Preparation method of perovskite solar cell
The PCBM film is preheated and heated annealed through continuous laser scanning technology, which solves the particle agglomeration and pore problems caused by crystal defects in perovskite solar cells, and significantly improves the performance of perovskite solar cells.
Patent Information
- Application Number
- CN202411192058.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-03
AI Technical Summary
The crystal defects that are common in the manufacturing process of perovskite solar cells lead to particle agglomeration and holes in the electron transport layer, affecting the charge recombination and improvement of perovskite solar cells' performance.
The PCBM film is preheated and heated annealed by continuous laser scanning technology. By adjusting the laser power and scanning path, local low-temperature heating is achieved, reducing the occurrence of particle agglomeration and pore phenomena, and forming a more uniform film layer.
It effectively reduces particle agglomeration and pore phenomena, and improves the performance of perovskite solar cells, including improving open circuit voltage, photoelectric conversion efficiency, fill factor and conductivity.
Smart Images

Figure CN119072206A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor optoelectronic technology, and in particular to a method for preparing a perovskite solar cell. Background Art
[0002] Perovskite solar cells have unparalleled advantages in terms of their excellent photovoltaic performance and low production cost, and have become the rising star of the next generation of photovoltaic technology. Charge recombination caused by the common crystal defects in perovskite solar cells is still one of the main factors limiting the further improvement of the performance of perovskite solar cells. The emergence of these undesirable defects is inevitable in the solution-based film preparation method, especially with the upgrading of perovskite manufacturing. This effect will cause particle agglomeration and holes in the electron transport layer, especially the PCBM electron transport layer, which makes it difficult for the performance of perovskite solar cells to reach the ideal expectations, and there is still room for improvement.
[0003] Therefore, a method is needed to reduce the crystal defects generated during the manufacturing process of perovskite solar cells to improve the performance of perovskite solar cells. Summary of the invention
[0004] In order to solve the problem that crystal defects are inevitably generated during the manufacturing process of perovskite solar cells, causing particle agglomeration and holes in the electron transport layer, resulting in unsatisfactory performance of the perovskite solar cell, the present invention provides a method for preparing a perovskite solar cell.
[0005] The present invention provides a method for preparing a perovskite solar cell, comprising the following steps: forming an electron transport layer; the step of forming the electron transport layer comprises: forming a PCBM film; using continuous laser scanning to preheat the PCBM film; and heating and annealing the PCBM film to form the electron transport layer.
[0006] Optionally, the continuous laser is a continuous linear laser; the area of the spot projected by the continuous laser on the PCBM film is smaller than the area of the PCBM film; the linear laser scans back and forth on the surface of the PCBM film so that the laser scanning path covers the entire surface of the PCBM film; and the heating annealing uses a hot stage annealing.
[0007] Optionally, the linear laser reciprocates 1 to 10 times.
[0008] Optionally, the scanning movement speed of the linear laser is 1mm / s-20mm / s.
[0009] Optionally, the scanning movement acceleration of the linear laser is 1 mm / S 2 -20mm / S2 .
[0010] Optionally, the power of the laser emitting the linear laser is 50mW-700mW.
[0011] Optionally, in the step of using continuous laser to scan the PCBM film for preheating, a linear laser scanner is used for scanning; the linear laser scanner includes: a carrier suitable for carrying a solar cell substrate to be scanned; the solar cell substrate is at least formed with the PCBM film; a laser emitter suitable for emitting the linear laser; a bracket installed on the carrier and connected to the laser emitter; the bracket includes: a horizontal guide rail for adjusting the horizontal position of the laser emitter; and a vertical guide rail for adjusting the vertical distance between the laser emitter and the solar cell substrate.
[0012] Optionally, the method for preparing a perovskite solar cell also includes the following steps: providing a transparent base plate; forming a transparent conductive layer on the transparent base plate; or providing a transparent base plate with a transparent conductive layer formed thereon; then, forming a hole transport layer on the transparent conductive layer; forming a perovskite absorption layer on the hole transport layer; forming the electron transport layer on the perovskite absorption layer; forming a hole blocking layer on the electron transport layer; and forming a metal electrode on the hole blocking layer.
[0013] Optionally, the steps of forming the perovskite absorption layer include: spin coating a perovskite precursor solution; spin coating the perovskite precursor solution in two steps; adding a perovskite reaction solution during the second step of spin coating the precursor solution; and heating and annealing a thin film formed by a mixture of the perovskite precursor solution and the perovskite reaction solution after spin coating.
