Ternary lithium ion battery electrolyte and ternary lithium ion battery containing same
By using compound A containing Se=O bond as a film forming additive in the ternary lithium-ion battery electrolyte, a protective interface film is formed, which solves the problem of damage to the battery by reactive oxygen radicals at high temperature and high voltage, and improves the battery Low temperature and high temperature cycle performance.
Patent Information
- Application Number
- CN202411491553.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-24
- Publication Date
- 2024-12-03
AI Technical Summary
The performance of high-nickel ternary lithium-ion batteries deteriorates at high temperatures and high voltages, mainly due to the damage of reactive oxygen radicals on the electrode-electrolyte interface and the decomposition of electrolytes, which leads to accelerated side reactions and affects the cycling performance of the battery.
Compound A containing structural formula I or structural formula II is used as film forming additives. This compound A forms a protective interface film on the electrode surface to reduce the damage of reactive oxygen radicals, and captures reactive oxygen radicals through Se=O bonds to improve the battery's Low temperature and high temperature cycle performance.
It significantly improves the low-temperature discharge performance of ternary lithium-ion batteries and the cycling performance under high temperature and high voltage, extends the service life of the battery and improves the stability of the electrode-electrolyte interface.
Smart Images

Figure CN119069809A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of ternary lithium ion batteries, and in particular relates to a ternary lithium ion battery electrolyte and a ternary lithium ion battery containing the electrolyte. Background Art
[0002] Lithium-ion batteries have been widely used in many fields such as consumer electronics, energy storage systems, and electric vehicles due to their advantages such as high energy density and long cycle life. In particular, with the rapid development of the electric vehicle industry, the market demand for increasing driving range is growing, which further promotes the pursuit of higher energy density battery technology. In lithium-ion batteries, although graphite negative electrode materials can already provide relatively high capacity (≥350mAh / g), the capacity of positive electrode materials has become one of the key factors restricting the improvement of overall energy density. In order to overcome this bottleneck, researchers turned their attention to high-nickel ternary layered oxide materials, which have high discharge capacity (≥180mAh / g) and voltage platform (3.8V), making high-nickel ternary lithium-ion batteries the preferred power source for electric vehicles, portable electronic devices and other fields.
[0003] However, the performance of high-nickel ternary lithium-ion batteries will significantly decline under high temperature and high voltage working conditions. This may be because as the voltage increases, especially when using high-nickel ternary layered oxides as the positive electrode, the electrode material may undergo an irreversible phase change and produce reactive oxygen radicals. These reactive oxygen radicals have a destructive effect on the electrode-electrolyte interface, which will accelerate the aging of the positive electrode material, trigger side reactions, and lead to a decline in battery performance. At the same time, the high temperature environment exacerbates the occurrence rate of the above process and accelerates the decomposition of the electrolyte, which will further damage the battery performance.
[0004] Therefore, there is an urgent need for a ternary lithium-ion battery electrolyte and a ternary lithium-ion battery containing the electrolyte to solve the deficiencies of the prior art. Summary of the invention
[0005] In view of the above problems, the object of the present invention is to provide a ternary lithium ion battery electrolyte and a ternary lithium ion battery containing the electrolyte, wherein the ternary lithium ion battery electrolyte can enable the ternary lithium ion battery to have good low-temperature discharge performance and excellent cycle performance at high temperature and high voltage.
[0006] To achieve the above objectives, the present invention provides a ternary lithium-ion battery electrolyte in a first aspect, comprising an electrolyte lithium salt, a non-aqueous organic solvent, and a film-forming additive, wherein the film-forming additive contains a compound A represented by structural formula I or structural formula II:
[0007]
[0008] Among them, R1 ~R 2 are independently selected from hydrogen, alkyl, 3 ~R 4 is selected from alkyl, and m and n are each independently selected from 0 or 1.
