Method for improving energy density of silicon-based negative electrode by reserving gap in current collector
By leaving a gap on the current collector and preparing conductive MXene-rGO-CNT composites, the problem of the impact of volume changes in silicon negative electrodes is solved, the energy density and cycle life of lithium-ion batteries are improved, and the electromagnetic shielding performance is enhanced.
Patent Information
- Application Number
- CN202411274606.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-12-03
AI Technical Summary
The large-scale application of silicon negative electrodes in lithium-ion batteries is caused by the expansion and contraction caused by huge volume changes during the cycle, which affects its reversible capacity and cycle life. The existing current collector design lacks effective void reservations, which limits lithium. The rapid embedding and deintercalation of ions reduces fast charging performance.
The space is reserved on the current collector, and the conductive MXene-rGO-CNT composite material is prepared, and the PMMA microsphere template method and heat treatment technology are used to form the MXene-rGO-CNT composite material with a three-dimensional hollow structure, providing expansion reserved space and constructing Conductive network improves the energy density of the silicon-based negative electrode.
The energy density and cycle life of the silicon-based negative electrode are improved, the fast charging performance of the battery is optimized, and the electromagnetic shielding performance is enhanced through the porous structure.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of current collectors, and in particular to a method for reserving gaps on current collectors to increase the energy density of silicon-based negative electrodes. Background Art
[0002] Graphite has become the negative electrode active material for most lithium-ion power and energy storage batteries on the market due to its advantages such as a stable discharge platform, high gram capacity and low price. At present, the reversible specific capacity of graphite negative electrode materials is close to the theoretical specific capacity of 372mA·h / g. In recent years, with the vigorous development of the new energy industry, the demand for high energy density lithium-ion batteries has increased. The development of high specific capacity negative electrode materials to replace graphite has become an important choice for the research and development of high energy density lithium-ion batteries. Silicon has great potential as a negative electrode material in secondary batteries. It has the advantages of being green, non-toxic and harmless, and having abundant reserves on the earth. Especially for lithium-ion batteries, the theoretical specific capacity of silicon negative electrode at room temperature is as high as 3579 mA·h / g, and the working potential is low. It is considered to be one of the ideal negative electrode materials.
[0003] However, the large-scale application of silicon negative electrodes in lithium-ion batteries still faces several key difficulties. Among them, the biggest challenge affecting the industrialization of silicon negative electrodes is the large volume change of silicon during the cycle. Compared with the volume change of only 12% of the graphite negative electrode, the volume change of the silicon negative electrode is as high as 300%, which means that during the charge and discharge cycle, the silicon negative electrode will undergo huge expansion and contraction, causing it to be severely broken and pulverized, causing the silicon particles to lose electrical contact with the current collector, thereby affecting its reversible capacity and cycle life. Although improving the reversible capacity of silicon-based negative electrodes can enhance the energy density and cruising range of batteries to a certain extent, the existing current collector design lacks effective gap reservation, which limits the rapid insertion and extraction of lithium ions, thereby reducing the fast charging performance and failing to meet the market demand for fast charging.
[0004] Therefore, we propose a method to reserve gaps on the current collector to improve the energy density of silicon-based anodes. Summary of the invention
[0005] The purpose of the present invention is to provide a method for reserving gaps on a current collector to increase the energy density of a silicon-based negative electrode, so as to solve the problems raised in the above-mentioned background technology.
