Low-temperature lithium iron phosphate positive electrode material as well as preparation method and application thereof
By doping zirconate and rhodium chloride in lithium iron phosphate batteries, combined with Rh3+ doping and two calcining processes, the problem of limited lithium ion migration in low-temperature environments is solved, and the discharge capacity and cycle stability of the battery are significantly improved. , suitable for applications in low temperature environments.
Patent Information
- Application Number
- CN202411545572.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-01
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-11-01
AI Technical Summary
Under low temperature environment, the lithium ion migration of lithium iron phosphate batteries is limited, resulting in an increase in internal resistance and a significant decrease in discharge capacity, affecting the startup and operation efficiency of the battery.
Using low-temperature lithium iron phosphate positive electrode material, the internal stress is reduced, the Li+ detachment/embedding rate is improved, and the conductivity and crystallization are optimized through Rh3+ doping. The grid structure is combined with two calcining processes to improve crystallinity and density.
At -20℃, the discharge specific capacity of the low-temperature lithium iron phosphate positive electrode material is significantly improved, with a charge and discharge ratio of 0.1C at 128~132 mAh/g, a charge and discharge ratio of 1.0C at 91~96 mAh/g, and a charge and discharge ratio of 2.0C at 74 ~77 mAh/g, improving the cycling stability and electrochemical performance of the battery at low temperatures.
Smart Images

Figure CN119069692A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of energy storage batteries, and specifically relates to a low-temperature lithium iron phosphate positive electrode material and a preparation method and application thereof. Background Art
[0002] In low temperature environments, such as high altitude areas, winter, or specific industries such as mining, navigation, and aerospace, the performance of ordinary lithium iron phosphate batteries will be affected. This is because under low temperature conditions, the migration of lithium ions in lithium iron phosphate materials is restricted, resulting in an increase in the internal resistance of the battery. This increase in internal resistance will significantly reduce the discharge capacity of the battery. Studies have shown that when the temperature drops to -20°C, the available capacity of lithium iron phosphate batteries may drop to about one-third of that at room temperature; and when the temperature drops further to -40°C, its capacity may only be about 20% of that at room temperature. Therefore, low temperature environments pose a challenge to the startup and operating efficiency of batteries. Summary of the invention
[0003] The present invention overcomes the above technical problems and provides a low-temperature lithium iron phosphate positive electrode material and a preparation method and application thereof. The low-temperature lithium iron phosphate positive electrode material battery of the present invention has a high discharge specific capacity at low temperatures.
[0004] The present invention solves the above technical problems through the following technical solutions.
[0005] The invention provides a low-temperature lithium iron phosphate positive electrode material, comprising the following raw materials in molar mass parts: 100 parts of iron phosphate, 50-55 parts of lithium carbonate, 3-7 parts of zirconate, and 1-4 parts of rhodium (III) chloride salt complex.
[0006] The zirconate is at least one of tetraethoxy zirconium and zirconium n-propoxide.
[0007] In some preferred embodiments, the low-temperature lithium iron phosphate positive electrode material includes the following raw materials in molar mass parts: 100 parts of iron phosphate, 50.5-53.5 parts of lithium carbonate, 4-6 parts of zirconate, and 1-2.5 parts of rhodium (III) chloride salt complex.
[0008] The present invention uses zirconate to dope the positive electrode material. Compared with inorganic zirconium doping, the material has a lower calcination temperature and is easier to operate, but it is usually more difficult to control the crystal form. Zirconium doping can reduce the internal side reactions of the positive electrode material and improve the Li + The extraction / embedding rate is reduced because Zr doping helps to anchor lattice oxygen and inhibit oxidation precipitation; while zirconium doping has little effect on the discharge capacity of the positive electrode material, but can improve the cycle stability of the material.
[0009] In the present invention, the rhodium (III) salt complex is at least one of a rhodium (III) chloride sodium salt complex, a rhodium (III) chloride potassium salt complex and a rhodium (III) chloride ammonium salt complex.
