Negative electrode active material and preparation method thereof, negative electrode, battery and electric device
The use of graphite powder and amorphous carbon fillers to densify natural graphite particles addresses the expansion issue, improving cycle life and rate performance by minimizing electrolyte consumption and side reactions, achieving high efficiency and retention rates.
Patent Information
- Application Number
- CN202310639235.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-31
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-05-31
AI Technical Summary
Natural graphite negative electrode materials experience large volume expansion during battery cycling, leading to reduced cycle life and rate performance due to internal pores that reopen, causing increased electrolyte consumption and side reactions.
A negative electrode active material is prepared by granulating natural graphite with graphite powder and optional amorphous carbon fillers, followed by carbonization to densify the graphite particles and coat them with a carbon layer, reducing internal pores and minimizing electrolyte interaction.
The solution effectively inhibits electrochemical expansion, enhances cycle life, and improves rate performance by reducing electrolyte consumption and side reactions, with charge and discharge efficiency exceeding 80% and capacity retention above 86% after 1000 cycles.
Smart Images

Figure CN119069694A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of batteries, and in particular to a negative electrode active material and a preparation method thereof, a negative electrode, a battery and an electrical device. Background Art
[0002] Among battery negative electrode materials, natural graphite has a high degree of graphitization and high specific capacity, and is cheaper than artificial graphite. However, due to the large grain size of natural graphite and the presence of many pores inside the particles, the high-rate capacity of natural graphite is low. In addition, during the battery cycle, due to the presence of pores in natural graphite particles, natural graphite expands both externally and internally, resulting in large electrochemical expansion, which causes natural graphite particles to continuously expose new reaction interfaces, resulting in a short battery cycle life. Reducing the internal pores of natural graphite particles can effectively improve the defects of natural graphite in electrochemical expansion and cycle life.
[0003] At present, the fillers used to fill the pores inside natural graphite include amorphous carbon formed by carbonization of asphalt or resin. During the long-term cycle of the battery, due to repeated expansion, the pores will inevitably open again, exposing the amorphous carbon interface filled. Amorphous carbon has a large specific surface area, which will bring more side reactions, causing the amount of electrolyte digestion to increase, thus shortening the battery life to a certain extent. In addition, the density of amorphous carbon as a pore filler for natural graphite is usually not high, which will affect the rate performance of the battery to a certain extent.
[0004] Therefore, there is an urgent need to improve the filling technology of the internal pores of natural graphite. Summary of the invention
[0005] Aiming at the problem that the natural graphite negative electrode material in the prior art is prone to large volume expansion during battery cycling, which affects the cycle life and rate performance of the battery, the present invention provides a negative electrode active material and a preparation method, a negative electrode, a battery and an electrical device.
[0006] In order to achieve the above-mentioned object, the present invention provides a negative electrode active material in a first aspect, the negative electrode active material comprising: graphite particles, and a carbon layer covering the graphite particles;
[0007] There are holes inside the graphite particles, and the holes are filled with fillers;
[0008] The filler includes graphite powder and optionally amorphous carbon.
[0009] A second aspect of the present invention provides a method for preparing a negative electrode active material, comprising:
[0010] (1) granulating a natural graphite raw material and a filler to obtain graphite particles;
[0011] (2) mixing the graphite particles with an organic carbon source to obtain graphite particles coated with an organic carbon source;
[0012] (3) carbonizing the graphite particles coated with the organic carbon source to obtain a negative electrode active material;
[0013] Wherein, the internal pores of the graphite particles are filled with the filler;
[0014] The filler includes graphite powder, optionally asphalt and optionally resin.
[0015] The third aspect of the present invention provides a negative electrode active material prepared by the method described in the second aspect.
[0016] A fourth aspect of the present invention provides a negative electrode, comprising a negative electrode current collector, and an active material layer disposed on the negative electrode current collector;
[0017] Wherein, the active material layer contains the negative electrode active material described in the first aspect or the third aspect.
[0018] A fifth aspect of the present invention provides a battery, comprising the negative electrode described in the fourth aspect.
[0019] A sixth aspect of the present invention provides an electrical device, comprising the battery described in the fifth aspect.
[0020] Through the above technical solution, the present invention uses graphite powder and optional amorphous carbon as pore fillers of graphite particles to densify the graphite particles, thereby obtaining a negative electrode active material, which can achieve the following beneficial effects:
[0021] (1) The negative electrode active material provided by the present invention has internal pores of graphite particles contained therein filled and densified, so that the electrochemical expansion space of graphite particles is greatly reduced during the cycle, thereby effectively reducing the expansion phenomenon, solving the expansion problem of graphite negative electrode, and extending the cycle life of the battery;
[0022] (2) The negative electrode active material provided by the present invention uses graphite powder as the main filler of the pores of graphite particles. Compared with the amorphous carbon filler in the prior art, the graphite powder has a smaller specific surface area and produces fewer side reactions during the operation of the battery, which can reduce the consumption of the electrolyte, increase the cycle life of the battery, and improve the rate performance of the battery;
[0023] (3) The graphite powder used as the main filler in the negative electrode active material provided by the present invention can be an industrial by-product graphite powder, for example, the artificial graphite fine powder obtained in the powder screening process during the preparation of artificial graphite can be directly used. While realizing the reuse of artificial graphite by-products, it can also avoid the asphalt or resin crushing process required in the existing technical solution using amorphous carbon as the main filler, and can also reduce the cost of subsequent graphitization;
[0024] (4) The negative electrode active material provided by the present invention has a coated carbon layer on the surface, which is beneficial to improving the cycle life and initial charge and discharge efficiency of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present invention but do not constitute a limitation of the present invention. In the accompanying drawings:
[0026] Figure 1 This is a SEM test image of the negative electrode active material P1 prepared in Example 1 of the present invention after ion cutting.