[0009] Compared with the prior art, the film-forming additive of the ternary lithium-ion battery electrolyte of the present invention contains compound A shown in structural formula I or structural formula II, and the compound A can be oxidized on the electrode surface before the solvent to form a thinner interface layer, which has a better lithium ion transmission efficiency, is not easy to shrink holes at low temperatures, can maintain the lithium ion transmission channel at low temperatures, and improve the low temperature performance of the ternary lithium-ion battery. At the same time, the compound A contains selenium, which exhibits high chemical reaction activity and low reduction potential. These characteristics enable compound A to more effectively form a protective interface film on the negative electrode surface. The formed interface film can significantly reduce the direct contact between the electrolyte and the electrode material, thereby effectively reducing the incidence of side reactions and improving the cycle performance of the battery. In addition, the Se=O bond in compound A can quickly react with the generated active oxygen free radicals and capture these active oxygen free radicals. This characteristic is particularly important for reducing the damage caused by active oxygen free radicals to the electrode-electrolyte interface, especially under high voltage or high temperature conditions. Therefore, the ternary lithium ion battery electrolyte of the present invention can not only improve the low temperature performance of the ternary lithium ion battery, but also enhance the stability of the electrode-electrolyte interface, and effectively solve the problems caused by active oxygen free radicals under high voltage and high temperature. Therefore, the ternary lithium ion battery electrolyte of the present invention is applied to the ternary lithium ion battery, which can make the ternary lithium ion battery have better low temperature discharge performance and excellent cycle performance under high temperature and high voltage.
[0010] Further, the alkyl group of the present invention is selected from at least one of methyl, ethyl, propyl, isopropyl, butyl, sec-butyl, tert-butyl, pentyl and cyclohexyl. Preferably, the alkyl group of the present invention is selected from methyl, ethyl and propyl.
[0011] Furthermore, the compound A of the present invention is at least one selected from compounds 1 to 8:
[0012]
[0013] Furthermore, the mass percentage of compound A of the present invention in the electrolyte of a ternary lithium-ion battery is 0.1-5%. If the content is lower than 0.1%, it is insufficient to form an effective interface film, while too high a concentration may cause the interface film to be too thick, thereby increasing the internal resistance of the battery. Specifically, the mass percentage of compound A in the electrolyte of a ternary lithium-ion battery may be, but is not limited to, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%.
[0014] Furthermore, the electrolyte lithium salt of the present invention includes lithium hexafluorophosphate (LiPF 6 ), lithium perchlorate (LiClO 4 ), lithium tetrafluoroborate (LiBF 4 ), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium methanesulfonate (LiMS), lithium trifluoromethanesulfonate, lithium fluorosulfonate, lithium bis(oxalatoborate) (LiBOB), lithium difluorooxalatoborate (LiDFOB), lithium difluorophosphate (LiPO 2 F 2 ), lithium difluorobis(oxalate)phosphate (LiDFOP), lithium diphosphate (Li 2 HPO 4 ) and at least one of a lower aliphatic carboxylic acid lithium. The lower aliphatic carboxylic acid lithium may be, but is not limited to, lithium acetate and lithium propionate. Lithium hexafluorophosphate has the characteristics of high conductivity, good electrochemical stability and good compatibility with graphite negative electrode, so the electrolyte lithium salt of the present invention is preferably lithium hexafluorophosphate.
[0015] Furthermore, the mass percentage of the electrolyte lithium salt of the present invention in the ternary lithium ion battery electrolyte is 5 to 30%. The electrolyte lithium salt is the main ion source in the ternary lithium ion battery electrolyte and provides the transmission of lithium ions. The content of lithium salt in the range of 5 to 30% can ensure that the electrolyte has sufficient ionic conductivity without increasing the viscosity of the electrolyte. Specifically, the mass percentage of the electrolyte lithium salt in the ternary lithium ion battery electrolyte can be but is not limited to 5%, 10%, 15%, 20%, 25%, 30%.
