Electrolyte-free Si-Sn-SWCNTs negative electrode material as well as preparation method and application thereof

Through the use of electrolyte-free Si-Sn-SWCNTs negative electrode materials, the performance attenuation problem caused by volume changes in the electrochemical cycle of lithium-ion battery negative electrode materials is solved, and the high energy density and stability of all-solid-state batteries are achieved, which improves the The dynamics and cycling performance of the battery.

CN119069680APending Publication Date: 2024-12-03WUHAN GULI NEW ENERGY TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411307148.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-19
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The volume changes in the existing lithium-ion battery anode materials during the electrochemical cycle lead to material rupture and electrode degradation, resulting in rapid attenuation of battery performance, and the energy density and stability of high-capacity anode materials in all-solid state batteries are insufficient.

Method used

The electrolyte-free Si-Sn-SWCNTs negative electrode material is used to form an excellent mixed ion-electronic conductor through the synergistic effect of Si and Sn composite materials and SWCNTs, and the electrolyte-free sheet negative electrode material is prepared by using SWCNTs as a binder. in sulfide all-solid state batteries.

Benefits of technology

It significantly improves the dynamic performance and cycle stability of all-solid-state batteries, increases surface capacity and material utilization, reduces void generation during the cycle, maintains electrical connections, and improves the overall performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069680A_ABST
    Figure CN119069680A_ABST
Patent Text Reader

Abstract

The invention provides an electrolyte-free Si-Sn-SWCNTs negative electrode material as well as a preparation method and application thereof, and belongs to the technical field of lithium-sulfur battery negative electrode materials. The electrolyte-free type Si-Sn-SWCNTs negative electrode material comprises a Si-Sn composite material and SWCNTs, wherein the Si-Sn composite material and the SWCNTs Wherein the Si-Sn composite material comprises a mixture of Si and Sn. According to the preparation method, Si powder and Sn powder are mixed through a simple ball milling method to obtain a Si-Sn composite material, SWCNTs are used as a binder to form slurry, the slurry is coated on a copper foil, and the electrolyte-free Si-Sn-SWCNTs negative electrode material is prepared. The electrolyte-free Si-Sn-SWCNTs negative electrode material is prepared by combining the advantages of pure Si and pure Sn and matching with SWCNTs, and the electrolyte-free Si-Sn-SWCNTs negative electrode material can show excellent dynamic performance and cycling stability when being applied to an all-solid-state battery. In addition, the Si-Sn composite material is used as the negative electrode material, and no solid electrolyte is added, so that the all-solid-state battery can show higher surface capacity and higher material utilization rate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of sulfur-lithium battery negative electrode materials, and in particular to an electrolyte-free Si-Sn-SWCNTs negative electrode material and a preparation method and application thereof. Background Art

[0002] Currently, commercial lithium-ion batteries mainly use graphite as the negative electrode, and their energy density has gradually approached the theoretical limit (~280 Wh kg -1 ), and the most feasible way to further improve the energy density of lithium-ion batteries is to replace the traditional graphite negative electrode with high-capacity materials, such as metal Li, Si, Sn, Mg, Al, Bi, Zn and Sb. However, a common problem of these negative electrode materials is that during the electrochemical cycle, the volume of the material will change dramatically, causing the material to break / crush and expose new surfaces to the liquid electrolyte, which in turn leads to severe electrode degradation and continuous electrolyte / electrode interface reactions, as well as rapid attenuation of battery performance. All-solid-state batteries are considered to be a key technology in the future. The use of solid electrolytes instead of carbonate-based liquid electrolytes has great potential to update the positive / negative electrode materials of current lithium-ion batteries and achieve high energy density and high safety batteries. Among them, sulfide-based solid electrolytes have high room temperature ionic conductivity (>10 -3 S cm -1 ) and excellent mechanical ductility, especially sulfide solid electrolytes (SSEs) cannot flow like liquid electrolytes, which has significant advantages in alleviating repeated electrolyte / electrode interface reactions caused by volume changes. This completely different chemical-mechanical environment makes this type of high-capacity anode material more stable in all-solid-state batteries. To date, most sulfide all-solid-state batteries studied have electrodes based on powder mixtures, which include mechanical mixing of active materials, solid electrolytes and conductive carbon additives. In order to establish an effective ion / electron permeation network, inactive ingredients (solid electrolytes and carbon conductive agents) usually account for a large proportion of the electrodes, which significantly reduces the energy density of high-capacity anode materials. Summary of the invention

[0003] In view of the deficiencies of the above-mentioned prior art, the present invention provides an electrolyte-free Si-Sn-SWCNTs negative electrode material and a preparation method and application thereof, utilizing the respective advantages of Si and Sn negative electrode materials, and synergizing Si-Sn composite materials with SWCNTs as negative electrode materials for all-solid-state batteries, which can enable the all-solid-state batteries to exhibit excellent kinetic performance and cycle stability.