[0006] In order to solve the above technical problems, the present invention provides the following technical solutions: A method for reserving gaps on a current collector to increase the energy density of a silicon-based negative electrode comprises the following steps: Step S1: Stir lithium fluoride and hydrochloric acid evenly, add Ti3AlC2, heat to 35-40°C, stir evenly, centrifuge and wash, collect the precipitate, and obtain Ti3C2T x Sediment; Step S2: In an argon environment, Ti3C2T x The precipitate was ultrasonically stripped and centrifuged to collect the upper Ti3C2T x The suspension is freeze-dried to obtain Mxene powder; Step S3: Mix the MXene powder and the polymethyl methacrylate solution evenly, add deionized water, stir evenly under an argon environment, centrifuge, collect the precipitate, add graphene oxide and deionized water, stir evenly under an argon environment, then add carbon nanotubes, stir evenly under an argon environment, centrifuge, collect the upper suspension and freeze-dry to obtain a PMMA@MXene-GO-CNT composite material; heat-treat the PMMA@MXene-GO-CNT composite material under an argon environment to obtain a MXene-rGO-CNT composite material; Step S4: Stir polyacrylic acid and pure water to obtain glue solution; add 1 / 2 mass parts of MXene-rGO-CNT composite material, 1 / 2 mass parts of conductive carbon black and graphite, stir evenly, add the remaining mass parts of MXene-rGO-CNT composite material and conductive carbon black, stir evenly, add sodium hydroxide solution, stir evenly, add isopropanol and pure water, stir evenly to obtain coating slurry; Step S5: coating the coating slurry on the copper foil, and after drying, forming a MXene-rGO-CNT coating to obtain a current collector; Step S6: coating the active slurry on the surface of the current collector and obtaining a pole piece after drying.
[0007] Furthermore, in step S1, Ti3C2T x The specific preparation process of the precipitate includes the following steps: stirring lithium fluoride and hydrochloric acid at 550-650 r / min for 25-35 minutes, adding Ti3AlC2 within 4-6 minutes, heating to 35-40°C, stirring for 45-55 hours, first centrifugally washing with 1 mol / L dilute hydrochloric acid for 2-4 times, and then centrifugally washing with deionized water until the pH is 7-8, each centrifugation washing speed is 3200-3800 r / min, the centrifugation washing time is 5-10 minutes, collecting the precipitate to obtain Ti3C2T x Sediment.
[0008] Furthermore, in step S1, the material-liquid ratio of lithium fluoride and hydrochloric acid is (2.8-3.6): (15-25) g / mL, the concentration of hydrochloric acid is 10-12 mol / L, and the material-liquid ratio of Ti3AlC2 and hydrochloric acid is (1.5-2.5): (15-25) g / mL.
[0009] Furthermore, in step S2, the specific preparation process of MXene powder includes the following steps: in an argon environment, Ti3C2T x The precipitate was subjected to ultrasonic stripping for 20-40 min and centrifuged at 3200-3800 r / min for 10-20 min to collect the upper Ti3C2T x The suspension was freeze-dried to obtain Mxene powder.
[0010] Furthermore, in step S3, the specific preparation process of the MXene-rGO-CNT composite material includes the following steps: mixing the MXene powder and the polymethyl methacrylate solution evenly, adding deionized water, stirring at 4000-4500 r / min for 1.5-2.5 h in an argon environment, centrifuging at a speed of 3200-3800 r / min for 20-40 min, collecting the precipitate, adding graphene oxide and deionized water, stirring at 4000-4500 r / min for 1.5-2. 5h, then add carbon nanotubes, stir at 4000-4500r / min for 1.5-2.5h in an argon environment, centrifuge at 3200-3800r / min for 10-20min, collect the upper suspension and freeze-dry to obtain PMMA@MXene-GO-CNT composite material; in an argon environment, heat treat the PMMA@MXene-GO-CNT composite material at 400-500℃ for 0.5-1.5h to obtain a MXene-rGO-CNT composite material.
[0011] In the above technical scheme, the PMMA microsphere structure is introduced by evenly mixing MXene powder and polymethyl methacrylate solution, and graphene oxide (GO) and carbon nanotube (CNT) materials are added during the solution blending process to construct a conductive network to form a PMMA@MXene-GO-CNT core-shell structure composite material; then, the PMMA@MXene-GO-CNT composite material is heat-treated in an Ar environment to in-situ pyrolyze the PMMA microspheres, and at the same time, GO is thermally reduced to rGO to obtain a MXene-rGO-CNT composite material with a three-dimensional hollow structure.
[0012] Furthermore, in step S3, the solvent of the polymethyl methacrylate solution is acetone, the solute is PMMA microspheres, and the concentration thereof is 50 mg / mL.
[0013] Furthermore, in step S3, the mass of the Mxene powder is 0.5-1.5wt% of the polymethyl methacrylate solution.
