Application of polyazine compound in electrolyte, electrolyte, preparation method and application of electrolyte, lithium ion battery and electric equipment
By using polyazine compounds in the electrolyte, the problem of poor cycling stability of ternary positive electrode materials under high pressure is solved. By forming Li3N and complexing tetravalent nickel ions, the battery impedance and oxidation and decomposition are reduced, and the battery performance is improved.
Patent Information
- Application Number
- CN202310643696.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-31
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-05-31
AI Technical Summary
The existing ternary positive electrode materials have poor cycle stability under high pressure, and the electrolyte is easily oxidized and decomposed, resulting in high impedance of the battery, reduced energy density, and it is difficult to find stable high-pressure additives.
Polyazine compounds are used as key components in the electrolyte, which have low nitrogen and nitrogen single bond energy, which can easily form electrochemical reactions on the surface of the electrode sheet, generate Li3N to reduce the battery impedance, and capture tetravalent nickel ions through nitrogen atom complexation. , prevent oxidation and decomposition.
It effectively reduces the battery impedance, improves the cycle stability and battery performance of the ternary positive electrode under high pressure, and polyazine compounds are universal in different electrolyte systems.
Smart Images

Figure CN119069790A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of lithium batteries, and in particular to an electrolyte and a preparation method and application thereof. Background Art
[0002] Ternary cathode materials have always received extensive attention in the industry due to their higher theoretical specific capacity. Among them, ternary cathode materials are more popular due to their higher charge cut-off voltage (up to 4.5V), which can greatly improve the energy density of the battery. However, the existing electrolyte system is based on carbonate solvents and lithium hexafluorophosphate, which are prone to oxidative decomposition at a high voltage of 4.5V, generating by-products, increasing the cathode impedance, and accelerating the consumption of the electrolyte. At the same time, the acidic impurities in the electrolyte will cause the metal in the cathode material to dissolve and cause structural collapse, which will reduce the energy density of the battery and deteriorate the cycle performance.
[0003] To address this problem, there are currently three main solutions: First, use organic solvents with higher oxidation potentials to replace or partially replace carbonate solvents, such as sulfones, nitriles, etc.; second, use lithium salts with better stability and no by-products (such as hydrofluoric acid, etc.) to replace or partially replace lithium hexafluorophosphate, such as lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), etc.; third, use positive electrode film-forming additives, such as CN104282939A discloses a fluorinated additive, and US20120009485A1P discloses a phosphate additive.
[0004] The non-carbonate solvents in the above scheme 1 have a low dielectric constant, which is not conducive to lithium ion transmission and is easily reduced at the negative electrode. The lithium salts in scheme 2 are prone to corroding the aluminum current collector under high voltage. The difficulty of scheme 3 lies in finding a suitable high-voltage additive that can form a stable solid interface film on the positive electrode surface. For example, fluorinated additives are expensive, and due to the presence of fluorine atoms, they are prone to produce acid in the electrolyte, inducing metal dissolution at the positive electrode; in addition, fluorinated additives are often not stable enough at high temperatures.
[0005] Therefore, it is necessary to develop an electrolyte that can reduce battery impedance and improve the cycling stability of the ternary positive electrode under high voltage. Summary of the invention
[0006] The purpose of the present invention is to overcome the problems of high battery impedance and poor cycle stability of ternary positive electrodes under high voltage in the prior art, and to provide an electrolyte and a preparation method and application thereof.
[0007] In order to achieve the above object, the first aspect of the present invention provides an application of a polyazine compound in an electrolyte, wherein the polyazine compound has a structure shown in formula (1):
[0008]
[0009] Wherein, V1 and V2 are each independently selected from C or N;
[0010] wherein R1, R2, R4 and R5 are each independently selected from H, substituted or unsubstituted C1 to C 10 Alkyl, substituted or unsubstituted C2 to C 10 Alkenyl, substituted or unsubstituted C2 to C 10 substituted or unsubstituted phenyl, substituted or unsubstituted C2 to C 10 A keto group or an ester group, or R4 and R5 are combined with the nitrogen atom to which they are attached to form a six-membered nitrogen heterocyclic ring containing two nitrogen atoms;
[0011] Wherein, R3 and R6 are each independently selected from H, or R3 and R6 are each independently formed with the C atom to which they are connected to form a carbonyl group.
[0012] A second aspect of the present invention provides an electrolyte, wherein the electrolyte comprises a solvent A, a solvent B, a lithium salt, a polyazine compound and an optional non-azine additive;
[0013] Wherein, the polyazine compound has a structure shown in formula (1):
[0014]
[0015] Wherein, V1 and V2 are each independently selected from C or N;
[0016] wherein R1, R2, R4 and R5 are each independently selected from H, substituted or unsubstituted C1 to C 10 Alkyl, substituted or unsubstituted C2 to C 10 Alkenyl, substituted or unsubstituted C2 to C 10 substituted or unsubstituted phenyl, substituted or unsubstituted C2 to C 10 A keto group or an ester group, or R4 and R5 are combined with the nitrogen atom to which they are attached to form a six-membered nitrogen heterocyclic ring containing two nitrogen atoms;
[0017] Wherein, R3 and R6 are each independently selected from H, or R3 and R6 are each independently formed with the C atom to which they are connected to form a carbonyl group.
