Sealing assembly and sealing method of alkali metal ion battery

By using metal plating and sealing glass with low softening temperature and high thermal expansion coefficient in the sealing assembly of alkali metal ion batteries, the problem of cracks caused by the difference in aging, fragility, corrosion and thermal expansion in the prior art is solved, and the problem of cracks caused by differences in aging, fragility, corrosion and thermal expansion is improved. Battery sealing and energy density.

CN119069905APending Publication Date: 2024-12-03CAMEL GRP WUHAN OPTICS VALLEY R&D CENT CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411258237.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing alkali metal ion battery sealing technology has problems such as aging failure, fragility and corrosion, and cracks, especially due to insufficient sealing and stability caused by poor thermal expansion coefficient of the material.

Method used

Design a sealing assembly for alkali metal ion batteries, using metal plating to cover the top cover and pole columns, and sealing glass with low softening temperature and high thermal expansion coefficient is added therebetween, so as to reduce the difference in thermal expansion coefficient through the transition of metal plating and improve sealing performance and corrosion resistance while reducing battery cover pack thickness and mass.

Benefits of technology

It improves the corrosion resistance and sealing of the battery, reduces the crack problems caused by thermal expansion differences, and improves product yield and energy density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069905A_ABST
    Figure CN119069905A_ABST
Patent Text Reader

Abstract

The invention discloses a sealing assembly and a sealing method of an alkali metal ion battery. The sealing assembly of the alkali metal ion battery comprises a top cover, a pole, sealing glass and a metal coating, wherein the top cover is provided with a through hole; the pole penetrates through the through hole; the sealing glass is positioned between the top cover and the pole; the metal coating is plated on the surface of the top cover and located between the top cover and the sealing glass, and / or plated on the surface of the pole and located between the pole and the sealing glass; the thermal expansion coefficient of the metal coating is smaller than that of the top cover and that of the pole and larger than that of the sealing glass. According to the embodiment of the invention, the sealing glass is designed to play a sealing role and an insulating role, so that the corrosion resistance and the sealing performance are improved, the thickness and the mass of the cover group are reduced, the internal space of the battery is favorably improved, and the energy density of the alkali metal ion battery is improved. And the metal coating is arranged, so that the difference of thermal expansion coefficients between two adjacent structures is reduced, defects such as cracks are avoided, and the product yield and the product quality are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of batteries, and in particular to a sealing component and a sealing method for an alkali metal ion battery. Background Art

[0002] Currently, the sealing of the pole and the top cover of the existing alkali metal ion battery mostly adopts the traditional plastic sealing technology, but plastic parts are easily corroded and aged. At the same time, the thermal expansion coefficient of most plastics is much higher than that of the metal materials used for the top cover and the pole, and it is easy to cause deformation due to temperature changes or alternating stress during vibration, and its sealing is difficult to ensure.

[0003] In recent years, some alkali metal ion batteries have been sealed with ceramic metallization, but this process is complicated, and the corrosion resistance of metallization materials is poor, and ceramics are fragile. At the same time, welding between metal and ceramic involves the use of brazing materials, which easily leads to the appearance of multi-layer interfaces between the two. Therefore, the application of alkali metal ion batteries sealed with ceramic metallization has many technical difficulties such as material optimization, active brazing material development, brazing process and component design. In addition, there is metal-glass sealing technology, in which glass and metal surfaces can form chemical bonds, and its airtightness is better than the physical seal of plastic sealing. At the same time, it has low cost and excellent electrical insulation. However, in the glass sealing technology of alkali metal ion batteries, the key is that the difference in thermal expansion coefficient between the sealing glass and the metal shell cover and metal pole is too high, which will generate stress during the cooling process and cause glass cracks. Research on this technical difficulty focuses on the research of low softening temperature and high expansion coefficient glass powder, but it has not solved the key technical difficulties of the above-mentioned alkali metal ion battery glass sealing.

[0004] In summary, the existing sealing method between the top cover and the pole has technical problems such as easy aging and failure, easy brittleness and corrosion, and easy cracking. Summary of the invention

[0005] The purpose of this application is to overcome the above-mentioned technical deficiencies, propose a sealing component and sealing method for alkali metal ion batteries, and solve the technical problems of easy aging failure, easy brittleness and corrosion, and easy cracking in the prior art.