[0014] Furthermore, in step S3, the mass ratio of MXene powder, graphene oxide, deionized water and carbon nanotubes is 1:5:(15-25):3.
[0015] Furthermore, in step S4, the specific preparation process of the coating slurry includes the following steps: stirring polyacrylic acid and pure water at a speed of 1000-1200r / min for 9-11min to obtain a glue solution; adding 1 / 2 mass fraction of MXene-rGO-CNT composite material, 1 / 2 mass fraction of conductive carbon black and graphite, stirring at a speed of 3000-3200r / min for 19-21min, adding the remaining mass fraction of MXene-rGO-CNT composite material and conductive carbon black, stirring at a speed of 3000-3200r / min for 29-31min, adding sodium hydroxide solution, stirring at a speed of 3000-3200r / min for 89-91min, adding isopropanol and pure water, stirring at a speed of 400-600r / min for 29-31min, to obtain a coating slurry.
[0016] Furthermore, in step S4, the solid content of the coating slurry is 10%; the mass ratio of polyacrylic acid to pure water is 1:(3-4); the total mass of the MXene-rGO-CNT composite material, conductive carbon black and graphite is 1.5 times the mass of the glue; the mass ratio of the MXene-rGO-CNT composite material and conductive carbon black is 9:1; the mass of graphite is 17-18% of the total mass of the MXene-rGO-CNT composite material and conductive carbon black.
[0017] Furthermore, in step S4, the amount of solid sodium hydroxide added is 7% of the mass of the glue solution, the concentration of the sodium hydroxide solution is 8wt%, the mass ratio of isopropanol to pure water is 1:28, and the amount of isopropanol used is 15% of the total mass of the coating slurry.
[0018] Furthermore, in step S5, the thickness of the MXene-rGO-CNT coating is 0.5-1.0 μm.
[0019] Furthermore, in step S6, the preparation method of the active slurry is as follows: The dried active material, binder and conductive agent are ground and mixed evenly, deionized water is added, and grinding is continued for 3-5 minutes to obtain active slurry.
[0020] Furthermore, in step S6, the active material is active silicon, the binder is sodium alginate, the conductive agent is acetylene black, the mass ratio of the active material, the binder and the conductive agent is 6:2:2, and the solid content of the active slurry is 52-54%.
[0021] Furthermore, in step S6, the coating process uses a SZQ four-sided coater, and the total thickness of the electrode is 150 µm.
[0022] Furthermore, the drying temperature is 80-120°C.
[0023] Compared with the prior art, the present invention has the following beneficial effects: 1. A method for reserving gaps on a current collector to improve the energy density of a silicon-based negative electrode of the present invention comprises selecting conductive MXene nanosheets and graphene oxide mixed shells to be assembled on polymethyl methacrylate microspheres, and carbon nanotubes assist in constructing a conductive network to prepare a PMMA@MXene-GO-CNT composite material with a three-dimensional core-shell structure; a MXene-rGO-CNT composite material is obtained by a sacrificial template method and heat treatment. During the preparation process, the pyrolysis and freeze-drying process of the PMMA microsphere template is performed to make the MXene-rGO-CNT composite material have macroscopic pores and microscopic hollow sphere structures, thereby obtaining a lower density (0.26 g / cm 3 ).
[0024] 2. A method of reserving gaps on a current collector to increase the energy density of a silicon-based negative electrode according to the present invention. The MXene-rGO-CNT composite material has the characteristics of being lightweight. Due to the introduction of a hollow structure, the composite material has a lower density, and the hollow structure reserves space for the expansion of the silicon-based negative electrode during the cycle. MXene, rGO and CNT have good electrical conductivity. rGO and CNT are staggered on the surface of MXene nanosheets to form a complete conductive path, giving the MXene-rGO-CNT composite material excellent electrical conductivity. Pre-coating a two-dimensional / three-dimensional structured MXene-rGO / MXene-rGO-CNT coating on the surface of the copper foil effectively increases the energy density of the battery and optimizes the cycle life of the battery.