[0018] A third aspect of the present invention provides a method for preparing an electrolyte, the method comprising:
[0019] Lithium salt, polyazine compound and optional non-azine additive are added into a solvent to obtain an electrolyte.
[0020] The fourth aspect of the present invention provides an electrolyte prepared by the preparation method described in the third aspect of the present invention.
[0021] The fifth aspect of the present invention provides a use of the electrolyte described in the second aspect and the fourth aspect of the present invention in a lithium ion battery.
[0022] A sixth aspect of the present invention provides a lithium battery, comprising the electrolyte described in the second and fourth aspects of the present invention.
[0023] The seventh aspect of the present invention provides an electrical device, comprising the lithium-ion battery described in the sixth aspect of the present invention; wherein the electrical device includes transportation vehicles and digital products, preferably selected from pure electric vehicles, hybrid vehicles, electric bicycles, and laptop computers.
[0024] Through the above technical solution, the present invention can produce the following beneficial effects:
[0025] 1. The polyazine compounds of the present invention have multiple nitrogen atoms in the six-membered ring, and the nitrogen-nitrogen single bond formed by them has a relatively low bond energy of about 200 kJ / mol, which is much lower than the carbon-carbon single bond (about 346 kJ / mol) and the carbon-oxygen single bond (356 kJ / mol). Therefore, it is easier to undergo electrochemical reactions and break bonds on the surface of the battery's pole piece. In other words, the molecular structure of the present invention will preferentially undergo electrochemical reactions at the positive and negative electrodes compared to carbonate molecules, especially ethylene carbonate (EC), and the reaction products will form a solid electrolyte interface film.
[0026] 2. The polyazine compounds of the present invention are rich in nitrogen atoms, so they can generate a large amount of Li3N after electrochemical reaction on the surface of the electrode. Li3N has extremely high ionic conductivity (1.3×10 -5 S / cm), while the ionic conductivity of Li2CO3 generated by the reduction of EC is only 1×10 -8 S / cm, which is much lower than Li3N. Therefore, the interface film formed by the polyazine compound is more conducive to conducting lithium ions and reducing the impedance of the battery.
[0027] 3. When the ternary material is charged to 4.5V, a large amount of tetravalent nickel ions will be formed. The high-valent metal ions are highly oxidizing and will oxidize carbonate solvents, consume active lithium and electrolyte, and ultimately cause the battery capacity to decay rapidly. The polyazine compound has multiple nitrogen atoms, and the lone electron pairs on the nitrogen atoms provide complexing sites, while the six-membered ring provides space for complexing metal ions. Therefore, the tetravalent nickel ions dissolved by the positive electrode due to high voltage and acidity of the electrolyte can be efficiently captured in the electrolyte to generate a structurally stable organic metal chelate, thereby preventing its oxidation of the electrolyte, reducing the generation of by-products in the battery system, and improving the cycle stability of the ternary positive electrode under high voltage.
[0028] 4. Due to the substitution of alkyl groups on the N atom, the polyazine compounds have good compatibility with the electrolyte body (organic carbonate molecules), can be used in different electrolyte systems, and have universal applicability.
[0029] The combined effects listed above enable the polyazine compounds of the present invention to effectively improve the battery performance after being added to the electrolyte of a ternary material high-voltage battery.
[0030] The polyazine compounds of the present invention are directed to ternary materials, which can be LiNi 0.5 Co 0.2 Mn 0.3 O2(NCM523 type), LiNi 0.6 Co 0.2 Mn 0.2 O2(NCM622 type), LiNi 0.8 Co 0.1 Mn 0.1 O2(NCM811 type), LiNi 0.85 Co 0.075 Mn 0.075 O2; the negative electrode can be artificial graphite, natural graphite, mesophase carbon microbeads (MCMB), silicon-carbon negative electrode, etc.
[0031] The content of Li3N in the polyazine compound of the present invention when forming a film at the negative electrode is much higher than that in the film at the positive electrode, which is more conducive to the conduction and embedding of lithium ions at the negative electrode side. DETAILED DESCRIPTION
[0032] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0033] In the present invention, the terms involved are uniformly interpreted as follows:
[0034] Polyazines are six-membered heterocyclic compounds containing 2-4 nitrogen atoms.
[0035] As mentioned above, the first aspect of the present invention provides an application of a polyazine compound in an electrolyte, wherein the polyazine compound has a structure shown in formula (1):
[0036]
[0037] Wherein, V1 and V2 are each independently selected from C or N;
[0038] wherein R1, R2, R4 and R5 are each independently selected from H, substituted or unsubstituted C1 to C 10 Alkyl, substituted or unsubstituted C2 to C 10 Alkenyl, substituted or unsubstituted C2 to C 10 substituted or unsubstituted phenyl, substituted or unsubstituted C2 to C 10 A keto group or an ester group, or R4 and R5 are combined with the nitrogen atom to which they are attached to form a six-membered nitrogen heterocyclic ring containing two nitrogen atoms;
[0039] Wherein, R3 and R6 are each independently selected from H, or R3 and R6 are each independently formed with the C atom to which they are connected to form a carbonyl group.
