Phase regulation and control method for mixed co-heating roasting of waste ternary lithium battery and lithium iron phosphate positive electrode material
Through the co-heat roasting method of waste ternary lithium batteries and lithium iron phosphate batteries, the self-oxidation reduction reaction is used to solve the problem of recycling valuable metals in the existing technology, and efficient and green metal recycling is achieved, and the process flow is simplified. Improves metal purity.
Patent Information
- Application Number
- CN202411173259.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-12-03
AI Technical Summary
The prior art is difficult to efficiently and greenly recover valuable metals from the positive electrode materials mixed with waste ternary lithium batteries and lithium iron phosphate batteries. The energy consumption of pyrometallurgy is high and toxic gases are generated. The hydrometallurgy process is complex and may cause secondary pollution. .
Co-heating roasting method of waste ternary lithium batteries and lithium iron phosphate batteries is adopted, and the co-heating roasting of lithium iron phosphate batteries is carried out in a constant temperature and constant pressure under a nitrogen atmosphere after full discharge, disassembly, preheating treatment, crushing and screening, and co-heating roasting is carried out in a nitrogen atmosphere. The reduction of iron ions is carried out in a self-oxidation reduction reaction with the oxidation of high-valent transition metals in ternary lithium batteries, achieving efficient recovery of valuable metals.
It realizes efficient and green recycling of valuable metals, simplifies the process flow, avoids the use of added agents, meets the production and processing needs, and improves the purity of metals.
Smart Images

Figure CN119069857A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of waste lithium-ion battery recycling, and in particular to a method for controlling the phase of a mixture of waste ternary lithium batteries and lithium iron phosphate positive electrode materials co-heated and roasted. Background Art
[0002] In recent years, with the country's vigorous promotion of the "dual carbon" goal and the vigorous development of new energy industries represented by electric vehicles in China, the production and sales of lithium-ion batteries in China have experienced rapid explosive growth. Among them, ternary lithium batteries and lithium iron phosphate batteries have the largest installed capacity, accounting for about 90% of the total market. Due to process requirements, a large amount of reductants and oxidants are usually required to participate in the reaction during the recycling process. Therefore, how to utilize the properties of the electrode materials themselves and extract valuable metals from the electrode materials in a targeted manner with little or no introduction of external agents has become the main research direction today.
[0003] The methods for recycling positive electrode materials of ternary lithium batteries mainly include pyrometallurgy and hydrometallurgy. However, pyrometallurgy recovers metals through high-temperature reduction or salt-assisted roasting, which has the advantages of simple process and large processing volume, but also has the problems of high energy consumption and possible production of toxic gases; hydrometallurgy uses chemical solutions to leach metals from batteries, and separates and purifies them through solvent extraction, chemical precipitation, ion exchange and other steps. It has the advantages of low energy consumption and high material purity, but the process is complicated and may produce secondary pollution. At present, there are no reports on how to recover valuable metals from the mixed positive electrode materials of waste ternary lithium batteries and lithium iron phosphate batteries.
[0004] Therefore, it is urgent to develop a phase control process for co-firing ternary lithium batteries and lithium iron phosphate positive electrode materials, so as to achieve efficient and green recovery of valuable metals. Summary of the invention
[0005] Based on the above problems, the present invention provides a phase control method for mixed co-heat roasting of waste ternary lithium batteries and lithium iron phosphate positive electrode materials.