[0010] Furthermore, the rhodium (III) chloride sodium salt complex is sodium hexachlororhodium (III) salt (CAS No.: 14972-70-4).
[0011] Furthermore, the rhodium (III) chloride potassium salt complex is potassium pentachlororhodium (III) acid (CAS No.: 65980-75-8) or potassium hexachlororhodium (III) acid (CAS No.: 13845-07-3).
[0012] Furthermore, the rhodium (III) chloride ammonium salt complex is dichloropentylamine rhodium (III) chloride (CAS No.: 13820-95-6), hexaammine rhodium (III) chloride (CAS No.: 13820-96-7) or ammonium chlororhodate (CAS No.: 15336-18-2).
[0013] In the present invention, Rh 3+ (Outer electron configuration: 4d 6 ) and Fe 2+ (Outer electron configuration: 3d 6 ), the number of electrons filled in the outermost d orbital is the same, the ionic radius is similar, and a certain amount of Rh 3+ After doping, the original lattice structure will not be destroyed or cause major changes; at the same time, compared with Fe 2+ , Rh 3+ The conductivity of ions will be better, which is beneficial to improve the conductivity of the material; and a certain amount of doping can shorten the Li + diffusion path, thereby increasing the Li + However, excessive rhodium doping as a heteroatom may even lead to local lattice distortion, which will reduce the number of effective lithium ions that can be extracted / embedded in the material, thus affecting the discharge capacity of the positive electrode material. In addition, excessive heteroatom doping will partially occupy the Li + 's location, and Li + Too many heteroatoms occupying the sites will hinder the diffusion channels of lithium ions and be detrimental to the rate performance of electrode materials.
[0014] In the present invention, at -20°C and a charge / discharge rate of 0.1C, the discharge capacity of a half-cell with the low-temperature lithium iron phosphate positive electrode material as the positive electrode is 128-132 mAh / g, and in some preferred embodiments is 129-132.8 mAh / g.
[0015] In the present invention, at -20°C and a charge-discharge rate of 1.0C, the discharge capacity of a half-cell with the low-temperature lithium iron phosphate positive electrode material as the positive electrode is 91-96 mAh / g, and in some preferred embodiments is 93-95.6 mAh / g.
[0016] In the present invention, at -20°C and a charge-discharge rate of 2.0C, the discharge capacity of a half-cell with the low-temperature lithium iron phosphate positive electrode material as the positive electrode is 74-77 mAh / g, and in some preferred embodiments is 75-76.8 mAh / g.
[0017] The present invention also provides a method for preparing a low-temperature lithium iron phosphate positive electrode material, comprising the following steps: S1. Wet-grinding iron phosphate and lithium carbonate, and then adding zirconate and rhodium (III) chloride salt complex to obtain a slurry; S2. spray drying the slurry to obtain a precursor powder; S3. The precursor powder is initially calcined at 550-600°C for 2-4 hours and ball-milled, and then secondary calcined at 720-760°C and kept warm for 8-10 hours. After annealing, a low-temperature lithium iron phosphate positive electrode material is obtained.
[0018] Among them, the double calcination can improve the crystallinity and density of the positive electrode material, and the double calcination helps to reduce the internal stress of the material, which can help the doped zirconium and rhodium elements to be more evenly distributed in the lattice of the positive electrode material.
[0019] In S1, the wet grinding is followed by sieving, wherein the sieved particle size is 200-300 meshes.
[0020] In S1, the solid content of the slurry is 35-45%.
[0021] In S2, the inlet air temperature of the spray drying is 200-250°C, and the outlet air temperature of the spray drying is 90-110°C.
[0022] In S3, preferably, the temperature of the primary calcination is 550-600° C., and the time of the primary calcination is 2-3 hours.
[0023] In S3, preferably, the temperature of the secondary calcination is 720-750° C., and the holding time of the secondary calcination is 8-9 h.
