Multi-doped laser crystal capable of realizing mid-infrared laser output and preparation method thereof

Through the calcium fluoride crystal co-doped with yotterbium sterbium, the energy transfer of ytterbium ions and holmium ions and the deactivation of terbium ions is solved, and the problem of difficult output of mid-infrared lasers in the prior art is achieved, and the efficiency of the ~3μm band is achieved Stable laser output has important application prospects.

CN119070128APending Publication Date: 2024-12-03NINGBO RADIUM CRYSTAL TECHNOLOGY CO LTD
3 Cites 0 Cited by

Patent Information

Application Number
CN202411048714.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing technology is difficult to achieve mid-infrared laser output, especially in the ~3μm band. The laser transition formed by Er3+ ions is linear spectrum, making it difficult to form a broadband spectrum. Ho3+ and Dy3+ doped laser crystals cannot be effective due to the lack of a pump source. The output of mid-infrared laser light, the lower energy level life of Er3+ and Ho3+ ions leads to the self-termination of the laser transition.

Method used

Calcium fluoride crystals co-doped with yotterbium terbium (Yb3+, Ho3+, Tb3+), ytterbium ions are used as sensitized ions, holmium ions are used as activation ions, and terbium ions are used as deactivated ions. The 2F5 ytterbium ions is prepared by temperature gradient method. The energy transfer of energy to the 5I6 energy level of the holmium ions. The incorporation of terbium ions reduces the lifetime of the 5I7 energy level of the holmium ions, achieving a fully solid state, efficient and stable laser output in the ~3μm mid-infrared band.

Benefits of technology

It realizes efficient and stable laser output in the ~3μm mid-infrared band, reduces research and production costs, and uses commercial lasers as pumping sources, which are suitable for scientific research, military, medical and optical communication fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119070128A_ABST
    Figure CN119070128A_ABST
Patent Text Reader

Abstract

The invention discloses a multi-doped crystal capable of realizing mid-infrared laser output and a preparation method thereof, the crystal is an ytterbium, holmium and terbium co-doped calcium fluoride crystal, x is equal to 0-50at.% and is the molar percentage of ytterbium ions in calcium ions in a matrix; y is equal to 0.01-5at.% and is the molar percentage of holmium ions in calcium ions in the matrix; and z is 0.001-5at.% and is the molar percentage of terbium ions in calcium ions in the matrix. In the laser crystal, holmium ions are used as activating ions, ytterbium ions are used as sensitizing ions, and terbium ions are used as deactivating ions. Compared with an existing laser crystal, the ytterbium, holmium and terbium co-doped fluoride crystal can utilize a mature semiconductor pumping source to achieve middle-infrared band efficient laser output.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of laser crystal materials, and in particular to an ytterbium, holmium, and terbium co-doped laser crystal capable of realizing mid-infrared laser output and a preparation method thereof. Background Art

[0002] Mid-infrared lasers in the ~3μm band have very important application backgrounds and significant demands in scientific research, military, remote sensing, medical treatment, optical communications, environmental monitoring, material processing and other fields, and have become a key area of ​​research and development for various countries. At present, the rare earth ions that can achieve mid-infrared laser output in this band mainly include Ho 3+ , Er 3+ 、Dy 3+ Plasma. Among them, Er 3+ The most researched is Er, because it has a suitable commercial LD ​​pump source, but 3+ The laser transition formed by ions under normal conditions is a linear spectrum and is difficult to form a broadband spectrum. So far, there has been no report of ultrafast femtosecond (fs) mode-locked laser output in crystals. 3+ 、Dy 3+ In the doped laser crystal, the lack of pump source restricts the laser output in the ~3μm band. 3+ 、Ho 3+ When ions achieve mid-infrared laser in the ~3μm band, the lifetime of the lower energy level is much longer than that of the upper energy level, making it difficult to form a particle number inversion, and ultimately leading to the problem of self-termination of the laser transition.

[0003] Ho 3+ Doping to achieve mid-infrared laser output requires a matrix material with low phonon energy, which can reduce non-radiative transitions caused by multi-phonon relaxation. Therefore, the present invention preferably uses fluoride or oxide crystals with low phonon energy as the matrix material to achieve mid-infrared laser output. Summary of the invention

[0004] The purpose of the present invention is to provide a multi-doped laser crystal that can achieve mid-infrared laser output, that is, a ytterbium, holmium, and terbium co-doped laser crystal and a preparation method thereof, which can achieve efficient and stable output of ~3μm mid-infrared band laser, and has very important application prospects in scientific research, military, medical treatment, optical communications and other fields.

