Preparation method of ferroelectric memory based on lithium niobate film

By using a probe to apply voltage to write, erase and read data, the problem of lack of ferroelectric memory in the prior art is solved, and the lithium niobate domain wall is realized The utilization of conductive properties has promoted the development of homogeneous photoelectric integration of lithium niobate.

CN119072133APending Publication Date: 2024-12-03ANHUI UNIVERSITY OF TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411191781.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

There are few related reports on the preparation of ferroelectric memory based on lithium niobate films in the prior art, and there is a lack of effective preparation methods.

Method used

By designing a ferroelectric memory preparation method based on lithium niobate film, the memory cell is stacked by a substrate, metal film I, lithium niobate film layer and metal film II, and a probe is used to apply voltage to write, erase and read Get data and use the conductive properties of the lithium niobate domain wall to achieve storage function.

Benefits of technology

This method makes full use of the conductive performance improvement of the lithium niobate domain wall, promotes the development of homogeneous photoelectric integration of lithium niobate, and realizes efficient preparation and data storage of ferroelectric memories.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119072133A_ABST
    Figure CN119072133A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of microelectronic device manufacturing, and particularly relates to a preparation method of a ferroelectric memory based on a lithium niobate thin film, a memory unit structure is formed by stacking a substrate, a metal thin film I, a lithium niobate thin film layer and a metal thin film II in sequence from bottom to top, and the polarization intensity Ps direction is in a plane; the preparation method comprises the following steps: S1, a writing stage; the domain wall is written below the lithium niobate film and is in contact with the lower surface of the metal film II and the upper surface of the metal film I; s2, an erasing stage: erasing the domain wall; s3, a reading stage; and the probe is removed, and the conductive state between the metal film II and the metal film I is read. The method provided by the invention is scientific and reasonable in design, the prepared ferroelectric memory can fully utilize the advantage of the lithium niobate domain wall in the aspect of improving the conductivity, and the method provided by the invention promotes the development of lithium niobate homogeneous photoelectric integration.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of microelectronic device manufacturing, and in particular relates to a method for preparing a ferroelectric memory based on a lithium niobate film. Background Art

[0002] Ferroelectric memory is a type of non-volatile memory. It has become a research focus in the aerospace and military fields because of its advantages such as fast read and write speed, long write life, no data loss in power-off state, operation in harsh environments and low power consumption. Lithium niobate is a multifunctional ferroelectric crystal material. Due to its excellent nonlinear effect and electro-optical effect, lithium niobate film is used to prepare various light-regulating devices and is known as "optical silicon". In recent years, the improvement of the conductive properties of lithium niobate domain walls has shown that lithium niobate has certain development prospects in the field of microelectronic device manufacturing. The commercialization of chip-level lithium niobate films combined with micro-nano processing technology has promoted the development of lithium niobate homogeneous optoelectronic integration.

[0003] In the prior art, there are few reports on the preparation of ferroelectric memory based on lithium niobate thin film. Based on this, the inventors hope to design a method for preparing a ferroelectric memory based on lithium niobate thin film. Summary of the invention

[0004] The purpose of the present invention is to overcome the above problems existing in the conventional technology and provide a method for preparing a ferroelectric memory based on a lithium niobate thin film.

[0005] In order to achieve the above technical objectives and the above technical effects, the present invention is implemented through the following technical solutions:

[0006] The present invention provides a method for preparing a ferroelectric memory based on a lithium niobate film. The memory unit structure is composed of a substrate, a metal film I, a lithium niobate film layer and a metal film II stacked from bottom to top. The polarization intensity P s The direction is within the plane; the preparation method specifically comprises the following steps:

[0007] S1, writing phase, recorded as phase “1”;

[0008] Initial polarization intensity P of lithium niobate thin film layer s Direction to the right; using scheme 1 in which the probe applies positive pressure or scheme 2 in which the probe applies negative pressure;

[0009] Solution 1: When the probe is applied with a positive voltage and contacts the surface of lithium niobate, the probe is required to be located on the right side of the metal film II. At this time, the lithium niobate on the left side of the probe has an electric field distribution that is in the same direction as its initial polarization intensity P. s The opposite component leads to the polarization intensity P of lithium niobate on the left side of the probe. s The direction is deflected by 180°, and a polarized region appears; the domain wall has a polarization intensity Ps The interface of adjacent regions with different directions. At this time, the domain wall is written below the lithium niobate film and contacts the lower surface of the metal film II and the upper surface of the metal film I. Because the domain wall has a better conductivity than the body domain, the metal film II and the metal film I can conduct electricity from top to bottom.