[0006] In order to achieve the above technical objectives, this application adopts the following technical solutions: In a first aspect, the present application provides a sealing assembly for an alkali metal ion battery, comprising a top cover, a pole, a sealing glass, and a metal coating: A top cover, wherein the top cover has a through hole; A pole, the pole passing through the through hole; Sealing glass, the sealing glass is located between the top cover and the pole; and A metal coating, wherein the metal coating is located between the top cover and the sealing glass and / or between the pole and the sealing glass, and the thermal expansion coefficient of the metal coating is greater than the thermal expansion coefficient of the sealing glass.

[0007] In some embodiments of the present application, the pole includes an upper cylinder and a lower cylinder, the upper cylinder is coaxially connected to the lower cylinder, the diameter of the lower cylinder is larger than the inner diameter of the through hole, the diameter of the upper cylinder is smaller than the inner diameter of the through hole, and the upper cylinder passes through the through hole.

[0008] In some embodiments of the present application, the metal coating covers the outer side wall of the upper column and the upper surface of the lower column, and the pole is in contact with the sealing glass through the metal coating.

[0009] In some embodiments of the present application, the material of the pole includes copper, aluminum or aluminum alloy, and the thermal expansion coefficient of the pole is greater than the thermal expansion coefficient of the metal coating.

[0010] In some embodiments of the present application, the metal coating covers a portion of the lower surface of the top cover and the inner side wall of the through hole, and the top cover is in contact with the sealing glass through the metal coating.

[0011] In some embodiments of the present application, the material of the top cover includes aluminum or aluminum alloy, and the thermal expansion coefficient of the top cover is greater than the thermal expansion coefficient of the metal coating.

[0012] In some embodiments of the present application, the material of the metal coating includes nickel, nickel alloy, chromium-iron alloy or titanium alloy, and the thermal expansion coefficient of the metal coating is not greater than 120% of the thermal expansion coefficient of the sealing glass.

[0013] In some embodiments of the present application, the thickness of the metal coating is not less than 50 μm.

[0014] In some embodiments of the present application, the top cover further has a liquid injection hole and an explosion-proof valve, the through hole is located at the center of the top cover, and the liquid injection hole and the explosion-proof valve are located at the edge of the top cover.

[0015] In a second aspect, the present application further provides a sealing method for an alkali metal ion battery, which is used to obtain a sealing assembly for an alkali metal ion battery as described in any one of the embodiments in the first aspect, comprising the following steps: Plating a metal coating on the lower surface and the inner side wall of the top cover, and / or plating the metal coating on the outer side wall and the upper surface of the pole; Sequentially mount the sealing glass and the top cover on the outer side of the pole; The top cover, the sealing glass and the top cover are placed in a sealing mold, filled with a protective atmosphere, and heated and sealed.

[0016] Compared with the prior art, the technical solution provided by this application has the following beneficial technical effects: The embodiment of the present application designs sealing glass between the metal top cover and the pole of the alkali metal ion battery, which plays a sealing role and an insulating role at the same time, improves corrosion resistance and sealing, reduces the thickness and mass of the cover group, and is conducive to increasing the internal space of the battery and improving the energy density of the alkali metal ion battery. At the same time, a metal coating is set on the contact surface between the top cover and the sealing glass, and the contact surface between the pole and the sealing glass. The difference in thermal expansion coefficient between the two adjacent structures is reduced through the transition of the metal coating, avoiding the large difference in thermal expansion coefficient between the shell cover metal and the sealing glass, resulting in cracks and other defects, thereby improving the product yield and product quality. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the technical solution in this application, the following is a brief introduction to the drawings required for use in the embodiments: Figure 1 It is a structural schematic diagram of a sealing assembly of an alkali metal ion battery provided in an embodiment of the present application; Figure 2 is a top view of a sealing assembly of an alkali metal ion battery provided in an embodiment of the present application; Figure 3 This is a disassembly schematic diagram of a sealing assembly of an alkali metal ion battery provided in an embodiment of the present application; Figure 4 It is an enlarged schematic diagram of a sealing component of an alkali metal ion battery provided in an embodiment of the present application.

[0018] Reference numerals: 1-top cover, 2-pole, 3-sealing glass, 4-metal coating, 5-liquid injection hole, 6-explosion-proof valve; 11-through hole, 21-upper column, 22-lower column. DETAILED DESCRIPTION

[0019] In order to make the purpose, technical solution and advantages of the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0020] Those skilled in the art will appreciate that in this specification, the wording "including" is an open-ended expression, which means that the described features exist but does not exclude other features. The directional words "up", "down", "left", "right", etc. are exemplary directions based on the drawings. Features defined as "first" and "second" implicitly include one or more of the features. Singular expressions can also be used in the plural. "Multiple" means two or more. The terms "installed", "connected", and "connected" can be fixed connections, detachable connections, or integrated connections; they can be directly connected, or indirectly connected through an intermediate medium, or they can be internal connections between two elements. In addition, "connected" can include wireless connections.