[0025] 3. The present invention provides a method for reserving gaps on the current collector to increase the energy density of the silicon-based negative electrode. When the electromagnetic wave is inside the material, the hollow porous structure provides more propagation space and paths for the electromagnetic wave entering the composite material, thereby enhancing the multiple reflection and scattering effects that occur when the electromagnetic wave propagates inside the material, thereby changing and increasing the propagation path of the electromagnetic wave inside the material, causing the electromagnetic wave to lose more energy inside the material. Finally, only a very small amount of electromagnetic waves can penetrate the MXene-rGO-CNT composite material, which can reduce the penetration of the electromagnetic wave and improve the electromagnetic shielding performance of the material. DETAILED DESCRIPTION
[0026] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] It should be noted that the purchase manufacturers of all raw materials involved in the present invention are not subject to any special restrictions and exemplarily include: lithium fluoride: CAS No. 7789-24-4, purchased from Nanjing Taiye Chemical New Materials Co., Ltd.; Ti3AlC2: particle size 5-10 μm, brand MAX-Ti3AlC2, purchased from Shandong Starry Metal Materials Co., Ltd.; polymethyl methacrylate: Japan Mitsubishi Rayon LP-3104, purchased from Dongguan Shunqi Plastic Raw Materials Co., Ltd.; graphene oxide: model MG-GO-01, thickness 1nm, single layer diameter 0.5μm, purchased from Shanghai Maoguo Nano Technology Co., Ltd.; carbon nanotubes: inner diameter 10-20nm, tube length 5-15μm, purchased from Shanghai Maoguo Nano Technology Co., Ltd.; polyacrylic acid: solid content 25%, purchased from Wuhan Proloff Biotechnology Co., Ltd.; conductive carbon black: SUPER P Li (Swiss Termega), purchased from Guangdong Lvwei New Materials Technology Co., Ltd.; graphite: particle size 5-10μm, purchased from Luoyang Tongrun Information Technology Co., Ltd.; copper foil: T2 copper foil, thickness 8μm, purchased from Shandong Huiya Metal Technology Co., Ltd.; active silicon: item number Brofos-Si-50, particle size 50nm, sourced from Bohuas Nanotechnology (Ningbo) Co., Ltd.; acetylene black: model HCY-80, purchased from Tianjin Huacai Chemical Co., Ltd.
[0028] Embodiment 1: A method for increasing the energy density of a silicon-based negative electrode by reserving gaps on a current collector, comprising the following process: Step S1: 2.8 g lithium fluoride and 15 mL 10 mol / L hydrochloric acid were stirred at 550 r / min for 25 min, 1.5 g Ti3AlC2 was added within 4 min, heated to 35 ° C, stirred for 45 h, centrifuged and washed twice with 1 mol / L dilute hydrochloric acid, and then centrifuged and washed with deionized water until pH = 7, each centrifugal washing speed was 3200 r / min, the centrifugal washing time was 5 min, and the precipitate was collected to obtain Ti3C2T x Sediment; Step S2: In an argon environment, Ti3C2T x The precipitate was subjected to ultrasonic stripping for 20 min and centrifuged at 3200 r / min for 10 min to collect the upper Ti3C2T x The suspension is freeze-dried to obtain Mxene powder; Step S3: 1 g of MXene powder and 99 g of 50 mg / mL polymethyl methacrylate solution were mixed evenly, 15 mL of deionized water was added, and the mixture was stirred at 4000 r / min for 1.5 h in an argon environment, and centrifuged at 3200 r / min for 20 min. The precipitate was collected, 5 g of graphene oxide and 15 mL of deionized water were added, and the mixture was stirred at 4000 r / min for 1.5 h in an argon environment, and then 3 g of carbon nanotubes were added. The mixture was stirred at 4000 r / min for 1.5 h in an argon environment, and centrifuged at 3200 r / min for 10 min. The upper suspension was collected and freeze-dried to obtain a PMMA@MXene-GO-CNT composite material; the PMMA@MXene-GO-CNT composite material was heat-treated at 400°C for 0.5 h in an argon environment to obtain a MXene-rGO-CNT composite material; Step S4: 1.95g polyacrylic acid and 5.85g pure water were stirred at a speed of 1000r / min for 9min to obtain a glue solution; 4.5g MXene-rGO-CNT composite material, 0.5g conductive carbon black and 1.7g graphite were added, and stirred at a speed of 3000r / min for 19min, 4.5g MXene-rGO-CNT composite material and 0.5g conductive carbon black were added, and stirred at a speed of 3000r / min for 29min, 8wt% sodium hydroxide solution (solid addition amount is 7% of the glue solution mass) was added, and stirred at a speed of 3000r / min for 89min, isopropanol and pure water were added at a mass ratio of 1:28 (the amount of isopropanol is 15% of the total mass of the coating slurry), and stirred at a speed of 400r / min for 29min to obtain a coating slurry with a solid content of 10%; Step S5: coating the coating slurry on a copper foil, and drying at 80° C. to form a MXene-rGO-CNT coating to obtain a current collector; Step S6: Grind the dried 6 g active silicon, 2 g sodium alginate and 2 g acetylene black, mix well, add deionized water, and continue grinding for 3 minutes to obtain an active slurry with a solid content of 52%; apply the active slurry on the surface of the current collector, use a SZQ four-sided coater with a 150 µm surface to evenly apply the active slurry, and after drying at 80°C, obtain a pole piece.