[0016] Furthermore, the non-aqueous organic solvent of the present invention includes at least one of carbonate, carboxylate and ether compounds. Carbonate, carboxylate and ether compounds generally have good lithium salt solubility, which can ensure that the concentration of lithium ions in the electrolyte is sufficiently high, thereby providing good conductivity. In addition, carbonate compounds generally have a higher boiling point, which helps to improve the thermal stability of the electrolyte; carboxylate compounds have a lower viscosity, which can improve the fluidity and wettability of the electrolyte; ether compounds can remain liquid over a wide temperature range, which is beneficial to the use of batteries in high and low temperature environments. Therefore, by reasonably selecting and proportioning these different types of non-aqueous organic solvents, the conductivity and cycle life of ternary lithium-ion batteries can be optimized.
[0017] Further, the carbonate compounds of the present invention include cyclic carbonates and chain carbonates. Specifically, the cyclic carbonates may be, but are not limited to, ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), pentylene carbonate, vinylene carbonate (VC) or their derivatives; chain carbonates include, but are not limited to, dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), and propylene carbonate.
[0018] Furthermore, the carboxylate compounds of the present invention include at least one of cyclic carboxylates and chain carboxylates. The cyclic carboxylates may specifically include but are not limited to at least one of γ-butyrolactone (GBL), γ-valerolactone (GVL), and δ-valerolactone (DVL); the chain carboxylates include but are not limited to methyl acetate (MAC), ethyl acetate (EA), propyl acetate (PA), butyl acetate (BA), propyl propionate (PP), and butyl propionate (BP).
[0019] Furthermore, the ether compounds of the present invention include cyclic ethers or chain ethers. The cyclic ethers may specifically include but are not limited to 1,3-dioxolane (DOL), 1,4-dioxolane (DX), crown ethers, tetrahydrofuran (THF), 2-methyltetrahydrofuran (2-CH 3 -THF), 2-trifluoromethyltetrahydrofuran (2-CF 3 -THF); the chain ether may specifically include but is not limited to dimethoxymethane, diethoxymethane, ethoxymethoxymethane, ethylene glycol di-n-propyl ether, ethylene glycol di-n-butyl ether, and diethylene glycol dimethyl ether.
[0020] Furthermore, the ternary lithium ion battery electrolyte of the present invention also includes an auxiliary agent, which is selected from vinylene carbonate (VC), vinylene carbonate (VEC), fluoroethylene carbonate (FEC), vinyl sulfite (ES), 1,3-propane sultone (PS), 1,3-propylene sultone (PES), 1,4-butane sultone (BS), vinyl sulfate (DTD), succinic anhydride (SA), maleic anhydride (MA), 2-methylmaleic anhydride (MMA), methyl carbonate-2-propynyl ester (MPC), tetravinylsilane (TES), triallyl isocyanurate (TAIC), hexamethylene diisocyanate At least one of ester (HDI), o-phenanthroline, p-phenylene diisocyanate (TDI), 2,4-toluene diisocyanate (MDI), N-phenylbis(trifluoromethanesulfonyl)imide (LiTFSI), diethylene sulfate (DES), phenyl methanesulfonate (BMS), dipropylene sulfate (DPS), hydroquinone difluorosulfonate, triallyl phosphate (TAP), tripropargyl phosphate (TPP), 2,4-butane sultone (BES), isocyanoethyl methacrylate, methylene disulfonate, tris(trimethylsilyl)borate, tris(trimethylsilyl)phosphate, and tris(vinyldimethylsilyl)phosphate. On the basis of film-forming additives, the introduction of additives can further improve the performance of ternary lithium-ion batteries. For example, VC and FEC can form a uniform and stable SEI film on the surface of the negative electrode, which can further improve the cycle performance of ternary lithium-ion batteries; PS and BS can form a more stable interface film at high temperature, reduce the decomposition of the electrolyte and gas generation, thereby further improving the stability of ternary lithium-ion batteries at high temperatures; MA can reduce the viscosity of the electrolyte and improve the fluidity of the electrolyte at low temperatures, thereby further improving the low-temperature discharge performance of ternary lithium-ion batteries. Therefore, by reasonably selecting and proportioning additives, the cycle performance, high-temperature performance, conductivity, low-temperature performance, etc. of ternary lithium-ion batteries can be significantly improved.