[0005] The first object of the present invention can be achieved by the following technical solutions:

[0006] A multi-doped laser crystal capable of realizing mid-infrared laser output, the crystal is ytterbium, holmium, and terbium (Yb 3+ 、Ho 3+ , Tb 3 + ) co-doped calcium fluoride crystals;

[0007] Among them, x is the molar percentage of ytterbium ions in the matrix calcium fluoride crystal, x=0-50at.%; y is the molar percentage of holmium ions in the matrix calcium ions, y=0.01-5at.%; z is the molar percentage of terbium ions in the matrix calcium ions, z=0.001-5at.%.

[0008] Furthermore, in the multi-doped laser crystal, x=1.0-10.0 at.%, y=0.5-5.0 at.%, and z=0.01-1.0 at.%.

[0009] Furthermore, in the multi-doped laser crystal, ytterbium ions serve as sensitizing ions, holmium ions serve as activating ions, and terbium ions serve as deactivating ions.

[0010] Furthermore, the multi-doped laser crystal is used to achieve all-solid-state laser output in the mid-infrared band of ∼3 μm.

[0011] The second object of the present invention can be achieved by adopting the following technical solutions:

[0012] A method for preparing a multi-doped laser crystal capable of realizing mid-infrared laser output, wherein the crystal is ytterbium Yb 3+ , holmium Ho 3+ , Terbium Tb 3+ The co-doped calcium fluoride crystal, the preparation method comprises the following steps:

[0013] S1, using YbF3, HoF3, TbF3, CaF2 raw materials with a purity greater than 99.99%, calculate the required mass of each raw material according to the stoichiometric ratio and weigh them accurately;

[0014] S2, grinding the weighed raw materials thoroughly to make them evenly mixed, and then loading them into a crucible;

[0015] S3, put the crucible into the hot field of the high temperature furnace and align it horizontally;

[0016] S4, close the furnace door, evacuate the furnace, and fill it with inert gas as a protective atmosphere;

[0017] S5, raising the temperature until the raw materials are melted, and performing a constant temperature heat treatment to ensure that all the raw materials in the crucible are melted; slowly cooling down to allow the melt in the crucible to crystallize from bottom to top; after the crystal growth is completed, slowly cooling down to room temperature, and taking out the crystal, which is the ytterbium, holmium, and terbium co-doped calcium fluoride crystal capable of realizing mid-infrared laser output.

[0018] Preferably, the Yb-containing 3+ 、Ho 3+ , Tb 3+The purity of the raw material is 5N. 5N purity has less impurities than chemical analysis purity and 4N purity raw materials, which can avoid problems such as difficulty in obtaining crystals and poor crystal quality due to the reaction of impurities with crucibles and raw materials during the growth process.

[0019] Preferably, the grinding in S2 is carried out in an agate mortar, and the grinding time is 45 min-60 min.

[0020] Preferably, the inert gas described in S4 is high-purity argon.

[0021] Preferably, the constant temperature described in S5 is maintained for a time of 2-10 hours to ensure that all the raw materials in the crucible are melted.

[0022] Preferably, the slow cooling in S5 is cooling at a rate of 0.2-2.0° C. / h to ensure that the melt in the crucible grows and crystallizes better.

[0023] Compared with the prior art, the present invention has the following advantages:

[0024] 1. The present invention proposes for the first time a ytterbium, holmium, and terbium co-doped mid-infrared laser crystal. Ytterbium ions are used as sensitizing ions, holmium ions are used as activating ions, and terbium ions are used as deactivating ions. Figure 1 Energy transfer diagram, ytterbium ions can be excited by 980nm LD. 2 F 5 / 2 energy level transfers energy to the holmium ion 5 I6 energy level makes the holmium ion 5 I6→ 5 The I7 transition emits fluorescence at around 3 μm. The incorporation of terbium ions makes the holmium ions 5 The lifetime of the I7 energy level is greatly reduced, which is conducive to achieving particle number inversion and realizing all-solid-state, efficient and stable laser output in the mid-infrared band of ~3μm.

[0025] 2. The Ytterbium, Holmium, and Terbium co-doped Calcium Fluoride crystals prepared by the present invention are easy to grow in large size and have high repeatability. They can be processed into high-quality wafers or laser rods for laser experiments, which reduces the research and production costs to a certain extent.