[0024] In S3, the orbital speed of the ball mill is 200-250 rpm, the rotation speed is 450-490 rpm, and the ball mill adopts a planetary ball mill.
[0025] In S3, the ball milling time is 4 to 6 hours.
[0026] In S3, the annealing temperature is 400-460°C, and the temperature is kept at the annealing temperature for 1-4 hours; preferably, the annealing temperature is 400-420°C, and the temperature is kept at the annealing temperature for 2-3 hours, and finally cooled to room temperature.
[0027] The application of the low-temperature lithium iron phosphate positive electrode material as mentioned above or the low-temperature lithium iron phosphate positive electrode material prepared by the preparation method of the low-temperature lithium iron phosphate positive electrode material as mentioned above in mining engineering vehicles, military equipment, polar exploration equipment, electric bicycles, electric vehicles, ships, aerospace, satellites or power grid energy storage systems.
[0028] On the basis of being in accordance with the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention.
[0029] Compared with the prior art, the present invention has the following beneficial effects:
[0030] 1. The present invention selects an appropriate amount of rhodium doping, because Rh 3+ The ionic radius of Fe 2+ This doping will not destroy the lattice structure of the material. Doping can also shorten the diffusion path of lithium ions and accelerate their diffusion rate, thereby improving the discharge performance of the positive electrode material under low temperature conditions. The present invention selects zirconate doping because zirconium doping helps anchor lattice oxygen and inhibit oxidation precipitation, thereby improving the cycle stability of the material.
[0031] 2. The doping raw materials are all organic metal compounds, which make it difficult for the positive electrode material to crystallize, so the calcination process needs to be strictly controlled. The present invention deeply explores the influence of the temperature and time of the primary calcination and the secondary calcination on the crystallinity of the positive electrode material, optimizes the density of the positive electrode material and the calcined crystal to improve the stability and electrochemical cycle performance of the positive electrode material.
[0032] 3. The low-temperature lithium iron phosphate positive electrode material provided by the present invention has good cycle performance; at -20°C: at a charge and discharge rate of 0.1C, the discharge specific capacity of the half-cell with the low-temperature lithium iron phosphate positive electrode material as the positive electrode is 128~132 mAh / g; at a charge and discharge rate of 1.0C, the discharge specific capacity of the half-cell with the low-temperature lithium iron phosphate positive electrode material as the positive electrode is 91~96 mAh / g; at a charge and discharge rate of 2.0C, the discharge specific capacity of the half-cell with the low-temperature lithium iron phosphate positive electrode material as the positive electrode is 74~77 mAh / g. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is a SEM image of the low-temperature lithium iron phosphate positive electrode material prepared in Example 1.
[0034] Figure 2 This is the SEM image of the low-temperature lithium iron phosphate positive electrode material prepared in Comparative Example 3.
[0035] Figure 3 This is the SEM image of the low-temperature lithium iron phosphate positive electrode material prepared in Comparative Example 5.
[0036] Figure 4 This is the SEM image of the low-temperature lithium iron phosphate positive electrode material prepared in Comparative Example 9.
[0037] Figure 5 This is the SEM image of the low-temperature lithium iron phosphate positive electrode material prepared in Comparative Example 10. DETAILED DESCRIPTION
[0038] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and carefully in combination with preferred embodiments below, but the protection scope of the present invention is not limited to the following specific embodiments.
[0039] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0040] The "range" disclosed in the present invention is defined in the form of a lower limit and an upper limit, and a given range is defined by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundaries of a particular range. The range defined in this way can be inclusive or exclusive of end values, and can be combined arbitrarily, that is, any lower limit can be combined with any upper limit to form a range. For example, if a range of 60-120 and 80-110 is listed for a specific parameter, it is understood that the range of 60-110 and 80-120 is also expected. In addition, if the minimum range values 1 and 2 are listed, and if the maximum range values 3, 4 and 5 are listed, the following ranges can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present invention, unless otherwise specified, the numerical range "ab" represents an abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" represents that all real numbers between "0-5" have been fully listed herein, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0041] If not otherwise specified, all embodiments and optional embodiments of the present invention can be combined with each other to form a new technical solution.