[0021] Furthermore, the mass percentage of the auxiliary agent of the present invention in the ternary lithium ion battery electrolyte is 0.1-5%. For example, the content of the auxiliary agent can be but not limited to 0.1%, 0.6%, 0.8%, 1.2%, 1.6%, 2%, 2.6%, 3.2%, 3.6%, 4%, 4.5%, 5%.
[0022] Correspondingly, the second aspect of the present invention also provides a ternary lithium-ion battery, including a positive electrode and a negative electrode, and also includes the ternary lithium-ion battery electrolyte mentioned above, the active material of the positive electrode is a high-nickel ternary layered oxide, and the maximum charging voltage of the ternary lithium-ion battery is 4.5V.
[0023] Compared with the prior art, the ternary lithium-ion battery electrolyte of the present invention can not only improve the low-temperature performance of the ternary lithium-ion battery, but also enhance the stability of the electrode-electrolyte interface and effectively solve the problems caused by active oxygen free radicals under high voltage and high temperature. Therefore, the ternary lithium-ion battery of the present invention has good low-temperature discharge performance and excellent cycle performance under high temperature and high voltage.
[0024] Furthermore, the structural formula of the high nickel ternary layered oxide of the present invention is LiNi x Co y Mn 1-x-y M z O 2 , wherein 0.6≤x<0.9, x+y<1, 0≤z<0.08, and M is at least one of Al, Mg, Zr and Ti.
[0025] Furthermore, the active material of the negative electrode of the present invention includes at least one of a carbon-based negative electrode, a silicon-based negative electrode, a tin-based negative electrode and a lithium negative electrode. The carbon-based negative electrode may include graphite, hard carbon, soft carbon, graphene, mesophase carbon microspheres, etc.; the silicon-based negative electrode may include silicon materials, silicon oxides, silicon-carbon composite materials and silicon alloy materials, etc.; the tin-based negative electrode may include tin, tin carbon, tin oxygen, tin metal compounds; the lithium negative electrode may include metallic lithium or lithium alloys, wherein the lithium alloy may specifically be at least one of lithium silicon alloys, lithium sodium alloys, lithium potassium alloys, lithium aluminum alloys, lithium tin alloys and lithium indium alloys. DETAILED DESCRIPTION
[0026] In order to further illustrate the purpose, technical scheme and beneficial effects of the present invention, the present invention will be further described below in conjunction with specific examples. It should be noted that, if specific conditions are not specified in the examples and comparative examples, they can be carried out according to conventional conditions or conditions recommended by the manufacturer, and if the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be obtained commercially.
[0027] Example 1
[0028] This embodiment provides a method for preparing a ternary lithium-ion battery, the steps comprising:
[0029] (1) The ternary material LiNi 0.8 Co 0.1 Mn 0.1 Zr 0.03 O 2 , conductive agent SuperP, adhesive PVDF and carbon nanotubes (CNT) are mixed evenly in a mass ratio of 96.5:1.5:1:1 to form a lithium-ion battery positive electrode slurry with a certain viscosity, which is coated on the aluminum foil for current collector, and the coating amount is 324g / m 2, dried at 85°C and then cold pressed; then trimmed, cut into pieces, and slit, and then dried at 85°C for 4 hours under vacuum conditions, and the tabs were welded to make positive electrode sheets that meet the requirements;
[0030] (2) artificial graphite and silicon are mixed in a mass ratio of 90:10, and then mixed with a conductive agent SuperP, a thickener CMC, and an adhesive SBR (styrene-butadiene rubber latex) in a mass ratio of 95:1.5:1.0:2.5 to make a slurry, which is mixed evenly, and the mixed slurry is applied on both sides of a copper foil, and then dried and rolled to obtain a negative electrode sheet, thereby making a negative electrode sheet that meets the requirements;