[0026] The Ytterbium, Holmium and Terbium co-doped laser crystal of the present invention uses calcium fluoride as the matrix material, and holmium ions are used as activation ions to emit light in the mid-infrared band; ytterbium ions are used as sensitizing ions. 2 F 5 / 2 Energy levels and holmium ions 5 The dipole interaction between the I6 energy levels transfers energy to the neighboring holmium ions. 5 I6 energy level, then radiate to 5I7 energy level, emitting ~3μm photons, so commercial lasers can be used as pump sources to achieve high-power mid-infrared laser output; terbium ions are used as deactivation ions to make the holmium ions 5 The lifetime of the I7 energy level is greatly reduced, which is conducive to achieving population inversion, reducing the laser threshold, and achieving efficient laser output. Compared with existing laser crystals, the Yb-H-Tb co-doped laser crystal of the present invention can use mature semiconductor pump sources to achieve efficient laser output in the mid-infrared band, and has very important application backgrounds and major demands in the fields of scientific research, military, medical treatment, optical communications, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 Yb in the present invention 3+ 、Ho 3+ , Tb 3+ Energy transfer diagram;

[0028] Figure 2 is the fluorescence spectrum of the crystal in Example 1 of the present invention.

[0029] Figure 3 It is the fluorescence decay curve spectrum of the crystal in Example 1 of the present invention. DETAILED DESCRIPTION

[0030] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is described in detail below in conjunction with the drawings and specific embodiments in the embodiments of the present invention. The following embodiments are implemented on the premise of the technical scheme of the present invention, and detailed implementation methods and specific operation processes are given, but the protection scope of the present invention is not limited to the following embodiments.

[0031] A ytterbium holmium terbium (Yb 3+ 、Ho 3+ , Tb 3+ ) co-doped laser crystal, wherein x=0-50at.%, which is the molar percentage of ytterbium ions in the matrix calcium fluoride crystal; y=0.01-5at.%, which is the molar percentage of holmium ions in the matrix calcium ions; z=0.001-5at.%, which is the molar percentage of terbium ions in the matrix calcium ions.

[0032] Ytterbium ions act as sensitizing ions, holmium ions act as activating ions, and terbium ions act as deactivating ions.

[0033] The laser crystal is used to achieve all-solid-state laser output in the mid-infrared band of ~3μm.

[0034] Example 1

[0035] The present invention adopts the temperature gradient method to grow Yb 0.03 Ho 0.015 Tb 0.0025Ca 0.9525 F 2.0475 , specifically prepared by the following method:

[0036] Growth of Yb by Temperature Gradient Method 0.03 Ho 0.015 Tb 0.0025 Ca 0.9525 F 2.0475 Crystal, the initial raw materials are 5N purity YbF3, HoF3, TbF3 and CaF2 single crystal particles, according to the chemical formula Yb 0.03 Ho 0.015 Tb 0.0025 Ca 0.9525 F 2.0475 Calculate the mass of each raw material and weigh it accurately. Put the weighed raw materials into a graphite crucible, evacuate the furnace, fill it with high-purity argon as a protective atmosphere, heat up to 1430℃ at a rate of 300℃ / h, keep the temperature constant for 4 hours until the raw materials are completely melted, grow at a cooling rate of 0.2℃ / h, and the growth time is 120h. After the growth is completed, slowly cool down and take out the crystal.

[0037] The prepared Yb 0.03 Ho 0.015 Tb 0.0025 Ca 0.9525 F 2.0475 The crystal was optically processed and the spectrum and fluorescence lifetime were tested. The fluorescence spectrum was as follows: Figure 2 As shown, the broad and smooth 2.7-3.1 μm band emission indicates that Yb 0.03 Ho 0.015 Tb 0.0025 Ca 0.9525 F 2.0475 The crystal is suitable as a gain medium for mid-infrared lasers; the fluorescence decay curve is as follows Figure 3 As shown in Figure 2, the addition of Tb ions effectively reduces the laser lower energy level. 5 The fluorescence lifetime of I7 is conducive to the inversion of the number of particles in the laser energy level. Therefore, Yb-H-Tb co-doped calcium fluoride laser crystal can become a new mid-infrared laser gain material suitable for LD pumping, achieving efficient and stable laser output.

[0038] Example 2

[0039] Growth of Yb by Temperature Gradient Method 0.20 Ho 0.010 Tb 0.0010 Ca 0.7890 F 2.2110 , specifically prepared by the following method:

[0040] Growth of Yb by Temperature Gradient Method 0.20 Ho 0.010 Tb0.0010 Ca 0.7890 F 2.2110 Crystal, the initial raw materials are 5N purity YbF3, HoF3, TbF3 and CaF2 single crystal particles, according to the chemical formula Yb 0.20 Ho 0.010 Tb 0.0010 Ca 0.7890 F 2.2110 Calculate the mass of each raw material and weigh it accurately. Put the weighed raw materials into a graphite crucible, evacuate the furnace, fill it with high-purity argon as a protective atmosphere, heat it up to 1430℃ at a rate of 300℃ / h, keep it at a constant temperature for 4 hours until the raw materials are completely melted, and grow it at a cooling rate of 1℃ / h. The growth time is 120h. After the growth is completed, slowly cool it down and take out the crystal. Processing a piece of Yb with good optical quality 0.20 Ho 0.010 Tb 0.0010 Ca 0.7890 F 2.2110 The crystals were subjected to spectral and fluorescence lifetime tests.