[0027] Figure 2 This is a SEM test image of the negative electrode active material DP1 prepared in Comparative Example 1 of the present invention after ion cutting. DETAILED DESCRIPTION
[0028] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0029] A first aspect of the present invention provides a negative electrode active material, the negative electrode active material comprising: graphite particles, and a carbon layer covering the graphite particles;
[0030] There are holes inside the graphite particles, and the holes are filled with fillers;
[0031] The filler includes graphite powder and optionally amorphous carbon.
[0032] The negative electrode active material provided by the present invention is mainly composed of graphite particles, the internal pores of the graphite particles are filled with specific fillers, and the surface of the graphite particles is coated with a carbon layer. At the microscopic level, the negative electrode active material is in a granular form, and preferably, the particle shape of the negative electrode active material is spherical or ellipsoidal.
[0033] According to the present invention, in the negative electrode active material, the graphite particles are prepared using natural graphite as a raw material. Preferably, the graphite particles are spherical graphite particles.
[0034] In the present invention, the natural graphite is preferably natural flake graphite.
[0035] In the present invention, the spherical graphite should be understood according to the definition of "spherical graphite" well known to those skilled in the art in the fields of graphite materials and batteries.
[0036] According to the present invention, in the negative electrode active material, the average particle size of the graphite particles is 8-35 μm. If the average particle size of the graphite particles is too large, the ion migration path will be too long during the battery cycle, which is not conducive to the dynamic performance of the battery; if the average particle size of the graphite particles is too small, the specific surface area of the graphite particles will increase, resulting in increased electrolyte consumption, thereby reducing the initial charge and discharge efficiency and cycle life of the battery. Preferably, the average particle size of the graphite particles is 10-30 μm.
[0037] In the present invention, the average particle size refers to the median diameter (D50), which can be measured by a laser particle size analyzer.
[0038] According to the present invention, in the negative electrode active material, the carbon layer is coated on the surface of the graphite particles, which can reduce the specific surface area of the graphite particles, increase the active sites, and help improve the initial charge and discharge efficiency and cycle life of the battery. In the present invention, the carbon layer should not be too thick, as a larger thickness will lead to the formation of a thicker SEI film, thereby reducing the initial charge and discharge efficiency of the battery. Preferably, the thickness of the carbon layer is 1-100 nm.
[0039] In the present invention, the thickness of the carbon layer can be measured by transmission electron microscopy (TEM).
[0040] According to the present invention, in the negative electrode active material, the internal pores of the graphite particles are filled with graphite powder and optional amorphous carbon. The use of this specific filler to densify the graphite particles can greatly reduce the electrochemical expansion space of the graphite particles during the battery cycle, thereby effectively inhibiting the expansion of the graphite negative electrode and extending the cycle life of the battery. Preferably, based on the total weight of the negative electrode active material, the content of the filler in the negative electrode active material is 5-15% by weight, and more preferably 7-10% by weight.
[0041] According to the present invention, in one embodiment, the filler can be entirely graphite powder. Using graphite powder as a filler can compact the internal pores of the graphite particles, reduce the irreversible expansion of the graphite particles due to multiple cycles, inhibit and significantly delay the reopening of the pores, and when the pores of the graphite particles open to expose the filler interface, since the filled graphite powder reacts less with the electrolyte, compared to the method of mainly using amorphous carbon as a filler, the consumption of the electrolyte can be reduced, thereby increasing the cycle life of the battery.
[0042] In another embodiment, the filler may be a mixture of graphite powder and amorphous carbon. An appropriate amount of amorphous carbon can provide more ion diffusion paths, thereby increasing the migration rate of ions in graphite. However, when the proportion of amorphous carbon in the filler is too high, it will lead to increased electrolyte consumption and reduce the cycle life of the battery. Preferably, based on the total weight of the filler, the content of the graphite powder in the filler is 90-100% by weight, and more preferably 95-100% by weight.
[0043] According to the present invention, the average particle size of the filler is 0.5-3 μm, preferably 1-2 μm.
[0044] According to the present invention, preferably, the graphitization degree of the graphite powder is ≥ 94%, which can enable the battery to obtain higher initial charge and discharge efficiency and capacity.