[0004] To achieve the above purpose, the specific technical solutions of the present invention are as follows:

[0005] In a first aspect, the present invention provides an electrolyte-free Si-Sn-SWCNTs negative electrode material, wherein the negative electrode material comprises a Si-Sn composite material and SWCNTs (single-walled carbon nanotubes); wherein the Si-Sn composite material comprises a mixture of Si and Sn; and the mass ratio of the Si-Sn composite material to SWCNTs is (99.5~99.8):(0.2~0.5).

[0006] Preferably, the method for preparing the Si-Sn composite material comprises the following steps: in an inert atmosphere, mixing Si powder and Sn powder, and ball-milling the mixture into a mixed powder to obtain a Si-Sn composite material, denoted as Si-Sn.

[0007] More preferably, the mass ratio of the Si powder to the Sn powder is (2-3):(3-4).

[0008] Further preferably, the specific operation of the ball milling is: using zirconium dioxide ball milling beads, the diameters of the zirconium dioxide ball milling beads are 4 / 10 / 15 mm respectively, the mass ratio of ball milling beads to materials is 30:1, the ball milling speed is 500 rpm, the time is 12~24h, each rotation is 30 min, and stop for 5 min.

[0009] Sn and Si have the advantages of high natural abundance, large weight / volume capacity, and low average working potential as negative electrode materials. Therefore, they have also been widely studied as high-energy negative electrode materials in sulfide all-solid-state batteries. + When considering the diffusion and electron transport of electrolyte-free anode active materials, two main differences between them should be considered: the electronic conductivity of semiconductor Si is much lower than that of metallic Sn, but the Li + The diffusion rate is much better than that of Sn. Therefore, the present invention forms a hybrid composed of Sn and Si to form an excellent mixed ion-electron conductor. In addition, the present invention uses a ball-milled mixture of Si and Sn as an active material and SWCNTs as a binder to prepare an electrolyte-free thin-sheet negative electrode material, which is applied to sulfide all-solid-state batteries; wherein SWCNTs can improve the structural stability of Si-Sn composite materials relative to ordinary PVDF binders, and better maintain electrical connections by reducing the gaps generated during the cycle, so that the electrolyte-free Si-Sn-SWCNTs negative electrode material can exhibit enhanced reaction kinetics and cycle stability.

[0010] In a second aspect, the present invention provides a method for preparing the electrolyte-free Si-Sn-SWCNTs negative electrode material, comprising the following steps: dispersing the Si-Sn composite material and SWCNTs in a solvent and mixing them evenly to obtain a slurry, casting the slurry on a copper foil, and vacuum drying at 90-110° C. to obtain an electrolyte-free Si-Sn-SWCNTs negative electrode material.

[0011] Preferably, the solvent is N-methyl-2-pyrrolidone.

[0012] Preferably, the drying time is 12 h.

[0013] In a third aspect, the present invention provides the application of the electrolyte-free Si-Sn-SWCNTs negative electrode material in the negative electrode of an all-solid-state battery.

[0014] In a fourth aspect, the present invention provides an all-solid-state battery, comprising an electrolyte-free Si-Sn-SWCNTs negative electrode material.

[0015] Preferably, the all-solid-state battery further comprises a cathode material and a dual solid-state electrolyte.

[0016] Further preferably, the dual solid-state electrolyte includes a positive electrode side solid electrolyte and a negative electrode side solid electrolyte; wherein the positive electrode side solid electrolyte is Li3InCl6, and the negative electrode side solid electrolyte is Li6PS5Cl.

[0017] Further preferably, the positive electrode material is a composite material, and the composite material includes: LiNi 0.8 Co0 .1 Mn 0.1 O2 (NCM811), positive electrode side solid electrolyte and vapor grown carbon fiber (VGCF).