[0042] Unless otherwise specified, all technical features and optional technical features of the present invention can be combined with each other to form a new technical solution.
[0043] If not otherwise specified, all steps of the present invention may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0044] If there is no special explanation, the "include" and "comprising" mentioned in the present invention represent open-ended or closed-ended expressions. For example, the "include" and "comprising" may represent that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0045] If not specifically stated, in the present invention, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0046] [Positive electrode material and preparation method] Example 1 1. The low-temperature lithium iron phosphate positive electrode material of this embodiment is composed of the following raw materials in molar mass parts: 100 parts of iron phosphate, 52.5 parts of lithium carbonate, 4.25 parts of zirconate, and 1.9 parts of rhodium (III) chloride salt complex.
[0047] In this embodiment, the rhodium (III) chloride salt complex is 0.8 parts of sodium hexachlororhodium (III) salt and 1.1 parts of potassium hexachlororhodium (III) salt.
[0048] In this embodiment, the zirconate is tetraethoxy zirconium.
[0049] 2. The method for preparing the low-temperature lithium iron phosphate positive electrode material of this embodiment comprises the following steps: S1. Wet-grind the iron phosphate and lithium carbonate, sieve through a 300-mesh sieve twice, add zirconate and rhodium (III) chloride salt complex and mix to obtain a slurry having a solid content of 36%; S2. The slurry was spray dried, the air inlet temperature of the spray drying was 200°C, and the air outlet temperature was 90°C to obtain a precursor powder; S3. The precursor powder was initially calcined at 560°C for 3 hours, the planetary ball mill had an orbital speed of 250 rpm and a rotation speed of 450 rpm, and ball milled for 4 hours. It was then secondary calcined at 740°C and kept warm for 8 hours. It was then annealed to 420°C and kept warm for 2 hours, and then cooled to room temperature to obtain a low-temperature lithium iron phosphate positive electrode material.
[0050] See the SEM image of the low-temperature lithium iron phosphate positive electrode material in this embodiment. Figure 1 , the crystal surface of the material in the figure is smoother and rounder, the grains are evenly distributed and neatly arranged, for example, the sizes of some particles are 222nm, 365nm, 322nm, and 374nm.
[0051] Example 2 The low-temperature lithium iron phosphate positive electrode material of this embodiment is composed of the following raw materials in molar mass parts: 100 parts of iron phosphate, 50.5 parts of lithium carbonate, 5.3 parts of zirconate, and 1.1 parts of rhodium chloride (III) salt complex. Among them, the rhodium chloride (III) salt complex is 0.8 parts of hexaammine rhodium chloride (III) and 0.3 parts of ammonium chlororhodate. Other steps and parameters are the same as in Example 1.
[0052] Example 3 The rhodium chloride (III) salt complex in the raw materials of this embodiment is 1.1 parts of sodium hexachlororhodium (III) acid and 0.8 parts of hexaammine rhodium (III) chloride, and the other steps and parameters are the same as those in Example 1.
[0053] Example 4 The raw materials in this embodiment include 1.1 parts of potassium hexachlororhodium (III) salt complex and 0.8 parts of ammonium chlororhodium salt. The other steps and parameters are the same as those in Example 1.
[0054] Example 5 The zirconate in the raw material of this embodiment is replaced by zirconium n-propoxide, and the other steps and parameters are the same as those in Example 1.
[0055] Example 6 The sieved particle size in S1 of the preparation method of this embodiment is 200 mesh, and the other steps and parameters are the same as those in Example 1.
[0056] Example 7 The sieved particle size in S1 of the preparation method of this embodiment is 250 mesh, and the other steps and parameters are the same as those in Example 1.
