Electrolyte, sodium ion battery and electric equipment

By adding imine and organic amines with C-N bonds or C=N double bonds to the sodium ion battery electrolyte, adsorbing and neutralizing moisture and HF, the problem of deterioration in the performance of sodium ion battery in high humidity environments is solved, and the battery is improved stability and cycle life.

CN119069801APending Publication Date: 2024-12-03GREE ALTAIRNANO NEW ENERGY INC
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410967611.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

In a high humidity environment, sodium ion batteries are prone to reacting with sodium salt to form HF, which leads to damage to the electrolyte, affecting the battery performance and cycle life. The stability of the existing electrolyte is insufficient, resulting in capacity attenuation and increased internal resistance.

Method used

Imine and organic amine containing C-N bonds or C=N double bonds are added as stabilizers. The imine absorbs moisture and HF by forming hydrogen bonds, neutralizes free acid HF, and reduces the water and acid content in the electrolyte. , improve the stability of the electrolyte.

Benefits of technology

It effectively reduces the side reactions of the electrolyte, reduces the internal resistance of the battery, extends the cycle life, and improves the battery capacity retention rate and gas production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004952197890000081
    Figure BDA0004952197890000081
  • Figure BDA0004952197890000091
    Figure BDA0004952197890000091
Patent Text Reader

Abstract

The invention relates to the field of sodium-ion batteries, and discloses an electrolyte, a sodium-ion battery and electric equipment. The electrolyte comprises an electrolyte sodium salt, an organic solvent, imine containing a C-N bond or a C = N double bond, and organic amine. According to the stabilizer-containing sodium-ion battery electrolyte provided by the invention, the adsorption type stabilizer imine is introduced and can form hydrogen bonds with H2O and HF molecules, and H2O and HF are adsorbed and stabilized through an intermolecular acting force, so that the purpose of protecting other components of the electrolyte is achieved; reaction type stabilizer organic amine is introduced and can be neutralized with free acid HF generated by side reaction according to the alkalinity of the reaction type stabilizer organic amine; the two stabilizing effects reduce the content of water and acid in the electrolyte, so that the side reaction of the electrolyte is reduced, the stability of the electrolyte is improved, the internal resistance is reduced, the capacity deterioration of the battery is reduced, and the cycle life of the battery is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of sodium ion batteries, and in particular to an electrolyte, a sodium ion battery and an electrical device. Background Art

[0002] With the introduction of the dual carbon concepts of "carbon neutrality" and "carbon peak", energy storage has received widespread attention as an important force to promote the realization of the "dual carbon" strategic goals. Among electrochemical energy storage methods, lithium-ion batteries have been widely industrialized, but due to the low abundance of lithium in the earth's crust and high dependence on imports, their future development space is limited, and a new battery is urgently needed to solve this problem.

[0003] Sodium-ion batteries are expected to complement and effectively replace lithium-ion batteries with their abundant sodium resources, low prices, and environmental friendliness. Sodium-ion batteries can be divided into different systems, such as layered oxide systems, Prussian blue compound systems, tunnel oxide systems, and polyanion systems, according to different positive electrode materials. The layered oxide system has become the best positive electrode material for sodium-ion batteries due to its high energy density and excellent rate performance, but layered oxides also have the disadvantage of being easy to absorb moisture. Especially in areas with high air humidity, the battery production environment is more difficult to control. Water has a huge destructive effect on the electrolyte. It reacts with sodium salts to generate HF, which will destroy the solid electrolyte interface film (SEI film), causing a series of problems such as capacity decay and battery deterioration. Therefore, in order to further improve the performance of sodium-ion batteries, adding stabilizers that stabilize water and acid to the electrolyte is one of the most effective ways to solve the damage of water to the performance of sodium-ion batteries. Summary of the invention

[0004] In view of this, the purpose of the present application is to provide an electrolyte, which can react with water and HF generated in the battery manufacturing process by adding a stabilizer, thereby reducing the side reactions of the electrolyte, improving the stability of the electrolyte, improving the battery bulging phenomenon, and reducing the internal resistance, reducing the capacity deterioration of the battery, and improving the cycle life of the battery;

[0005] Another object of the present application is to provide a sodium ion battery and electrical equipment prepared based on the above electrolyte.