[0040] Preferably, V1 is C, V2 is N; or V1 and V2 are both N.
[0041] R1, R2, R4 and R5 are each independently selected from H, substituted or unsubstituted C1 to C8 alkyl, substituted or unsubstituted C2 to C8 alkenyl, substituted or unsubstituted C2 to C8 alkynyl, substituted or unsubstituted phenyl, substituted or unsubstituted C2 to C8 keto or ester, or R4 and R5 are combined with the N atoms to which they are connected to form a six-membered nitrogen heterocycle containing two N atoms.
[0042] More preferably, the polyazine compound is selected from 1,2,4,5-tetramethyl-1,2,4,5-tetrazine, 1,4-diacetyl-2,5-dimethyl-1,2,4,5-tetrazine, 1,4-diacetyl-2,5-diethyl-1,2,4,5-tetrazine, 1,4-dimethyl-2,5-bis(phenylmethyl)-1,2,4,5-tetrazine, 1,2,3,4,5,6 -hexamethyl-1,2,4,5-tetrazine, 2,3-dimethyloctahydropyridazine[1,2-a]-1,2,4,5-tetrazine, 1,5-dimethyl-2,4-bis(phenylmethyl)-1,2,4,5-tetrazine-3,6-dione, 1,2,4,5-tetrazine-3,6-dione, hexahydro-1,2-dimethylpyridazine or hexahydro-1,2,4-trimethyl-1,2,4-triazine.
[0043] According to a particularly preferred embodiment of the present invention, the polyazine compound is selected from 1,2,4,5-tetramethyl-1,2,4,5-tetrazine, 1,4-diacetyl-2,5-dimethyl-1,2,4,5-tetrazine, 1,4-diacetyl-2,5-diethyl-1,2,4,5-tetrazine, 1,4-diacetyl-2,5-diethyl-1,2,4,5-tetrazine or 1,2,3,4,5,6-hexamethyl-1,2,4,5-tetrazine.
[0044] Wherein, in the polyazine compound, the bond energy of the nitrogen-nitrogen single bond is lower than 356 kJ / mol, preferably lower than 346 kJ / mol, and more preferably 200 kJ / mol.
[0045] A second aspect of the present invention provides an electrolyte, wherein the electrolyte comprises a solvent A, a solvent B, a lithium salt, a polyazine compound and an optional non-azine additive;
[0046] Wherein, the polyazine compound has a structure shown in formula (1):
[0047]
[0048] Wherein, V1 and V2 are each independently selected from C or N;
[0049] wherein R1, R2, R4 and R5 are each independently selected from H, substituted or unsubstituted C1 to C 10 Alkyl, substituted or unsubstituted C2 to C 10 Alkenyl, substituted or unsubstituted C2 to C 10 substituted or unsubstituted phenyl, substituted or unsubstituted C2 to C 10 A keto group or an ester group, or R4 and R5 are combined with the nitrogen atom to which they are attached to form a six-membered nitrogen heterocyclic ring containing two nitrogen atoms;
[0050] Wherein, R3 and R6 are each independently selected from H, or R3 and R6 are each independently formed with the C atom to which they are connected to form a carbonyl group.
[0051] Preferably, V1 is C, V2 is N; or V1 and V2 are both N;
[0052] R1, R2, R4 and R5 are each independently selected from H, substituted or unsubstituted C1 to C8 alkyl, substituted or unsubstituted C2 to C8 alkenyl, substituted or unsubstituted C2 to C8 alkynyl, substituted or unsubstituted phenyl, substituted or unsubstituted C2 to C8 keto or ester, or R4 and R5 are combined with the N atoms to which they are connected to form a six-membered nitrogen heterocycle containing two N atoms.
[0053] More preferably, the polyazine compound is selected from 1,2,4,5-tetramethyl-1,2,4,5-tetrazine, 1,4-diacetyl-2,5-dimethyl-1,2,4,5-tetrazine, 1,4-diacetyl-2,5-diethyl-1,2,4,5-tetrazine, 1,4-dimethyl-2,5-bis(phenylmethyl)-1,2,4,5-tetrazine, 1,2,3,4,5,6 - hexamethyl-1,2,4,5-tetrazine, 2,3-dimethyloctahydropyridazine[1,2-a]-1,2,4,5-tetrazine, 1,5-dimethyl-2,4-bis(phenylmethyl)-1,2,4,5-tetrazine-3,6-dione, 1,2,4,5-tetrazine-3,6-dione, hexahydro-1,2-dimethylpyridazine or hexahydro-1,2,4-trimethyl-1,2,4-triazine;
[0054] According to a particularly preferred embodiment of the present invention, the polyazine compound is selected from 1,2,4,5-tetramethyl-1,2,4,5-tetrazine, 1,4-diacetyl-2,5-dimethyl-1,2,4,5-tetrazine, 1,4-diacetyl-2,5-diethyl-1,2,4,5-tetrazine, 1,4-diacetyl-2,5-diethyl-1,2,4,5-tetrazine or 1,2,3,4,5,6-hexamethyl-1,2,4,5-tetrazine.