[0057] Example 8 In S3 of the preparation method of this embodiment, the initial calcination is carried out at 550° C. for 3 h, and the other steps and parameters are the same as those in Example 1.
[0058] Example 9 In S3 of the preparation method of this embodiment, the initial calcination is performed at 580° C. for 2 h, and the other steps and parameters are the same as those in Example 1.
[0059] Example 10 In S3 of the preparation method of this embodiment, the initial calcination is carried out at 600° C. for 2 h, and the other steps and parameters are the same as those in Example 1.
[0060] Embodiment 11 The ball milling time in S3 of the preparation method of this embodiment is 5 hours, and the other steps and parameters are the same as those in Example 1.
[0061] Example 12 The ball milling time in S3 of the preparation method of this embodiment is 6 hours, and the other steps and parameters are the same as those in Example 1.
[0062] Example 13 The secondary calcination in S3 of the preparation method of this embodiment is calcined at 720° C. for 8 h, and the other steps and parameters are the same as those in Example 1.
[0063] Embodiment 14 The secondary calcination in S3 of the preparation method of this embodiment is calcined at 730° C. for 8 h, and the other steps and parameters are the same as those in Example 1.
[0064] Embodiment 15 The secondary calcination in S3 of the preparation method of this embodiment is calcined at 750° C. for 8 h, and the other steps and parameters are the same as those in Example 1.
[0065] Comparative Example 1 The low-temperature lithium iron phosphate positive electrode material of this comparative example is composed of the following raw materials in molar mass parts: 100 parts of iron phosphate, 51 parts of lithium carbonate and 4.7 parts of zirconate. Other steps and parameters are the same as those in Example 1.
[0066] Comparative Example 2 The low-temperature lithium iron phosphate positive electrode material of this comparative example is composed of the following raw materials in molar mass parts: 100 parts of iron phosphate, 52.5 parts of lithium carbonate and 1.9 parts of rhodium chloride (III) salt complex; the rhodium chloride (III) salt complex is 0.9 parts of sodium hexachlororhodium (III) acid and 1.0 parts of potassium hexachlororhodium (III) acid. Other steps and parameters are the same as those in Example 1.
[0067] Comparative Example 3 The low-temperature lithium iron phosphate positive electrode material of this comparative example is composed of the following raw materials in molar mass parts: 100 parts of iron phosphate, 52.5 parts of lithium carbonate, 5.25 parts of zirconate, and 5.0 parts of rhodium chloride (III) salt complex; the rhodium chloride (III) salt complex is 3.4 parts of hexaammine rhodium chloride (III) and 1.6 parts of ammonium chlororhodate. Other steps and parameters are the same as those in Example 1.
[0068] The SEM image of the low-temperature lithium iron phosphate positive electrode material prepared in this comparative example is shown in Figure 2 ,It can be seen in the figure that the surface of the grains is unevenly distributed, with many inclusions and poor crystallinity. For example, the sizes of some particles are 163nm, 604nm, 235nm, and 296nm.
[0069] Comparative Example 4 In this comparative example, the zirconate in the raw material is replaced by tetrabutyl zirconate, and the other steps and parameters are the same as those in Example 1.
[0070] Comparative Example 5 In S3 of the preparation method of this comparative example, the initial calcination is performed at 610° C. for 2 h, and the other steps and parameters are the same as those in Example 1.
[0071] The SEM image of the low-temperature lithium iron phosphate positive electrode material prepared in this comparative example is shown in Figure 3 ,It can be seen in the figure that the grains are overgrown and the grains are too large, for example, the sizes of some grains are 935nm, 1.1μm, 163nm, and 225nm.
[0072] Comparative Example 6 In S3 of the preparation method of this comparative example, the initial calcination is performed at 620° C. for 2 h, and the other steps and parameters are the same as those in Example 1.