[0010] Solution 2: When the probe is applied with a negative voltage and contacts the surface of lithium niobate, the probe is required to be located on the left side of the metal film II. At this time, the lithium niobate on the right side of the probe has an electric field distribution that is different from its initial polarization intensity P. s The opposite component leads to the polarization intensity P of lithium niobate on the right side of the probe. s The direction is deflected by 180°, and a polarized area appears; the domain wall is written under the lithium niobate film, contacting the lower surface of the metal film II and the upper surface of the metal film I; because the domain wall has a better conductivity than the body domain, the metal film II and the metal film I can conduct electricity from top to bottom at this time;

[0011] S2, erasing phase, recorded as phase “0”;

[0012] For the "1" state formed in Scheme 1, the probe needs to apply negative pressure to contact the polarized area or the surrounding area to achieve domain wall erasure, thereby converting it to the "0" state. When erasing the domain wall, the electric field distribution of the probe is different from the polarization intensity P of the polarized area. s The component in the opposite direction, the polarization intensity P of the polarization area s Deflection occurs again, so that the domain wall below the metal film II is erased or deviates from the metal film II, and the metal film II and the metal film I are not conductive above and below;

[0013] For the "1" state formed in Scheme 2, the probe needs to apply positive pressure to contact the polarized area or the surrounding area to achieve domain wall erasure, thereby converting it to the "0" state. When erasing the domain wall, the electric field distribution of the probe is different from the polarization intensity P of the polarized area. s The component in the opposite direction, the polarization intensity P of the polarization area s Deflection occurs again, so that the domain wall below the metal film II is erased or deviates from the metal film II, and the metal film II and the metal film I are not conductive above and below;

[0014] S3, reading phase;

[0015] Remove the probe and read the conductive state between metal film II and metal film I; let the conductive state be "1" and the non-conductive state be "0";

[0016] “1” reading: The domain wall has a better conductivity than the lithium niobate bulk material. When the domain wall contacts the metal film I and the metal film II, the metal film II and the metal film I are considered to be in a conductive state.

[0017] “0” reading: When the domain wall is erased or is far enough away from the metal film II, the metal film I and the metal film II are in a non-conductive state.

[0018] Furthermore, in the writing stage and the erasing stage, when the probe is applied with voltage and contacts lithium niobate, the probe / lithium niobate / metal film II is in an open circuit state; the probe / lithium niobate / metal film I is in an open circuit state; the power supply connected to the probe is not connected to metal film I or metal film II to form a loop.

[0019] Furthermore, during the writing and erasing phases, the probes can be replaced by thin films made of any conductive objects.

[0020] Furthermore, in the writing stage, when the prepared conductive domain wall is not in strict contact with the metal film II or the metal film I, it still has good conductivity; within the conductive range, there is a certain distance between the conductive domain wall and the metal film I or the metal film II.

[0021] Furthermore, in the reading stage, the read information, such as the current, penetrates the thickness of the lithium niobate layer from top to bottom. The storage unit "1" reading structure is composed of metal film II / domain wall / metal film I stacked up and down; the storage unit "0" reading structure is composed of metal film II / lithium niobate body / metal film I stacked up and down.

[0022] Further, during the erasing phase, the area contacted by the probe is within the polarization area, or in an area surrounding the polarization area.

[0023] Furthermore, in the erasing stage, the memory cell write and erase structure is composed of a probe / lithium niobate; if the metal film I or the metal film II is removed, the domain wall preparation and erasing process can still be completed by the probe to which a voltage is applied.