[0021] The purpose of this application is to overcome the above-mentioned technical deficiencies, propose a sealing component and sealing method for alkali metal ion batteries, and solve the technical problems of easy aging failure, easy brittleness and corrosion, and easy cracking in the prior art.

[0022] In order to achieve the above technical objectives, this application adopts the following technical solutions: In a first aspect, the present application provides a sealing assembly for an alkali metal ion battery, such as Figure 1 and Figure 2 As shown, Figure 1 It is a structural schematic diagram of a sealing assembly of an alkali metal ion battery provided in an embodiment of the present application; Figure 2 It is a top view of a sealing assembly of an alkali metal ion battery provided in an embodiment of the present application.

[0023] A sealing assembly for an alkali metal ion battery, comprising a top cover 1, a pole 2, a sealing glass 3 and a metal coating 4: A top cover 1, wherein the top cover 1 has a through hole 11; A pole 2, wherein the pole 2 passes through the through hole 11; Sealing glass 3, the sealing glass 3 is located between the top cover 1 and the pole 2; and The metal coating 4 is located between the top cover 1 and the sealing glass 3 and / or between the pole 2 and the sealing glass 3 , and the thermal expansion coefficient of the metal coating 4 is greater than the thermal expansion coefficient of the sealing glass 3 .

[0024] The embodiment of the present application designs a sealing glass 3 between the metal top cover 1 and the pole 2 of the alkali metal ion battery, which plays a sealing role and an insulating role at the same time, improves the corrosion resistance and sealing performance, reduces the thickness and mass of the cover group, and is conducive to increasing the internal space of the battery and improving the energy density of the alkali metal ion battery. At the same time, a metal coating 4 is set on the contact surface between the top cover 1 and the sealing glass 3, and the contact surface between the pole 2 and the sealing glass 3. The difference in thermal expansion coefficient between the two adjacent structures is reduced by the transition of the metal coating 4, avoiding the large difference in thermal expansion coefficient between the shell cover metal and the sealing glass 3, resulting in cracks and other defects, thereby improving the product yield and product quality.

[0025] This embodiment is applicable to alkali metal ion batteries and other batteries. Alkali metal ion batteries include lithium ion batteries, sodium ion batteries, potassium ion batteries, etc.

[0026] In the drawings of the present application, a cylindrical battery is taken as an example, but in fact it can also be applied to square aluminum shell batteries and batteries of other shapes.

[0027] like Figure 3 and Figure 4 As shown, Figure 3 This is a disassembly schematic diagram of a sealing assembly of an alkali metal ion battery provided in an embodiment of the present application; Figure 4 It is an enlarged schematic diagram of a sealing component of an alkali metal ion battery provided in an embodiment of the present application.

[0028] In some embodiments of the present application, the pole 2 includes an upper cylinder 21 and a lower cylinder 22, the upper cylinder 21 is coaxially connected to the lower cylinder 22, the diameter of the lower cylinder 22 is larger than the inner diameter of the through hole 11, the diameter of the upper cylinder 21 is smaller than the inner diameter of the through hole 11, and the upper cylinder 21 passes through the through hole 11.

[0029] In some embodiments of the present application, the metal coating 4 covers the outer wall of the upper column 21 and the upper surface of the lower column 22 , and the pole 2 is in contact with the sealing glass 3 through the metal coating 4 .

[0030] In some embodiments of the present application, the material of the pole 2 includes copper, aluminum or aluminum alloy, and the thermal expansion coefficient of the pole 2 is greater than the thermal expansion coefficient of the metal coating 4 .

[0031] In this embodiment, the pole 2 and the top cover 1 are connected by a sealing glass 3. The pole 2 is made of aluminum / aluminum alloy or copper, and consists of two sections of columns. The cross-section is in an "inverted T" shape. The diameter of the lower column 22 is greater than that of the upper column by more than 212 mm, which can facilitate the welding of the surface of the lower column 22 and the pole ear.

[0032] The sealing glass 33 is lead-free phosphate glass with low softening temperature and high thermal expansion coefficient, and plays the role of insulation and sealing.