[0045] In the present invention, all graphite powders that meet the above-mentioned limiting conditions can be used as the filler in the negative electrode active material of the present invention. In a preferred embodiment of the present invention, the graphite powder can be artificial graphite fine powder obtained in the powder screening process during the preparation of artificial graphite. The artificial graphite fine powder is a by-product in the preparation process of artificial graphite, which is already a fine particle graphitized product. The artificial graphite fine powder is directly used as a filler, which can avoid the asphalt or resin (as a filler precursor) crushing process required in the prior art using amorphous carbon as the main filler.
[0046] The negative electrode active material provided by the present invention is mainly composed of graphite particles densified with specific fillers (graphite powder and optional amorphous carbon). Compared with graphite particles densified mainly with amorphous carbon, the former has significantly reduced electrochemical expansion during battery cycling and produces fewer side reactions, which can make the battery have a longer cycle life and better rate performance. Specifically, the charge and discharge efficiency at 25°C and 3C rate conditions can be increased to more than 80%, and the capacity retention rate after 1000 cycles at 25°C and 1C charge and discharge conditions can be increased to more than 86%.
[0047] A second aspect of the present invention provides a method for preparing a negative electrode active material, comprising:
[0048] (1) granulating a natural graphite raw material and a filler to obtain graphite particles;
[0049] (2) mixing the graphite particles with an organic carbon source to obtain graphite particles coated with an organic carbon source;
[0050] (3) carbonizing the graphite particles coated with the organic carbon source to obtain a negative electrode active material;
[0051] Wherein, the internal pores of the graphite particles are filled with the filler;
[0052] The filler includes graphite powder, optionally asphalt and optionally resin.
[0053] According to the present invention, in step (1), during the granulation process, the natural graphite raw material wraps the filler, and is granulated to form graphite particles whose internal pores are filled with the filler.
[0054] According to the present invention, in step (1), the granulation process is preferably a spheroidization process of natural graphite raw materials. Preferably, the granulation process comprises:
[0055] The natural graphite raw material is subjected to spheroidization treatment, and the filler is added during the spheroidization process, so that the natural graphite raw material wraps the filler to obtain graphite particles.
[0056] According to the present invention, in the above-mentioned preferred granulation process, the filler is added during the spheroidization process, the natural graphite raw material and the filler are fully mixed, and at the same time, the spheroidizing wheel of the spheroidizing equipment collides, rubs and shears the natural graphite raw material, and the filler is wrapped into the natural graphite raw material to obtain spherical graphite particles filled with graphite powder, optional asphalt and optional resin.
[0057] According to the present invention, in step (1), the natural graphite raw material is a conventional raw material for preparing spherical graphite, preferably natural flake graphite.
[0058] According to the present invention, in step (1), preferably, the weight ratio of the filler: (the filler + the natural graphite raw material) is (10-30): 100, preferably (15-20): 100. When the above ratio is met, it is beneficial to obtain graphite particles with better densification effect.
[0059] According to the present invention, in one embodiment, the filler can be entirely graphite powder, and graphite powder is used as the pore filler of graphite particles. After subsequent carbonization treatment, the graphite structure of the graphite powder itself remains unchanged, and is filled in the pores as a filler in the form of graphite, which can increase the capacity of natural graphite, reduce the irreversible expansion of graphite particles due to multiple cycles, inhibit and significantly delay the reopening of the pores, and when the pores of the graphite particles open to expose the filler interface, since the filled graphite powder reacts less with the electrolyte, the consumption of the electrolyte can be reduced, thereby increasing the cycle life of the battery.
[0060] In another embodiment, the filler can also be a mixture of graphite powder, asphalt and / or resin, and this mixture is used as a filler for the holes of graphite particles. After subsequent carbonization treatment, the graphite structure of the graphite powder itself remains unchanged, and the asphalt and / or resin is converted into amorphous carbon, that is, a mixture of graphite powder and amorphous carbon is formed as a filler to fill the holes. An appropriate amount of amorphous carbon can provide more ion diffusion paths, thereby increasing the migration rate of ions in graphite, but when the proportion of amorphous carbon in the filler is too high, it will lead to increased consumption of electrolyte and reduce the cycle life of the battery.
[0061] According to the present invention, in step (1), the content of the graphite powder in the filler is 90-100% by weight, preferably 95-100% by weight. In the present invention, in the case where the filler contains asphalt and / or resin, in the above ratio, the amount of asphalt and / or resin other than graphite powder is calculated by the weight of amorphous carbon converted after subsequent carbonization.
[0062] According to the present invention, in step (1), when the filler contains asphalt and / or resin, the asphalt and / or resin is preferably heated and softened before the granulation.
[0063] According to the present invention, the average particle size of the filler is 0.5-3 μm, preferably 1-2 μm. If the average particle size of the filler is too large, the fluidity of the filler will be poor, and it will be difficult to be fully wrapped by the natural graphite raw material, so that the graphite particles obtained by granulation still have holes inside; if the average particle size of the filler is too small, the filler will fly during the granulation process, and it will also be difficult to be fully wrapped by the natural graphite raw material, thereby reducing the compacting effect of the graphite particles obtained by granulation.
[0064] According to the present invention, preferably, the graphitization degree of the graphite powder is ≥ 94%, which can enable the battery to obtain higher initial charge and discharge efficiency and capacity.