[0006] In order to solve the above technical problems / achieve the above purposes or at least partially solve the above technical problems / achieve the above purposes, as the first aspect of the present application, an electrolyte is provided, comprising an electrolyte sodium salt, an organic solvent, an imine containing a CN bond or a C=N double bond, and an organic amine.

[0007] Optionally, the mass percentage content of the imine is 0.2-2.8%, and the mass percentage content of the organic amine is 0.1-3.2%.

[0008] Further optionally, the imine includes polyimide (PI) and / or polyethyleneimine (PEI), and the organic amine includes ethylenediamine (EDA) and / or ethanolamine (MEA).

[0009] As a second aspect of the present application, a sodium ion battery is provided, comprising a positive electrode sheet, a negative electrode sheet, a separator, and the electrolyte described in the present application.

[0010] Optionally, the active material of the positive electrode plate includes a layered oxide material. Further optionally, the chemical formula of the layered oxide material is Na x M 1-y-z Fe y Mn z O 2 ; wherein M is selected from one or more of Co, Ni, Cu, Mg, Zn, Al, Sn, Ga, Cr, Sr, V and Ti, 0 <x≤1,0≤y<1,0≤z<1,y+z≤1。

[0011] Optionally, the active material of the negative electrode plate includes one or more of hard carbon, titanium-based oxide negative electrode material, and alloy negative electrode material.

[0012] As a third aspect of the present application, an electrical device is provided, comprising the sodium ion battery described in the present application, wherein the sodium ion battery provides electrical energy for the electrical device.

[0013] The present application provides a sodium ion battery electrolyte containing a stabilizer, wherein an adsorption stabilizer imine is introduced to react with H 2 O and HF molecules form hydrogen bonds, and H is adsorbed and stabilized by intermolecular forces. 2 O and HF are added to protect other components of the electrolyte; the introduction of reactive stabilizer organic amine can neutralize the free acid HF produced by the side reaction according to its alkalinity; the two-way stabilization reduces the content of water and acid in the electrolyte, thereby reducing the side reaction of the electrolyte, improving the stability of the electrolyte, and at the same time reducing the internal resistance, reducing the capacity deterioration of the battery, and increasing the cycle life of the battery. DETAILED DESCRIPTION

[0014] The present application discloses an electrolyte, a sodium ion battery and an electrical device. Those skilled in the art can refer to the content of this article and appropriately improve the process parameters to achieve it. It is particularly important to point out that all similar substitutions and modifications are obvious to those skilled in the art, and they are all deemed to be included in this application. The products, processes and applications described in this application have been described through preferred embodiments. Relevant personnel can obviously modify or appropriately change and combine the preparation methods described herein without departing from the content, spirit and scope of this application to realize and apply the technology of this application. Obviously, the described embodiments are part of the embodiments of this application, not all of them. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0015] It should be noted that, in this article, if relational terms such as "first" and "second", "step 1" and "step 2", and "(1)" and "(2)" appear, they are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "comprise", "include" or any other variants thereof are intended to cover non-exclusive inclusion, so that the process, method, article or equipment including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or equipment. In the absence of further restrictions, the elements defined by the sentence "comprise one..." do not exclude the presence of other identical elements in the process, method, article or equipment including the elements. At the same time, the embodiments in this application and the features in the embodiments may be combined with each other without conflict.

[0016] During the production of sodium-ion batteries, excessive humidity causes water to react with sodium salts to generate excessive HF, which corrodes the metal parts inside the battery, destroys the battery material structure, and affects the density of the battery's SEI film, increasing the battery's internal resistance and shortening its cycle life. On the other hand, the metastable double bonds in the electrolyte solvent react with water to form complexes, causing problems such as battery capacity decay and performance deterioration. In addition, the increased water content reacts with the electrolyte, and the side reactions cause severe gas production and battery bulging.