[0033] This method abandons traditional plastic parts and uses sealing glass 3 for sealing, which improves the corrosion resistance and sealing of the structure; at the same time, it eliminates some metal components in the traditional sealing structure, reduces the mass and thickness, and is beneficial to improving the internal space utilization of the battery and thus improving the battery energy density.

[0034] In some embodiments of the present application, the metal coating 4 covers a portion of the lower surface of the top cover 1 and the inner side wall of the through hole 11 , and the top cover 1 is in contact with the sealing glass 3 through the metal coating 4 .

[0035] In some embodiments of the present application, the material of the top cover 1 includes aluminum or aluminum alloy, and the thermal expansion coefficient of the top cover 1 is greater than the thermal expansion coefficient of the metal coating 4 .

[0036] In this embodiment, the top cover 1 is made of aluminum / aluminum alloy, and is provided with a liquid injection hole 5 and an explosion-proof valve 6. The outer wall of the upper cylinder 21 and the upper surface of the lower cylinder 22 in the pole 2 are designed with a metal coating 4, and the inner wall and the lower surface of the top cover 1 are also designed with a metal coating 4. The radius of the metal coating 4 on the lower surface of the top cover 1 is equal to the radius of the lower cylinder 22 in the pole 2, that is, the metal coating 4 on the surface of the top cover 1 in this direction completely overlaps with the metal coating 4 on the surface of the pole 2.

[0037] In some embodiments of the present application, the material of the metal coating 4 includes nickel, nickel alloy, chromium-iron alloy or titanium alloy, and the thermal expansion coefficient of the metal coating 4 is not greater than 120% of the thermal expansion coefficient of the sealing glass 3 .

[0038] In some embodiments of the present application, the thickness of the metal coating layer 4 is not less than 50 μm.

[0039] In this embodiment, the metal coating 4 is made of nickel or nickel alloy, whose thermal expansion coefficient is lower than that of metal aluminum and copper, and the nickel plating process is mature and simple. The coating thickness is greater than 50 μm, and its thermal expansion coefficient is within 20% of the thermal expansion coefficient of the sealing glass 3.

[0040] The metal coating 4 may be made of nickel alloy in the embodiment, or other metals or alloys that meet the thermal expansion coefficient requirement, and the thermal expansion coefficient is higher than the thermal expansion coefficient of the sealing glass 3 by less than 20%, such as chromium-iron alloy, titanium alloy, etc.

[0041] By selecting a suitable material, the difference in thermal expansion coefficient between the metal coating 4 and the sealing glass 3 can be small, and the difference in thermal expansion coefficient between the metal coating 4 and the top cover 1 and the difference in thermal expansion coefficient between the metal coating 4 and the pole 2 can also be small. When the difference in thermal expansion coefficient in the latter two cases is less than 20% of the thermal expansion coefficient of the metal coating 4, the metal coating 4 can play a good transition effect.

[0042]

[0043] Table 1 As shown in Table 1, the battery top cover 1 of the embodiment and the comparative example was tested for pressure insulation and sealing before and after high-temperature storage (40°C, 60 days). Comparative Example 1 is a battery cover group sealed by a traditional method using plastic parts, Comparative Example 2 is a glass-sealed battery cover group made without a metal coating 4, and the embodiment is a glass-sealed cover group designed with a metal coating 4 as described above. From Comparative Example 1, it can be seen that the use of traditional plastic parts for sealing has a mature process and good airtightness, but after high-temperature storage, the airtightness decreases rapidly due to plastic aging. From Comparative Example 2, it can be seen that the battery cover group sealed with glass has a small difference in airtightness after high-temperature storage, but the product yield is reduced due to the large difference in thermal expansion coefficients between the shell cover metal and the sealing glass. After the pole 21 and the cover plate 2 are designed with a metal coating 4, the product yield is significantly improved, and good airtightness is still shown after high-temperature storage. This design effectively solves the problem of cracks caused by the large difference in thermal expansion coefficients between the shell cover metal and the sealing glass, thereby reducing the product yield.

[0044] In some embodiments of the present application, the top cover 1 further has a liquid injection hole 5 and an explosion-proof valve 6 , the through hole 11 is located at the center of the top cover 1 , and the liquid injection hole 5 and the explosion-proof valve 6 are located at the edge of the top cover 1 .