[0065] According to the present invention, all graphite powders that meet the above-mentioned limiting conditions can be used for the filler. In a preferred embodiment of the present invention, the graphite powder can be an artificial graphite fine powder obtained in the powder screening process during the preparation of artificial graphite. In the present invention, the preparation process of the artificial graphite can refer to the raw materials (for example, oil-based coke, coal-based coke, etc.), processes and parameters in the artificial graphite preparation process known to technicians in the fields of graphite materials and batteries, and usually mainly include a crushing process, a shaping process, a graphitization process and a powder screening process performed in sequence, wherein the artificial graphite fine powder obtained in the powder screening process is a by-product, and its average particle size is usually 1-3μm, and there is no good place yet. The present invention directly uses the artificial graphite fine powder as a hole filler for graphite particles, which can avoid the crushing process required in the prior art to use asphalt and / or resin as the main filler (crushing the asphalt and / or resin to a suitable particle size through the crushing process), and can reduce the process and cost of graphitizing the asphalt and / or resin filler after the hole filling, and realize the improvement of the utilization rate of artificial graphite by-products.
[0066] According to the present invention, in the filler, the average particle size of the asphalt and / or resin is 0.5-3 μm.
[0067] According to the present invention, among the fillers, the selection range of the asphalt is relatively wide, and the filler asphalt commonly used in the prior art using amorphous carbon as the main filler can be selected.
[0068] According to the present invention, the range of the resin to be selected from the filler is also wide, and the filler resin commonly used in the prior art using amorphous carbon as the main filler can be selected, for example, phenolic resin, furfural resin and epoxy resin.
[0069] According to the present invention, in step (2), the organic carbon source can be selected from asphalt and / or resin. In the present invention, the asphalt and / or resin used as the organic carbon source can be selected from the same materials as the asphalt and / or resin used as the filler in the above step (1).
[0070] According to the present invention, in step (2), preferably, the weight ratio of the organic carbon source: (the graphite particles + the organic carbon source) is (0.5-5):100.
[0071] According to the present invention, in step (2), the conditions of the carbonization treatment include: a temperature of 1100-1200° C., and an oxygen content in the carbonization atmosphere of less than 400 ppm.
[0072] The method for preparing negative electrode active materials provided by the present invention uses graphite powder, optional asphalt and optional resin as fillers, and the filling is preferably carried out during the spheroidization process of natural graphite raw materials. The obtained graphite particles containing fillers are coated with an organic carbon source and carbonized, and the graphite particles are densified with graphite powder and optional amorphous carbon. The electrochemical expansion of the negative electrode active material obtained in the battery cycle process is significantly reduced, and there are fewer side reactions, so that the battery can have a longer cycle life and better rate performance.
[0073] The third aspect of the present invention provides a negative electrode active material prepared by the method described in the second aspect.
[0074] According to the present invention, the structure, composition and performance of the negative electrode active material prepared by the method described in the second aspect are the same as those of the negative electrode active material described in the first aspect of the present invention, and will not be described in detail here.
[0075] A fourth aspect of the present invention provides a negative electrode, comprising a negative electrode current collector, and an active material layer disposed on the negative electrode current collector;
[0076] Wherein, the active material layer contains the negative electrode active material described in the first aspect or the third aspect.
[0077] According to the present invention, in some embodiments, the active material layer in the negative electrode may also contain other negative electrode active materials other than the negative electrode active material provided by the present invention, including but not limited to at least one of carbon materials other than graphite, silicon-based materials, tin-based materials, and lithium-containing composite materials. Among them, the carbon material other than graphite may include but not limited to at least one of carbon fiber, soft carbon, hard carbon, mesophase carbon microspheres, and graphene; the silicon-based material may include but not limited to at least one of elemental silicon, silicon oxide, silicon alloy, and composite silicon; the tin-based material may include but not limited to tin oxide and / or tin alloy.
[0078] According to the present invention, the negative electrode current collector in the negative electrode can be any conventional negative electrode current collector for batteries, and the present invention does not specifically limit its material selection and specification parameters. For example, the negative electrode current collector can be copper foil, preferably carbon-coated copper foil.
[0079] Compared with conventional negative electrodes, the negative electrode provided by the present invention has the advantages of low expansion, low thickness change rate during the battery cycle, and less side reactions with the electrolyte, which can make the battery have a longer cycle life and better rate performance.
[0080] A fifth aspect of the present invention provides a battery, comprising the negative electrode described in the fourth aspect.
[0081] In the present invention, further, the battery is preferably a lithium ion battery or a sodium ion battery.
[0082] A sixth aspect of the present invention provides an electrical device, comprising the battery described in the fifth aspect.
[0083] The present invention will be described in detail below by way of examples. In the following examples and comparative examples, unless otherwise specified, all reagents used are commercially available products.
[0084] Artificial graphite fine powder-1 (filler): obtained from the sieving step in the preparation process of artificial graphite (based on petroleum coke raw material), with an average particle size (D50) of 1.2 μm and a graphitization degree of 95%.
[0085] Artificial graphite fine powder-2 (filler): taken from the powder screening step in the preparation process of artificial graphite (based on petroleum coke raw materials) (the preparation raw materials, preparation process and preparation parameters are the same as those of the above-mentioned graphite powder-1), with an average particle size (D50) of 2.5μm and a degree of graphitization of 95%.