[0024] Furthermore, in the erasing stage, when the probe contacts the "1" polarization region, the polarization region will be partially erased; when the probe contacts outside the "1" polarization region, the "1" polarization region will be completely erased, and new polarization regions will appear in other areas around the probe.

[0025] The beneficial effects of the present invention are:

[0026] The present invention provides a method for preparing a ferroelectric memory based on a lithium niobate film. The preparation method is scientifically and reasonably designed. The prepared ferroelectric memory can fully utilize the advantages of lithium niobate domain walls in improving electrical conductivity. The method of the present invention promotes the development of lithium niobate homogeneous optoelectronic integration.

[0027] Of course, any product implementing the present invention does not necessarily need to achieve all of the above advantages at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0029] Figure 1 A schematic diagram of writing and erasing a lithium niobate memory cell;

[0030] Figure 2 Schematic diagram for reading a lithium niobate memory cell;

[0031] Figure 3 Schematic diagram of the probe being put under positive pressure to contact lithium niobate to write "1";

[0032] Figure 4 A schematic diagram of a probe being contacted with a polarization region under negative pressure and writing "0";

[0033] Figure 5 A schematic diagram of a probe being contacted with a polarized peripheral area under negative pressure and writing "0";

[0034] Figure 6 Schematic diagram of the probe being subjected to negative pressure to contact lithium niobate to write "1";

[0035] Figure 7 A schematic diagram of a probe being contacted with a polarized region under positive pressure and writing "0";

[0036] Figure 8 A schematic diagram of a probe being contacted with a polarized peripheral area under positive pressure and writing "0";

[0037] Fig. 9 This is the piezoelectric atomic force microscope image of array “1”. DETAILED DESCRIPTION

[0038] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0039] The present invention includes two modules: writing, erasing and reading. The memory cell structure is as follows: Figure 1 As shown, it is composed of metal film II / lithium niobate film layer / metal film I / substrate stacked up and down. Polarization intensity P s The direction lies within the surface.

[0040] The memory preparation method specifically includes the following steps:

[0041] Phase "1" (writing phase):

[0042] Background: Lithium niobate applied electric field and lithium niobate polarization intensity P s The direction is opposite, and the magnitude exceeds the coercive electric field of lithium niobate, making the polarization intensity of lithium niobate P s The direction is deflected by 180°, and lithium niobate polarization occurs. The area where the polarization intensity direction is deflected is called the polarization area.

[0043] like Figure 1 As shown, the initial polarization intensity P of the lithium niobate film layer s Direction right.

[0044] like Figure 1 As shown in (a), when the probe is applied with positive pressure and contacts the surface of lithium niobate, the probe is required to be located on the right side of the metal film 2. At this time, the lithium niobate on the left side of the probe has an electric field distribution that is in the same direction as its initial polarization intensity P. s The opposite component leads to the polarization intensity P of lithium niobate on the left side of the probe. s The direction is deflected by 180°, and a polarized region appears, which is represented by the dark schematic diagram. The domain wall has a polarization intensity P s At the interface of adjacent regions with different directions, the domain wall is written below the lithium niobate film and contacts the lower surface of metal film II and the upper surface of metal film I. Because the domain wall has a better conductivity than the bulk domain, metal film II and metal film I can conduct electricity from top to bottom.

[0045] Or, if Figure 1 As shown in (b), when the probe is applied with a negative voltage to contact the lithium niobate surface, the probe is required to be located on the left side of the metal film II. At this time, the lithium niobate on the right side of the probe has a component of the probe electric field distribution that is opposite to its initial polarization direction, resulting in the polarization intensity P of the lithium niobate on the right side of the probe. s The direction is deflected by 180°, and a polarized area appears, which is represented by the dark schematic diagram. The domain wall is written below the lithium niobate film, contacting the lower surface of metal film II and the upper surface of metal film I. Because the domain wall has a better conductivity than the bulk domain, metal film II and metal film I can conduct electricity from top to bottom.

