Surface treatment method for improving photoelectric property of perovskite

By using 2-(1-cyclohexenyl)ethylammonium salt solution to treat the perovskite film to form a low-dimensional cover layer, the problem of insufficient photoelectric performance and stability of perovskite is solved, and the perovskite film is realized Efficient repair and passivation are suitable for solar cells and LED fields, reducing raw material costs and suitable for large-scale commercial applications.

CN119072202AActive Publication Date: 2024-12-03SHANGHAI JIAOTONG UNIV

Patent Information

Application Number
CN202311147195.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-09-06
Publication Date
2024-12-03
Estimated Expiration
2043-09-06

AI Technical Summary

Technical Problem

While improving the photoelectric properties of perovskites, the commonly used n-octamine hydroiodate treatment method makes it difficult to prepare subsequent hole transport layers, and the stability of perovskites to light, heat and water is still insufficient, which limits the Its commercial application.

Method used

The surface of the perovskite film is treated with 2-(1-cyclohexenyl)ethylammonium salt solution, and the low-dimensional cover layer is formed by annealing to repair and passivate the defects on the surface of the film, and improve its stability and photoelectric properties.

Benefits of technology

It has achieved all-round defect repair of perovskite films, improved its photoelectric conversion performance and stability, is suitable for solar cells, LEDs and other fields, and reduced raw material costs, and is suitable for large-scale commercial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119072202A_ABST
    Figure CN119072202A_ABST
Patent Text Reader

Abstract

The invention provides a surface treatment method for improving the photoelectric property of perovskite, and the method comprises the following steps: S1, coating the surface of a perovskite film with a 2-(1-cyclohexenyl) ethyl ammonium salt solution, and carrying out the surface treatment; and S2, after the solvent on the surface of the perovskite thin film is removed, annealing is carried out. According to the method, the surface of the thin film is treated by using the solution of the 2-(1-cyclohexenyl) ethyl ammonium salt, and the thin layer with multiple defects on the surface is converted into a more stable low-dimensional covering layer, so that the defects on the surface of the thin film are repaired and passivated, and the stability and the photoelectric property of perovskite are improved. The perovskite thin film treated by the method has low surface defect density and good stability, and the treated thin film has obviously enhanced photoelectric conversion performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of perovskite photovoltaics, relates to a surface treatment method for improving the photoelectric performance of perovskite, and specifically designs a method for improving the photoelectric performance of a perovskite film by repairing and passivating surface defects of the perovskite film. Background Art

[0002] Metal halide perovskites possess almost all the properties required for photoelectric conversion applications, such as high absorption coefficient, long carrier diffusion length and high defect tolerance. Therefore, they are considered to be one of the candidate materials for the next generation of solar cells, LEDs and other fields. However, the intrinsic sensitivity of three-dimensional perovskites to light, heat, water and oxygen limits their commercial application. In contrast, low-dimensional perovskites, although their photoelectric properties are poor, have better stability. Researchers have found that forming a low-dimensional (two-dimensional, one-dimensional) covering layer on the surface of three-dimensional perovskites can not only improve the stability of three-dimensional perovskites to light, heat, water and oxygen, but the covered low-dimensional perovskites can also passivate the defects on the surface of perovskites and improve the photoelectric properties of three-dimensional perovskites. Despite this, the current methods still face certain shortcomings. For example, the treatment of the perovskite surface with n-octylamine hydroiodide (OAI), one of the most commonly used treatment materials, has improved stability and photoelectric properties, but due to its long organic alkane chain, it brings new challenges to the preparation of subsequent hole transport layers. Therefore, exploring a method that can improve the stability and photoelectric properties of perovskite without introducing new problems is particularly important for promoting the commercial application of perovskite. Summary of the invention

[0003] In view of the defects of the prior art, the present invention relates to a surface treatment method for improving the photoelectric performance of perovskite, which is a method for repairing and passivating the defects on the surface of a perovskite film. The surface of the film is treated with a solution of 2-(1-cyclohexenyl)ethylammonium salt, and a thin layer with many defects on the surface is converted into a more stable low-dimensional covering layer, thereby achieving repair and passivation of the surface defects of the film, thereby improving the stability and photoelectric performance of the perovskite.