[0029] Embodiment 2: A method for increasing the energy density of a silicon-based negative electrode by reserving gaps on a current collector, comprising the following process: Step S1: 3.2 g lithium fluoride and 20 mL 11 mol / L hydrochloric acid were stirred at 600 r / min for 30 min, 2 g Ti3AlC2 was added within 5 min, heated to 38 °C, stirred for 48 h, first centrifuged and washed 3 times with 1 mol / L dilute hydrochloric acid, and then centrifuged and washed with deionized water until pH = 7.5, each centrifugation washing speed was 3500 r / min, the time was 8 min, and the precipitate was collected to obtain Ti3C2T x Sediment; Step S2: In an argon environment, i3 C2T x The precipitate was subjected to ultrasonic stripping for 30 min, centrifuged at 3500 r / min for 15 min, and the upper layer of T i3 C2T x The suspension is freeze-dried to obtain Mxene powder; Step S3: 2 g of MXene powder and 134 g of 50 mg / mL polymethyl methacrylate solution were mixed evenly, 40 mL of deionized water was added, and the mixture was stirred at 4200 r / min for 2 h in an argon environment, and centrifuged at 3500 r / min for 30 min. The precipitate was collected, 10 g of graphene oxide and 40 mL of deionized water were added, and the mixture was stirred at 4200 r / min for 2 h in an argon environment, and then 6 g of carbon nanotubes were added. The mixture was stirred at 4200 r / min for 2 h in an argon environment, and centrifuged at 3500 r / min for 15 min. The upper suspension was collected and freeze-dried to obtain a PMMA@MXene-GO-CNT composite material; the PMMA@MXene-GO-CNT composite material was heat-treated at 450°C for 1 h in an argon environment to obtain a MXene-rGO-CNT composite material; Step S4: 1.7g polyacrylic acid and 6.12g pure water are stirred at a speed of 1100r / min for 10min to obtain a glue solution; 4.5g MXene-rGO-CNT composite material, 0.5g conductive carbon black and 1.73g graphite are added, and stirred at a speed of 3100r / min for 20min, 4.5g MXene-rGO-CNT composite material and 0.5g conductive carbon black are added, and stirred at a speed of 3100r / min for 30min, 8wt% sodium hydroxide solution (solid addition amount is 7% of the glue solution mass) is added, and stirred at a speed of 3100r / min for 90min, isopropanol and pure water are added at a mass ratio of 1:28 (the amount of isopropanol is 15% of the total mass of the coating slurry), and stirred at a speed of 500r / min for 30min to obtain a coating slurry with a solid content of 10wt%; Step S5: coating the coating slurry on a copper foil, and drying at 100° C. to form a MXene-rGO-CNT coating to obtain a current collector; Step S6: Grind the dried 6 g active silicon, 2 g sodium alginate and 2 g acetylene black, mix well, add deionized water, and continue grinding for 4 minutes to obtain an active slurry with a solid content of 53 wt%; apply the active slurry on the surface of the current collector, use a SZQ four-sided coater with a 150 µm surface to evenly apply the active slurry, and dry at 100 ° C to obtain a pole piece.