[0046] Phase "0" (erase phase):

[0047] The domain wall below the metal film II is erased. Figure 1 (a) When erasing domain walls, the probe needs to be subjected to negative pressure to contact the polarized area or the surrounding area in Figure 1(a). Because the electric field distribution of the probe is different from the polarization intensity P in the polarized area, sComponents in opposite directions, Figure 1 (a) Polarization intensity P of the polarization region s The direction changes again, such as Figure 1 As shown in (c), the domain wall below the metal film II is erased or deviates from the metal film II, and the metal film II and the metal film I are not conductive above and below.

[0048] right Figure 1 (b) When erasing domain walls, the probe needs to be pressed positively to contact the polarized region or surrounding area in Figure 1(b). The electric field distribution of the probe is related to the polarization intensity P in the polarized region. s Components in opposite directions, Figure 1 (b) Polarization intensity P of the polarization region s The direction changes again, such as Figure 1 As shown in (d), the domain wall below the metal film II is erased or deviates from the metal film II, and the metal film II and the metal film I are not conductive above and below.

[0049] Reading phase:

[0050] Remove the probe and read the conductive state between metal film II and metal film I. Let the conductive state be "1" and the non-conductive state be "0".

[0051] "1" reading: The domain wall has a better conductivity than the lithium niobate body material. When the domain wall contacts the metal film II and the metal film I, the metal film II and the metal film I are considered to be in a conductive state. Figure 2 (a) and Figure 2 (c) as shown.

[0052] "0" reading: When the domain wall is erased or far enough away from the metal film II, the metal film II and the metal film I are in a non-conductive state. Figure 2 (b) and Figure 2 (d) as shown.

[0053] Generally speaking, Figure 2 (a) The conductivity of the head-to-head domain wall (adjacent polarization strength directions are opposite) is higher than Figure 2 (c) The conductivity of tail-to-tail domain walls (adjacent polarization intensities are opposite) is 3-4 orders of magnitude, Figure 2 (a) When the read state is "1", compared to Figure 2 (a), can be Figure 2 The metal film II and the metal film I in (c) are considered to be non-conductive, and the read state is "0".

[0054] When the probe is applied with voltage and contacts lithium niobate, the probe / lithium niobate / metal film II is in an open circuit state. The probe / lithium niobate / metal film I is in an open circuit state. The power supply connected to the probe is not connected to metal film I or metal film II to form a loop.

[0055] The probe can be replaced by a thin film made of any conductive object.

[0056] The prepared conductive domain wall still has good conductivity when it is not in strict contact with the metal film II or the metal film I. Within the conductive range, the conductive domain wall can be at a certain distance from the metal film I or the metal film II.

[0057] For example, the current reads information by penetrating the thickness of the lithium niobate layer from top to bottom. The storage unit "1" read structure is composed of metal film II / domain wall / metal film I stacked up and down. The storage unit "0" read structure is composed of metal film II / lithium niobate body / metal film I stacked up and down.

[0058] The area contacted by the probe may be within the polarization region, or in the area surrounding the polarization region.

[0059] The memory cell write and erase structure is composed of a probe / lithium niobate. If the metal film I or the metal film II is removed, the domain wall preparation and erasing process can still be completed by the probe to which a voltage is applied.

[0060] When the probe contacts the "1" polarization area, the polarization area will be partially erased. When the probe contacts outside the "1" polarization area, the "1" polarization area will be completely erased, and new polarization areas will appear in other areas around the probe.

[0061] The relevant specific embodiments of the present invention are as follows:

[0062] The specifications of lithium niobate film are 500nm thick x cut lithium niobate film layer / 100nm thick gold film / 2m thick silicon dioxide substrate / 500m thick lithium niobate substrate.

[0063] Example 1

[0064] Writing "1": A chromium film with a thickness of 500nm is plated on the surface of the lithium niobate film through micro-nano processing technology. Along the direction of the initial polarization intensity Ps, the conductive probe is located 500nm from the right boundary line of the chromium film and contacts the lithium niobate film. The probe is applied with a positive voltage of 60V for 0.01s. The head-to-head domain wall is written into the lithium niobate, contacting the chromium film and the gold film. Figure 3 shown.