[0086] Asphalt: high temperature asphalt (softening point is 200°C), average particle size is 0.5μm.
[0087] Phenolic resin: The average particle size is 3 μm.
[0088] Natural flake graphite: carbon content 97%, average particle size of large flakes (D50) is 70μm, and average particle size of small flakes (D50) is 37μm.
[0089] Example 1
[0090] This example is used to illustrate the preparation of negative electrode active materials
[0091] (1-1) natural flake graphite is added into a mixer, and a filler (artificial graphite fine powder-1) is added and mixed, and then the obtained mixture is added into a spheroidizing device for spheroidizing treatment. Under the collision, friction and shearing action of the spheroidizing wheel on the natural flake graphite, the filler is wrapped into the natural flake graphite to obtain spherical graphite particles (D50 is 18 μm) with filler densification; wherein the weight ratio of filler: (filler + natural flake graphite) is 20:100;
[0092] (1-2) mixing the spherical graphite particles obtained in step (1-1) with asphalt (the temperature of the asphalt is 200° C.) to obtain asphalt-coated graphite particles; wherein the weight ratio of asphalt: (asphalt + spherical graphite particles) is 2.5:100;
[0093] (2) The asphalt-coated graphite particles obtained in step (1-2) are carbonized (the carbonization temperature is 1150° C., and the oxygen content in the carbonization atmosphere is less than 150 ppm) to obtain a negative electrode active material (denoted as P1).
[0094] P1 has an ellipsoidal appearance and contains filler (graphite powder, D50 is 1.2μm) densified graphite particles (D50 of graphite particles is 18μm), and the outer surface of the graphite particles is covered with a carbon layer (the average thickness of the carbon layer is 40nm); based on the total weight of P1, the content of filler in the graphite particles is 9.8% by weight; the content of graphite powder in the filler is 100% by weight.
[0095] P1 was ion cut and then SEM tested. The results are as follows: Figure 1 As shown, in Figure 1 It can be seen that there are no obvious holes inside the graphite particles in P1, indicating that the artificial graphite fine powder-1 is wrapped into the interior of the graphite particles and realizes the densification of the graphite particles.
[0096] Example 2
[0097] (1-1) natural flake graphite is added into a mixer, and a filler (artificial graphite fine powder-1) is added and mixed, and then the obtained mixture is added into a spheroidizing device for spheroidizing treatment, and the filler is wrapped into the natural flake graphite under the collision, friction and shearing action of the spheroidizing wheel on the natural flake graphite, so as to obtain spherical graphite particles (D50 is 18 μm) with filler densification; wherein the weight ratio of filler: (filler + natural flake graphite) is 15:100;
[0098] (1-2) mixing the spherical graphite particles obtained in step (1-1) with asphalt (the temperature of the asphalt is 200° C.) to obtain asphalt-coated graphite particles; wherein the weight ratio of asphalt: (asphalt + spherical graphite particles) is 2.5:100;
[0099] (2) The asphalt-coated graphite particles obtained in step (1-2) are carbonized (the carbonization temperature is 1150° C., and the oxygen content in the carbonization atmosphere is less than 150 ppm) to obtain a negative electrode active material (denoted as P2).
[0100] P2 has an ellipsoidal appearance and contains filler (graphite powder, D50 is 1.2μm) densified graphite particles (D50 of graphite particles is 18μm), and the outer surface of the graphite particles is covered with a carbon layer (the average thickness of the carbon layer is 40nm); based on the total weight of P2, the content of filler in the graphite particles is 7.8% by weight; the content of graphite powder in the filler is 100% by weight.
[0101] Example 3
[0102] (1-1) natural flake graphite is added into a mixer, and a filler (artificial graphite fine powder-1) is added and mixed, and then the obtained mixture is added into a spheroidizing device for spheroidizing treatment, and the filler is wrapped into the natural flake graphite under the collision, friction and shearing action of the spheroidizing wheel on the natural flake graphite, so as to obtain spherical graphite particles (D50 is 18 μm) with filler densification; wherein the weight ratio of filler: (filler + natural flake graphite) is 10:100;
[0103] (1-2) mixing the spherical graphite particles obtained in step (1-1) with asphalt (the temperature of the asphalt is 200° C.) to obtain asphalt-coated graphite particles; wherein the weight ratio of asphalt: (asphalt + spherical graphite particles) is 2.5:100;
[0104] (2) The asphalt-coated graphite particles obtained in step (1-2) are carbonized (the carbonization temperature is 1150° C., and the oxygen content in the carbonization atmosphere is less than 150 ppm) to obtain a negative electrode active material (denoted as P3).
[0105] P3 has an ellipsoidal appearance and contains filler (graphite powder, D50 is 1.2μm) densified graphite particles (D50 of graphite particles is 18μm), and the outer surface of the graphite particles is covered with a carbon layer (the average thickness of the carbon layer is 40nm); based on the total weight of P3, the content of filler in the graphite particles is 5.5% by weight; the content of graphite powder in the filler is 100% by weight.