[0030] Embodiment 3: A method for increasing the energy density of a silicon-based negative electrode by reserving gaps on a current collector, comprising the following process: Step S1: 3.6 g lithium fluoride and 25 mL 12 mol / L hydrochloric acid were stirred at 650 r / min for 35 min, 2.5 g Ti3AlC2 was added within 6 min, heated to 40 °C, stirred for 55 h, first centrifuged and washed 4 times with 1 mol / L dilute hydrochloric acid, and then centrifuged and washed with deionized water until pH = 8, each centrifugation washing speed was 3800 r / min, the time was 10 min, and the precipitate was collected to obtain T i3 C2T x Sediment; Step S2: In an argon environment, i3 C2T x The precipitate was subjected to ultrasonic stripping for 40 min, centrifuged at 3800 r / min for 20 min, and the upper layer of T i3 C2T x The suspension is freeze-dried to obtain Mxene powder; Step S3: 2 g of MXene powder and 134 g of 50 mg / mL polymethyl methacrylate solution were mixed evenly, 50 mL of deionized water was added, and the mixture was stirred at 4500 r / min for 2.5 h in an argon environment, and centrifuged at 3800 r / min for 10 min. The precipitate was collected, 10 g of graphene oxide and 50 mL of deionized water were added, and the mixture was stirred at 4500 r / min for 2.5 h in an argon environment, and then 6 g of carbon nanotubes were added. The mixture was stirred at 4500 r / min for 2.5 h in an argon environment, and centrifuged at 3800 r / min for 15 min. The upper suspension was collected and freeze-dried to obtain a PMMA@MXene-GO-CNT composite material; the PMMA@MXene-GO-CNT composite material was heat-treated at 500°C for 1.5 h in an argon environment to obtain a MXene-rGO-CNT composite material; Step S4: 1.572g polyacrylic acid and 6.288g pure water were stirred at a speed of 1200r / min for 11min, 4.5g MXene-rGO-CNT composite material, 0.5g conductive carbon black and 1.79g graphite were added, and stirred at a speed of 3200r / min for 21min, 4.5g MXene-rGO-CNT composite material and 0.5g conductive carbon black were added, and stirred at a speed of 3200r / min for 31min, 8wt% sodium hydroxide solution (solid addition amount is 7% of the mass of the glue solution) was added, and stirred at a speed of 3200r / min for 91min, isopropanol and pure water were added at a mass ratio of 1:28 (the amount of isopropanol is 15% of the total mass of the coating slurry), and stirred at a speed of 600r / min for 31min to obtain a coating slurry with a solid content of 10wt%; Step S5: coating the coating slurry on a copper foil, and drying at 120° C. to form a MXene-rGO-CNT coating to obtain a current collector; Step S6: Grind the dried 6 g active silicon, 2 g sodium alginate and 2 g acetylene black, mix well, add deionized water, and continue grinding for 5 min to obtain an active slurry with a solid content of 54%; apply the active slurry on the surface of the current collector, use a SZQ four-sided coater with a 150 µm surface to evenly apply the active slurry, and dry at 120°C to obtain a pole piece.
[0031] Comparative Example 1: A method for increasing the energy density of a silicon-based negative electrode by reserving gaps on a current collector, comprising the following processes: Compared with Example 2, Comparative Example 1 does not include steps S1-S5, the current collector in step S6 is replaced with a double-glazed copper foil, and the other steps are the same as those in Example 2.
[0032] Comparative Example 2: A method for increasing the energy density of a silicon-based negative electrode by reserving gaps on a current collector, comprising the following processes: Compared with Example 2, no carbon nanotubes are added in step S3 of Comparative Example 2 to obtain a MXene-rGO composite material with a two-dimensional structure, and the other steps are the same as those of Example 2.
