Lithium ion battery heat-resistant diaphragm and preparation method thereof
By applying melamine formaldehyde resin microspheres and functional additives on the lithium-ion battery separator, the problems of unstable thermal size of the lithium-ion battery separator and poor affinity are solved, and the high energy density and thermal safety of lithium-ion batteries are achieved Sex improvement.
Patent Information
- Application Number
- CN202411293341.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-12-03
AI Technical Summary
The existing lithium-ion battery separators have unstable thermal dimensions and poor electrolyte affinity under the demands of high energy density and high power output, which cannot meet the safety and energy density improvement of lithium batteries in the future development.
Polyolefin separators are used to combine with melamine formaldehyde resin microspheres and functional additives. By coating melamine formaldehyde resin microspheres on both sides of the polyolefin separators, the heat shrinkage rate is significantly reduced and the wettability of the electrolyte is improved, forming a high temperature resistant and lightweight Composite diaphragm.
It significantly reduces the heat shrinkage rate of the polyolefin separator, improves the thermal safety and energy density of the battery, reduces the weight, and improves the mass-specific energy density of the battery.
Smart Images

Figure CN119069945A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion battery diaphragms, and in particular to a heat-resistant diaphragm for lithium ion batteries and a preparation method thereof. Background Art
[0002] With the development of the times and technology, people's demand for consumer electronics, power batteries and energy storage equipment is increasing. Lithium-ion batteries are widely used because of their high energy density and long cycle life. The diaphragm is one of the core materials of lithium-ion batteries. Its main function is to separate the positive and negative electrodes of the battery. It is a thin film with a microporous structure while ensuring the passage of lithium ions. The performance of the diaphragm determines the interface structure and internal resistance of the battery, and affects the capacity and cycle of the battery.
[0003] At present, polyolefin separators such as polypropylene separators (PP) and polyethylene separators (PE) are mainly used commercially. However, due to their thermal dimensional instability and poor affinity for electrolytes, they cannot meet the needs of high energy density and high power output. The future development direction of lithium batteries is to improve safety and energy density. The current mainstream solution is to coat the separator base film. Among them, water-based ceramics are the most commonly used for high temperature resistance, but the ceramic coating has a high density, which is not conducive to improving the battery energy density.
[0004] Therefore, it is necessary to develop a heat-resistant separator for lithium-ion batteries to further improve the energy density of lithium-ion batteries. Summary of the invention
[0005] In view of this, the present application provides a lithium-ion battery heat-resistant diaphragm and a preparation method thereof, which are used to solve the problem of how to improve the energy density of lithium-ion batteries.
[0006] In order to achieve the above technical objectives, this application adopts the following technical solutions: In a first aspect, the present application provides a heat-resistant separator for a lithium-ion battery, comprising a polyolefin separator and melamine formaldehyde resin microspheres and functional additives coated on both sides of the polyolefin separator.
[0007] Preferably, the functional additive includes one or more of a dispersant, a wetting agent, and a binder.
[0008] Preferably, the preparation method of melamine formaldehyde resin microspheres comprises the following steps: S1. adding melamine powder to a formaldehyde solution, heating for reaction, and obtaining a prepolymer methylol melamine solution; S2. adding an acidic catalyst to the prepolymer methylol melamine solution, stirring for reaction, obtaining a suspension, separating the suspension into solid and liquid, and then washing and drying to obtain melamine formaldehyde resin microspheres.
[0009] Preferably, in step S1, the heating reaction temperature is 60-80°C and the reaction time is 20-40 min.
[0010] Preferably, in step S1, the amount of catalyst added is 0.25‰ to 2.5‰ of the total volume of the solvent.
[0011] Preferably, in step S2, the acidic catalyst includes one or more of hydrochloric acid, formic acid, and acetic acid.
[0012] In a second aspect, the present application provides a method for preparing a heat-resistant diaphragm for a lithium-ion battery, comprising the following steps: dispersing melamine formaldehyde resin microspheres into an aqueous solution, adding a functional additive, and mixing evenly to obtain a slurry; coating the slurry on a polyolefin diaphragm substrate to obtain a wet composite film, and after drying, a heat-resistant diaphragm for a lithium-ion battery is obtained.