[0031] (3) In a glove box filled with nitrogen (O 2 <1ppm,H 2 O<1ppm), ethylene carbonate (EC), ethyl methyl carbonate (EMC), butylene carbonate (BC), propyl propionate (PP), and butyl acetate (BA) were mixed in a mass ratio of 4:3:2:4:2 to obtain a mixed solvent as a non-aqueous organic solvent, and then film-forming additives and auxiliary agents were added to obtain a mixed solution. The mixed solution was sealed and packaged and placed in a quick freezer (-4°C) for 2 hours, then taken out and placed in a glove box filled with nitrogen (O 2 <1ppm,H 2 O<1ppm), slowly add lithium hexafluorophosphate (LiPF 6 ), and after being evenly mixed, a ternary lithium-ion battery electrolyte is prepared;
[0032] (4) The positive electrode sheet, negative electrode sheet and separator are laminated to form a ternary lithium-ion battery with a thickness of 4.7 mm, a width of 55 mm and a length of 60 mm. The battery is vacuum-baked at 75°C for 10 h and the electrolyte of the ternary lithium-ion battery is injected. After standing for 24 h, the battery is charged to 4.5 V with a constant current of 0.1 C (180 mA), and then charged at a constant voltage of 4.5 V until the current drops to 0.05 C (90 mA); then discharged to 3.0 V with 0.2 C (180 mA), and the charge and discharge are repeated twice. Finally, the battery is charged to 3.8 V with 0.2 C (180 mA) to obtain a ternary lithium-ion battery.
[0033] The formulas of the ternary lithium-ion battery electrolytes of Examples 1 to 19 and Comparative Examples 1 to 5 are shown in Table 1, wherein the preparation processes of the ternary lithium-ion battery electrolytes, positive electrode sheets, negative electrode sheets, and ternary lithium-ion batteries of Examples 2 to 19 and Comparative Examples 1 to 5 are exactly the same as those of Example 1.
[0034] Table 1 Compositions of the ternary lithium ion battery electrolytes of the embodiments and comparative examples
[0035]
[0036] The structure of DTD is as follows:
[0037]
[0038] The ternary lithium-ion batteries prepared in Examples 1 to 19 and Comparative Examples 1 to 5 were subjected to high temperature storage performance test, high temperature cycle performance test, room temperature cycle performance test, and low temperature discharge performance test under the following conditions. The results are shown in Table 2.
[0039] High temperature storage performance test :
[0040] At room temperature (25°C), the ternary lithium-ion battery was charged and discharged at 0.5C / 0.5C (the battery discharge capacity was recorded as C 0 ), the upper limit voltage is 4.5V, then the battery is charged to 4.5V under 0.5C constant current and constant voltage conditions, and the battery thickness is measured (the thickness is recorded as D 0 ); Place the battery in a 60°C oven for 30 days, take it out and measure the battery thickness (the thickness is recorded as D 1 ) ; Place the battery in a 25°C environment and discharge it at 0.5C (the discharge capacity is recorded as C 1 ); continue to charge and discharge the ternary lithium-ion battery at 0.5C / 0.5C at room temperature (25°C) (the battery discharge capacity is recorded as C 2 ), with the upper limit voltage being 4.5 V, calculate the capacity retention rate, capacity recovery rate and thickness expansion rate.
[0041] Capacity retention rate = (C 1 / C 0 ) × 100%;
[0042] Capacity recovery rate = (C 2 / C 0 ) × 100%;
[0043] Thickness expansion rate = (D 1 / D 0 ) × 100%
[0044] Normal temperature cycle performance test :
[0045] At room temperature (25°C), the ternary lithium-ion battery was charged and discharged at 1.0C / 1.0C (the battery discharge capacity is C 0 ), the upper limit voltage is 4.5V, and then 1.0C / 1.0C charging and discharging is performed at room temperature for 500 cycles (the battery discharge capacity is C 1 ), calculate the capacity retention rate.