[0033] Experiment: Take the pole pieces obtained in Examples 1-3 and Comparative Examples 1-2, cut them into discs with a diameter of 12 mm with a punching machine, put them into an Ar-protected glove box (oxygen and water contents are both below 0.1), and assemble the battery using a sealing machine in the order of negative electrode shell, negative electrode sheet, diaphragm, positive electrode sheet, gasket, spring and positive electrode shell. The sealing pressure is 1000 Psi. During the assembly process, a drop of electrolyte needs to be added to each side of the diaphragm to ensure the infiltration effect of the electrolyte; wherein the model of the battery shell is CR2032 (purchased from Foshan Jiaying Battery Co., Ltd.), the negative electrode sheet is the pole sheet prepared by the present invention, the positive electrode sheet is a lithium iron phosphate positive electrode sheet (model is Dongyangguang P321), the diaphragm is Celgard 2400 material, and the preparation method of the electrolyte is: 1 mol / L LiPF6 is dissolved in a mixture of EC / DEC / EMC=1:1:1, and 5% FEC is added as an additive. The battery charge and discharge performance was tested using a LAND CT2001A battery tester (Wuhan Landian). At 0.2C, the battery was cycled 1, 9, 23, and 50 times, respectively, to determine the reversible capacity with a voltage range of 2.0–3.65 V.
[0034] Test Results
[0035] According to the data in the above table, we can clearly draw the following conclusions: Compared with Examples 1-3, the reversible capacity of the products obtained in Comparative Examples 1 and 2 decreased, indicating that pre-coating a two-dimensional / three-dimensional structured MXene-rGO / MXene-rGO-CNT coating on the copper foil surface can enhance the reversible capacity of the silicon-based negative electrode, thereby increasing the energy density of the battery, extending the driving range, improving the fast charging performance, and optimizing the cycle life of the battery.
[0036] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process method article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process method article or device.
[0037] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for increasing the energy density of a silicon-based negative electrode by reserving gaps on a current collector, characterized in that: The steps include: Step S1: Stir lithium fluoride and hydrochloric acid evenly, add Ti3AlC2, heat to 35-40°C, stir evenly, centrifuge and wash, collect the precipitate, and obtain Ti3C2T x Sediment; Step S2: In an argon environment, Ti3C2T x The precipitate was ultrasonically stripped and centrifuged to collect the upper Ti3C2T x The suspension is freeze-dried to obtain Mxene powder; Step S3: Mix the MXene powder and the polymethyl methacrylate solution evenly, add deionized water, stir evenly under an argon environment, centrifuge, collect the precipitate, add graphene oxide and deionized water, stir evenly under an argon environment, then add carbon nanotubes, stir evenly under an argon environment, centrifuge, collect the upper suspension and freeze-dry to obtain a PMMA@MXene-GO-CNT composite material; heat-treat the PMMA@MXene-GO-CNT composite material under an argon environment to obtain a MXene-rGO-CNT composite material; Step S4: Stir polyacrylic acid and pure water to obtain glue solution; add 1 / 2 mass parts of MXene-rGO-CNT composite material, 1 / 2 mass parts of conductive carbon black and graphite, stir evenly, add the remaining mass parts of MXene-rGO-CNT composite material and conductive carbon black, stir evenly, add sodium hydroxide solution, stir evenly, add isopropanol and pure water, stir evenly to obtain coating slurry; Step S5: coating the coating slurry on the copper foil, and after drying, forming a MXene-rGO-CNT coating to obtain a current collector; Step S6: coating the active slurry on the surface of the current collector and obtaining a pole piece after drying.
2. The method of claim 1 for increasing the energy density of a silicon-based negative electrode by reserving gaps on a current collector, characterized in that: In step S1, Ti3C2T x The specific preparation process of the precipitate includes the following steps: stirring lithium fluoride and hydrochloric acid at 550-650 r / min for 25-35 minutes, adding Ti3AlC2 within 4-6 minutes, heating to 35-40°C, stirring for 45-55 hours, first centrifugally washing with 1 mol / L dilute hydrochloric acid for 2-4 times, and then centrifugally washing with deionized water until the pH is 7-8, each centrifugation washing speed is 3200-3800 r / min, the centrifugation washing time is 5-10 minutes, collecting the precipitate to obtain Ti3C2T x Sediment.
