0.13% 400+760 5+10 Comparative Example 8 0.13% 400+770 5+10
[0096] Please refer to Table 2. Compared with Comparative Examples 7 and 8, Example 1 has milder calcination conditions under the condition of achieving similar vanadium doping amount. For example, when calcining at 400°C to promote grain nucleation, Example 1 requires significantly less calcination time than Comparative Examples 7 or 8. When calcining at a higher temperature to promote the growth of nucleated grains, Example 1 requires significantly less calcination temperature and time than Comparative Examples 7 or 8. This shows that compared with vanadium pentoxide or ammonium metavanadate, the preparation method of the present application can reduce the energy consumption and time required for doping by using anhydrous vanadium citrate as a vanadium doping carrier, and effectively reduce the preparation cost.
[0097] Example 1 compared with Comparative Example 1:
[0098] See also Figure 1(a) and (c) in the figure, under the conditions of 3-4.5V and 0.2C, the discharge capacity of the first cycle of comparative example 1 is 198mAh / g, the coulombic efficiency is 82.2%, the capacity retention rate after 100 cycles is 75%, and the capacity retention rate after 300 cycles is 40%. Please refer to Figure 1 In (b) and (c), under the conditions of 3-4.5V and 0.2C, the discharge capacity of Example 1 in the first cycle is 203mAh / g, the coulombic efficiency is 82.5%, the capacity retention rate after 100 cycles is 85%, and the capacity retention rate after 300 cycles is 49%. Please refer to Figure 1 In (d), when reaching 10C, the capacity of Example 1 is 119.0 mAh / g, while that of Comparative Example 1 is only 84.4 mAh / g. This indicates that after Example 1 is modified by vanadium doping using anhydrous vanadium citrate as a doping carrier, the first coulombic efficiency, capacity retention rate and rate performance of the obtained positive electrode material are significantly improved.
[0099] See also Figure 1 In (e) and (f), under the conditions of 3-4.5V and 0.2C, the peaks near 3.8V, 4.1V and 4.3V represent H1-M, M-H2 and H2-H3 phase transitions, respectively. As charging proceeds, a hexagonal-monoclinic-hexagonal structural transition occurs in Comparative Example 1, accompanied by a large anisotropic lattice mutation, which is an important cause of microcracks. The degree of H2-H3 phase transition in Example 1 is low, and the curves of different cycle numbers have a high degree of overlap, indicating that vanadium doping with anhydrous vanadium citrate as the doping carrier suppresses the adverse phase transition during the charge and discharge process, and improves the reversibility of the phase transition and the structural stability.
[0100] See also Figure 1 In (g), the ohmic impedance (R0) of comparative example 1 is 1.871Ω, and the charge transfer impedance (R ct ) is 181.1Ω, R0 of Example 1 is 12.03Ω, R ct is 151.1Ω, that is, Example 1 has a relatively smaller charge transfer impedance. Figure 1 In (h), the internal resistance of the battery in comparative example 1 increases significantly as the cycle progresses, which is one of the reasons for the decrease in capacity.
[0101] Example 2 is compared with Comparative Example 2:
[0102] See also Figure 2 In (a) and (c), at 3-4.3V, 0.2C, the discharge capacity of the first cycle of comparative example 2 is 173.2mAh / g, the coulombic efficiency is 76.1%, and the capacity retention rate after 100 cycles is 97.1%. Please refer to Figure 2In (b) and (c), the discharge capacity of Example 2 in the first cycle is 188.6 mAh / g, the coulombic efficiency is 78.3%, and the capacity retention rate after 100 cycles is 98.2%. Please refer to Figure 2 (d) in the figure shows that under the conditions of 3-4.5V and 0.2C, the discharge capacity of the first cycle of Comparative Example 2 is 204.7mAh / g, the coulombic efficiency is 81.9%, and the capacity retention rate after 200 cycles is 35.7%. The discharge capacity of the first cycle of Example 2 is 206.4mAh / g, the coulombic efficiency is 82.7%, and the capacity retention rate after 200 cycles is 42.6%. This shows that after Example 2 is subjected to vanadium doping modification using anhydrous vanadium citrate as the doping carrier, the first coulombic efficiency and capacity retention rate of the obtained positive electrode material are significantly improved.
[0103] See also Figure 2 In (e) and (f), the degree of H2-H3 phase transition in Example 2 is lower than that in Comparative Example 2, and the curves of different cycle numbers have a high degree of overlap, indicating that vanadium doping with anhydrous vanadium citrate as the doping carrier suppresses the adverse phase transition during the charge and discharge process and improves the structural stability.
[0104] See also Figure 2 In (g), when reaching 10C, the capacity of Example 2 is 116.1 mAh / g, while that of Comparative Example 2 is only 106.1 mAh / g. This indicates that after Example 2 is subjected to vanadium doping modification using anhydrous vanadium citrate as a doping carrier, the rate performance of the obtained positive electrode material is significantly improved.
[0105] See also Figure 2 In (h), the ohmic impedance (R0) of comparative example 2 is 1.237Ω, and the charge transfer impedance (R ct ) is 208.2Ω, R0 of Example 2 is 1.361Ω, R ct is 200.1Ω, that is, Example 2 has a relatively smaller charge transfer impedance. After ten cycles, SEI is formed. Figure 2 In (i), the (R0) of Comparative Example 2 is 1.062Ω, R SEI is 21.61Ω, R ct is 75.6Ω, while R0 of Example 2 is 3.683Ω, R SEI is 35.06Ω, R ct It is 29.5Ω, which shows that the internal resistance of the battery increases with the progress of the cycle. However, under the same conditions, the impedance of Example 2 is smaller than that of Comparative Example 2, indicating that after the vanadium doping modification using anhydrous vanadium citrate as the doping carrier in Example 2, R ct The charge transfer resistance is reduced, the lithium ion diffusion is accelerated, and thus the rate performance is better.