[0017] Based on the above problems in the production process of existing sodium ion batteries, the present invention introduces imine substances containing CN bonds or C=N double bonds into the electrolyte. 2 O and HF molecules have strong polarity. Such stabilizers can react with H 2 O and HF molecules form N…HF(O), F(O)…HN or F(O)…HC hydrogen bonds, and adsorb and stabilize H through intermolecular forces.2 O, HF, to achieve the purpose of protecting other components of the electrolyte. At the same time, the present application also introduces a reactive stabilizer organic amine substance, which is alkaline and can neutralize the free acid HF produced by the side reaction, thereby reducing the content of water and acid in the electrolyte, improving the stability of the electrolyte, reducing the internal resistance, and improving the cycle performance of the battery. Therefore, in the first aspect of the present application, an electrolyte is provided, including an electrolyte sodium salt, an organic solvent, an imine containing a CN bond or a C=N double bond, and an organic amine.

[0018] In certain embodiments of the present application, the mass percentage content of the imine is 0.2-2.8%, the mass percentage content of the organic amine is 0.1-3.2%, the mass percentage content of the electrolyte sodium salt is 3-15%, and the balance is an organic solvent. In other embodiments of the present application, the mass percentage content of the imine is 0.2-0.4%, the mass percentage content of the organic amine is 0.1-0.2%, the mass percentage content of the electrolyte sodium salt is 9%, and the balance is an organic solvent.

[0019] In some other embodiments of the present application, the imine includes polyimide (PI) and / or polyethyleneimine (PEI), and the organic amine includes ethylenediamine (EDA) and / or ethanolamine (MEA).

[0020] In some other embodiments of the present application, the electrolyte sodium salt includes one or more of sodium hexafluorophosphate, sodium perchlorate, sodium tetrafluoroborate, sodium trifluoromethanesulfonate, sodium bis(trifluoromethylsulfonylimide), sodium bis(oxalatoborate), sodium difluorophosphate, sodium difluorooxalatoborate, sodium difluorobis(oxalatophosphate) and sodium bis(fluorosulfonylimide); optionally, the electrolyte sodium salt includes two or more types, each sodium salt having the same proportion, for example, a mixed sodium salt having a weight ratio of sodium hexafluorophosphate to sodium bis(trifluoromethylsulfonylimide of 1:1.

[0021] In some other embodiments of the present application, the organic solvent includes a cyclic compound and a linear compound, and the volume ratio of the two is 2:8 to 8:2. The cyclic compound includes one or more of propylene carbonate (PC), ethylene carbonate (EC), γ-butyrolactone (GBL), sulfolane (TMS), and fluoroethylene carbonate (FEC); the linear compound includes one or more of dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), methyl propyl carbonate (MPC), ethyl acetate (EA), propyl propionate (PP), ethyl propionate (EP), propyl acetate (PA), methyl propionate (MP), 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (HFE-458), and 2,2-difluoroethyl acetate (DFEA). In some other embodiments of the present application, the organic solvent includes ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC), and the weight ratio is EC:PC:EMC:DEC = 10:20:30:40.

[0022] In the second aspect of the present application, a sodium-ion battery is provided, which includes a positive electrode sheet, a negative electrode sheet, a separator, and the electrolyte of the present application.

[0023] In some embodiments of the present application, the active material of the positive electrode sheet includes a layered oxide material. In some other embodiments of the present application, the chemical formula of the layered oxide material is Na x M 1-y-z Fe y Mn z O 2 ; wherein, M is selected from one or more of Co, Ni, Cu, Mg, Zn, Al, Sn, Ga, Cr, Sr, V, and Ti, 0 < x ≤ 1, 0 ≤ y < 1, 0 ≤ z < 1, and y + z ≤ 1. In some other embodiments of the present application, the layered oxide material is sodium nickel iron manganese oxide. In some other embodiments of the present application, the active material of the positive electrode sheet includes a layered oxide material, a binder, and a conductive agent, which are mixed with N-methylpyrrolidone according to a mass ratio of 95:2.5:2.5 to form a slurry, coated on a current collector and dried to obtain the positive electrode sheet.