[0106] Example 4
[0107] (1-1) natural flake graphite is added into a mixer, and a filler (artificial graphite fine powder-2) is added and mixed, and then the obtained mixture is added into a spheroidizing device for spheroidizing treatment, and the filler is wrapped into the natural flake graphite under the collision, friction and shearing action of the spheroidizing wheel on the natural flake graphite, so as to obtain spherical graphite particles (D50 is 18 μm) with a filler densified; wherein the weight ratio of filler: (filler + natural flake graphite) is 10:100;
[0108] (1-2) mixing the spherical graphite particles obtained in step (1-1) with asphalt (the temperature of the asphalt is 200° C.) to obtain asphalt-coated graphite particles; wherein the weight ratio of asphalt: (asphalt + spherical graphite particles) is 2.5:100;
[0109] (2) The asphalt-coated graphite particles obtained in step (1-2) are carbonized (the carbonization temperature is 1150° C., and the oxygen content in the carbonization atmosphere is less than 150 ppm) to obtain a negative electrode active material (denoted as P4).
[0110] P4 has an ellipsoidal appearance and contains filler (graphite powder, D50 is 2.5μm) densified graphite particles (D50 of graphite particles is 18μm), and the outer surface of the graphite particles is covered with a carbon layer (the average thickness of the carbon layer is 40nm); based on the total weight of P4, the content of filler in the graphite particles is 5.5% by weight; the content of graphite powder in the filler is 100% by weight.
[0111] Example 5
[0112] (1-1) natural flake graphite is added into a mixer, and a filler (artificial graphite fine powder-1 and 200°C asphalt in a weight ratio of 99:1) is added and mixed, and then the resulting mixture is added into a spheroidizing device for spheroidization treatment. Under the collision, friction and shearing action of the spheroidizing wheel on the natural flake graphite, the filler is wrapped into the natural flake graphite to obtain spherical graphite particles (D50 is 18μm) with filler densification; wherein the weight ratio of filler: (filler + natural flake graphite) is 10:100; the weight of the asphalt in step (1-1) is based on the weight of amorphous carbon converted after subsequent carbonization;
[0113] (1-2) mixing the spherical graphite particles obtained in step (1-1) with asphalt (the temperature of the asphalt is 200° C.) to obtain asphalt-coated graphite particles; wherein the weight ratio of asphalt: (asphalt + spherical graphite particles) is 2.5:100;
[0114] (2) The mixture obtained in step (1-2) is subjected to carbonization treatment (carbonization temperature is 1150° C., and the oxygen content in the carbonization atmosphere is less than 150 ppm) to obtain a negative electrode active material (denoted as P5).
[0115] P5 has an ellipsoidal appearance and contains fillers (graphite powder, D50 is 1.2μm; amorphous carbon, D50 is 3μm) densified graphite particles (D50 of graphite particles is 18μm), and the outer surface of the graphite particles is covered with a carbon layer (the average thickness of the carbon layer is 40nm); based on the total weight of P5, the content of filler in the graphite particles is 5.5% by weight; the content of graphite powder in the filler is 99% by weight.
[0116] Example 6
[0117] (1-1) natural flake graphite is added into a mixer, and a filler (artificial graphite fine powder-1 and 200°C asphalt in a weight ratio of 89:11) is added and mixed, and then the resulting mixture is added into a spheroidizing device for spheroidization treatment. Under the collision, friction and shearing action of the spheroidizing wheel on the natural flake graphite, the filler is wrapped into the natural flake graphite to obtain spherical graphite particles (D50 is 18μm) with filler densification; wherein the weight ratio of filler: (filler + natural flake graphite) is 10:100; the weight of the asphalt in step (1-1) is based on the weight of amorphous carbon converted after subsequent carbonization;
[0118] (1-2) mixing the spherical graphite particles obtained in step (1-1) with asphalt (the temperature of the asphalt is 200° C.) to obtain asphalt-coated graphite particles; wherein the weight ratio of asphalt: (asphalt + spherical graphite particles) is 2.5:100;
[0119] (2) The asphalt-coated graphite particles obtained in step (1-2) are carbonized (the carbonization temperature is 1150° C., and the oxygen content in the carbonization atmosphere is less than 150 ppm) to obtain a negative electrode active material (denoted as P6).
[0120] P6 has an ellipsoidal appearance and contains fillers (graphite powder, D50 is 1.2μm; amorphous carbon, D50 is 3μm) densified graphite particles (D50 of graphite particles is 18μm), and the outer surface of the graphite particles is covered with a carbon layer (the average thickness of the carbon layer is 40nm); based on the total weight of P6, the content of filler in the graphite particles is 5.5% by weight; the content of graphite powder in the filler is 89% by weight.
[0121] Comparative Example 1
[0122] The method of Example 1 is different in that no filler is added during the spheroidization of natural flake graphite in step (1-1), unfilled spherical graphite particles are obtained in step (1-1), and the unfilled spherical graphite particles are sequentially subjected to step (1-2) and step (2). Other operating processes and parameters are the same as those of Example 1, to obtain a negative electrode active material (denoted as DP1).