[0013] Preferably, the functional additive accounts for 1-10% of the slurry mass, and the melamine formaldehyde resin microspheres account for 2-40% of the slurry mass.
[0014] Preferably, the thickness of the polyolefin separator is 5-35 μm.
[0015] Preferably, the particle size D50 of the melamine formaldehyde resin microspheres is 0.05 μm-5 μm.
[0016] The beneficial effects of the present application are as follows: The present application significantly reduces the thermal shrinkage of the polyolefin separator by using melamine formaldehyde resin microspheres and polyolefin separators, and the thermal shrinkage is ≤5% at 180°C, thereby improving the thermal safety of the battery cell; the present application has excellent wettability to the electrolyte, the electrolyte absorption rate is 122.3~486.1%, and the ion conductivity is 0.5~3.0 mS / cm; in addition, the composite separator coating is light in weight, with a gram weight of 0.8-9.8 g / m 2 , reducing the weight of the diaphragm helps to improve the mass-specific energy density of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 A flow chart of a method for preparing a heat-resistant separator for a lithium-ion battery provided by the present invention; Figure 2 This is the SEM image of Celgard's 10 um PE separator; Figure 3 The SEM image of the PE diaphragm surface coated with MF resin microspheres; Figure 4 The SEM image of the cross section of the PE diaphragm coated with MF resin microspheres; Figure 5 Actual photos of PE separator, ceramic-PE, and MF resin-PE separator before and after heating at 180 °C for 30 min. DETAILED DESCRIPTION
[0018] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0019] The present application provides a heat-resistant diaphragm for a lithium-ion battery, comprising a polyolefin diaphragm and melamine formaldehyde resin microspheres and functional additives coated on both sides of the polyolefin diaphragm.
[0020] The present application significantly reduces the thermal shrinkage rate of the polyolefin separator by using melamine formaldehyde resin microspheres and polyolefin separators, thereby improving the thermal safety of the battery monomer. At the same time, the heat-resistant separator of the lithium-ion battery obtained by the composite of melamine formaldehyde resin microspheres and polyolefin separators has low density, which helps to improve the mass energy density of the battery; the defects of the existing lithium-ion battery polyolefin separators that are easy to shrink when heated and the ceramic modified separators that are high in gram weight are improved.
[0021] In some embodiments, the functional additives include one or more of a dispersant, a wetting agent, and a binder. The dispersant and the wetting agent are one or more of fluoroalkyl methoxy alcohol ether, polyoxyethylene alkylamine, polyether modified silicone, sodium aryl naphthalene sulfonate, sodium dodecylbenzene sulfonate, sodium dodecyl sulfate, sodium perfluorooctanoate, nonylphenol polyoxyethylene ether, sodium butyl naphthalene sulfonate, polyacrylate, polyethylene glycol, and sodium carboxymethyl cellulose; the binder is one or more of styrene-butadiene rubber, sodium carboxymethyl cellulose, lithium polyacrylate, and polyacrylonitrile multipolymer.
[0022] In the present application, the PE diaphragm serves as the skeleton of the supporting substrate. The hydrophilicity of the polyolefin diaphragm is very poor, and a functional additive needs to be added to the above-mentioned MF resin microsphere aqueous dispersion to help the MF resin microspheres adhere to the surface of the PE diaphragm, thereby obtaining a high temperature resistant, relatively light and thin composite diaphragm.
[0023] In some embodiments, the method for preparing melamine formaldehyde resin microspheres comprises the following steps: S1. Add melamine powder to formaldehyde solution for ultrasonic dispersion, and then heat to react to obtain a prepolymer methylol melamine solution; S2. Add an acid catalyst to the prepolymer methylol melamine solution, stir to react, obtain a suspension, separate the suspension into solid and liquid, and then wash and dry to obtain melamine formaldehyde resin microspheres.