[0045] In a second aspect, the present application further provides a sealing method for an alkali metal ion battery, which is used to obtain a sealing assembly for an alkali metal ion battery as described in any one of the embodiments in the first aspect, comprising the following steps: A metal coating 4 is plated on the lower surface and the inner side wall of the top cover 1, and / or, the metal coating 4 is plated on the outer side wall and the upper surface of the pole 2; The sealing glass 3 and the top cover 1 are sequentially mounted on the outer side of the pole 2; The top cover 1, the sealing glass 3 and the top cover 1 are placed in a sealing mold, filled with a protective atmosphere, and heated and sealed.

[0046] Compared with the prior art, the technical solution provided by this application has the following beneficial technical effects: The embodiment of the present application designs a sealing glass 3 between the metal top cover 1 and the pole 2 of the alkali metal ion battery, which plays a sealing role and an insulating role at the same time, improves the corrosion resistance and sealing performance, reduces the thickness and mass of the cover group, and is conducive to increasing the internal space of the battery and improving the energy density of the alkali metal ion battery. At the same time, a metal coating 4 is set on the contact surface between the top cover 1 and the sealing glass 3, and the contact surface between the pole 2 and the sealing glass 3. The difference in thermal expansion coefficient between the two adjacent structures is reduced by the transition of the metal coating 4, avoiding the large difference in thermal expansion coefficient between the shell cover metal and the sealing glass 3, resulting in cracks and other defects, thereby improving the product yield and product quality.

[0047] Those skilled in the art will appreciate that the various operations, methods, steps, measures, and schemes in the processes discussed in this application may be alternated, modified, rearranged, decomposed, combined, or deleted.

[0048] The specific implementation methods of the present application described above do not constitute a limitation on the protection scope of the present application. Any other corresponding changes and modifications made according to the technical concept of the present application should be included in the protection scope of the claims of the present application.

Claims

1. A sealing assembly for an alkali metal ion battery, characterized in that: include: A top cover, wherein the top cover has a through hole; A pole, the pole passing through the through hole; Sealing glass, the sealing glass is located between the top cover and the pole; as well as A metal coating, the metal coating is coated on the surface of the top cover and is located between the top cover and the sealing glass, and / or is coated on the surface of the pole and is located between the pole and the sealing glass; the thermal expansion coefficient of the metal coating is smaller than the thermal expansion coefficient of the top cover and the pole, and larger than the thermal expansion coefficient of the sealing glass.

2. The sealing assembly of an alkali metal ion battery according to claim 1, characterized in that: The pole comprises an upper cylinder and a lower cylinder, the upper cylinder is coaxially connected with the lower cylinder, the diameter of the lower cylinder is larger than the inner diameter of the through hole, the diameter of the upper cylinder is smaller than the inner diameter of the through hole, and the upper cylinder passes through the through hole.

3. The sealing assembly of an alkali metal ion battery according to claim 2, characterized in that: The metal coating covers the outer side wall of the upper column and the upper surface of the lower column, and the pole is in contact with the sealing glass through the metal coating.

4. The sealing assembly of an alkali metal ion battery according to claim 2, characterized in that: The material of the pole includes copper, aluminum or aluminum alloy.

5. The sealing assembly of an alkali metal ion battery according to claim 1, characterized in that: The metal plating layer covers a portion of the lower surface of the top cover and the inner side wall of the through hole, and the top cover is in contact with the sealing glass through the metal plating layer.

6. The sealing assembly of an alkali metal ion battery according to claim 5, characterized in that: The material of the top cover includes aluminum or aluminum alloy.

7. The sealing assembly of an alkali metal ion battery according to claim 1, characterized in that: The material of the metal coating includes nickel, nickel alloy, chromium-iron alloy or titanium alloy, and the thermal expansion coefficient of the metal coating is not greater than 120% of the thermal expansion coefficient of the sealing glass.

8. The sealing assembly of an alkali metal ion battery according to claim 7, characterized in that: The thickness of the metal coating is not less than 50 μm.

9. The sealing assembly of an alkali metal ion battery according to claim 1, characterized in that: The top cover also has a liquid injection hole and an explosion-proof valve. The through hole is located at the center of the top cover, and the liquid injection hole and the explosion-proof valve are located at the edge of the top cover.

10. A sealing method for an alkali metal ion battery, characterized in that: The method for obtaining the sealing assembly of the alkali metal ion battery according to any one of claims 1 to 9 comprises the following steps: Plating a metal coating on the lower surface and the inner wall of the top cover, and / or plating the metal coating on the outer wall and the upper surface of the pole; Sequentially mount the sealing glass and the top cover on the outer side of the pole; The top cover, the sealing glass and the top cover are placed in a sealing mold, filled with a protective atmosphere, and heated and sealed.