[0018] Further preferably, the positive electrode side solid electrolyte is Li3InCl6; the preparation method of Li3InCl6 is as follows: an aqueous solution containing LiCl and InCl3·4H2O is mixed in a molar ratio of 3:1, and dried to obtain Li3InCl6.

[0019] Further preferably, the LiNi 0.8 Co 0.1 Mn 0.1 The mass ratio of O2, positive electrode side solid electrolyte, and vapor-grown carbon fiber is 60:35:5.

[0020] Compared with the prior art, the present invention is beneficial in that:

[0021] The present invention rationally utilizes the advantages of Si or Sn as the negative electrode material, and combines Si-Sn composite materials with SWCNTs to prepare electrolyte-free Si-Sn-SWCNTs negative electrode materials, which are applied to all-solid-state batteries. The synergistic effect between Si, Sn and SWCNTs can enable the all-solid-state battery to exhibit excellent kinetic performance and cycle stability. In addition, since the Si-Sn composite material is used as the negative electrode material without adding a solid electrolyte, the all-solid-state battery can exhibit a higher surface capacity and a higher material utilization rate. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 XRD spectra of Sn, Si and Si-Sn composites;

[0023] Figure 2 Schematic diagram of electrolyte-free Si-Sn-SWCNTs anode material for Li-In alloy solid-state full battery;

[0024] Figure 3 The electrochemical performance test results of B3; 3a is the selected constant current charge and discharge voltage curve of B3; 3b is the cycle performance of B3 at 0.1C;

[0025] Figure 4 The electrochemical performance test results of B4; 4a is the selected constant current charge and discharge voltage curve of B4; 4b is the cycle performance of B4 at 0.1C;

[0026] Figure 5 The electrochemical performance test results of B1 and B2; 5a is the comparison of the constant current charge and discharge voltage curves of B1 and B2 in the first cycle; 5b is the cycle performance of B2 at 0.1C; 5c is the cycle performance of B1 at 0.1C;

[0027] Figure 6 This is the cycle performance diagram of B5 at 0.1C;

[0028] Figure 7 is the cycle performance diagram of A1 at 0.5C;

[0029] Figure 8 This is the rate performance diagram of A1. DETAILED DESCRIPTION

[0030] The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] The present invention provides an electrolyte-free Si-Sn-SWCNTs negative electrode material, wherein the negative electrode material comprises a Si-Sn composite material and SWCNTs (single-walled carbon nanotubes); wherein the Si-Sn composite material comprises a mixture of Si and Sn; and the mass ratio of the Si-Sn composite material to the SWCNTs is (99.5-99.8):(0.2-0.5).

[0032] In the following specific embodiments, the preparation method of the Si-Sn composite material comprises the following steps: in an inert atmosphere, Si powder and Sn powder are mixed, ball-milled into a mixed powder, and a Si-Sn composite material is obtained; the mass ratio of the Si powder to the Sn powder is 2:3; the specific operation of the ball milling is: using zirconium dioxide ball milling beads, the diameters of the zirconium dioxide ball milling beads are 4 / 10 / 15 mm, respectively, the mass ratio of the ball milling beads to the material is 30:1, the ball milling speed is 500 rpm, the time is 12~24 h, each rotation is 30 min, and the stop time is 5 min.

[0033] Example 1

[0034] An electrolyte-free Si-Sn-SWCNTs negative electrode material, the preparation steps are as follows:

[0035] (1) Preparation of Si-Sn composite materials: In an argon environment, Si powder and Sn powder were mixed in a mass ratio of 2:3 and mechanically ball milled at 500 rpm for 24 h to obtain Si-Sn composite materials. Figure 1 The XRD patterns of Si-Sn composite material, Si powder and Sn powder are compared. Figure 1 It can be seen that the XRD spectrum of the Si-Sn composite material is a simple combination of the XRD spectra of Si powder and Sn powder, indicating that the ball milling treatment will not cause alloy reaction between Si powder and Sn powder.

[0036] (2) Preparation of negative electrode materials: The Si-Sn composite material and SWCNTs were dispersed in N-methyl-2-pyrrolidone at a mass ratio of 99.8:0.2, stirred evenly to obtain a slurry, cast the slurry on a copper foil, and vacuum dried at 110 °C for 12 h to obtain an electrolyte-free Si-Sn-SWCNTs negative electrode material.