[0024] In the present application, melamine formaldehyde resin microspheres are obtained by catalytic polymerization of melamine and formaldehyde in an acidic environment; in step S1, the formaldehyde solution is an aqueous solution of formaldehyde, and the ultrasonic dispersion time is 1-5 minutes; in step S2, the stirring reaction time is 0.5-2 hours.
[0025] In the present application, the specific operation after obtaining the suspension is as follows: after the suspension is centrifuged, the precipitate is washed with a washing solvent (one or more of deionized water and ethanol), and then dried.
[0026] In some embodiments, in step S1, the heating reaction temperature is 60-80°C, and the reaction time is 20-40 min.
[0027] In some embodiments, in step S1, the amount of catalyst added is 0.25‰ to 2.5‰ of the total volume of the solvent.
[0028] In some embodiments, in step S2, the acidic catalyst includes one or more of hydrochloric acid, formic acid, and acetic acid.
[0029] In a second aspect, the present application provides a method for preparing a heat-resistant diaphragm for a lithium-ion battery, comprising the following steps: dispersing melamine formaldehyde resin microspheres into an aqueous solution, adding a functional additive, and mixing evenly to obtain a slurry; coating the slurry on a polyolefin diaphragm substrate to obtain a wet composite film, and after drying, a heat-resistant diaphragm for a lithium-ion battery is obtained.
[0030] The present application disperses the synthesized submicron melamine formaldehyde resin microspheres in an aqueous solution, adds a dispersant, a wetting agent and a binder to prepare a slurry, and then coats the slurry on a polyolefin diaphragm to obtain a composite diaphragm. The composite diaphragm can significantly reduce the thermal shrinkage of the polyolefin diaphragm and improve the thermal safety of the battery cell. In addition, the composite diaphragm coating is light in weight, which helps to improve the mass energy density of the battery.
[0031] In the present application, the drying process is: after the wet composite film is placed at room temperature for drying for 30 minutes, it is transferred to a blast oven for drying to obtain a heat-resistant separator for lithium-ion batteries; wherein the blast oven drying temperature is 80°C and the drying time is 5 to 15 minutes.
[0032] In some embodiments, the functional additive accounts for 1-10% of the slurry by weight, and the melamine formaldehyde resin microspheres account for 2-40% of the slurry by weight.
[0033] The present invention has no special limitation on the specifications of the polyolefin separator, and a commercially available polyolefin separator can be used; however, in some embodiments, the thickness of the polyolefin separator is 5-35 μm; in the embodiments of the present application, a 10 μm thick PE separator is selected as the base membrane.
[0034] In some embodiments, the particle size D50 of the melamine formaldehyde resin microspheres is 0.05 μm-5 μm.
[0035] The present solution is further described below through specific embodiments.
[0036] Example 1 A heat-resistant diaphragm for a lithium-ion battery comprises a polyolefin diaphragm, melamine formaldehyde resin microspheres coated on the polyolefin diaphragm, and functional additives; the functional additives comprise a dispersant, a wetting agent, and a binder.
[0037] The present application provides a method for preparing a heat-resistant separator for a lithium-ion battery, comprising the following steps: 2 g of melamine formaldehyde resin microsphere (MF microsphere) powder was added to deionized water to prepare a suspension with a solid content of 16.7%. Subsequently, 1.5% of a polycarboxylic acid dispersant and 1.5% of a polyether-modified silane wetting agent were added, and the mixture was transferred to a magnetic stirrer and stirred for 12 h. After the mixture was evenly mixed (no obvious precipitation was produced after the mixture was left to stand for half an hour), 5% of a polyacrylonitrile binder was added, and the mixture was stirred for 6 h to obtain a water-based coating slurry for MF resin microspheres. The above slurry was coated on a 10 μm thick PE separator by an automatic coating machine. The obtained wet film was first placed at room temperature for 30 min (25 ℃ room temperature). After there was no water mark on the surface of the composite separator, it was transferred to an 80 ℃ forced air oven for vacuum drying for 10 min to obtain a PE composite separator coated with MF resin microspheres on one side. The above coating steps were repeated to obtain a PE composite separator coated with MF resin microspheres on both sides. The thickness of the front and back coatings was 4 μm, and the total thickness of the composite separator was 18 μm.