[0055] Wherein, the lithium salt is selected from lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium tetrafluoroborate or lithium perchlorate; preferably lithium hexafluorophosphate.
[0056] Preferably, the solvent A is selected from cyclic carbonates, preferably selected from ethylene carbonate, propylene carbonate, 1,2-butene carbonate; more preferably ethylene carbonate.
[0057] Preferably, the solvent B is selected from linear carbonates, preferably dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, methyl propyl carbonate; more preferably ethyl methyl carbonate.
[0058] Preferably, the non-oxazine additive is selected from propylene sulfite, 1,3-propylene sultone (PST), diethylene sulfate (DTD), and ethylene methane disulfonate (MMDS); more preferably, propylene sulfite.
[0059] Among them, based on the total amount of the electrolyte, the mass concentration of the solvent A is 25-35%; the mass concentration of the solvent B is 50-65%; the mass concentration of the polyazine compound is 0.1-10%, preferably 0.5-3%; the mass concentration of the lithium salt is 6-15%, and the mass concentration of the non-azine additive is 0-5%.
[0060] The mass ratio of the solvent A to the solvent B is 1:(1-3); preferably 1:(2-2.5). The appropriate mass ratio can ensure that the solvent system formed by the solvent A and the solvent B has both a low viscosity and a high dielectric constant, and the prepared electrolyte has good conductivity.
[0061] A third aspect of the present invention provides a method for preparing an electrolyte, the method comprising:
[0062] Lithium salt, polyazine compound and optional non-azine additive are added into a solvent to obtain an electrolyte.
[0063] In some embodiments of the present invention, preferably, the lithium salt is selected from lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium tetrafluoroborate or lithium perchlorate; more preferably lithium hexafluorophosphate;
[0064] In some embodiments of the present invention, preferably, the polyazine compound has a structure shown in formula (1):
[0065]
[0066] Wherein, V1 and V2 are each independently selected from C or N;
[0067] wherein R1, R2, R4 and R5 are each independently selected from H, substituted or unsubstituted C1 to C 10 Alkyl, substituted or unsubstituted C2 to C 10 Alkenyl, substituted or unsubstituted C2 to C 10 substituted or unsubstituted phenyl, substituted or unsubstituted C2 to C 10 A keto group or an ester group, or R4 and R5 are combined with the nitrogen atom to which they are attached to form a six-membered nitrogen heterocyclic ring containing two nitrogen atoms;
[0068] wherein R3 and R6 are each independently selected from H, or R3 and R6 each independently form a carbonyl group with the C atom to which they are connected;
[0069] In some embodiments of the present invention, preferably, the non-oxazine additive is selected from propylene sulfite, 1,3-propylene sultone (PST), diethylene sulfate (DTD), and ethylene methane disulfonate (MMDS); more preferably, propylene sulfite.
[0070] In some embodiments of the present invention, preferably, the solvent is a mixed solvent made of solvent A and solvent B; preferably, the mass ratio of solvent A to solvent B is 1:(1-3); more preferably 1:(2-2.5).
[0071] In some embodiments of the present invention, preferably, in parts by weight, the solvent A is 25-35 parts; the solvent B is 50-65 parts; the lithium salt is 6-15 parts; the polyazine compound is 0.1-10 parts, preferably 0.5-3 parts; and the non-azine additive is 0-5 parts.
[0072] The fourth aspect of the present invention provides an electrolyte prepared by the preparation method described in the third aspect of the present invention.
[0073] The fifth aspect of the present invention provides a use of the electrolyte described in the second aspect and the fourth aspect of the present invention in a lithium ion battery.
[0074] A sixth aspect of the present invention provides a lithium battery, comprising the electrolyte described in the second and fourth aspects of the present invention.
[0075] Wherein, the lithium battery includes a positive electrode sheet and a negative electrode sheet.
[0076] The active material contained in the positive electrode sheet is a ternary material; a solid electrolyte (SEI) film can be generated on the surface of the negative electrode sheet; and the components of the solid electrolyte (SEI) film include Li3N.
[0077] The seventh aspect of the present invention provides an electrical device, comprising the lithium-ion battery described in the sixth aspect of the present invention; wherein the electrical device includes transportation vehicles and digital products, preferably selected from pure electric vehicles, hybrid vehicles, electric bicycles, and laptop computers.
[0078] The present invention will be described in detail below through examples. In the following examples, the raw materials of ethylene carbonate and ethyl methyl carbonate are commercially available products of Xinzhoubang Company; the raw material of lithium hexafluorophosphate is commercially available products of Duofuduo Company; and the raw material of polyazine compound is commercially available products of HONEST JOY HOLDINGS LIMITED Company.