[0065] Reading "1": Remove the probe, chromium film / head-to-head domain wall / gold film conducts electricity.

[0066] Method 1 for writing "0": The probe contacts the "1" polarization area and is applied with a voltage of negative 60V for 0.01s. The polarization intensity direction of the "1" polarization area on the left side of the probe deflects 180° again. The "1" polarization area on the right side may expand to the surrounding area depending on the magnitude and duration of the applied voltage. The head-to-head domain wall under the metal film II, i.e. the chromium film, is erased. The head-to-head domain wall is located at the position where the probe contacts, away from the chromium film. Figure 4 shown.

[0067] Method 2 for writing "0": The probe contacts the outer peripheral area of ​​the "1" polarization area, and a voltage of negative 60V is applied for 0.01s. The polarization intensity direction of the "1" polarization area on the left side of the probe is deflected 180° again. A new polarization area may be generated on the right side of the probe due to the distribution of the external electric field. The head-to-head domain wall under the metal film II, that is, the chromium film, is erased. The head-to-head domain wall is located at the position where the probe contacts, away from the chromium film. Figure 5 shown.

[0068] Read "0": Remove the probe, the chromium film / lithium niobate layer / gold film is not conductive.

[0069] Example 2

[0070] Writing "1": A 500nm thick chromium metal film is plated on the surface of the lithium niobate film using micro-nano processing technology. s The conductive probe is located 500nm from the left boundary of the chromium film and contacts the lithium niobate film. The probe is applied with a voltage of negative 60V for 0.01s. The tail-to-tail domain wall is written into the lithium niobate, contacting the chromium film and the gold film. Figure 6 shown.

[0071] Reading "1": chromium film / tail-to-tail domain wall / gold film is conductive.

[0072] Method 1 for writing "0": The probe contacts the "1" polarization region, and a positive voltage of 60V is applied for 0.01s. The polarization intensity direction of the "1" polarization region on the right side of the probe deflects 180° again, and the "1" polarization region on the left side of the probe may expand depending on the magnitude and duration of the applied voltage. The tail-to-tail domain wall under the metal film II, i.e. the chromium film, is erased. The tail-to-tail domain wall is located at the position where the probe contacts, away from the chromium film. Figure 7 shown.

[0073] Method 2 for writing "0": The probe contacts the outer peripheral area of ​​the "1" polarization area, and a voltage of 60V is applied to it for 0.01s. The polarization intensity direction of the "1" polarization area on the right side of the probe is deflected 180° again. A new polarization area may be generated on the left side of the probe due to the distribution of the external electric field. At this time, the tail-to-tail domain wall under the metal film II, i.e., the chromium film, is erased. The tail-to-tail domain wall is located at the position where the probe contacts, away from the chromium film. Figure 8 shown.

[0074] Read "0": Remove the probe, the chromium film / lithium niobate layer / gold film is not conductive.

[0075] The lithium niobate film writes the array "1", and its piezoelectric atomic force microscope image is as follows Fig. 9 shown.