[0046] Capacity retention rate = (C 1 / C 0 ) × 100%
[0047] High temperature cycle performance test :
[0048] Under the condition of over-temperature (50℃), the ternary lithium-ion battery was charged and discharged at 1.0C / 1.0C (the battery discharge capacity is C 0 ), the upper limit voltage is 4.5V, and then 1.0C / 1.0C charging and discharging is performed at room temperature for 400 cycles (the battery discharge capacity is C 1 ), calculate the capacity retention rate.
[0049] Capacity retention rate = (C 1 / C 0 ) × 100%
[0050] Low temperature performance test :
[0051] At room temperature (25°C), the ternary lithium-ion battery was charged and discharged at 0.5C / 0.5 (the battery cut-off voltage was 3.0V and the discharge capacity was C 0 ), the upper limit voltage is 4.5V (cut-off current 0.05C). Then the battery is fully charged to 4.5V (cut-off current 0.05C) at 0.5C at room temperature (25℃), and then the battery is transferred to -20℃ and left for 4 hours, and discharged to 3.0V at 0.5C, with a discharge capacity of C 1 , calculate the capacity retention rate.
[0052] Capacity retention rate = (C 1 / C 0 )×100%
[0053] Table 2 Ternary lithium-ion battery performance test results
[0054]
[0055] As can be seen from Table 2, compared with Comparative Example 1, the ternary lithium-ion batteries of Examples 1 to 8 have relatively good cycle performance under high temperature and high pressure, and have good low-temperature discharge performance. This is because the ternary lithium-ion battery electrolyte of the present invention contains compound A shown in structural formula I or structural formula II, and the compound A can be oxidized on the electrode surface before the solvent to form a thinner interface layer. The interface layer has a better lithium ion transmission efficiency, is not easy to shrink holes at low temperatures, can maintain the lithium ion transmission channel at low temperatures, and improves the low-temperature performance of the ternary lithium-ion battery. At the same time, the compound A contains selenium, which exhibits high chemical reaction activity and low reduction potential. These characteristics enable compound A to more effectively form a protective interface film on the surface of the negative electrode. The formed interface film can significantly reduce the direct contact between the electrolyte and the electrode material, thereby effectively reducing the incidence of the secondary interface film reaction and improving the cycle performance of the battery. In addition, the Se=O bond in compound A can react quickly with the generated active oxygen free radicals and capture these active oxygen free radicals. This property is particularly important for reducing the damage caused by active oxygen free radicals to the electrode-electrolyte interface, especially under high voltage or high temperature conditions. Therefore, the ternary lithium ion battery of the present invention has good low-temperature discharge performance and excellent cycle performance under high temperature and high voltage.
[0056] By comparing Example 10 with Examples 13 to 16, it can be seen that adding auxiliary agents on the basis of the film-forming additives of the present invention can further improve the high-temperature storage performance, high-temperature cycle performance, low-temperature performance, lithium ion cycle performance of the ternary lithium-ion battery, and the expansion rate is lower.
[0057] By comparing Examples 13 to 14 with Examples 17 to 19, it can be seen that when VC / SA mixed additives are used in the electrolyte of the ternary lithium-ion battery, the high temperature performance of the ternary lithium-ion battery is greatly improved, and the expansion rate is further improved.
[0058] By comparing Example 5, Example 15, and Comparative Example 5, it can be seen that if only DTD is used as an auxiliary agent, it cannot effectively improve the cycle performance of the ternary lithium-ion battery under high temperature and high pressure. This is because compared with sulfur atoms, selenium atoms have lower electronegativity and larger atomic radius. Selenium has the characteristics of high chemical reactivity, lower reduction potential, and is more likely to form a protective layer interface at the negative electrode. In addition, the S=O bond is not easy to react with active oxygen, and thus cannot effectively inhibit the side effects of oxygen free radicals on the electrode electrolyte interface. Therefore, if the electrolyte of the ternary lithium-ion battery only contains DTD, it cannot effectively improve the cycle performance of the ternary lithium-ion battery under high temperature and high pressure.