[0024] In some embodiments of the present application, the active material of the negative electrode sheet includes one or more of hard carbon, a titanium-based oxide negative electrode material, and an alloy-based negative electrode material. In some other embodiments of the present application, the active material of the negative electrode sheet includes hard carbon, a thickening agent, a binder, and a conductive agent, which are mixed with deionized water according to a mass ratio of 94:2:2:2 to form a slurry, coated on a current collector and dried to obtain the positive electrode sheet.

[0025] In certain embodiments of the present application, the thickener, binder, and conductive agent can be selected with reference to conventional substances in the battery field, such as polyvinylidene fluoride, styrene-butadiene rubber latex, conductive carbon black SP, graphene, carbon nanotubes, carboxymethyl cellulose, and the like.

[0026] In certain embodiments of the present application, the sodium ion battery is a soft-pack battery, which adopts the method of coating the positive electrode with the negative electrode, and the positive electrode sheet and the negative electrode sheet are stacked into a single cell by a Z-type lamination process, and the separator is separated between adjacent positive and negative electrode sheets, and then encapsulated with aluminum-plastic film, injected with liquid, and formed to prepare a soft-pack sodium battery.

[0027] In the third aspect of the present application, an electric device is provided, comprising the lithium-ion battery described in the present application, wherein the lithium-ion battery provides electric energy for the electric device. The electric device may be various devices or equipment driven by the lithium-ion battery, including but not limited to electric vehicles, electric vehicles, self-balancing vehicles, flatbed vehicles, aircraft, lighting equipment, household appliances, etc.

[0028] In each group of comparative experiments provided in this application, unless otherwise specified, other experimental conditions, materials, etc. are kept consistent except for the differences indicated in each group, so as to provide comparability. The experimental materials and reagents used in the examples can be obtained from commercial channels unless otherwise specified.

[0029] The following is a further description of an electrolyte, a sodium ion battery and an electrical device provided in the present application.

[0030] Embodiment 1:

[0031] 1. Sodium ion battery electrolyte containing stabilizer

[0032] The electrolyte is composed of electrolyte sodium salt, stabilizer and organic solvent:

[0033] The organic solvent is composed of ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) in a weight ratio of EC:PC:EMC:DEC=10:20:30:40, and the organic solvent accounts for 90.7% of the total mass of the electrolyte.

[0034] The electrolyte sodium salt is sodium hexafluorophosphate (NaPF 6 ), sodium bis(trifluoromethanesulfonimide) (NaN(CF 3 SO 2 ) 2 ) by weight ratio NaPF 6 :NaN(CF 3 SO 2 ) 2 =1:1 composition, sodium salt accounts for 9% of the total mass of the electrolyte.

[0035] The stabilizer is composed of a first additive polyimide (PI) accounting for 0.2% of the total mass of the electrolyte and a second additive ethylenediamine (EDA) accounting for 0.1% of the total mass of the electrolyte.

[0036] The electrolyte was prepared in an argon-protected glove box (H 2 O≤0.1ppm, O 2 During the preparation, the components constituting the organic solvent are firstly mixed uniformly according to the mass fractions, and then the first and second additives are added, and then the sodium salt is slowly added and fully stirred to form a mixed solution, that is, a sodium ion battery electrolyte is obtained.

[0037] 2. Sodium-ion soft-pack battery

[0038] The sodium ion battery comprises a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte.