[0038] Wherein, the preparation method of melamine formaldehyde resin microspheres is as follows: S1. Add 19.6 g of formaldehyde solution and 400 mL of water into a 1000 mL two-necked flask, stir magnetically and disperse ultrasonically, and heat to 80 °C in a water bath; then, add 5.0 g of melamine powder and react for 30 min to generate prepolymer hydroxymethyl melamine; S2. Add 0.35 mL of formic acid catalyst to the prepolymer hydroxymethyl melamine solution to adjust the pH value of the system. After 5 minutes, the transparent solution becomes turbid. Continue stirring for 50 minutes to obtain a milky white turbid solution and stop the reaction. Transfer the suspension in the reaction flask to a centrifuge tube and centrifuge it at 13,000 rpm for 3 minutes using a high-speed centrifuge. Wash the obtained precipitate with deionized water and ethanol alternately twice. Transfer the above product to an oven at 80°C and dry it for 12 hours to obtain white powdery MF resin microspheres. Figure 3 , is a scanning electron microscope (SEM) image of the MF resin particles prepared in this embodiment. It can be seen that the obtained MF nanoparticles are all spherical, with an average D50 of 598 nmnm; the thickness of the PE composite diaphragm obtained in Example 1 is measured to be 18 μm.
[0039] Example 2 Embodiment 2 differs from Embodiment 1 in that the particle size of the melamine formaldehyde resin microspheres is different, and comprises the following steps: 2 g of melamine formaldehyde resin microsphere (MF microsphere) powder was added to deionized water to prepare a suspension with a solid content of 16.7%. Subsequently, 1.5% of a polycarboxylic acid dispersant and 1.5% of a polyether-modified silane wetting agent were added, and the mixture was transferred to a magnetic stirrer and stirred for 12 h. After the mixture was evenly mixed (no obvious precipitation was produced after the mixture was left to stand for half an hour), 5% of a polyacrylonitrile binder was added, and the mixture was stirred for 6 h to obtain a water-based coating slurry for MF resin microspheres. The above slurry was coated on a 10 μm thick PE separator by an automatic coating machine. The obtained wet film was first placed at room temperature for 30 min (25 ℃ room temperature). After there was no water mark on the surface of the composite separator, it was transferred to an 80 ℃ forced air oven for vacuum drying for 10 min to obtain a PE composite separator coated with MF resin microspheres on one side. The above coating steps were repeated to obtain a PE composite separator coated with MF resin microspheres on both sides. The thickness of the front and back coatings was 4 μm, and the total thickness of the composite separator was 18 μm.
[0040] Wherein, the preparation method of melamine formaldehyde resin microspheres is as follows: S1. Add 19.6 g of formaldehyde solution and 400 mL of water into a 1000 mL two-necked flask, stir magnetically and disperse ultrasonically, and heat to 80 °C in a water bath; then, add 5.0 g of melamine powder and react for 30 min to generate prepolymer hydroxymethyl melamine; S2. Add 0.4 mL of formic acid catalyst to the prepolymer hydroxymethyl melamine solution to adjust the pH value of the system. After 5 minutes, the transparent solution becomes turbid. Continue stirring for 50 minutes to obtain a milky white turbid solution and stop the reaction. Transfer the suspension in the reaction flask to a centrifuge tube and centrifuge it at 13,000 rpm for 3 minutes using a high-speed centrifuge. Wash the obtained precipitate with deionized water and ethanol alternately twice. Transfer the above product to an oven at 80°C and dry it for 12 hours to obtain white powdery MF resin microspheres. Figure 3 , is a scanning electron microscope (SEM) image of the MF resin particles prepared in this embodiment. It can be seen that the obtained MF nanoparticles are all spherical, with an average D50 of 361 nmnm; the thickness of the PE composite diaphragm obtained in Example 1 is measured to be 18 μm.