[0004] The objective of the present invention is achieved through the following technical solutions:

[0005] In a first aspect, the present invention provides a surface treatment method for improving the photoelectric performance of perovskite, the method comprising the following steps:

[0006] S1, applying a 2-(1-cyclohexenyl)ethylammonium salt solution on the surface of the perovskite film for surface treatment;

[0007] S2. After removing the solvent from the surface of the perovskite film, annealing is performed.

[0008] As an embodiment of the present invention, in step S1, the solvent in the 2-(1-cyclohexenyl)ethylammonium salt solution includes at least one of chloroform and isopropanol.

[0009] As an embodiment of the present invention, in step S1, the 2-(1-cyclohexenyl)ethylammonium salt includes at least one of 2-(1-cyclohexenyl)ethylammonium iodide (CHEAI), 2-(1-cyclohexenyl)ethylammonium bromide (CHEABr), CHEA2PbI4, and CHEA2PbBr4.

[0010] Furthermore, CHEA2PbI4 and CHEA2PbBr4 are two-dimensional perovskites generated by halogen salts of 2-(1-cyclohexenyl)ethylamine and lead halides (PbI2, PbBr2).

[0011] As an embodiment of the present invention, in step S1, the concentration of 2-(1-cyclohexenyl)ethylammonium salt in the 2-(1-cyclohexenyl)ethylammonium salt solution is 0.5-10 g / L.

[0012] As an embodiment of the present invention, in step S1, the coating amount of the 2-(1-cyclohexenyl)ethylammonium salt solution is 0.01-0.03 mL / cm 2 .

[0013] In some embodiments, the coating amount of the 2-(1-cyclohexenyl)ethylammonium salt solution is 0.02-0.025 mL / cm 2 .

[0014] As an embodiment of the present invention, in step S1, the perovskite film includes an organic-inorganic hybrid lead-halogen perovskite film and an all-inorganic cesium-lead-halogen perovskite film.

[0015] In some embodiments, the perovskite film is a formamidinium lead iodide (FAPbI3) perovskite film.

[0016] As an embodiment of the present invention, in step S1, the coating method includes at least one of a spin coating method and a coating method.

[0017] As an embodiment of the present invention, when the spin coating method is used, the rotation speed is 1000-6000 rpm and the time is 5-60s; when the coating method is used, the gas flow used to assist the coating includes at least one of dry air and inert gas.

[0018] In the present invention, the auxiliary gas flow includes at least one of nitrogen and argon.

[0019] As an embodiment of the present invention, in step S2, when the coating method is adopted, airflow can be used to assist in removing the surface solvent; when the spin coating method is adopted, the film will rotate at high speed, and the excess solvent will be directly thrown off the film during the rotation process, and the remaining solvent will be dried by air convection during the spin coating process.

[0020] As an embodiment of the present invention, in step S2, the annealing temperature is 60-120°C and the time is 0.5-10 min.

[0021] In some embodiments, the annealing temperature is 100° C. and the annealing time is 0.5-2 min.

[0022] The present invention uses 2-(1-cyclohexenyl)ethylammonium salt to post-treat the surface of a perovskite film, uses 2-(1-cyclohexenyl)ethylammonium salt to chemically react with the surface of the perovskite to repair and passivate defects on the surface of the film, forms a passivation layer on the surface of the film and at the grain boundary, improves the stability of the perovskite by inhibiting ion migration in the perovskite and blocking water and oxygen, and improves the photoelectric performance of the perovskite by promoting the separation and extraction of carriers.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] 1. Since the impurity phase in the perovskite film will become the recombination center of the carriers and the site for inducing phase separation of the perovskite, it is crucial to eliminate the impurity phase remaining on the surface of the film during the preparation process to improve the photoelectric conversion performance and stability of the perovskite. The 2-(1-cyclohexenyl)ethylammonium salt used in the present invention can not only react with the uncoordinated lead halide and the residual lead halide on the surface of the film to generate a low-dimensional perovskite, but also react with the impurity phase (yellow phase) to convert the impurity phase into a low-dimensional perovskite, thereby achieving all-round defect repair of the film, thereby improving its photoelectric conversion performance and stability.