[0039] The process humidity is 22% and the process temperature is 25°C. Preparation of positive electrode sheets for sodium ion batteries: Sodium nickel iron manganese oxide, polyvinylidene fluoride, conductive agent Super-P and N-methylpyrrolidone are mixed in a mass ratio of 95:2.5:2.5, and a slurry is obtained by stirring. The slurry is coated on the current collector aluminum foil on a coating machine and then dried. The positive electrode sheets are obtained by cold pressing, cutting, sheeting, powdering and sheet selection.

[0040] Preparation of negative electrode sheets for sodium ion batteries: hard carbon is used as the negative electrode active material, mixed with thickener CMC, binder SBR (styrene-butadiene rubber latex), conductive agent Super-P and deionized water in a mass ratio of 94:2:2:2, and a slurry is obtained by stirring. The slurry is coated on the current collector aluminum foil on a coater and then dried. The negative electrode sheets are obtained after cold pressing, cutting, sheet making, powder sweeping and sheet selection.

[0041] The positive electrode is coated with the negative electrode, and the positive electrode and the negative electrode are stacked into a single cell by a Z-type stacking process. The separator is placed between adjacent positive and negative electrode sheets, and then aluminum-plastic film packaging, liquid injection, and chemical formation are performed to prepare a soft-pack sodium battery.

[0042] Embodiment 2:

[0043] 1. Sodium ion battery electrolyte containing stabilizer

[0044] The electrolyte is composed of electrolyte sodium salt, stabilizer and organic solvent:

[0045] The organic solvent is composed of ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) in a weight ratio of EC:PC:EMC:DEC=10:20:30:40, and the organic solvent accounts for 90.4% of the total mass of the electrolyte.

[0046] The electrolyte sodium salt is sodium hexafluorophosphate (NaPF 6 ), sodium bis(trifluoromethanesulfonimide) (NaN(CF 3 SO 2 ) 2 ) by weight ratio NaPF 6 :NaN(CF 3 SO 2 ) 2 =1:1 composition, sodium salt accounts for 9% of the total mass of the electrolyte.

[0047] The stabilizer is composed of a first additive polyimide (PI) accounting for 0.4% of the total mass of the electrolyte and a second additive ethylenediamine (EDA) accounting for 0.2% of the total mass of the electrolyte.

[0048] The electrolyte was prepared in an argon-protected glove box (H 2 O≤0.1ppm, O 2 During the preparation, the components constituting the organic solvent are firstly mixed uniformly according to the mass fractions, and then the first and second additives are added, and then the sodium salt is slowly added and fully stirred to form a mixed solution, that is, a sodium ion battery electrolyte is obtained.

[0049] 2. Sodium-ion soft-pack battery

[0050] The sodium ion battery comprises a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte.

[0051] The process humidity is 22% and the process temperature is 25°C. Preparation of positive electrode sheets for sodium ion batteries: Sodium nickel iron manganese oxide, polyvinylidene fluoride, conductive agent Super-P and N-methylpyrrolidone are mixed in a mass ratio of 95:2.5:2.5, and a slurry is obtained by stirring. The slurry is coated on the current collector aluminum foil on a coating machine and then dried. The positive electrode sheets are obtained by cold pressing, cutting, sheeting, powdering and sheet selection.

[0052] Preparation of negative electrode sheets for sodium ion batteries: hard carbon is used as the negative electrode active material, mixed with thickener CMC, binder SBR (styrene-butadiene rubber latex), conductive agent Super-P and deionized water in a mass ratio of 94:2:2:2, and a slurry is obtained by stirring. The slurry is coated on the current collector aluminum foil on a coater and then dried. The negative electrode sheets are obtained after cold pressing, cutting, sheet making, powder sweeping and sheet selection.

[0053] The positive electrode is coated with the negative electrode, and the positive electrode and the negative electrode are stacked into a single cell by a Z-type stacking process. The separator is placed between adjacent positive and negative electrode sheets, and then aluminum-plastic film packaging, liquid injection, and chemical formation are performed to prepare a soft-pack sodium battery.