[0073] Comparative Example 7 In S3 of the preparation method of this comparative example, the initial calcination is performed at 540° C. for 3 h, and the other steps and parameters are the same as those in Example 1.
[0074] Comparative Example 8 The ball milling time in S3 of the preparation method of this comparative example is 8 hours, and the other steps and parameters are the same as those in Example 1.
[0075] Comparative Example 9 The secondary calcination in S3 of the preparation method of this comparative example is calcination at 780° C. for 8 h, and the other steps and parameters are the same as those in Example 1.
[0076] The SEM image of the low-temperature lithium iron phosphate positive electrode material prepared in this comparative example is shown in Figure 4 ,It can be seen in the figure that the grains are overgrown and the inclusions are large, for example, the sizes of some particles are 113nm, 621nm, 937nm, 410nm, and 879nm.
[0077] Comparative Example 10 In S3 of the preparation method of this comparative example, the precursor powder is calcined at 750° C. for 10 h without secondary calcination. The other steps and parameters are the same as those in Example 1.
[0078] The SEM image of the low-temperature lithium iron phosphate positive electrode material prepared in this comparative example is shown in Figure 5 ,The grains in the figure have poor crystallinity and even large areas of collapse.,For example, the sizes of some particles are 76.7nm, 235nm, 291nm, 407nm, and 703nm.
[0079] Test Case The positive electrode materials prepared in the above examples and comparative examples are prepared into button-type half-cells, and the preparation steps are as follows: (1) Adding solvent N-methylpyrrolidone (NMP) to a low-temperature lithium iron phosphate positive electrode material: acetylene black: polyvinylidene fluoride in a mass ratio of 8:1:1 to adjust the viscosity to 4000-8000 mPa·s to prepare a positive electrode slurry; (2) The positive electrode slurry is evenly coated on one surface (perpendicular to the thickness direction) of the aluminum foil (positive electrode current collector) and dried, and then rolled and sheared to obtain a positive electrode sheet containing a positive electrode film layer.
[0080] (3) Using lithium hexafluorophosphate-ethyl methyl carbonate as the electrolyte and polypropylene as the isolation membrane, the prepared positive electrode sheet and negative lithium sheet are combined to make a button half-cell.
[0081] The button half-cell was tested with a Blue Electric device in a voltage range of 2.0V to 3.8V with a discharge capacity of 0.1C, 1.0C and 2.0C (measured at -20°C). The test results are shown in Table 1 below.
[0082]
[0083] According to the data in Table 1, the following conclusions can be drawn: In Comparative Example 1, no rhodium (III) chloride salt complex was used in the preparation of the positive electrode material, which may be the reason for its lower specific capacity at high rate discharge.
[0084] In Comparative Example 2, since zirconate is not added, the lattice stability of the positive electrode material after calcination is poor.
[0085] In Comparative Example 3, the amount of rhodium (III) chloride salt complex added is too much, which may cause excessive occupation of lithium ion sites by heteroatoms, change the electronic structure, and even cause local lattice distortion, hindering the diffusion channel of lithium ions, which is not conducive to the rate performance of the electrode material.
[0086] In Comparative Example 4, the zirconate used is tetrabutyl zirconate. Compared with tetraethoxy zirconium and zirconium n-propoxide, the addition of this zirconate still leads to poor crystallinity of the positive electrode material even after two calcinations.
[0087] In Comparative Examples 5 to 7, the initial calcination temperature is improperly set, whether too high or too low, which is not conducive to the crystallinity of the positive electrode material. Too high a temperature may lead to excessive grain growth and crystal structure distortion, while too low a temperature may lead to poor crystallinity.
[0088] In Comparative Example 8, the ball milling time was too long, resulting in the positive electrode material having too small a particle size and a high density after secondary calcination.
[0089] In Comparative Example 9, the secondary calcination temperature is too high, which may cause excessive grain growth and reduce the active sites of the material, thereby affecting its electrochemical performance.