[0079] Example 1
[0080] (1) Preparation of electrolyte
[0081] 30g of ethylene carbonate (EC) and 70g of ethyl methyl carbonate (EMC) were mixed into a mixed solvent, and 14.4g of lithium hexafluorophosphate was added to the mixed solvent. Then 2.32g (mass percentage 2%) of 1,2,4,5-tetramethyl-1,2,4,5-tetrazine (as shown in Formula 2) was added thereto. The electrolyte was recorded as I1.
[0082]
[0083] (2) Preparation of batteries
[0084] The carbon-coated silicon material, the conductive agent super-p, the thickener sodium carboxymethyl cellulose (CMC), and the binder styrene-butadiene rubber (SBR) were mixed uniformly in a mass ratio of 100:2:2:3, and the obtained paste was evenly coated on the copper foil as the negative electrode current collector, and dried in a vacuum oven at 60°C for 24 hours to obtain a negative electrode sheet.
[0085] LiNi cathode 0.5 Co 0.2 Mn 0.3 O2, i.e. NCM523 type, NCM523, carbon nanotubes (CNT) and polyvinylidene fluoride (PVDF) are uniformly mixed in a mass ratio of 100:2:2, the obtained paste is uniformly coated on an aluminum foil as a positive electrode current collector, and dried in a vacuum oven at 60°C for 24 hours to obtain a positive electrode sheet.
[0086] Preparation of soft-pack battery: The battery cell was wound to obtain a silicon negative electrode soft-pack lithium battery of model SL523450. In an argon glove box with water and oxygen content less than 5ppm, 3g of electrolyte I1 was injected into the soft-pack battery with airbag to prepare the battery P1 for cycle test.
[0087] Formation process: The simulated battery is first charged to 1.5V at 45mA (0.05C) and maintained at 1.5V for 10h to allow the electrolyte to fully infiltrate the battery electrode. After sufficient aging, the battery is first charged at a smaller current of 9mA (C / 100) for 15h to form a stable and complete SEI film, then charged to 4.5V at 45mA (0.05C) and then discharged to 3V.
[0088] Example 2
[0089] The electrolyte was prepared in the same manner as in Example 1, except that the additive was 2.32 g (2% by mass) 1,4-diacetyl-2,5-dimethyl-1,2,4,5-tetrazine (as shown in Formula 3), to obtain electrolyte I2. The battery preparation and formation process were the same as in Example 1, to prepare soft pack battery P2.
[0090]
[0091] Example 3
[0092] The electrolyte was prepared in the same manner as in Example 1, except that the additive was 2.32 g (2% by mass) 1,4-diacetyl-2,5-diethyl-1,2,4,5-tetrazine (as shown in Formula 4), to obtain electrolyte I3. The battery preparation and formation process were the same as in Example 1, to prepare soft pack battery P3.
[0093]
[0094] Example 4
[0095] The electrolyte was prepared in the same manner as in Example 1, except that the additive was 2.32 g (2% by mass) 1,2,3,4,5,6-hexamethyl-1,2,4,5-tetrazine (as shown in Formula 5), to obtain electrolyte I4. The battery preparation and formation process were the same as in Example 1, to prepare soft pack battery P4.
[0096]
[0097] Example 5
[0098] The electrolyte was prepared in the same manner as in Example 1, except that the additives were 2.32 g (2% by mass) 1,2,3,4,5,6-hexamethyl-1,2,4,5-tetrazine (as shown in Formula 5) and 1.16 g (1% by mass) 1,3-propane sultone (PS), to obtain electrolyte I5. The battery preparation and formation process were the same as in Example 1, to prepare soft pack battery P5.
[0099] Example 6
[0100] The electrolyte was prepared in the same manner as in Example 1, except that the additive was 2.32 g (2% by mass) of 1,2,4,5-tetrazine-3,6-dione (as shown in Formula 6, the nitrogen atom in the six-membered ring is connected to an active hydrogen), to obtain electrolyte I6. The battery preparation and formation process were the same as in Example 1, to obtain battery P6.
[0101]
[0102] Example 7
[0103] The electrolyte was prepared in the same manner as in Example 1, except that the additive was 2.32 g (mass percentage 2%) of 1,4-dimethyl-2,5-bis(phenylmethyl)-1,2,4,5-tetrazine (structure shown in Formula 7, with a bulky group attached to the nitrogen atom in the six-membered ring), to obtain electrolyte I7. The battery preparation and formation process were the same as in Example 1, to obtain battery P7.
[0104]
[0105] Example 8
[0106] The electrolyte was prepared in the same manner as in Example 1, except that the additive was 2.32 g (2% by mass) of hexahydro-1,2-dimethylpyridazine (as shown in Formula 8, the six-membered ring contains two nitrogen atoms), to obtain electrolyte I8. The battery preparation and formation process were the same as in Example 1, to obtain battery P8.