[0054] Embodiment 3:

[0055] 1. Sodium ion battery electrolyte containing stabilizer

[0056] The electrolyte is composed of electrolyte sodium salt, stabilizer and organic solvent:

[0057] The organic solvent is composed of ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) in a weight ratio of EC:PC:EMC:DEC=10:20:30:40, and the organic solvent accounts for 90.7% of the total mass of the electrolyte.

[0058] The electrolyte sodium salt is sodium hexafluorophosphate (NaPF 6 ), sodium bis(trifluoromethanesulfonimide) (NaN(CF 3 SO 2 ) 2 ) by weight ratio NaPF 6 :NaN(CF 3 SO 2 ) 2 =1:1 composition, sodium salt accounts for 9% of the total mass of the electrolyte.

[0059] The stabilizer is composed of a first additive polyimide (PI) accounting for 0.2% of the total mass of the electrolyte and a second additive ethanolamine (MEA) accounting for 0.1% of the total mass of the electrolyte.

[0060] The electrolyte was prepared in an argon-protected glove box (H 2 O≤0.1ppm, O 2 During the preparation, the components constituting the organic solvent are firstly mixed uniformly according to the mass fractions, and then the first and second additives are added, and then the sodium salt is slowly added and fully stirred to form a mixed solution, that is, a sodium ion battery electrolyte is obtained.

[0061] 2. Sodium-ion soft-pack battery

[0062] The sodium ion battery comprises a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte.

[0063] The process humidity is 22% and the process temperature is 25°C. Preparation of positive electrode sheets for sodium ion batteries: Sodium nickel iron manganese oxide, polyvinylidene fluoride, conductive agent Super-P and N-methylpyrrolidone are mixed in a mass ratio of 95:2.5:2.5, and a slurry is obtained by stirring. The slurry is coated on the current collector aluminum foil on a coating machine and then dried. The positive electrode sheets are obtained by cold pressing, cutting, sheeting, powdering and sheet selection.

[0064] Preparation of negative electrode sheets for sodium ion batteries: hard carbon is used as the negative electrode active material, mixed with thickener CMC, binder SBR (styrene-butadiene rubber latex), conductive agent Super-P and deionized water in a mass ratio of 94:2:2:2, and a slurry is obtained by stirring. The slurry is coated on the current collector aluminum foil on a coater and then dried. The negative electrode sheets are obtained after cold pressing, cutting, sheet making, powder sweeping and sheet selection.

[0065] The positive electrode is coated with the negative electrode, and the positive electrode and the negative electrode are stacked into a single cell by a Z-type stacking process. The separator is placed between adjacent positive and negative electrode sheets, and then aluminum-plastic film packaging, liquid injection, and chemical formation are performed to prepare a soft-pack sodium battery.

[0066] Embodiment 4:

[0067] 1. Sodium ion battery electrolyte containing stabilizer

[0068] The electrolyte is composed of electrolyte sodium salt, stabilizer and organic solvent:

[0069] The organic solvent is composed of ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) in a weight ratio of EC:PC:EMC:DEC=10:20:30:40, and the organic solvent accounts for 90.4% of the total mass of the electrolyte.

[0070] The electrolyte sodium salt is sodium hexafluorophosphate (NaPF 6 ), sodium bis(trifluoromethanesulfonimide) (NaN(CF 3 SO 2 ) 2 ) by weight ratio NaPF 6 :NaN(CF 3 SO 2 ) 2 =1:1 composition, sodium salt accounts for 9% of the total mass of the electrolyte.

[0071] The stabilizer is composed of a first additive polyimide (PI) accounting for 0.4% of the total mass of the electrolyte and a second additive ethanolamine (MEA) accounting for 0.2% of the total mass of the electrolyte.

[0072] The electrolyte was prepared in an argon-protected glove box (H 2 O≤0.1ppm, O 2 During the preparation, the components constituting the organic solvent are firstly mixed uniformly according to the mass fractions, and then the first and second additives are added, and then the sodium salt is slowly added and fully stirred to form a mixed solution, that is, a sodium ion battery electrolyte is obtained.