[0041] Comparative Example 1 A lithium-ion battery separator, the other contents are the same as those of Example 1, except that the melamine formaldehyde resin microspheres are replaced with ceramic micropowders to obtain a double-sided ceramic-PE separator, namely the lithium-ion battery separator, with a thickness of 16 μm.
[0042] Test and Evaluation Taking a PE diaphragm with a thickness of 10 μm and the double-sided ceramic-PE diaphragm of Comparative Example 1 as comparative examples, the heat-resistant diaphragm for lithium-ion batteries obtained in Example 1 was tested for morphology, thickness, air permeability, gram weight, thermal stability, etc.
[0043] Specifically, the air permeability of the diaphragm was tested using the American Gurley 4110N air permeability tester. The air permeability of the diaphragm reflects the tortuosity of the internal pores of the diaphragm and the true path of ion diffusion, which is proportional to the ionic conductivity and can be evaluated by the Gurley value. The Gurley value refers to the time required for a certain amount of air to pass through a unit area of the diaphragm under a certain specified pressure, in seconds. The gram weight of the diaphragm was calculated by slicing + weighing. The diaphragm was cut into discs with a diameter of 16.5 mm using a cutting machine and weighed one by one. The thickness of the diaphragm was tested using a handheld thickness gauge. See Table 1 for the implementation results of this case.
[0044] Table 1 Test results of physical parameters of different diaphragms
[0045] The surface and cross-sectional morphologies of the PE separator and MF-PE composite separator were observed under a cold-field scanning electron microscope.
[0046] See also Figure 2 as well as Figure 4 , Figure 2 This is the SEM image of the PE diaphragm; Figure 3 The SEM image of the PE diaphragm surface coated with MF resin microspheres; Figure 4 The SEM image of the cross section of the PE diaphragm coated with MF resin microspheres. Figure 2 It can be seen that the SEM image of the commercial PE separator prepared by the wet process shows a large number of evenly distributed pores on the membrane surface; Figure 3 It can be seen that the MF resin microspheres are attached relatively smoothly, and no exposed PE base film can be seen at all, indicating that the slurry formula has good coatability for polyolefin separators. At the same time, there are a large number of tiny pores between the staggered accumulation of MF resin microspheres, which provide abundant channels for the transmission of lithium ions. Figure 4 The cross-sectional view of the double-sided PE composite diaphragm coated with MF resin microspheres is similar to a sandwich structure, with the MF resin microspheres constituting the upper and lower coatings and the PE base film being the middle layer.
[0047] Specifically, the bulk impedance of the composite membrane was tested on an electrochemical workstation (Bio-Logic VSP-300) by electrochemical impedance spectroscopy (EIS), and its ionic conductivity was obtained. A stainless steel symmetrical cell was assembled for testing. The frequency range was 106~10-1 Hz, the AC amplitude was 10 mV, and the ionic conductivity was calculated as follows: σ = D / RS Wherein, σ represents the ionic conductivity of the membrane; D represents the thickness of the membrane; R is the horizontal intercept of the Nyquist plot; S represents the area of the membrane. The ionic conductivities of the PE and MF-PE membranes were measured to be 0.34 mS / cm and 0.72 mS / cm, respectively. The ionic conductivities of the PE, ceramic, MF-PE Example 1 and MF-PE Example 2 were measured to be 0.34 mS / cm, 0.45 mS / cm, 0.72 mS / cm and 0.64 mS / cm, respectively. Due to the small particle size of the microspheres in MF-PE Example 2, the pores of the polyolefin membrane were partially blocked, resulting in a lower ionic conductivity than that of MF-PE Example 1.