[0006] A phase control method for mixed co-heat roasting of waste ternary lithium batteries and lithium iron phosphate positive electrode materials, comprising the following steps:
[0007] S1: Fully discharge the used ternary lithium battery and lithium iron phosphate battery;
[0008] S2: Dismantle the used ternary lithium batteries and lithium iron phosphate batteries after they are fully discharged;
[0009] S3: Take out the disassembled positive electrode sheets respectively and cut them into pieces;
[0010] S4: preheating the shredded positive electrode sheets of the ternary lithium battery and the positive electrode sheets of the lithium iron phosphate battery respectively;
[0011] S5: further crushing and screening the positive electrode powder of the ternary lithium battery and the positive electrode powder of the lithium iron phosphate battery after the preheating treatment;
[0012] S6: Evenly mix the sieved positive electrode powder of the ternary lithium battery and the positive electrode powder of the lithium iron phosphate battery according to different molar ratios;
[0013] S7: The uniformly mixed positive electrode powder is subjected to a constant temperature and pressure co-heating calcination treatment under a nitrogen atmosphere to obtain a co-heating calcination product containing lithium and a high-valent transition metal after redox.
[0014] In one embodiment, in step S3, the size of the cut positive electrode sheet is 1 to 9 cm 2 .
[0015] In one embodiment, the preheating treatment is to preheat the shredded ternary lithium battery positive electrode sheets and lithium iron phosphate battery positive electrode sheets in an oxygen-free atmosphere, and the preheating treatment includes a heating rate of 10°C / min, a treatment temperature of 500°C, and a treatment pressure of normal pressure.
[0016] In one of the embodiments, in step S5, a sieve is used to sieve the positive electrode powder of the ternary lithium battery and the positive electrode powder of the lithium iron phosphate battery after the preheating treatment, and the aperture of the sieve is 200 meshes.
[0017] In one of the embodiments, in step S6, the molar ratio of the ternary material to lithium iron phosphate is 1:1 to 1:3.
[0018] In one embodiment, in step S7, the co-calcination temperature increase rate is 10°C / min.
[0019] In one embodiment, in step S7, the inert gas during the constant temperature and pressure treatment is nitrogen, the flow rate is 250 mL / min, and the gas pressure is normal pressure.
[0020] In one embodiment, in step S7, the constant temperature and constant pressure treatment time is 30 to 150 minutes.
[0021] In one embodiment, in step S7, the temperature of the constant temperature and constant pressure treatment is 500-700°C.
[0022] The above-mentioned phase control method for mixed co-thermal roasting of waste ternary lithium batteries and lithium iron phosphate positive electrode materials utilizes the reducibility of ferrous ions in lithium iron phosphate and the oxidizability of high-valent transition metals in ternary lithium batteries to act as reductants and oxidants for self-oxidation-reduction reactions. The process is simple and the reduction roasting efficiency is high. It also realizes the efficient recovery of valuable metals from waste mixed lithium-ion battery electrode materials, and can meet the needs of production and processing. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a schematic diagram of the technical process of the present invention;
[0024] Figure 2 This is the XRD pattern of the co-calcined product in Example 1;
[0025] Figure 3 This is the XPS graph of Fe element in the co-calcined product in Example 1;
[0026] Figure 4 This is the XPS graph of Ni element in the co-calcined product in Example 1;
[0027] Figure 5 This is the XPS graph of the Co element in the co-calcined product in Example 1;
[0028] Figure 6 This is the XPS graph of the Mn element in the co-calcined product of Example 1. DETAILED DESCRIPTION
[0029] In order to make the above-mentioned purpose, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below.
[0030] As used herein, the term "prepared from" is synonymous with "comprising." As used herein, the terms "comprising," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.
[0031] When amount, concentration or other value or parameter is expressed as range, preferred range or a series of upper preferred value and lower preferred value limit range, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value and any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when disclosing range "1 to 5", described range should be interpreted as including range "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5" etc. When numerical range is described in this article, unless otherwise stated, the range is intended to include its end value and all integers and fractions within the range.
[0032] In addition, the indefinite articles "a" and "an" before the elements or components of the present invention have no restrictions on the quantity requirements (i.e. the number of occurrences) of the elements or components. Therefore, "a" or "an" should be interpreted as including one or at least one, and the elements or components in the singular form also include the plural form, unless the number is obviously intended to be in the singular form.