[0073] 2. Sodium-ion soft-pack battery

[0074] The sodium ion battery comprises a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte.

[0075] The process humidity is 22% and the process temperature is 25°C. Preparation of positive electrode sheets for sodium ion batteries: Sodium nickel iron manganese oxide, polyvinylidene fluoride, conductive agent Super-P and N-methylpyrrolidone are mixed in a mass ratio of 95:2.5:2.5, and a slurry is obtained by stirring. The slurry is coated on the current collector aluminum foil on a coating machine and then dried. The positive electrode sheets are obtained by cold pressing, cutting, sheeting, powdering and sheet selection.

[0076] Preparation of negative electrode sheets for sodium ion batteries: hard carbon is used as the negative electrode active material, mixed with thickener CMC, binder SBR (styrene-butadiene rubber latex), conductive agent Super-P and deionized water in a mass ratio of 94:2:2:2, and a slurry is obtained by stirring. The slurry is coated on the current collector aluminum foil on a coater and then dried. The negative electrode sheets are obtained after cold pressing, cutting, sheet making, powder sweeping and sheet selection.

[0077] The positive electrode is coated with the negative electrode, and the positive electrode and the negative electrode are stacked into a single cell by a Z-type stacking process. The separator is placed between adjacent positive and negative electrode sheets, and then aluminum-plastic film packaging, liquid injection, and chemical formation are performed to prepare a soft-pack sodium battery.

[0078] Comparative Example 1

[0079] 1. Conventional sodium ion battery electrolyte

[0080] The electrolyte is composed of electrolyte sodium salt and organic solvent:

[0081] The organic solvent is composed of ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) in a weight ratio of EC:PC:EMC:DEC=10:20:30:40, and the organic solvent accounts for 91% of the total mass of the electrolyte.

[0082] The electrolyte sodium salt is sodium hexafluorophosphate (NaPF 6 ), sodium bis(trifluoromethanesulfonimide) (NaN(CF 3 SO 2 ) 2 ) by weight ratio NaPF 6 :NaN(CF 3 SO 2 ) 2 =1:1 composition, sodium salt accounts for 9% of the total mass of the electrolyte.

[0083] The electrolyte was prepared in an argon-protected glove box (H 2 O≤0.1ppm, O 2During the preparation, the components constituting the organic solvent are firstly mixed uniformly according to their mass fractions, and then the sodium salt is slowly added and fully stirred to form a mixed solution, so as to obtain a sodium ion battery electrolyte.

[0084] 2. Sodium-ion soft-pack battery

[0085] The sodium ion battery comprises a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte.

[0086] The process humidity is 22% and the process temperature is 25°C. Preparation of positive electrode sheets for sodium ion batteries: Sodium nickel iron manganese oxide, polyvinylidene fluoride, conductive agent Super-P and N-methylpyrrolidone are mixed in a mass ratio of 95:2.5:2.5, and a slurry is obtained by stirring. The slurry is coated on the current collector aluminum foil on a coating machine and then dried. The positive electrode sheets are obtained by cold pressing, cutting, sheeting, powdering and sheet selection.

[0087] Preparation of negative electrode sheets for sodium ion batteries: hard carbon is used as the negative electrode active material, mixed with thickener CMC, binder SBR (styrene-butadiene rubber latex), conductive agent Super-P and deionized water in a mass ratio of 94:2:2:2, and a slurry is obtained by stirring. The slurry is coated on the current collector aluminum foil on a coater and then dried. The negative electrode sheets are obtained after cold pressing, cutting, sheet making, powder sweeping and sheet selection.

[0088] The positive electrode is coated with the negative electrode, and the positive electrode and the negative electrode are stacked into a single cell by a Z-type stacking process. The separator is placed between adjacent positive and negative electrode sheets, and then aluminum-plastic film packaging, liquid injection, and chemical formation are performed to prepare a soft-pack sodium battery.