[0048] Figure 5 The following are the actual photos of PE separator, ceramic-PE, and MF resin-PE separator before and after heating at 180 °C for 30 min. Figure 5 The experimental results show that the PE diaphragm obviously shrinks, melts and solidifies, changing from a round shape to a tiny light white plastic mass, while the ceramic-PE diaphragm and MF-PE diaphragm have basically no obvious shrinkage after heating, and the thermal shrinkage rate is only 4.8%. This shows that the organic resin MF-PE diaphragm obtained in the implementation case of the present invention can reach the level of thermal dimensional stability of the inorganic ceramic-PE diaphragm. As known to those skilled in the art, the diaphragm is an inert material of the battery system, and the gram weight of the diaphragm directly affects the mass energy density of the battery cell. When other conditions are the same, the smaller the gram weight, the higher the mass energy density.
[0049] The invention provides a heat-resistant diaphragm for a lithium-ion battery and a preparation method thereof. The components of the heat-resistant diaphragm for a lithium-ion battery include a polyolefin diaphragm, melamine formaldehyde resin microspheres and a plurality of functional additives. The steps are as follows: dispersing synthesized submicron-level melamine formaldehyde resin microspheres in an aqueous solution, adding a dispersant, a wetting agent and a binder to prepare a slurry; coating the slurry on a polyolefin diaphragm to obtain a composite diaphragm. The composite diaphragm of the invention can significantly reduce the thermal shrinkage of the polyolefin diaphragm, has excellent thermal dimensional stability, and improves the thermal safety of a battery cell; in addition, the composite diaphragm coating is light in weight, which helps to improve the energy density of the battery.
[0050] The above are only preferred specific implementations of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.
Claims
1. A heat-resistant separator for a lithium-ion battery, characterized in that: The invention comprises a polyolefin diaphragm and melamine formaldehyde resin microspheres and functional additives coated on two sides of the polyolefin diaphragm.
2. The heat-resistant separator for lithium-ion batteries according to claim 1, characterized in that: The functional additives include one or more of a dispersant, a wetting agent, and a binder.
3. The heat-resistant separator for lithium-ion batteries according to claim 1, characterized in that: The preparation method of the melamine formaldehyde resin microspheres comprises the following steps: S1. Add melamine powder to the formaldehyde solution and heat the reaction to obtain a prepolymer of hydroxymethyl melamine; S2. Add an acidic catalyst to the solution of the prepolymer hydroxymethyl melamine, stir the reaction to obtain a suspension, separate the suspension into solid and liquid, and then wash and dry to obtain the melamine formaldehyde resin microspheres.
4. The heat-resistant separator for lithium-ion batteries according to claim 3, characterized in that: In step S1, the heating reaction temperature is 60-80°C and the reaction time is 20-40 minutes.
5. The heat-resistant separator for lithium-ion batteries according to claim 3, characterized in that: In step S1, the amount of the catalyst added is 0.25‰ to 2.5‰ of the total volume of the solvent.
6. The heat-resistant separator for lithium-ion batteries according to claim 3, characterized in that: In step S2, the acidic catalyst includes one or more of hydrochloric acid, formic acid, and acetic acid.
7. A method for preparing a heat-resistant separator for a lithium-ion battery according to any one of claims 1 to 6, characterized in that: The following steps are involved: Dispersing the melamine formaldehyde resin microspheres into an aqueous solution, adding a functional additive, and mixing evenly to obtain a slurry; The slurry is coated on the polyolefin separator substrate to obtain a composite wet film, and after drying, the heat-resistant separator for lithium-ion batteries is obtained.
8. The method for preparing a heat-resistant separator for a lithium-ion battery according to claim 7, characterized in that: The functional additive accounts for 1-10% of the mass of the slurry, and the melamine formaldehyde resin microspheres account for 2-40% of the mass of the slurry.
9. The heat-resistant separator for lithium-ion batteries according to claim 7, characterized in that: The polyolefin separator has a thickness of 5-35 μm.
10. The method for preparing a heat-resistant separator for a lithium-ion battery according to claim 7, characterized in that: The particle size D50 of the melamine formaldehyde resin microspheres is 0.05 μm-5 μm.
Citation Information
Cited By
Lithium battery diaphragm with high heat resistance and low water absorption and preparation method thereof
CN119944237A