[0106] Example 3 compared with Comparative Example 3:
[0107] See also Figure 3 (a) and (c) in the figure, under the conditions of 3-4.5V and 1C, the discharge capacity of the first cycle of comparative example 3 is 181mAh / g, the coulombic efficiency is 81.9%, and the capacity retention rate after 200 cycles is 27%. Please refer to Figure 3 In (b) and (c), under the conditions of 3-4.5V and 1C, the discharge capacity of Example 3 in the first cycle is 175mAh / g, the coulombic efficiency is 83.1%, and the capacity retention rate after 200 cycles is 45%. Please refer to Figure 3 In (d), when reaching 10C, the capacity of Example 3 is 120 mAh / g, while that of Comparative Example 3 is only 108 mAh / g. This shows that after Example 3 is modified by vanadium doping with anhydrous vanadium citrate as the doping carrier, the first coulombic efficiency, capacity retention rate and rate performance of the obtained positive electrode material are significantly improved.
[0108] Example 4 is compared with Comparative Example 4:
[0109] See also Figure 4 (a) and (c) in the figure, under the conditions of 3-4.5V and 1C, the discharge capacity of the first cycle of comparative example 4 is 198mAh / g, and the capacity retention rate after 100 cycles is 50%. Please refer to Figure 4 In (b) and (c), under the conditions of 3-4.5V and 1C, the discharge capacity of Example 4 in the first cycle is 205mAh / g, and the capacity retention rate after 100 cycles is 77%. Please refer to Figure 4 In (d), when the temperature reaches 10C, the capacity of Example 4 is 125 mAh / g, while that of Comparative Example 4 is only 110 mAh / g. This indicates that after Example 4 is modified by vanadium doping with anhydrous vanadium citrate as the doping carrier, the capacity retention rate and rate performance of the obtained positive electrode material are significantly improved.
[0110] The above results show that after vanadium doping modification of ternary positive electrode materials (such as lithium nickel cobalt manganese oxide) using anhydrous vanadium citrate as a doping carrier, the resulting modified ternary positive electrode material has a relatively significant performance improvement. The preparation process of doping modification of ternary positive electrode materials using anhydrous vanadium citrate as a doping carrier in this application is simple and energy-saving, which is conducive to reducing production costs and being used for large-scale production.
[0111] The above implementation modes are only used to illustrate the technical solutions of the present application and are not intended to limit the present application. Although the present application has been described in detail with reference to the above preferred implementation modes, a person skilled in the art should understand that the technical solutions of the present application may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present application.
Claims
1. A method for preparing a vanadium-doped nickel-cobalt-manganese ternary positive electrode material, characterized in that: include: Providing a vanadium citrate aqueous solution, evaporating and crystallizing the vanadium citrate aqueous solution and performing a calcination to obtain anhydrous vanadium citrate; The anhydrous vanadium citrate is mixed with lithium nickel cobalt manganese oxide to obtain a mixture, and the mixture is subjected to secondary calcination to obtain the vanadium-doped nickel cobalt manganese ternary positive electrode material.
2. The preparation method according to claim 1, characterized in that The providing of the vanadium citrate aqueous solution comprises mixing vanadium pentoxide with citric acid, and heating the mixture to allow the vanadium pentoxide to react with the citric acid.
3. The preparation method according to claim 1, characterized in that: The temperature of the evaporation crystallization is 60° C. to 100° C., and the time is 2 h to 4 h.
4. The preparation method according to claim 1, characterized in that: The primary calcination is performed in an oxygen-containing atmosphere at a temperature of 180° C. to 220° C. for a time of 2 h to 3 h.
5. The preparation method according to claim 1, characterized in that: The particle size of the anhydrous vanadium citrate is 500nm to 800nm.
6. The preparation method according to claim 1, characterized in that: The mixing speed is 200 r / min to 300 r / min.
7. The preparation method according to claim 1, characterized in that: The secondary calcination is performed in an oxygen-containing atmosphere, the temperature of the secondary calcination is 400° C. to 730° C., and the time is 3 h to 6 h.
8. A vanadium-doped nickel-cobalt-manganese ternary positive electrode material, characterized in that: Prepared by the preparation method according to any one of claims 1 to 7, the molecular formula of the vanadium-doped nickel-cobalt-manganese ternary positive electrode material is LiNi x Co y Mn z V a O2, 0.8≤x≤0.96, 0.02≤y≤0.2, 0.02≤z≤0.2, 0.0013≤a≤0.0043.
9. A positive electrode sheet, comprising a positive electrode current collector and a positive electrode active material layer disposed on at least one surface of the positive electrode current collector, characterized in that: The positive electrode active material layer includes the vanadium-doped nickel-cobalt-manganese ternary positive electrode material as claimed in claim 8.
10. A lithium-ion battery, comprising an electrode assembly, wherein the electrode assembly comprises a separator and a negative electrode plate, characterized in that: It also includes the positive electrode sheet as described in claim 9, wherein the isolation film is arranged between the positive electrode sheet and the negative electrode sheet.
Citation Information
Patent Citations
Ternary composite positive electrode material of lithium ion battery and preparation method thereof
CN103259008A
Vanadium-doped Ni-Co-Mn lithium ion battery positive electrode material
CN107799739A
Preparation method of nickel-cobalt-manganese-aluminum composite positive electrode material co-coated with lithium manganese vanadium phosphate and carbon
CN110518206A
Manufacturing method of active material, active material and lithium ion secondary battery
JP2012004045A
Synthesis and characterization of vanadium complexes
US20220396593A1