[0123] DP1 has an ellipsoidal appearance and contains spherical graphite particles (D50 of graphite particles is 18 μm. DP1 was ion cut and then tested by SEM. The results are as follows: Figure 2 As shown, in Figure 2 As can be seen in the figure, there is no filler in the pores inside the graphite particles in DP1), and the outer surface of the graphite particles is covered with a carbon layer (the average thickness of the carbon layer is 40nm).
[0124] Comparative Example 2
[0125] (1-1) natural flake graphite is added into a mixer, and a filler (phenolic resin) is added and mixed, and then the obtained mixture is added into a spheroidizing device for spheroidization treatment, and the filler is wrapped into the natural flake graphite under the collision, friction and shearing action of the spheroidizing wheel on the natural flake graphite, so as to obtain spherical graphite particles (D50 is 18 μm) with filler densification; wherein the weight ratio of filler: (filler + natural flake graphite) is 20:100; the weight of the phenolic resin in step (1-1) is based on the weight of amorphous carbon converted after subsequent carbonization;
[0126] (1-2) mixing the spherical graphite particles obtained in step (1-1) with asphalt (the temperature of the asphalt is 200° C.) to obtain asphalt-coated graphite particles; wherein the weight ratio of asphalt: (asphalt + spherical graphite particles) is 2.5:100;
[0127] (2) The pitch-coated graphite particles obtained in step (1-2) are carbonized (the carbonization temperature is 1150° C., and the oxygen content in the carbonization atmosphere is less than 150 ppm) to obtain a negative electrode active material (denoted as DP2).
[0128] DP2 has an ellipsoidal appearance and contains graphite particles (D50 of graphite particles is 18 μm) densified with fillers (amorphous carbon, D50 is 3 μm), and the outer surface of the graphite particles is covered with a carbon layer (the average thickness of the carbon layer is 40 nm); based on the total weight of DP2, the content of fillers in the graphite particles is 9.8 wt%; the content of amorphous carbon in the filler is 100 wt%.
[0129] Comparative Example 3
[0130] The method of Example 1 is followed, except that no filler is added during the spheroidization of natural flake graphite in step (1-1), unfilled spherical graphite particles are obtained in step (1-1), and the unfilled spherical graphite particles and asphalt (the temperature of the asphalt is 200°C) are placed in a mixer and mixed evenly (wherein the weight ratio of asphalt: (asphalt + unfilled spherical graphite particles) is 2.5:100), and then the mixed product is placed in an elastic rubber tank for isostatic pressure treatment, and finally the obtained isostatic pressure product is subjected to step (2). The other operating processes and parameters are the same as those of Example 1, and a negative electrode active material (denoted as DP3) is obtained.
[0131] DP3 has an ellipsoidal appearance and contains spherical graphite particles (the average particle size of the graphite particles is 18μm, there is no filler inside, and the pores are dense after isostatic pressing), and the outer surface of the graphite particles is covered with a carbon layer (the average thickness of the carbon layer is 40nm).
[0132] Test Case
[0133] The negative electrode active materials P1-P6 and DP1-DP3 prepared in the above Examples 1-6 and Comparative Examples 1-3 were used to prepare negative electrodes, and then batteries were prepared to test the high-rate charge and discharge performance, cycle performance and expansion degree of the batteries.
[0134] Preparation of negative electrode: The negative electrode active materials P1-P6, DP1-DP3 were mixed with a conductive agent (ketjen black), a thickener (sodium carboxymethyl cellulose), a binder (styrene-butadiene rubber) etc. at a weight ratio of 96:1:1:2 to obtain a mixed powder. The mixed powder was then stirred with deionized water using a vacuum mixer to form a negative electrode slurry and evenly coated on a carbon-coated copper foil. The negative electrodes were prepared after baking and rolling (respectively designated as N1-N6 and DN1-DN3).
[0135] Preparation of the positive electrode: Lithium iron phosphate (LiFePO4), conductive agent (Ketjen black), and binder (polyvinylidene fluoride) are mixed in a weight ratio of 96:1.5:2.5 to obtain a mixed powder. The mixed powder is then mixed with N-methylpyrrolidone (NMP) using a vacuum mixer to form a positive electrode slurry and evenly coated on aluminum foil. The positive electrode is prepared after baking and rolling.
[0136] Preparation of electrolyte: Ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) were mixed in a volume ratio of 1:1:1 to prepare an electrolyte.
[0137] The above positive electrode, negative electrode (N1-N6, DN1-DN3), electrolyte and polypropylene separator were prepared into 1.5Ah laminated lithium batteries (respectively denoted as B1-B6, DB1-DB3), and the batteries were subjected to high-rate charge and discharge tests and cycle performance tests, respectively.
[0138] Conditions for high rate charge and discharge test:
[0139] (1) At 25°C, charge and discharge at 0.1C and calibrate the battery capacity;
[0140] (2) Charge to full charge at 0.1C, then discharge at 3C, calculate the discharge efficiency of the battery;
[0141] (3) Charge the battery to full charge at 3C and then discharge it at 0.1C. Calculate the charging efficiency of the battery.