[0037] Comparative Example 1

[0038] An electrolyte-free Si-Sn-PVDF negative electrode material, the preparation steps are as follows:

[0039] (1) Preparation of Si-Sn composite materials: In an argon environment, Si powder and Sn powder were mixed in a mass ratio of 2:3 and mechanically ball milled at 500 rpm for 24 h to obtain Si-Sn composite materials.

[0040] (2) Preparation of negative electrode material: Disperse Si-Sn composite material and PVDF in N-methyl-2-pyrrolidone at a mass ratio of 99.8:0.2, stir evenly to obtain slurry, cast the slurry on copper foil, and vacuum dry at 110 °C for 12 h to obtain electrolyte-free Si-Sn-PVDF negative electrode material.

[0041] Comparative Example 2

[0042] An electrolyte-free Si-SWCNTs negative electrode material, the preparation steps are as follows:

[0043] Si powder and SWCNTs were dispersed in N-methyl-2-pyrrolidone at a mass ratio of 99.8:0.2, stirred evenly to obtain a slurry, cast the slurry on a copper foil, and finally vacuum dried at 110 °C for 12 h to obtain an electrolyte-free Si-SWCNTs negative electrode material.

[0044] Comparative Example 3

[0045] An electrolyte-free Sn-SWCNTs negative electrode material, the preparation steps are as follows:

[0046] Sn powder and SWCNTs were dispersed in N-methyl-2-pyrrolidone at a mass ratio of 99.8:0.2, stirred evenly to obtain a slurry, cast the slurry on a copper foil, and finally dried in vacuum at 110 °C for 12 h to obtain an electrolyte-free Sn-SWCNTs negative electrode material.

[0047] Comparative Example 4

[0048] An electrolyte-free Si-Sn-SWCNTs negative electrode material, the preparation steps are as follows:

[0049] (1) Preparation of Si-Sn composite materials: In an argon environment, Si powder and Sn powder were mixed in a mass ratio of 2:3 and mechanically ball milled at 500 rpm for 24 h to obtain Si-Sn composite materials.

[0050] (2) Preparation of negative electrode materials: The Si-Sn composite material and SWCNTs were dispersed in N-methyl-2-pyrrolidone at a mass ratio of 99:1, stirred evenly to obtain a slurry, cast the slurry on a copper foil, and vacuum dried at 110 °C for 12 h to obtain an electrolyte-free Si-Sn-SWCNTs negative electrode material.

[0051] Application Examples

[0052] The negative electrode material obtained in Example 1 was used to prepare an all-solid-state battery by the following method, and the obtained all-solid-state battery was recorded as A1:

[0053] S1. Prepare a positive electrode side solid electrolyte: In an argon environment, mix aqueous solutions of LiCl and InCl3·4H2O in a molar ratio of 3:1, stir evenly and then dry to obtain a Li3InCl6 halide positive electrode side solid electrolyte;

[0054] S2. Preparation of positive electrode materials: In a glove box filled with argon, LiNi 0.8 Co 0.1 Mn 0.1 O2 (NCM811), positive electrode solid electrolyte Li3InCl6 and vapor grown carbon fiber (VGCF) were ground and mixed in a mass ratio of 60:35:5 to obtain a positive electrode material;

[0055] S3. Preparation of all-solid-state batteries: Take 70 mg of Li3InCl6 solid electrolyte powder on the positive electrode side and 80 mg of Li6PS5Cl solid electrolyte powder on the negative electrode side and place them in the solid-state battery mold in sequence, and pressurize them at 250 MPa; then add positive electrode materials on the Li3InCl6 layer side and place negative electrode materials on the Li6PS5Cl layer side, further pressurize the assembled full battery at 380 MPa, and finally apply a stacking pressure of 60 MPa on the mold for further electrochemical testing.

[0056] The negative electrode materials obtained in Example 1 and Comparative Examples 1 to 4 were used to prepare all-solid-state batteries by the following method. The obtained all-solid-state batteries were respectively denoted as B1, B2, B3, B4, and B5:

[0057] 100 mg of solid electrolyte powder Li6PS5Cl was placed in a solid-state battery mold and pressurized at 250 MPa; the negative electrode material was placed on one side of the solid electrolyte and a pressure of 380 MPa was applied; then the Li-In alloy was placed as a counter electrode on the other side of the solid electrolyte and a pressure of 125 MPa was applied; finally, a stacking pressure of 60 MPa was applied to the mold for further electrochemical testing. Figure 2 Schematic diagram of the internal structure of the electrolyte-free Si-Sn-SWCNTs negative electrode material for Li-In alloy all-solid-state battery.