[0076] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A method for preparing a ferroelectric memory based on a lithium niobate thin film, characterized in that: The memory cell structure is composed of a substrate, a metal film I, a lithium niobate film layer, and a metal film II stacked from bottom to top. The polarization intensity P s The direction is within the plane; the preparation method specifically comprises the following steps: S1, writing phase, recorded as "1" phase; The initial polarization intensity Ps of the lithium niobate thin film layer is directed to the right; the scheme 1 in which the probe applies positive pressure or the scheme 2 in which the probe applies negative pressure is adopted; Solution 1: When the probe is applied with a positive voltage and contacts the surface of lithium niobate, the probe is required to be located on the right side of the metal film II. At this time, the lithium niobate on the left side of the probe has an electric field distribution that is in the same direction as its initial polarization intensity P. s The opposite component leads to the polarization intensity P of lithium niobate on the left side of the probe. s The direction is deflected by 180°, and a polarized region appears; The domain wall has a polarization intensity P s The interface of adjacent regions with different directions. At this time, the domain wall is written below the lithium niobate film and contacts the lower surface of the metal film II and the upper surface of the metal film I. Because the domain wall has a better conductivity than the body domain, the metal film II and the metal film I can conduct electricity from top to bottom. Solution 2: When the probe is applied with a negative voltage and contacts the surface of lithium niobate, the probe is required to be located on the left side of the metal film II. At this time, the lithium niobate on the right side of the probe has an electric field distribution that is different from its initial polarization intensity P. s The opposite component leads to the polarization intensity P of lithium niobate on the right side of the probe. s The direction is deflected by 180°, and a polarized region appears; The domain wall is written below the lithium niobate film, contacting the lower surface of metal film II and the upper surface of metal film I; Since the domain wall has a better conductivity than the bulk domain, the metal film II and the metal film I can conduct electricity up and down; S2, erasing phase, recorded as "0" phase; For the "1" state formed in scheme 1, the probe needs to apply negative pressure to contact the polarized area or the surrounding area to achieve domain wall erasure, thereby converting it to the "0" state; when erasing the domain wall, the electric field distribution of the probe has a component in the opposite direction to the polarization intensity Ps of the polarized area, and the polarization intensity P s Deflection occurs again, so that the domain wall below the metal film II is erased or deviates from the metal film II, and the metal film II and the metal film I are not conductive above and below; For the "1" state formed by scheme 2, the probe needs to apply positive pressure to contact the polarized area or the surrounding area to achieve domain wall erasure, thereby converting it to the "0" state; when erasing the domain wall, the probe needs to be applied with positive pressure to contact the polarized area or the surrounding area; The electric field distribution of the probe exists in the polarization region with polarization intensity P s The component in the opposite direction, the polarization intensity P of the polarization area s Deflection occurs again, so that the domain wall below the metal film II is erased or deviates from the metal film II, and the metal film II and the metal film I are not conductive above and below; S3, reading phase; Remove the probe and read the conductive state between metal film II and metal film I; Let the conductive state be "1" and the non-conductive state be "0"; "1" reading: The domain wall has a better conductivity than the lithium niobate bulk material. When the domain wall contacts the metal film I and the metal film II, the metal film II and the metal film I are considered to be in a conductive state. "0" reading: When the domain wall is erased or is far enough away from the metal film II, the metal film I and the metal film II are in a non-conductive state.

2. The preparation method according to claim 1, characterized in that: During the writing and erasing stages, when voltage is applied to the probe and it contacts lithium niobate, the probe / lithium niobate / metal film II is in an open circuit state; the probe / lithium niobate / metal film I is in an open circuit state; the power supply connected to the probe is not connected to metal film I or metal film II to form a loop.

3. The preparation method according to claim 1, characterized in that: During the writing and erasing phases, the probes can be replaced by thin films made of any conductive objects.

4. The preparation method according to claim 1, characterized in that: In the writing stage, when the prepared conductive domain wall is not in strict contact with the metal film II or the metal film I, it still has good conductivity; In the conductive range, there is a certain distance between the conductive domain wall and the metal film I or the metal film II.

5. The preparation method according to claim 1, characterized in that: In the reading stage, the read information, such as the current, passes through the thickness of the lithium niobate layer from top to bottom. The reading structure of the storage unit "1" is composed of metal film II / domain wall / metal film I stacked up and down; the reading structure of the storage unit "0" is composed of metal film II / lithium niobate body / metal film I stacked up and down.

6. The preparation method according to claim 1, characterized in that: During the erasing phase, the area contacted by the probe is within the polarization region, or in the area surrounding the polarization region.

7. The preparation method according to claim 1, characterized in that: In the erase phase, the memory cell write and erase structure is composed of probe / lithium niobate; if metal film I or metal film II is removed, the domain wall preparation and erase process can still be completed by the probe to which voltage is applied.

8. The preparation method according to claim 1, characterized in that: During the erasing phase, when the probe contacts the "1" polarization region, the polarization region will be partially erased; when the probe contacts outside the "1" polarization region, the "1" polarization region will be completely erased, and new polarization regions will appear in other areas around the probe.