[0142] Cyclic performance test conditions:
[0143] The battery was mounted on a displacement sensor for thickness measurement. The battery was charged and discharged at 1C for 1000 cycles at 25°C, and the capacity retention rate of the battery was calculated. After the above cycles were completed, the displacement sensor data was recorded, and the thickness change rate of the battery was calculated based on the initial thickness of the battery and the thickness after the cycle.
[0144] The test results are shown in Table 1.
[0145] Table 1
[0146]
[0147] As can be seen from Table 1, the negative electrode active material provided by the present invention uses graphite powder as the main filler of the pores of graphite particles, which can effectively inhibit the expansion of the negative electrode during the battery cycle. Under the above test conditions, the thickness change rate of the battery after B1-B6 cycles for 1000 cycles is less than 0.8%, which is significantly lower than DB1-DB3. Due to the effective solution to the expansion problem of natural graphite negative electrodes, B1-B6 exhibits a higher cycle life, and the capacity retention rate after 1000 cycles at 25°C and 1C charge and discharge conditions is higher than 86%, and has excellent rate performance, and the charge and discharge efficiency at 25°C and 3C rate conditions is higher than 80%.
[0148] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A negative electrode active material, characterized in that: The negative electrode active material comprises: graphite particles, and a carbon layer covering the graphite particles; There are holes inside the graphite particles, and the holes are filled with fillers; The filler includes graphite powder and optionally amorphous carbon.
2. The negative electrode active material according to claim 1, wherein The particle shape of the negative electrode active material is spherical or ellipsoidal; Preferably, the graphite particles are spherical graphite particles.
3. The negative electrode active material according to claim 1 or 2, wherein The average particle size of the graphite particles is 8-35 μm, preferably 10-30 μm.
4. The negative electrode active material according to any one of claims 1 to 3, wherein The thickness of the carbon layer is 1-100 nm.
5. The negative electrode active material according to any one of claims 1 to 4, wherein: Based on the total weight of the negative electrode active material, the content of the filler in the negative electrode active material is 5-15 wt %, preferably 7-10 wt %.
6. The negative electrode active material according to any one of claims 1 to 5, wherein: Based on the total weight of the filler, the content of the graphite powder in the filler is 90-100 wt %, preferably 95-100 wt %.
7. The negative electrode active material according to any one of claims 1 to 6, wherein: The average particle size of the filler is 0.5-3 μm, preferably 1-2 μm; Preferably, the graphitization degree of the graphite powder is ≥94%; Preferably, the graphite powder is artificial graphite fine powder obtained in a powder screening process during the preparation of artificial graphite.
8. A method for preparing a negative electrode active material, characterized in that: include: (1) granulating a natural graphite raw material and a filler to obtain graphite particles; (2) mixing the graphite particles with an organic carbon source to obtain graphite particles coated with an organic carbon source; (3) carbonizing the graphite particles coated with the organic carbon source to obtain a negative electrode active material; Wherein, the internal pores of the graphite particles are filled with the filler; The filler includes graphite powder, optionally asphalt and optionally resin.
9. The preparation method according to claim 8, wherein: The granulation process includes: The natural graphite raw material is subjected to spheroidization treatment, and the filler is added during the spheroidization process, so that the natural graphite raw material wraps the filler to obtain graphite particles.
10. The preparation method according to claim 8 or 9, wherein: The natural graphite raw material is natural flake graphite; Preferably, the weight ratio of the filler: (the filler + the natural graphite raw material) is (10-30):100; Preferably, the organic carbon source is selected from asphalt and / or resin.
11. The preparation method according to any one of claims 8 to 10, wherein: In the filler, the content of the graphite powder is 90-100% by weight, preferably 95-100% by weight; Preferably, the average particle size of the filler is 0.5-3 μm, more preferably 1-2 μm; Preferably, the graphitization degree of the graphite powder is ≥94%; Preferably, the graphite powder is artificial graphite fine powder obtained in a powder screening process during the preparation of artificial graphite.
12. The preparation method according to any one of claims 8 to 11, wherein: The weight ratio of the organic carbon source: (the graphite particles + the organic carbon source) is (0.5-5):100; Preferably, the carbonization treatment conditions include: a temperature of 1100-1200° C., and an oxygen content in the carbonization atmosphere of less than 400 ppm.
13. A negative electrode active material prepared by the method according to any one of claims 8 to 12.
14. A negative electrode, comprising a negative electrode current collector, and an active material layer disposed on the negative electrode current collector; in, The active material layer contains the negative electrode active material according to any one of claims 1 to 7 and 13.
15. A battery comprising the negative electrode according to claim 14; preferably, the battery is a lithium ion battery or a sodium ion battery.
16. An electrical device comprising the battery according to claim 15.
Citation Information
Patent Citations
Graphite negative electrode material, preparation method thereof and lithium ion battery
CN114171738A
Negative electrode material, preparation method and electrochemical device comprising negative electrode material
CN114300685A
Cooking apparatus and method for controlling thereof
KR1020220153501A
Lithium-ion secondary battery and manufacturing method thereof
US20070003837A1
Cited By
Negative electrode material and secondary battery
WO2026124346A1