[0089] Experimental example:

[0090] The performance tests were performed on the batteries in Examples 1 to 4 and Comparative Example 1. The results of the battery 0.5C / 0.5C cycle test at room temperature are shown in Table 1. The results of the battery internal resistance test are shown in Table 2. The results of the volume change during the battery cycle at room temperature are shown in Table 3.

[0091] Performance testing method:

[0092] Battery internal resistance test: The battery is tested for internal resistance when it is fully charged, i.e., at SOC 100%.

[0093] Normal temperature cycle test: At room temperature, charge at 0.5C constant current and constant voltage; leave for 10 minutes; discharge at 0.5C constant current and leave for 10 minutes; repeat the charge and discharge steps. After reaching the number of cycles, measure the battery volume under the cabinet.

[0094] The above electrochemical tests were all completed using Titan 5V10A battery test cabinet.

[0095] Table 1

[0096]

[0097]

[0098] It can be seen from Table 1 that the battery of Comparative Example 1 does not contain an electrolyte containing a stabilizer, and at a relatively high process humidity, its capacity retention rate after 200 cycles is only 87.6%, while the capacity retention rate of the battery of the present application after 200 cycles is above 92.7%.

[0099] Table 2

[0100] Initial internal resistance (mΩ) Internal resistance of battery after 200 cycles (mΩ) Example 1 14.96 16.01 Example 2 14.76 15.82 Example 3 14.52 15.77 Example 4 14.59 15.84 Comparative Example 1 14.71 17.54

[0101] It can be seen from Table 2 that the internal resistance of the battery in Comparative Example 1 increased by 2.83 mΩ after 200 cycles, while the internal resistance of the battery of the present application increased by a maximum of 1.25 mΩ after 200 cycles, and the degree of increase in internal resistance was significantly reduced.

[0102] Table 3

[0103] Initial volume (mL) Cell volume after 200 cycles (mL) Example 1 28.3 30.1 Example 2 28.2 29.7 Example 3 28.3 30 Example 4 28 29.9 Comparative Example 1 27.8 32.6

[0104] It can be seen from Table 3 that the battery of Comparative Example 1 has a gas production of 4.8 mL after 200 cycles, while the maximum gas production of the battery of the present application is 1.9 mL after 200 cycles, which can significantly improve the battery bulging phenomenon.

[0105] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.

Claims

1. An electrolyte, characterized in that: The invention comprises electrolyte sodium salt, organic solvent, imine containing CN bond or C=N double bond, and organic amine.

2. The electrolyte according to claim 1, characterized in that The mass percentage content of the imine is 0.2-2.8%, and the mass percentage content of the organic amine is 0.1-3.2%.

3. The electrolyte according to claim 1 or 2, characterized in that The imine includes polyimide and / or polyethyleneimine.

4. The electrolyte according to claim 1 or 2, characterized in that The organic amine includes ethylenediamine and / or ethanolamine.

5. A sodium ion battery, characterized in that: It comprises a positive electrode sheet, a negative electrode sheet, a separator, and the electrolyte according to any one of claims 1 to 4.

6. The sodium ion battery according to claim 5, characterized in that: The active material of the positive electrode plate includes a layered oxide material.

7. The sodium ion battery according to claim 6, characterized in that: The chemical formula of the layered oxide material is Na x M 1-y-z Fe y Mn z O2; wherein M is selected from one or more of Co, Ni, Cu, Mg, Zn, Al, Sn, Ga, Cr, Sr, V and Ti, 0 <x≤1,0≤y<1,0≤z<1,y+z≤1。 8. The sodium ion battery according to claim 5, characterized in that: The active material of the negative electrode plate includes one or more of hard carbon, titanium-based oxide negative electrode material, and alloy negative electrode material.

9. An electrical device, characterized in that: The sodium ion battery comprises the sodium ion battery according to any one of claims 5 to 8, wherein the sodium ion battery provides electrical energy for the electrical equipment.

Citation Information

Cited By

  • High-temperature electrolyte additive, electrolyte and lithium ion battery

    CN122025811A