[0058] Electrochemical testing of all-solid-state batteries:

[0059] The electrochemical performance of all-solid-state batteries A1, B1~B5 were tested using Wuhan Blue Electric CT2001A battery tester. A1 operated in the voltage window of 2.0~4.2 V, with a fixed N / P ratio of ~1.2, the cycle performance was carried out at 0.5C, and the rate performance was carried out at 0.1, 0.2, 0.5, 0.8, and 1C; B1~B5 operated in the voltage window of -0.61~1.38 V, and the cycle performance was carried out at 0.1C.

[0060] Figure 3 The electrochemical performance test results of B3 are shown in Figure 3a, where 3a is the selected constant current charge-discharge voltage curve of B3; 3b is the cycle performance of B3 at 0.1C. The mass loading of Si powder in B3 is about 0.35 mg cm -2 ,Depend on Figure 3 b shows that at 0.1C, B3 can provide 3350 mAh g -1 The high initial charge capacity of Si-SWCNTs was achieved, but the capacity decayed sharply in subsequent cycles, with the capacity retention rate being only 59% after 160 cycles; this result indicates that the electrolyte-free Si-SWCNTs electrode cannot operate stably even at relatively low load levels. Figure 4 The electrochemical performance test results of B4 are shown in Figure 4a, where 4a is the selected constant current charge and discharge voltage curve of B4; 4b is the cycle performance of B4 at 0.1C. The mass loading of Sn powder in B4 is about 0.94 mgcm -2 ,Depend on Figure 4 b shows that at 0.1C, B4 can provide 800 mAh g -1 With a high initial charge capacity, B4 exhibited capacity fluctuations in the first 50 cycles; its capacity decayed slowly in the subsequent cycles; and after 200 cycles, its capacity retention rate was as high as 86.5%, which was superior to the electrolyte-free Si-SWCNTs electrode of B3. Figure 4 The results show that the electrolyte-free Sn-SWCNTs electrode exhibits relatively excellent cycling performance, which undergoes an electrode activation process during the initial cycle, which may be related to the Li + In summary, compared with the electrolyte-free Sn-SWCNTs electrode, the electrolytic-free Si-SWCNTs electrode has a higher surface capacity but poorer cyclability. This is because the electronic conductivity of Si is significantly lower than that of Sn, and the Li + The diffusion rate is much better than Sn.

[0061] In order to give full play to the respective advantages of Si and Sn, Si powder and Sn powder were mixed and matched with SWCNTs and PVDF to assemble into batteries B1 and B2 respectively. Figure 5 The electrochemical performance test results of B1 and B2; 5a is the comparison of the constant current charge and discharge voltage curves of B1 and B2 in the first cycle; 5b is the cycle performance of B2 at 0.1C; 5c is the cycle performance of B1 at 0.1C. Figure 5 a It can be seen that the polarization of B2 (electrolyte-free Si-Sn-PVDF negative electrode material) is greater than that of B1 (electrolyte-free Si-Sn-SWCNTs negative electrode material); Figure 5b and 5c show that after 50 deep charge and discharge cycles, the capacity retention rate of B2 is 42.1%, which is much lower than the capacity retention rate of B1 after 50 deep charge and discharge cycles (91.4%). Therefore, SWCNTs are more suitable as a binder for Si-Sn composite materials than PVDF. The preparation of negative electrode materials by using Si-Sn composite materials in conjunction with SWCNTs can improve the stability of the entire electrode structure and the cycle stability of the entire battery. In addition, Figure 6 is the cycle performance diagram of B5 at 0.1C, Figure 6 It can be seen that after 50 deep charge and discharge cycles, the capacity retention rate of B5 is only 85.1%, which is lower than the capacity retention rate of B1 after 50 deep charge and discharge cycles (91.4%). This result shows that increasing the amount of binder SWCNTs cannot enhance the cycle performance of the Si-Sn mixture.