[0025] 2. Using the method of the present invention to treat the perovskite film can not only repair and passivate the surface defects of the film, but the 2-(1-cyclohexenyl)ethylammonium salt in the present invention can also convert the residual lead halide at the grain boundary into a low-dimensional perovskite that grows vertically on the substrate, thereby achieving deep defect repair of the film; and the vertically grown low-dimensional perovskite provides a channel for the extraction of carriers (the in-plane mobility of carriers in the low-dimensional perovskite is much higher than the mobility between layers), thereby promoting the extraction of bulk carriers in the film and greatly improving the filling of the device.

[0026] 3. The present invention uses 2-(1-cyclohexenyl)ethylammonium salt to treat the perovskite film, so that the wettability of the treated film to chlorobenzene is almost unchanged, which is conducive to the large-area preparation of high-quality carrier transport layers.

[0027] 4. The perovskite treated by the method of the present invention has good wet and heat stability and can be widely used in solar cells, detectors, LEDs and other fields.

[0028] 5. The processing method of the present invention is conducive to the preparation of the subsequent hole transport layer of the perovskite film, so that the perovskite solar cell module prepared using the perovskite film has a higher fill factor and exhibits better performance.

[0029] 6. The raw material cost of the perovskite processed by the method of the present invention is low, which is conducive to large-scale commercial application.

[0030] 7. The present invention has low requirements on equipment, is simple to operate, and is conducive to large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Other features, objects and advantages of the present invention will become more apparent from the detailed description of non-limiting embodiments made with reference to the following drawings:

[0032] Figure 1 is the XRD pattern of CHEAI;

[0033] Figure 2 It is a characteristic diagram of CHEA2PbI4; wherein, Figure A is a physical diagram of CHEA2PbI4, and Figure B is the XRD and single crystal XRD diffraction diagram of CHEA2PbI4;

[0034] Figure 3 is a SEM image of the perovskite film obtained in Example 1;

[0035] Figure 4 is the X-ray diffraction pattern of the perovskite film obtained in Example 1;

[0036] Figure 5 is the contact angle of the perovskite film surface obtained in Example 1 to water;

[0037] Figure 6 The JV curve of the solar cell device prepared by the perovskite film obtained in Example 1;

[0038] Figure 7 It is a comparison diagram of the yellow phase perovskite film before and after treatment in Example 1; wherein, Figure A is a UV-visible absorption spectrum of the yellow phase perovskite film and the yellow phase film after CHEAI treatment, and Figure B is an XRD of the yellow phase perovskite film and the yellow phase film after CHEAI treatment;

[0039] Figure 8 The JV curve diagram of the solar cell module prepared by the perovskite film obtained in Example 2;

[0040] Fig. 9This is a physical picture of a solar cell module prepared using the perovskite film obtained in Example 2;

[0041] Fig.10 This is a graph of the electroluminescent efficiency of an LED device prepared from the perovskite film obtained in Example 3;

[0042] Fig.11 The contact angles of the perovskite film surface obtained by the comparative sample in Comparative Example 1, the OAI treatment and the 2-(1-cyclohexenyl)ethylammonium iodide (CHEAI) treatment to the commonly used hole transport layer solution;

[0043] Fig.12 The JV curves of the solar cell modules prepared by the control sample in Comparative Example 1, the perovskite thin film treated with OAI and the perovskite thin film treated with 2-(1-cyclohexenyl)ethylammonium iodide;

[0044] Fig.13 It is a comparison chart of the yellow phase perovskite film before and after treatment in Comparative Example 1; wherein, Figure A is the UV-visible absorption spectrum of the yellow phase perovskite film and the yellow phase film after being treated with CHEAI, and Figure B is the XRD of the yellow phase perovskite film and the yellow phase film after being treated with CHEAI. DETAILED DESCRIPTION

[0045] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. The following examples are implemented on the premise of the technical solution of the present invention, provide detailed implementation methods and specific operation processes, and will help those skilled in the art to further understand the present invention. It should be pointed out that the protection scope of the present invention is not limited to the following embodiments, and several adjustments and improvements made under the premise of the concept of the present invention all belong to the protection scope of the present invention.