3. The method of claim 1 for increasing the energy density of a silicon-based negative electrode by reserving gaps on a current collector, characterized in that: In step S1, the material-liquid ratio of lithium fluoride to hydrochloric acid is (2.8-3.6): (15-25) g / mL, the concentration of hydrochloric acid is 10-12 mol / L, and the material-liquid ratio of Ti3AlC2 to hydrochloric acid is (1.5-2.5): (15-25) g / mL.
4. The method of claim 1 for increasing the energy density of a silicon-based negative electrode by reserving gaps on a current collector, characterized in that: In step S2, the specific preparation process of MXene powder includes the following steps: in an argon environment, Ti3C2T x The precipitate was subjected to ultrasonic stripping for 20-40 min and centrifuged at 3200-3800 r / min for 10-20 min to collect the upper Ti3C2T x The suspension was freeze-dried to obtain Mxene powder.
5. The method of claim 1 for increasing the energy density of a silicon-based negative electrode by reserving gaps on a current collector, characterized in that: In step S3, the specific preparation process of the MXene-rGO-CNT composite material includes the following steps: mixing the MXene powder and the polymethyl methacrylate solution evenly, adding deionized water, stirring at 4000-4500 r / min for 1.5-2.5 h in an argon environment, centrifuging at a speed of 3200-3800 r / min for 20-40 min, collecting the precipitate, adding graphene oxide and deionized water, stirring at 4000-4500 r / min for 1.5-2.5 h in an argon environment. , then add carbon nanotubes, stir at 4000-4500r / min for 1.5-2.5h in an argon environment, centrifuge at 3200-3800r / min for 10-20min, collect the upper suspension and freeze-dry it to obtain a PMMA@MXene-GO-CNT composite material; in an argon environment, heat treat the PMMA@MXene-GO-CNT composite material at 400-500℃ for 0.5-1.5h to obtain a MXene-rGO-CNT composite material.
6. The method of claim 1 for increasing the energy density of a silicon-based negative electrode by reserving gaps on a current collector, characterized in that: In the step S3, the mass ratio of MXene powder, graphene oxide, deionized water and carbon nanotubes is 1:5:(15-25):
3.
7. The method of claim 1 for increasing the energy density of a silicon-based negative electrode by reserving gaps on a current collector, characterized in that: In the step S4, the specific preparation process of the coating slurry includes the following steps: stirring polyacrylic acid and pure water at a speed of 1000-1200r / min for 9-11min to obtain a glue solution; adding 1 / 2 mass fraction of MXene-rGO-CNT composite material, 1 / 2 mass fraction of conductive carbon black and graphite, stirring at a speed of 3000-3200r / min for 19-21min, adding the remaining mass fraction of MXene-rGO-CNT composite material and conductive carbon black, stirring at a speed of 3000-3200r / min for 29-31min, adding sodium hydroxide solution, stirring at a speed of 3000-3200r / min for 89-91min, adding isopropanol and pure water, stirring at a speed of 400-600r / min for 29-31min, and obtaining a coating slurry.
8. The method of claim 1 for increasing the energy density of a silicon-based negative electrode by reserving gaps on a current collector, characterized in that: In the step S4, the solid content of the coating slurry is 10%; the mass ratio of polyacrylic acid to pure water is 1:(3-4); the total mass of the MXene-rGO-CNT composite material, conductive carbon black and graphite is 1.5 times the mass of the glue; the mass ratio of the MXene-rGO-CNT composite material to the conductive carbon black is 9:1; the mass of the graphite is 17-18% of the total mass of the MXene-rGO-CNT composite material and the conductive carbon black.
9. The method of claim 1 for increasing the energy density of a silicon-based negative electrode by reserving gaps on a current collector, characterized in that: In step S6, the preparation method of the active slurry is as follows: The dried active material, binder and conductive agent are ground and mixed evenly, deionized water is added, and grinding is continued for 3-5 minutes to obtain active slurry.
10. The method of claim 1 for increasing the energy density of a silicon-based negative electrode by reserving gaps on a current collector, characterized in that: In the step S6, the active material is active silicon, the binder is sodium alginate, the conductive agent is acetylene black, and the mass ratio of the active material, the binder and the conductive agent is 6:2:2.