[0107]
[0108] Example 9
[0109] The electrolyte was prepared in the same manner as in Example 1, except that the additive was 2.32 g (2% by mass) of hexahydro-1,2,4-trimethyl-1,2,4-triazine (as shown in Formula 9, the six-membered ring contains three nitrogen atoms), to obtain electrolyte I9. The battery preparation and formation process were the same as in Example 1, to obtain battery P9.
[0110]
[0111] Comparative Example 1
[0112] The electrolyte was prepared in the same manner as in Example 1, except that no additive was added, to obtain electrolyte R1. The battery preparation and formation process were the same as in Example 1, to obtain battery RP1.
[0113] Comparative Example 2
[0114] The electrolyte was prepared in the same manner as in Example 5, except that only 1.16 g (1% by mass) of 1,3-propane sultone (PS) was added to obtain electrolyte R2. The battery preparation and formation process were the same as in Example 1, and battery RP2 was prepared.
[0115] Fully charged high temperature storage test
[0116] The electrolyte compositions in Examples 1-9 and Comparative Examples 1-3 are shown in Table 1
[0117] Table 1
[0118]
[0119]
[0120] After each experimental formation, the batteries P1-P9 and RP1-RP2 were charged at 0.5C (450mA) with a cut-off voltage of 4.5V, and then charged at a constant voltage of 4.5V with a cut-off current of 45mA. The fully charged batteries were placed in a constant temperature oven at 60°C for 5 days, with 10 batteries under each condition, and the results were averaged. The thickness of the batteries before and after storage was measured with a vernier caliper. The battery expansion rate (%) was calculated by subtracting the thickness before storage from the thickness after storage, and dividing the thickness difference by the thickness before storage to obtain the percentage. The experimental results are shown in Table 2
[0121] Table 2
[0122] Electrolyte No. Volume expansion rate (%) I1 23 I2 35 I3 32 I4 21 I5 17 I6 52 I7 44 I8 58 I9 54 R1 79 R2 66
[0123] (2) Nickel dissolution test
[0124] After disassembling the above batteries, the positive and negative electrode separators and the aluminum-plastic film were repeatedly rinsed with 5 mL of propylene glycol, and then the washing liquid was sent to the inductively coupled plasma spectrometer (ICP) for testing. The test instrument was the Thermo Fisher Inductively Coupled Plasma Spectrometer, and the test conditions were familiar to general testers. Ten batteries were tested under each condition, and the results were averaged. The experimental test results are shown in Table 3.
[0125] Table 3
[0126]
[0127]
[0128] (3) Battery high voltage cycle test
[0129] After each experimental formation, the airbags of the batteries P1-P9 and RP1-RP2 were removed and vacuum sealed, and the batteries were cycled 200 times at 1C (900mA) current between 3V and 4.5V (10 batteries under each condition, and the results were averaged). The tests were carried out in a 45°C constant temperature box. The capacity retention rate (%) was calculated by dividing the discharge capacity at the 200th cycle by the initial discharge capacity at the first cycle to obtain a percentage. The experimental test results are shown in Table 4.
[0130] Table 4
[0131] Electrolyte No. Capacity retention rate (%) I1 68 I2 60 I3 61 I4 71 I5 78 I6 62 I7 51 I8 44 I9 50 R1 30 R2 35
[0132] As can be seen from Table 2, the film-forming additive of the present invention significantly reduces the expansion rate of the high-nickel ternary battery during high-temperature storage at full charge, indicating that it successfully forms a solid electrolyte interface film on the surface of the pole piece before EC, thereby protecting the electrolyte, reducing the continuous occurrence of side reactions, and reducing the generation of gas, so it can reduce the expansion rate during battery storage and improve the high-temperature safety of the battery. The cycle performance test results in Table 4 also prove this point. In addition, the results of Example 5 (electrolyte I5) show that the additive of the present invention has a better effect when used in combination with PS. The results of Comparative Example 1 (electrolyte R1) show that without the additive, the battery cycle performance of the high-voltage positive electrode material is extremely poor. This is mainly because the dissolution of the positive electrode metal ions under high pressure cannot be suppressed, which is not conducive to the battery life.
[0133] As can be seen from Table 3, the additives of the present invention can reduce the dissolution of metal nickel during high-temperature storage of the battery due to their good metal ion complexing effect. Among them, due to the presence of acyl groups on nitrogen atoms, the electron-withdrawing effect of Examples 2 and 3 (electrolytes I2 and I3) reduces the electron cloud density of the six-membered ring in the polyazine compound, making its complexing effect on metal ions slightly inferior, and more metal nickel is dissolved in the battery. The result of Example 6 (electrolyte I6) is mainly better than that of Example 6 (electrolyte I6) because the presence of active hydrogen on nitrogen atoms will increase the acidity of the electrolyte; while Example 7 (electrolyte I7) is due to the excessive volume of the substituents on the nitrogen atoms and the excessive steric hindrance, making the complexing effect of the two on metal ions not as good as that of other embodiments. In addition, since the six-membered rings of Examples 8 and 9 contain only two and three nitrogen atoms respectively, there are fewer lone electron pairs, making their complexing effect on metal ions not as good as that of tetrazine molecules, so more metal nickel is dissolved.