[0046] The preparation method of 2-(1-cyclohexenyl)ethylammonium salt (i.e., CHEAI, CHEABr, CHEA2PbI4, CHEA2PbBr4) in the present invention is as follows:

[0047] Synthesis of CHEAI: Add 9.5 mL (55–58 wt%) of HI solution to 4 mL of ethanol and 1 mL of isopropanol solution, stir evenly, and slowly add 5 mL of 2-(1-cyclohexenyl)ethylamine in an ice-water bath (exothermic reaction, the ice-water bath is to avoid overheating of the solution), then heat to 75°C to dissolve, and after complete dissolution, cool to –20°C to crystallize. Finally, wash the resulting crystals with ether or ethyl acetate 5 times. Figure 1 This is the XRD pattern of CHEAI.

[0048] Synthesis of CHEABr: The synthesis of CHEABr is the same as that of CHEAI, except that HI acid solution is replaced by HBr solution.

[0049] Synthesis of CHEA2PbI4: 0.56 mmol of CHEAI was dissolved in 4 mL of ethanol to obtain solution A; 0.28 mmol of PbI2 was dissolved in 4 mL (55–58 wt%) of HI solution. After complete dissolution, 3 mL of ethanol was added and mixed to obtain solution B. After heating solution A and solution B to ~60°C, solution A was added to solution B to obtain solution C. Solution C was slowly cooled to obtain CHEA2PbI4 single crystals. Figure 2 The physical picture and XRD diagram of CHEA2PbI4.

[0050] Synthesis of CHEA2PbBr4: The synthesis of CHEA2PbBr4 is same as that of CHEA2PbI4, except that lead iodide and hydroiodic acid are replaced by lead bromide and hydrobromic acid respectively.

[0051] Note that among the preparation methods of the above reagents, the present invention only provides a preparation method that is simple to operate.

[0052] It should be noted that the comparative sample referred to in the present invention is a perovskite film sample obtained without any treatment on the surface of the perovskite film or a device prepared based on the film.

[0053] Example 1

[0054] Example 1 Taking a 3 g / L 2-(1-cyclohexenyl)ethylammonium iodide (CHEAI) chloroform solution as an example, a formamidinium lead iodide (FAPbI3) perovskite film is treated by spin coating, and the method comprises the following steps:

[0055] S1. Dissolve 3 mg of 2-(1-cyclohexenyl)ethylammonium iodide in 1 mL of chloroform to obtain solution A;

[0056] S2. Drop 0.1 mL of solution A onto a 2×2 cm 2 The surface of the perovskite film was then maintained at 5000 rpm for 20 seconds;

[0057] S3, annealing the spin-coated perovskite film at 100° C. for 1 minute.

[0058] Figure 3 The SEM images of the formamidinium lead iodide perovskite film obtained in Example 1 and the comparative sample show that vertically grown two-dimensional perovskite exists at the grain boundaries after CHEAI treatment. Figure 4 The X-ray diffraction patterns of the formamidinium lead iodide perovskite film obtained in Example 1 and the comparative sample show that the FAPbI3 obtained in Example 1 retains its original crystal structure, and the diffraction peak belonging to lead iodide disappears, and the diffraction peak of the two-dimensional perovskite appears at 5.19°; Figure 5 The contact angle test result of the formamidinium lead iodine perovskite film surface to water obtained in Example 1 shows that the contact angle increases significantly after CHEAI treatment, which is beneficial to improving the wet stability of the perovskite. Figure 6 Table 1 and Table 2 are respectively the JV curves and corresponding parameters of the formamidinium lead iodine perovskite solar cell obtained in Example 1. It can be seen that after treatment, the photoelectric conversion performance of the device is significantly improved.