[0014] Optionally, the transparent base plate includes glass; the material of the transparent conductive layer includes ITO or FTO; the material of the hole transport layer includes nickel oxide; the solute material of the perovskite precursor solution has a general formula of ABX3, wherein A is one or more of methylamine, methylamine, and cesium, B is lead or tin, and X is iodine or bromine; the material of the hole blocking layer includes PCB or SnO2; the material of the metal electrode includes gold, silver, copper or their alloys.
[0015] The beneficial effects of the technical solution provided by the present invention are:
[0016] The preparation method of the perovskite solar cell provided by the present invention, the step of forming an electron transport layer includes: forming a PCBM film; using a continuous laser to scan the PCBM film for preheating; heating and annealing the PCBM film to form the electron transport layer. By first using a continuous laser to preheat the PCBM film, and then using a conventional hot stage annealing process, the conventional annealing process is divided into two steps, and the linear laser scanning preheating continuous laser can achieve the effect of local low-temperature heating by adjusting the power, and the local low-temperature preheating gradually spreads to the entire film layer, which can make the particles in the PCBM film spread more evenly, greatly reduce the occurrence of particle agglomeration and hole phenomena, make the film layer smoother and more uniform, and thus improve the performance of the perovskite solar cell. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0018] Figure 1 A schematic diagram of a process for preparing a perovskite solar cell according to an embodiment of the present invention;
[0019] Figure 2 A schematic diagram of the state of a PCBM film layer being scanned by a linear laser in a method for preparing a perovskite solar cell according to an embodiment of the present invention;
[0020] Figure 3 A schematic structural diagram of a linear laser scanner used in a method for preparing a perovskite solar cell according to an embodiment of the present invention;
[0021] Figure 4 A schematic diagram of the structure of a perovskite solar cell prepared by a method for preparing a perovskite solar cell according to an embodiment of the present invention;
[0022] Figure 5 A scanning electron microscope image of an electron transport layer of a perovskite solar cell prepared by a method for preparing a perovskite solar cell according to an embodiment of the present invention;
[0023] Figure 6 This is a scanning electron microscope image of the electron transport layer of the perovskite solar cell prepared by the method of Comparative Example 1;
[0024] Figure 7 This is a scanning electron microscope image of the electron transport layer of the perovskite solar cell prepared by the method of Comparative Example 2;
[0025] Figure 8 JV curves of the perovskite solar cell prepared by the method for preparing a perovskite solar cell according to an embodiment of the present invention and the perovskite solar cell prepared by the methods of Comparative Examples 1 and 2. DETAILED DESCRIPTION
[0026] In order to solve the problem that crystal defects are inevitably generated during the manufacturing process of perovskite solar cells, causing particle agglomeration and holes in the electron transport layer, resulting in unsatisfactory performance of the perovskite solar cell, the present invention provides a method for preparing a perovskite solar cell.
[0027] The present invention provides a method for preparing a perovskite solar cell, comprising the following steps: forming an electron transport layer; the step of forming the electron transport layer comprises: forming a PCBM film; using continuous laser scanning to preheat the PCBM film; and heating and annealing the PCBM film to form the electron transport layer.
[0028] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] In the description of the present invention, it should be noted that the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inner", "outer", etc., indicating the orientation or positional relationship, are based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", and "third" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance.
[0030] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0031] In addition, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0032] Example
[0033] refer to Figure 1 This embodiment provides a method for preparing a perovskite solar cell, comprising the following steps:
[0034] forming an electron transport layer;
[0035] The step of forming an electron transport layer comprises:
[0036] Forming a PCBM film;
[0037] Scanning the PCBM film with a continuous laser to preheat it;
[0038] The PCBM film is heated and annealed to form the electron transport layer.
[0039] Specifically, in some embodiments, reference Figure 2 , a continuous laser 1 is used to scan and preheat the perovskite solar cell substrate 2 on the carrier 3, on which a PCBM film has been formed. Then, the perovskite solar cell substrate 2 is heated and annealed.