[0062] In order to demonstrate the application potential of Si-Sn-SWCNTs negative electrode materials in all-solid-state batteries, the present invention constructed a complete battery A1 by pairing it with commercial NCM811 positive electrode material. Figure 7 is the cycle performance diagram of A1 at 0.5C, Figure 7 It can be seen that at 0.5C, the mass loading of NCM811 in A1 is 11.3 mg cm -2 , the average coulombic efficiency of A1 after 200 cycles was 99.38%, and the capacity retention rate was 84.1%, showing good cycle performance; Figure 8 is the rate performance diagram of A1, Figure 8 It can be seen that A1 exhibits excellent rate performance, with specific capacities of 163, 155, 138, 84, and 60 mAh g at 0.1, 0.2, 0.5, 0.8, and 1 C, respectively. -1 At the same time, when the current density is restored to 0.1C, the specific capacity can be restored to 150 mAh g -1 Therefore, the Si-Sn-SWCNTs negative electrode material provided by the present invention is a very potential all-solid-state battery negative electrode material.

[0063] In summary, the present invention utilizes the respective advantages of pure Si and pure Sn, and through a simple ball milling method, Si powder and Sn powder are mixed to obtain a Si-Sn composite material, and SWCNTs are used as a binder to form a slurry coated on a copper foil to prepare an electrolyte-free Si-Sn-SWCNTs negative electrode material. The prepared electrolyte-free Si-Sn-SWCNTs negative electrode material is applied to an all-solid-state battery, wherein SWCNTs can improve the structural stability of the Si-Sn composite material relative to the ordinary PVDF binder, and better maintain electrical connection by reducing the gaps generated during the cycle, so that the electrolyte-free Si-Sn-SWCNTs negative electrode material can exhibit enhanced reaction kinetics and cycle stability. In addition, since the Si-Sn composite material is used as a negative electrode material without adding a solid electrolyte, the all-solid-state battery can exhibit a higher surface capacity and a higher material utilization rate.

[0064] The above specific embodiments describe the implementation of the present invention in detail, but the present invention is not limited to the specific details in the above embodiments. Within the scope of the claims and technical concept of the present invention, the technical solution of the present invention can be modified and changed in many simple ways, and these simple modifications all belong to the protection scope of the present invention.

Claims

1. An electrolyte-free Si-Sn-SWCNTs negative electrode material, It is characterized in that It comprises a Si-Sn composite material and SWCNTs; wherein the Si-Sn composite material comprises a mixture of Si and Sn; and the mass ratio of the Si-Sn composite material to the SWCNTs is (99.5-99.8): (0.2-0.5).

2. The electrolyte-free Si-Sn-SWCNTs negative electrode material according to claim 1, It is characterized in that The preparation method of the Si-Sn composite material comprises the following steps: in an inert atmosphere, Si powder and Sn powder are mixed, ball-milled into mixed powder, and the Si-Sn composite material is obtained.

3. The electrolyte-free Si-Sn-SWCNTs negative electrode material according to claim 2, It is characterized in that The mass ratio of the Si powder to the Sn powder is (2-3): (3-4).

4. A method for preparing an electrolyte-free Si-Sn-SWCNTs negative electrode material, It is characterized in that The method comprises the following steps: dispersing Si-Sn composite material and SWCNTs in a solvent and mixing them evenly to obtain slurry, casting the slurry on a copper foil, and vacuum drying at 90-110° C. to obtain an electrolyte-free Si-Sn-SWCNTs negative electrode material.

5. An all-solid-state battery, It is characterized in that The all-solid-state battery comprises the electrolyte-free Si-Sn-SWCNTs negative electrode material as described in any one of claims 1 to 3, or comprises the electrolyte-free Si-Sn-SWCNTs negative electrode material prepared by the method described in claim 4.

6. The all-solid-state battery according to claim 5, It is characterized in that The all-solid-state battery also includes a positive electrode material and a dual solid-state electrolyte.

7. The all-solid-state battery according to claim 6, It is characterized in that The dual solid electrolyte comprises a positive electrode side solid electrolyte and a negative electrode side solid electrolyte, wherein the positive electrode side solid electrolyte is Li 3 InCl 6 The solid electrolyte on the negative electrode side is Li 6 PS 5 Cl.

8. The all-solid-state battery according to claim 6, It is characterized in that The positive electrode material is a composite material, which includes: LiNi 0.8 Co 0.1 Mn 0.1 O 2 , solid electrolyte on the positive electrode side and vapor-grown carbon fiber.

9. The all-solid-state battery according to claim 8, It is characterized in that The LiNi 0.8 Co 0.1 Mn 0.1 O 2 The mass ratio of the positive electrode side solid electrolyte and the vapor-grown carbon fiber is 60:35:5.

Citation Information

Cited By

  • All-solid-state battery comprising fusible metal alloy