[0059] Table 1. Photoelectric conversion parameters of devices prepared before and after CHEAI treatment of perovskite films

[0060] PCE(%) FF(%) <![CDATA[J SC (mA cm -2 )]]> <![CDATA[V OC (V)]]> Comparison sample 22.87 82.70 25.83 1.07 CHEAI treatment 25.20 86.18 25.87 1.13

[0061] Yellow-phase perovskite conversion to 2D experiments

[0062] The CHEAI solution used in the above Example 1 to treat the perovskite film was used to treat the yellow phase perovskite film in the same manner.

[0063] Figure 7 A is the UV-visible absorption spectrum of the yellow phase and the film after the yellow phase was treated with CHEAI. It can be seen from the figure that after the CHEAI treatment, the light absorption characteristics of the yellow phase film have changed significantly. The absorption peak of the yellow phase at a wavelength of 385nm almost disappears, and new absorption peaks belonging to 2D perovskite appear at 509nm and 580nm, indicating that the yellow phase perovskite is converted into 2D perovskite after CHEAI treatment. Figure 7 B is the XRD pattern of the yellow phase and the film after the yellow phase was treated with CHEAI, which further proves that the yellow phase film is almost completely converted into 2D perovskite after CHEAI treatment.

[0064] Example 2

[0065] Example 2 Taking the preparation of a large-area component by treating a formamidine lead iodide perovskite film with a 2 g / L isopropanol solution of 2-(1-cyclohexenyl)ethylammonium iodide by spin coating as an example, the method comprises the following steps:

[0066] S1. Dissolve 2 mg of 2-(1-cyclohexenyl)ethylammonium iodide in 1 mL of chloroform to obtain solution A;

[0067] S2. Add 0.5 mL of solution A to a 5×5 cm 2 The surface of the perovskite film was then maintained at 5000 rpm for 20 seconds;

[0068] S3, annealing the spin-coated perovskite film at 100° C. for 2 minutes.

[0069] Figure 8Table 2 and Table 3 are respectively the JV curves and corresponding parameters of the solar cell module prepared from the formamidinium lead iodide perovskite film obtained in Example 2. It can be seen that after surface treatment with 2-(1-cyclohexenyl)ethylammonium iodide, the photoelectric conversion performance of the module is significantly improved. Fig. 9 This is a physical picture of a perovskite solar cell module prepared based on the perovskite film obtained in Example 2.

[0070] Table 2. 12.25 cm prepared perovskite films before and after CHEAI treatment 2 Photoelectric conversion parameter table of components

[0071] PCE(%) FF(%) <![CDATA[J SC (mA cm -2 )]]> <![CDATA[V OC (V)]]> Comparison sample 17.86 73.67 3.73 6.49 CHEAI treatment 20.77 84.06 3.73 6.62

[0072] Example 3

[0073] The method of this embodiment is the same as that of embodiment 1, except that the annealing time in step 3 is 30 seconds.

[0074] Fig.10 This is a graph of the electroluminescence efficiency of the LED device prepared with the formamidinium lead iodide perovskite film obtained in Example 3 at different voltages. It can be seen that the LED device prepared with the perovskite film treated with 2-(1-cyclohexenyl)ethylammonium iodide has significantly improved efficiency at the same voltage.

[0075] Comparative Example 1

[0076] The method of this comparative example is the same as that of Example 1, except that the formamidinium lead iodide perovskite film is treated with n-octyl hydroiodide (OAI) in the same manner as that of Example 1. Fig.11 The contact angles of the perovskite film surface obtained by the control sample in the comparative example, OAI treatment and 2-(1-cyclohexenyl)ethylammonium iodide treatment to the commonly used hole transport layer solution. It can be seen that the contact angle of the perovskite film surface obtained by 2-(1-cyclohexenyl)ethylammonium iodide treatment has almost no change, while the contact angle after OAI treatment increases from 9.9° to 43.6°. Good wettability is conducive to building a good interface contact. Fig.12 Table 3 and Table 4 are the JV curves and corresponding parameters of the perovskite solar cell modules prepared by the control sample in Comparative Example 1, the perovskite film treated with OAI and the perovskite film treated with 2-(1-cyclohexenyl)ethylammonium iodide. The solar cell module treated with 2-(1-cyclohexenyl)ethylammonium iodide shows better performance, with a fill factor (FF) exceeding 84%, which is much higher than the fill factor obtained by the control sample and the OAI treatment.