[0090] In Comparative Example 10, calcination was performed only once instead of twice. Compared with Example 1, the positive electrode material obtained by this method has poor crystallinity and uneven doping, resulting in poor structural stability.
[0091] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods. The specific embodiments described above further describe the purpose, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. Low-temperature lithium iron phosphate positive electrode material, characterized in that: The method comprises the following raw materials in molar mass parts: 100 parts of iron phosphate, 50-55 parts of lithium carbonate, 3-7 parts of zirconate, and 1-4 parts of rhodium (III) chloride salt complex.
2. The low-temperature lithium iron phosphate positive electrode material according to claim 1, characterized in that: The zirconate is at least one of tetraethoxy zirconium and zirconium n-propoxide; And / or, the rhodium (III) salt complex is at least one of a rhodium (III) chloride sodium salt complex, a rhodium (III) chloride potassium salt complex and a rhodium (III) chloride ammonium salt complex.
3. The low-temperature lithium iron phosphate positive electrode material according to claim 2, characterized in that: The rhodium (III) chloride sodium salt complex is sodium hexachlororhodium (III) acid; and / or, the rhodium (III) chloride potassium salt complex is potassium pentachlororhodium (III) acid or potassium hexachlororhodium (III) acid; And / or, the rhodium (III) chloride ammonium salt complex is dichloropentammine rhodium (III) chloride, hexaammine rhodium (III) chloride or ammonium chlororhodate.
4. The method for preparing a low-temperature lithium iron phosphate positive electrode material according to any one of claims 1 to 3, characterized in that: The following steps are involved: S1. Wet-grinding iron phosphate and lithium carbonate, and then adding zirconate and rhodium (III) chloride salt complex to obtain a slurry; S2. spray drying the slurry to obtain a precursor powder; S3. The precursor powder is initially calcined at 550-600°C for 2-4 hours and ball-milled, and then secondary calcined at 720-760°C and kept warm for 8-10 hours. After annealing, a low-temperature lithium iron phosphate positive electrode material is obtained.
5. The method for preparing a low-temperature lithium iron phosphate positive electrode material according to claim 4, characterized in that: The wet grinding is followed by sieving, wherein the sieved particle size is 200-300 meshes; And / or, the solid content of the slurry is 35-45%.
6. The method for preparing a low-temperature lithium iron phosphate positive electrode material according to claim 4, characterized in that: The inlet air temperature of the spray drying is 200-250°C, and the outlet air temperature of the spray drying is 90-110°C.
7. The method for preparing a low-temperature lithium iron phosphate positive electrode material according to claim 4, characterized in that: The ball milling adopts a planetary ball mill; The revolution speed of the ball mill is 200-250 rpm and the rotation speed is 450-490 rpm; The ball milling time is 4 to 6 hours.
8. The method for preparing a low-temperature lithium iron phosphate positive electrode material according to claim 4, characterized in that: The annealing temperature is 400-460° C., and the annealing temperature is maintained for 1-4 hours.
9. Use of the low-temperature lithium iron phosphate positive electrode material according to claims 1 to 3 or the low-temperature lithium iron phosphate positive electrode material prepared by the preparation method of the low-temperature lithium iron phosphate positive electrode material according to claims 4 to 8, characterized in that: Applications in mining engineering vehicles, military equipment, polar exploration equipment, electric bicycles, electric vehicles, ships, aerospace or power grid energy storage systems.
Citation Information
Patent Citations
High-capacity high-stability lithium manganate positive electrode material and preparation method thereof
CN103730654A
Modified positive electrode material for lithium iron phosphate battery and preparation method of modified positive electrode material and lithium-ion battery
CN106602027A
Carbon-coated lithium-containing transition metal phosphate cathode material and preparation method thereof
CN111342018A
Rapid composite coating modification method of lithium battery positive electrode material
CN112151781A
Composite lithium manganese iron phosphate positive electrode material as well as preparation method and application thereof