[0033] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0034] like Figure 1 As shown, the present invention provides a method for controlling the phases of co-baking waste ternary lithium batteries and lithium iron phosphate positive electrode materials. The present invention completely discharges the waste ternary lithium batteries and lithium iron phosphate batteries, disassembles and crushes them for pre-anaerobic heat treatment, crushes and screens them, and evenly mixes them to obtain waste lithium-ion battery electrode powder, which is then co-battered at normal pressure under anaerobic conditions.
[0035] Through the regulation of the co-thermal roasting process, the ferrous iron, nickel, cobalt, manganese, etc. in the mixed electrode powder are used as the only reactants. Under high-temperature nitrogen atmosphere conditions, the Fe2+ contained in the lithium iron phosphate is used to undergo an oxidation-reduction reaction with the Ni3+, Co3+, and Mn4+ in the ternary lithium battery to generate Fe3+ and Ni2+, Co2+, Mn2+ as well as elemental Ni and Co.
[0036] In a high-temperature oxygen-free environment, when the ternary lithium battery particles come into contact with the lithium iron phosphate particles, the Li+ in the ternary lithium battery particles increases its own disorder (entropy) due to the influence of thermodynamics, that is, Li+ diffuses and migrates between the two along the pores inside the two. When Li+ migrates from the hexagonally close-packed ternary lithium battery particles to the olivine-structured lithium iron phosphate particles, the lithium iron phosphate is transformed into a highly lithium-rich state, causing its lattice structure to collapse, and eventually causing part of the Fe2+ to be exposed or even escape from the olivine structure. When Fe2+ comes into contact with the surface of the ternary lithium battery particles, due to the reducing property of Fe2+, the high-valent nickel-cobalt-manganese oxide on the surface of the ternary lithium material is reduced to a low-valent nickel-cobalt-manganese oxide and part of the nickel-cobalt element due to the reduction property of Fe2+. At this time, because the reaction destroys the hexagonally close-packed ternary lithium crystal structure, it causes lamellar exfoliation, exposing more Li+ inside the crystal. The high temperature allows more Li+ to enter the lithium iron phosphate crystals, turning them into a lithium-rich state, which then causes structural collapse, resulting in a chain reaction - the ternary lithium battery and lithium iron phosphate powder undergo a self-oxidation-reduction reaction.
[0037] A phase control method for mixed co-heat roasting of waste ternary lithium batteries and lithium iron phosphate positive electrode materials, comprising the following steps:
[0038] S1: Fully discharge the used ternary lithium battery and lithium iron phosphate battery;
[0039] S2: Dismantle the used ternary lithium batteries and lithium iron phosphate batteries after they are fully discharged;
[0040] S3: Take out the disassembled positive electrode sheets and cut them into pieces; the size of the cut positive electrode sheets is 1 to 9 cm 2 .
[0041] S4: Preheating the shredded ternary lithium battery positive electrode sheets and lithium iron phosphate battery positive electrode sheets respectively; the preheating treatment is carried out in an oxygen-free atmosphere, and the preheating treatment includes a heating rate of 10°C / min, a treatment temperature of 500°C, and a treatment pressure of normal pressure.
[0042] S5: further crushing and sieving the preheated ternary lithium battery positive electrode powder and the lithium iron phosphate battery positive electrode powder; the aperture of the sieve is 200 meshes.
[0043] S6: Evenly mix the sieved positive electrode powder of the ternary lithium battery and the positive electrode powder of the lithium iron phosphate battery in a molar ratio of 1:1 to 1:3;
[0044] S7: The mixed positive electrode powder is subjected to constant temperature and constant pressure co-heating roasting treatment in a nitrogen atmosphere to obtain a co-heating roasting product containing lithium and high-valent transition metal after redox. The co-heating rate is 10°C / min; the inert gas during the constant temperature and constant pressure treatment is nitrogen, the flow rate is 250mL / min, and the gas pressure is normal pressure; the time of the constant temperature and constant pressure treatment is 30 to 150 minutes; the temperature of the constant temperature and constant pressure treatment is 500 to 700°C.