[0059] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention is described in detail with reference to the preferred embodiments, it is not limited to those listed in the embodiments. Those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A ternary lithium-ion battery electrolyte, characterized in that: The invention comprises an electrolyte lithium salt, a non-aqueous organic solvent, and a film-forming additive, wherein the film-forming additive contains a compound A represented by structural formula I or structural formula II: Wherein, R1-R2 are each independently selected from hydrogen and alkyl, R3-R4 are selected from alkyl, and m and n are each independently selected from 0 or 1.
2. The ternary lithium-ion battery electrolyte according to claim 1, characterized in that: The alkyl group is selected from at least one of a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, a sec-butyl group, a tert-butyl group, a pentyl group and a cyclohexyl group.
3. The ternary lithium-ion battery electrolyte according to claim 1, characterized in that: The compound A is selected from at least one of compounds 1 to 8:
4. The ternary lithium-ion battery electrolyte according to claim 1, characterized in that: The mass percentage of the compound A in the ternary lithium-ion battery electrolyte is 0.1-5%.
5. The ternary lithium-ion battery electrolyte according to claim 1, characterized in that: The electrolyte lithium salt includes at least one of lithium hexafluorophosphate, lithium perchlorate, lithium tetrafluoroborate, lithium bisfluorosulfonyl imide, lithium bistrifluoromethylsulfonyl imide, lithium methane sulfonate, lithium trifluoromethyl sulfonate, lithium fluorosulfonate, lithium bisoxalatoborate, lithium difluorooxalatoborate, lithium difluorophosphate, lithium difluorobisoxalatophosphate, lithium diphosphate and lithium lower aliphatic carboxylate.
6. The ternary lithium-ion battery electrolyte according to claim 1, characterized in that: The non-aqueous organic solvent includes at least one of carbonate, carboxylate and ether compounds.
7. The ternary lithium-ion battery electrolyte according to claim 1, characterized in that: The auxiliary agent is selected from vinylene carbonate, vinylene carbonate, fluoroethylene carbonate, vinyl sulfite, 1,3-propane sultone, 1,3-propylene sultone, 1,4-butane sultone, vinyl sulfate, succinic anhydride, maleic anhydride, 2-methylmaleic anhydride, methyl carbonate-2-propynyl ester, tetravinylsilane, triallyl isocyanurate, hexamethylene diisocyanate, o-phenanthroline, p-phenylene diisocyanate At least one of ester, 2,4-toluene diisocyanate, N-phenylbis(trifluoromethanesulfonyl)imide, vinyl bissulfate, phenyl methanesulfonate, bis-spiro propylene sulfate, hydroquinone difluorosulfonate, triallyl phosphate, tripropargyl phosphate, 2,4-butane sultone, isocyanoethyl methacrylate, methylene methanedisulfonate, tris(trimethylsilyl)borate, tris(trimethylsilyl)phosphate, and tris(vinyldimethylsilyl)phosphate.
8. A ternary lithium-ion battery, characterized in that: It comprises a positive electrode and a negative electrode, and also comprises a ternary lithium-ion battery electrolyte as described in any one of claims 1 to 7, the active material of the positive electrode is a high-nickel ternary layered oxide, and the maximum charging voltage of the ternary lithium-ion battery is 4.5V.
9. The ternary lithium-ion battery according to claim 8, characterized in that: The structural formula of the high nickel ternary layered oxide is LiNi x Co y Mn 1-x-y M z O2, wherein 0.6≤x<0.9, x+y<1, 0≤z<0.08, and M is at least one of Al, Mg, Zr and Ti.
10. The ternary lithium-ion battery according to claim 8, characterized in that: The active material of the negative electrode includes at least one of a carbon-based negative electrode, a silicon-based negative electrode, a tin-based negative electrode and a lithium negative electrode.
Citation Information
Cited By
Electrolyte and alkali metal ion secondary battery
CN119864506A
An electrolyte and an alkali metal ion secondary battery
CN119864506B