[0134] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. Application of a polyazine compound in an electrolyte, wherein: The polyazine compound has a structure shown in formula (1): Wherein, V1 and V2 are each independently selected from C or N; wherein R1, R2, R4 and R5 are each independently selected from H, substituted or unsubstituted C1 to C 10 Alkyl, substituted or unsubstituted C2 to C 10 Alkenyl, substituted or unsubstituted C2 to C 10 substituted or unsubstituted phenyl, substituted or unsubstituted C2 to C 10 A keto group or an ester group, or R4 and R5 are combined with the nitrogen atom to which they are attached to form a six-membered nitrogen heterocyclic ring containing two nitrogen atoms; Wherein, R3 and R6 are each independently selected from H, or R3 and R6 are each independently formed with the C atom to which they are connected to form a carbonyl group.
2. The use according to claim 1, wherein: V1 is C, V2 is N; or both V1 and V2 are N; Wherein, R1, R2, R4 and R5 are each independently selected from H, substituted or unsubstituted C1 to C8 alkyl, substituted or unsubstituted C2 to C8 alkenyl, substituted or unsubstituted C2 to C8 alkynyl, substituted or unsubstituted phenyl, substituted or unsubstituted C2 to C8 keto or ester, or R4 and R5 are combined with the N atoms to which they are connected to form a six-membered nitrogen heterocycle containing two N atoms.
3. The use according to claim 1 or 2, wherein: The polyazine compound is selected from 1,2,4,5-tetramethyl-1,2,4,5-tetrazine, 1,4-diacetyl-2,5-dimethyl-1,2,4,5-tetrazine, 1,4-diacetyl-2,5-diethyl-1,2,4,5-tetrazine, 1,4-dimethyl-2,5-bis(phenylmethyl)-1,2,4,5-tetrazine, 1,2,3,4,5,6-hexamethyl 1,2,4,5-tetrazine, 2,3-dimethyloctahydropyridazine [1,2-a]-1,2,4,5-tetrazine, 1,5-dimethyl-2,4-bis (phenylmethyl)-1,2,4,5-tetrazine-3,6-dione, 1,2,4,5-tetrazine-3,6-dione, hexahydro-1,2-dimethylpyridazine or hexahydro-1,2,4-trimethyl-1,2,4-triazine; Preferably, it is selected from 1,2,4,5-tetramethyl-1,2,4,5-tetrazine, 1,4-diacetyl-2,5-dimethyl-1,2,4,5-tetrazine, 1,4-diacetyl-2,5-diethyl-1,2,4,5-tetrazine, 1,4-diacetyl-2,5-diethyl-1,2,4,5-tetrazine or 1,2,3,4,5,6-hexamethyl-1,2,4,5-tetrazine.
4. The use according to any one of claims 1 to 3, wherein: In the polyazine compound, the bond energy of the nitrogen-nitrogen single bond is lower than 356 kJ / mol, preferably lower than 346 kJ / mol, and more preferably 200 kJ / mol.
5. An electrolyte, wherein The electrolyte comprises solvent A, solvent B, lithium salt, polyazine compound and optional non-azine additive; Wherein, the polyazine compound has a structure shown in formula (1): Wherein, V1 and V2 are each independently selected from C or N; wherein R1, R2, R4 and R5 are each independently selected from H, substituted or unsubstituted C1 to C 10 Alkyl, substituted or unsubstituted C2 to C 10 Alkenyl, substituted or unsubstituted C2 to C 10 substituted or unsubstituted phenyl, substituted or unsubstituted C2 to C 10 A keto group or an ester group, or R4 and R5 are combined with the nitrogen atom to which they are attached to form a six-membered nitrogen heterocyclic ring containing two nitrogen atoms; Wherein, R3 and R6 are each independently selected from H, or R3 and R6 are each independently formed with the C atom to which they are connected to form a carbonyl group.
6. The electrolyte according to claim 5, wherein V1 is C, V2 is N; or both V1 and V2 are N; Wherein, R1, R2, R4 and R5 are each independently selected from H, substituted or unsubstituted C1 to C8 alkyl, substituted or unsubstituted C2 to C8 alkenyl, substituted or unsubstituted C2 to C8 alkynyl, substituted or unsubstituted phenyl, substituted or unsubstituted C2 to C8 keto or ester, or R4 and R5 are combined with the N atoms to which they are connected to form a six-membered nitrogen heterocycle containing two N atoms.