[0045] By utilizing the self-oxidation-reduction reaction between ternary lithium battery and lithium iron phosphate powder, the mixed powder material itself is used to achieve efficient in-situ thermal reduction and oxidation, thereby effectively separating the valuable metal elements. The waste ternary lithium battery and lithium iron phosphate positive electrode material are co-thermally roasted.
[0046] In the co-calcination products, lithium, iron, nickel, cobalt and manganese elements exist in the form of Li3PO4, Fe3O4, NiO, Ni, CoO, Co and MnO, respectively.
[0047] It should be noted that during the co-heat roasting process of the mixed materials, the Fe2+ in the lithium iron phosphate crystals is completely relied on to reduce the high-valent Ni3+, Co3+, and Mn4+ in the ternary lithium battery using its own high reducibility. The conventional thermal reduction process can only process a single electrode material, and a considerable amount of reducing agent needs to be introduced from the outside to participate in the reaction. The present invention enhances the diffusion and migration behavior of Li+ in the lithium battery electrode material powder through a process thermal regulation process, so that the ternary material and the lithium iron phosphate material crystals are alternately transformed between the lithium-rich state and the lithium-poor state, thereby causing the crystal structure of the two to collapse, and the Fe2+ exposed in the lithium iron phosphate crystals is used to reduce the Ni3+, Co3+, and Mn4+ in the ternary lithium battery to obtain Ni2+, Co2+, Mn2+ and Ni, Co single substance mixed products. The obtained electrode material co-heat roasting product can be obtained by leaching and evaporation to obtain an industrial-grade metal salt product.
[0048] Example 1
[0049] A phase control method for mixed co-heat roasting of waste ternary lithium batteries and lithium iron phosphate positive electrode materials, comprising the following steps:
[0050] S1: Fully discharge the used ternary lithium battery and lithium iron phosphate battery;
[0051] S2: Dismantle the used ternary lithium batteries and lithium iron phosphate batteries after they are fully discharged;
[0052] S3: Take out the disassembled positive electrode sheets and cut them into pieces; the size of the cut positive electrode sheets is 1 to 9 cm 2 .
[0053] S4: preheating the shredded positive electrode sheet of the lithium iron phosphate battery; the preheating is performed in an oxygen-free atmosphere, the heating rate of the preheating is 10°C / min, the treatment temperature is 500°C, and the treatment pressure is normal pressure;
[0054] Similarly, the used ternary lithium batteries are completely discharged, and then the positive electrode sheets are manually separated and cut into pieces of 1 to 9 cm2 and preheated in an oxygen atmosphere.
[0055] S5: further crushing and sieving the preheated ternary lithium battery positive electrode powder and the lithium iron phosphate battery positive electrode powder; the aperture of the sieve is 200 meshes.
[0056] S6: Evenly mix the sieved positive electrode powder of the ternary lithium battery and the positive electrode powder of the lithium iron phosphate battery in a molar ratio of 1:1.5;
[0057] S7: The mixed positive electrode powder is subjected to a constant temperature and constant pressure co-heating roasting treatment in a nitrogen atmosphere to obtain a co-heating roasting product containing lithium and a high-valent transition metal after redox; the co-heating rate is 10°C / min; the inert gas during the constant temperature and constant pressure treatment is nitrogen, the flow rate is 250mL / min, and the gas pressure is normal pressure; the constant temperature and constant pressure treatment time is 90min; the constant temperature and constant pressure treatment temperature is 600°C;
[0058] In the co-calcination products, lithium, iron, nickel, cobalt and manganese elements exist in the form of Li3PO4, Fe3O4, NiO, Ni, CoO, Co and MnO, respectively.