[0077] Similarly, the method of treating the yellow phase with the CHEAI solution in Example 1 was adopted, CHEAI was replaced with the commonly used post-treatment amine salt OAI, and the yellow phase film was treated with OAI. Fig.13 A is the UV-visible absorption spectrum of the yellow phase film before and after OAI treatment. It can be seen that the absorption spectrum before and after treatment is still dominated by the yellow phase absorption spectrum, indicating that the main body of the yellow phase perovskite has not changed. A very weak absorption peak belonging to low-dimensional perovskite appears near 570nm, which mainly comes from a small amount of uncoordinated lead iodide on the surface of the yellow phase and a small amount of 2D perovskite generated by the reaction of OAI. Fig.13 The XRD patterns of the yellow phase in B before and after OAI treatment further prove that after OAI treatment, the film still maintains the yellow phase as the main component, with only a weak diffraction peak from 2D appearing around 3.8°, which is consistent with the conclusion of the UV-visible absorption spectrum. This shows that the commonly used OAI salt post-treatment can only convert the residual lead iodide and uncoordinated lead iodide into low-dimensional perovskite.

[0078] Table 3. 12.25 cm prepared perovskite films before and after different salt treatments 2 Photoelectric conversion parameter table of components

[0079] PCE(%) FF(%) <![CDATA[J SC (mA cm -2 )]]> <![CDATA[V OC (V)]]> Comparison sample 17.86 73.67 3.73 6.49 CHEAI treatment 20.77 84.06 3.73 6.62 OAI Processing 19.45 79.68 3.74 6.53

[0080] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art may make various modifications or variations within the scope of the claims, which do not affect the essence of the present invention.

Claims

1. A surface treatment method for improving the photoelectric performance of perovskite, characterized in that: The surface treatment method comprises the following steps: S1, applying a 2-(1-cyclohexenyl)ethylammonium salt solution on the surface of the perovskite film for surface treatment; S2. After removing the solvent from the surface of the perovskite film, annealing is performed.

2. The surface treatment method according to claim 1, characterized in that: In step S1, the solvent in the 2-(1-cyclohexenyl)ethylammonium salt solution includes at least one of chloroform and isopropanol.

3. The surface treatment method according to claim 1, characterized in that: In step S1, the 2-(1-cyclohexenyl)ethylammonium salt includes at least one of CHEAI, CHEABr, CHEA2PbI4, and CHEA2PbBr4.

4. The surface treatment method according to claim 1, characterized in that: In step S1, the concentration of 2-(1-cyclohexenyl)ethylammonium salt in the 2-(1-cyclohexenyl)ethylammonium salt solution is 0.5-10 g / L.

5. The surface treatment method according to claim 1, characterized in that: In step S1, the coating amount of the 2-(1-cyclohexenyl)ethylammonium salt solution is 0.01-0.03 mL / cm 2 .

6. The surface treatment method according to claim 1, characterized in that: In step S1, the perovskite film includes an organic-inorganic hybrid lead-halogen perovskite film and an all-inorganic cesium-lead-halogen perovskite film.

7. The surface treatment method according to claim 1, characterized in that: In step S1, the coating method includes at least one of a spin coating method and a coating method.

8. The surface treatment method according to claim 7, characterized in that: When the spin coating method is used, the spin coating speed is 1000-6000 rpm and the time is 5-60s; when the coating method is used, the gas flow used to assist the coating includes at least one of dry air and inert gas.

9. The surface treatment method according to claim 1, characterized in that: In step S2, the annealing temperature is 60-120°C and the time is 0.5-10 min.

10. A perovskite film prepared by the surface treatment method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • A-site doped halide perovskite type solar cell and preparation method thereof

    CN115942757A

  • Perovskite thin film preparation method, perovskite solar cell and laminated cell

    CN116456790A

  • Photoelectric conversion element and method for manufacturing the same, and solar cell using the photoelectric conversion element

    JP2015119023A

Cited By

  • Perovskite film surface treatment method based on micro-nano space confinement crystallization

    CN122476808A