7. The electrolyte according to claim 5 or 6, wherein The polyazine compound is selected from 1,2,4,5-tetramethyl-1,2,4,5-tetrazine, 1,4-diacetyl-2,5-dimethyl-1,2,4,5-tetrazine, 1,4-diacetyl-2,5-diethyl-1,2,4,5-tetrazine, 1,4-dimethyl-2,5-bis(phenylmethyl)-1,2,4,5-tetrazine, 1,2,3,4,5,6-hexamethyl 1,2,4,5-tetrazine, 2,3-dimethyloctahydropyridazine [1,2-a]-1,2,4,5-tetrazine, 1,5-dimethyl-2,4-bis (phenylmethyl)-1,2,4,5-tetrazine-3,6-dione, 1,2,4,5-tetrazine-3,6-dione, hexahydro-1,2-dimethylpyridazine or hexahydro-1,2,4-trimethyl-1,2,4-triazine; Preferably, it is selected from 1,2,4,5-tetramethyl-1,2,4,5-tetrazine, 1,4-diacetyl-2,5-dimethyl-1,2,4,5-tetrazine, 1,4-diacetyl-2,5-diethyl-1,2,4,5-tetrazine, 1,4-diacetyl-2,5-diethyl-1,2,4,5-tetrazine or 1,2,3,4,5,6-hexamethyl-1,2,4,5-tetrazine.
8. The electrolyte according to any one of claims 5 to 7, wherein: The lithium salt is selected from lithium hexafluorophosphate, lithium bis(fluorosulfonyl imide), lithium bis(trifluoromethanesulfonyl imide), lithium tetrafluoroborate or lithium perchlorate; preferably lithium hexafluorophosphate; Preferably, the solvent A is selected from cyclic carbonates, preferably ethylene carbonate, propylene carbonate, 1,2-butene carbonate; more preferably ethylene carbonate; Preferably, the solvent B is selected from linear carbonates, preferably dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, methyl propyl carbonate; more preferably ethyl methyl carbonate; Preferably, the non-oxazine additive is selected from propylene sulfite, 1,3-propylene sultone, vinylene sulfate, and ethylene methane disulfonate; more preferably, propylene sulfite.
9. The electrolyte according to any one of claims 5 to 8, wherein: Based on the total amount of the electrolyte, the mass concentration of the solvent A is 25-35%; the mass concentration of the solvent B is 50-65%; the mass concentration of the polyazine compound is 0.1-10%, preferably 0.5-3%; the mass concentration of the lithium salt is 6-15%, and the mass concentration of the non-azine additive is 0-5%.
10. The electrolyte according to any one of claims 5 to 9, wherein: The mass ratio of the solvent A to the solvent B is 1:(1-3); preferably 1:(2-2.5).
11. A method for preparing an electrolyte, the method comprising: Lithium salt, polyazine compound and optional non-azine additive are added into a solvent to obtain an electrolyte.
12. The method according to claim 11, wherein: The lithium salt is selected from lithium hexafluorophosphate, lithium bis(fluorosulfonyl imide), lithium bis(trifluoromethanesulfonyl imide), lithium tetrafluoroborate or lithium perchlorate; preferably lithium hexafluorophosphate; Preferably, the polyazine compound has a structure shown in formula (1): Wherein, V1 and V2 are each independently selected from C or N; wherein R1, R2, R4 and R5 are each independently selected from H, substituted or unsubstituted C1 to C 10 Alkyl, substituted or unsubstituted C2 to C 10 Alkenyl, substituted or unsubstituted C2 to C 10 substituted or unsubstituted phenyl, substituted or unsubstituted C2 to C 10 A keto group or an ester group, or R4 and R5 are combined with the nitrogen atom to which they are attached to form a six-membered nitrogen heterocyclic ring containing two nitrogen atoms; wherein R3 and R6 are each independently selected from H, or R3 and R6 each independently form a carbonyl group with the C atom to which they are connected; Preferably, the non-oxazine additive is selected from propylene sulfite, 1,3-propylene sultone, vinylene sulfate, and ethylene methane disulfonate; more preferably, propylene sulfite.
13. The method according to claim 11 or 12, wherein: The solvent is a mixed solvent made of solvent A and solvent B; preferably, the mass ratio of solvent A to solvent B is 1:(1-3); more preferably 1:(2-2.5).
14. The method according to any one of claims 11 to 13, wherein: In parts by weight, the solvent A is 25-35 parts; the solvent B is 50-65 parts; the lithium salt is 6-15 parts; the polyazine compound is 0.1-10 parts, preferably 0.5-3 parts; and the non-azine additive is 0-5 parts.
15. An electrolyte prepared by the method according to any one of claims 11 to 14.
16. A lithium ion battery comprising the electrolyte according to any one of claims 4 to 10 and 15.
17. An electrical device comprising the lithium-ion battery of claim 16; wherein: The electrical equipment includes transportation tools and digital products, preferably selected from pure electric vehicles, hybrid electric vehicles, electric bicycles, and laptop computers.
Citation Information
Patent Citations
High voltage electrolyte for lithium ion batteries
CN104282939A
Nonaqueous secondary battery and flame retardant for use in the same
CN102856586A
Electrolyte and battery
CN110391460A
Electrolyte additive, electrolyte and lithium ion battery
CN113328142A
Electrolyte for lithium ion battery, preparation method of electrolyte and lithium ion battery
CN113764736A