[0059] Example 2
[0060] A phase control method for mixed co-heat roasting of waste ternary lithium batteries and lithium iron phosphate positive electrode materials, comprising the following steps:
[0061] S1: Fully discharge the used ternary lithium battery and lithium iron phosphate battery;
[0062] S2: Dismantle the used ternary lithium batteries and lithium iron phosphate batteries after they are fully discharged;
[0063] S3: Take out the disassembled positive electrode sheets and cut them into pieces; the size of the cut positive electrode sheets is 1 to 9 cm 2 .
[0064] S4: preheating the shredded lithium iron phosphate battery positive electrode sheet; the preheating treatment is performed in a nitrogen atmosphere, the preheating rate is 10°C / min, the treatment temperature is 500°C, and the treatment pressure is normal pressure;
[0065] Similarly, the used ternary lithium battery is completely discharged, and then the positive electrode sheet is manually separated and cut into pieces of 1 to 9 cm2 and preheated in an air atmosphere.
[0066] S5: further crushing and sieving the preheated ternary lithium battery positive electrode powder and the lithium iron phosphate battery positive electrode powder; the aperture of the sieve is 200 meshes.
[0067] S6: Evenly mix the sieved positive electrode powder of the ternary lithium battery and the positive electrode powder of the lithium iron phosphate battery in a molar ratio of 1:1.2;
[0068] S7: The mixed positive electrode powder is subjected to a constant temperature and constant pressure co-heating roasting treatment in a nitrogen atmosphere to obtain a co-heating roasting product containing lithium and a high-valent transition metal after redox; the co-heating rate is 10°C / min; the inert gas during the constant temperature and constant pressure treatment is nitrogen, the flow rate is 250mL / min, and the gas pressure is normal pressure; the constant temperature and constant pressure treatment time is 120min; the constant temperature and constant pressure treatment temperature is 500°C;
[0069] In the co-calcination products, lithium, iron, nickel, cobalt and manganese elements exist in the form of Li3PO4, Fe3O4, NiO, Ni, CoO, Co and MnO, respectively.
[0070] Example 3
[0071] A phase control method for mixed co-heat roasting of waste ternary lithium batteries and lithium iron phosphate positive electrode materials, comprising the following steps:
[0072] S1: Fully discharge the used ternary lithium battery and lithium iron phosphate battery;
[0073] S2: Dismantle the used ternary lithium batteries and lithium iron phosphate batteries after they are fully discharged;
[0074] S3: Take out the disassembled positive electrode sheets and cut them into pieces; the size of the cut positive electrode sheets is 1 to 9 cm 2 .
[0075] S4: preheating the shredded lithium iron phosphate battery positive electrode sheet; the preheating treatment is performed in a nitrogen atmosphere, the preheating rate is 10°C / min, the treatment temperature is 500°C, and the treatment pressure is normal pressure;
[0076] Similarly, the used ternary lithium batteries were completely discharged, and then the positive electrode sheets were manually separated and cut into pieces of 1 to 9 cm2 and preheated in an air atmosphere.
[0077] S5: further crushing and sieving the preheated ternary lithium battery positive electrode powder and the lithium iron phosphate battery positive electrode powder; the aperture of the sieve is 200 meshes.
[0078] S6: Evenly mix the sieved positive electrode powder of the ternary lithium battery and the positive electrode powder of the lithium iron phosphate battery in a molar ratio of 1:2.2;
[0079] S7: The mixed positive electrode powder is subjected to a constant temperature and constant pressure co-heating roasting treatment in a nitrogen atmosphere to obtain a co-heating roasting product containing lithium and a high-valent transition metal after redox; the co-heating rate is 10°C / min; the inert gas during the constant temperature and constant pressure treatment is nitrogen, the flow rate is 250mL / min, and the gas pressure is normal pressure; the constant temperature and constant pressure treatment time is 60min; the constant temperature and constant pressure treatment temperature is 700°C;
[0080] In the co-calcined product, lithium, iron, nickel, cobalt and manganese elements exist in the form of Li3PO4, Fe3O4, NiO, Ni, CoO, Co and MnO, respectively.