[0041] The ytterbium, holmium, and terbium co-doped laser crystal of the present invention can utilize a mature semiconductor pump source to achieve efficient laser output in the mid-infrared band, and has very important application prospects in the fields of scientific research, military affairs, medical treatment, optical communications, etc.

[0042] The above description of the embodiments is to facilitate those skilled in the art to understand and use the present invention. However, the implementation of the present invention is not limited to the above embodiments. Any changes, modifications, substitutions, combinations, and simplifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention and without creative work should be within the scope of protection of the present invention.

Claims

1. A multi-doped laser crystal capable of achieving mid-infrared laser output, It is characterized in that The multi-doped laser crystal is Yb 3+ , holmium Ho 3+ , Terbium Tb 3+ Co-doped calcium fluoride crystals; Among them, x is the molar percentage of ytterbium ions in the matrix calcium fluoride crystal, x=0-50at.%; y is the molar percentage of holmium ions in the matrix calcium ions, y=0.01-5at.%; z is the molar percentage of terbium ions in the matrix calcium ions, z=0.001-5at.%.

2. The multi-doped laser crystal capable of achieving mid-infrared laser output according to claim 1, It is characterized in that In the multi-doped laser crystal, x=1.0-10.0 at.%, y=0.5-5.0 at.%, and z=0.01-1.0 at.%.

3. The multi-doped laser crystal capable of achieving mid-infrared laser output according to any one of claims 1 to 2, It is characterized in that In the multi-doped laser crystal, ytterbium ions serve as sensitizing ions, holmium ions serve as activating ions, and terbium ions serve as deactivating ions.

4. The multi-doped laser crystal capable of achieving mid-infrared laser output according to any one of claims 1 to 2, It is characterized in that The multi-doped laser crystal is used to achieve full solid-state laser output in the mid-infrared band of 3 μm.

5. A method for preparing a multi-doped laser crystal capable of achieving mid-infrared laser output, It is characterized in that The multi-doped laser crystal capable of achieving mid-infrared laser output as claimed in claim 1, wherein the crystal is ytterbium Yb 3+ , holmium Ho 3+ , Terbium Tb 3+ The co-doped calcium fluoride crystal, the preparation method thereof comprises the following steps: S1, YbF with purity greater than 99.99% 3 、HoF 3 , TbF 3 , CaF 2 Raw materials: calculate the required mass of each raw material according to the stoichiometric ratio and weigh it accurately; S2, grinding the weighed raw materials thoroughly to make them evenly mixed, and then loading them into a crucible; S3, put the crucible into the hot field of the high temperature furnace and align it horizontally; S4, close the furnace door, evacuate the furnace, and fill it with inert gas as a protective atmosphere; S5, raising the temperature until the raw material is melted, and performing constant temperature heat treatment to ensure that the raw material in the crucible is completely melted; then slowly lowering the temperature to allow the melt in the crucible to crystallize from bottom to top; after the crystal growth is completed, lowering the temperature to room temperature, and taking out the crystal, which is the multi-doped laser crystal capable of realizing mid-infrared laser output.

6. The method for preparing a multi-doped laser crystal capable of achieving mid-infrared laser output according to claim 5, It is characterized in that The inert gas described in S4 is high-purity argon.

7. The method for preparing a multi-doped laser crystal capable of achieving mid-infrared laser output according to claim 5, It is characterized in that The constant temperature described in S5 is to ensure that the constant temperature time for all the raw materials in the crucible are melted is 2-10 hours.

8. The method for preparing a multi-doped laser crystal capable of achieving mid-infrared laser output according to claim 5, It is characterized in that The slow cooling described in S5 is cooling at a rate of 0.2-2.0°C / h.

Citation Information

Patent Citations

  • Novel medium-infrared laser crystal of ytterbium, holmium and dysprosium-doped lead fluoride and preparation method of novel medium-infrared laser crystal

    CN109252219A

  • Fluoride laser glass containing eu or tb as deactivating agent for emission of ho 2.9mum light

    JP1994122531A

  • Rare-earth-doped ternary sulfides for mid-wave and long-wave IR lasers

    US10389082B1