[0081] The above-mentioned phase control method for mixed co-thermal roasting of waste ternary lithium batteries and lithium iron phosphate positive electrode materials utilizes the reducibility of ferrous ions in lithium iron phosphate and the oxidizability of high-valent transition metals in ternary lithium batteries to act as reductants and oxidants for self-oxidation-reduction reactions, laying the foundation for achieving efficient and green recycling of multiple metals. The method is simple and can meet the needs of production and processing.
[0082] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0083] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A phase control method for mixed co-heat roasting of waste ternary lithium batteries and lithium iron phosphate positive electrode materials, characterized in that: The following steps are involved: S1: Fully discharge the used ternary lithium battery and lithium iron phosphate battery; S2: Dismantle the used ternary lithium batteries and lithium iron phosphate batteries after they are fully discharged; S3: Take out the disassembled positive electrode sheets respectively and cut them into pieces; S4: preheating the shredded positive electrode sheets of the ternary lithium battery and the positive electrode sheets of the lithium iron phosphate battery respectively; S5: further crushing and screening the positive electrode powder of the ternary lithium battery and the positive electrode powder of the lithium iron phosphate battery after the preheating treatment; S6: Evenly mix the sieved positive electrode powder of the ternary lithium battery and the positive electrode powder of the lithium iron phosphate battery according to different molar ratios; S7: The uniformly mixed positive electrode powder is subjected to a constant temperature and pressure co-heating calcination treatment under a nitrogen atmosphere to obtain a co-heating calcination product containing lithium and a high-valent transition metal after redox.
2. The phase control method for mixed co-heat roasting of waste ternary lithium batteries and lithium iron phosphate positive electrode materials according to claim 1, characterized in that: In step S3, the size of the cut positive electrode sheet is 1 to 9 cm 2 .
3. The phase control method for mixed co-heat roasting of waste ternary lithium batteries and lithium iron phosphate positive electrode materials according to claim 1, characterized in that: In step S4, the preheating treatment is to heat treat the shredded ternary lithium battery positive electrode sheets and lithium iron phosphate battery positive electrode sheets in an oxygen-free atmosphere, and the preheating treatment includes a heating rate of 10°C / min, a treatment temperature of 500°C, and a treatment pressure of normal pressure.
4. The phase control method for mixed co-heat roasting of waste ternary lithium batteries and lithium iron phosphate positive electrode materials according to claim 1, characterized in that: In step S5, the ternary lithium battery positive electrode powder and the lithium iron phosphate battery positive electrode powder after the preheating treatment are screened respectively using a sieve, and the aperture of the sieve is 200 meshes.
5. The phase control method for mixed co-heat roasting of waste ternary lithium batteries and lithium iron phosphate positive electrode materials according to claim 1, characterized in that: In step S6, the molar ratio of the ternary material to lithium iron phosphate is 1:1 to 1:
3.
6. The phase control method for mixed co-heat roasting of waste ternary lithium batteries and lithium iron phosphate positive electrode materials according to claim 1, characterized in that: In step S7, the co-calcination temperature rise rate is 10°C / min.
7. The phase control method for mixed co-heat roasting of waste ternary lithium batteries and lithium iron phosphate positive electrode materials according to claim 1, characterized in that: In step S7, the inert gas during the constant temperature and constant pressure treatment is nitrogen, the flow rate is 250 mL / min, and the gas pressure is normal pressure.
8. The phase control method for mixed co-heat roasting of waste ternary lithium batteries and lithium iron phosphate positive electrode materials according to claim 1, characterized in that: In step S7, the constant temperature and constant pressure treatment time is 30 to 150 minutes.
9. The phase control method for mixed co-heat roasting of waste ternary lithium batteries and lithium iron phosphate positive electrode materials according to claim 1, characterized in that: In step S7, the temperature of the constant temperature and constant pressure treatment is 500-700°C.