[0040] The preparation method of the perovskite solar cell provided by the present invention, the step of forming an electron transport layer includes: forming a PCBM film; using a continuous laser to scan the PCBM film for preheating; heating and annealing the PCBM film to form the electron transport layer. By first using a continuous laser to preheat the PCBM film, and then using a conventional hot stage annealing process, the conventional annealing process is divided into two steps, and the linear laser scanning preheating continuous laser can achieve the effect of local low-temperature heating by adjusting the power, and the local low-temperature preheating gradually spreads to the entire film layer, which can make the particles in the PCBM film spread more evenly, greatly reduce the occurrence of particle agglomeration and hole phenomena, make the film layer smoother and more uniform, and thus improve the performance of the perovskite solar cell.
[0041] Furthermore, the continuous laser is a continuous linear laser; the area of the spot projected by the continuous laser on the PCBM film is smaller than the area of the PCBM film; the linear laser scans back and forth on the surface of the PCBM film so that the path of the laser scanning covers the entire surface of the PCBM film; and the heating annealing uses hot stage annealing. In the prior art, one annealing method for the electron transport layer is to use a pulsed laser to directly anneal the film in one step. Compared with a continuous laser, a pulsed laser has a larger output power and is suitable for laser marking, cutting, and film scribing. For film annealing, the energy is too high, which will inevitably produce particle agglomeration and holes, and may damage the film, and the cost is too high for optimizing agglomeration. The above defects can be effectively avoided by preheating with a continuous linear laser and then heating and annealing using conventional methods, such as hot stage annealing.
[0042] Specifically, in some embodiments, the power of the laser emitting the linear laser is 50mW-700mW. The laser can select a suitable power within an appropriate range for scanning preheating. If the laser power is too low, it is difficult for the scanning heating to provide sufficient energy and it is difficult to affect the film layer. If the laser power is too high, it will directly cause agglomeration or holes. Therefore, the laser power is within the range of 50mW-700mW, which can strike a balance between effectively affecting the film and avoiding directly causing agglomeration or holes.
[0043] Specifically, in some embodiments, the number of reciprocating motions of the linear laser is 1-10 times. One reciprocating motion means that the laser scans once in a specified direction and then scans once in the opposite direction, which is regarded as one reciprocating motion. If the number of reciprocating motions is too small, the energy provided by the scanning heating is likely to be insufficient, and it is difficult to affect the film layer; if the number of reciprocating motions is too large, it is easy to directly cause agglomeration or holes. Therefore, when the number of reciprocating motions of the linear laser is within the range of 1-10 times, a balance can be achieved between effectively affecting the film and avoiding directly causing agglomeration or holes.
[0044] Specifically, in some embodiments, the scanning movement speed of the linear laser is 1 mm / s-20 mm / s.
[0045] Specifically, in some embodiments, the scanning movement acceleration of the linear laser is 1 mm / S 2 -20mm / S 2 .
[0046] If the moving speed or acceleration is too fast, the irradiated PCBM film position will receive less energy and it will be difficult to have a practical impact; if the moving speed or acceleration is too slow, it is easy to accumulate too much energy at the irradiation point, directly causing agglomeration or holes. Therefore, the scanning speed of the linear laser is 1mm / S 2-20mm / S 2 The scanning movement acceleration is 1mm / S within the range of 2 -20mm / S 2 Within this range, a balance can be achieved between effectively affecting the film and avoiding directly causing agglomeration or voiding.
[0047] Specifically, in some embodiments, the laser scanning area is 2.4×2.4 cm 2 . It can completely cover the area of a conventional solar cell, that is, it can cover the entire surface of the PCBM film. Specifically, in some embodiments, refer to Figure 3 In the step of using continuous laser to scan the PCBM film for preheating, a linear laser scanner is used for scanning; the linear laser scanner includes:
[0048] A carrier, suitable for carrying a solar cell substrate to be scanned; the solar cell substrate is at least formed with the PCBM film;
[0049] A laser emitter 4, adapted to emit the linear laser;
[0050] A bracket is mounted on the carrier and connected to the laser emitter 4; the bracket includes:
[0051] A horizontal guide rail 6, used for adjusting the horizontal position of the laser transmitter;
[0052] The vertical guide rail 5 is used to adjust the vertical distance between the laser emitter and the solar cell substrate.
[0053] refer to Figure 1 and Figure 4 In a specific embodiment, the method for preparing a perovskite solar cell further includes the following steps:
[0054] Provide a transparent bottom plate (not shown in the figure);
[0055] Forming a transparent conductive layer 600 on the transparent substrate;
[0056] Alternatively, a transparent substrate having a transparent conductive layer 600 formed thereon is provided; then,
[0057] forming a hole transport layer 500 on the transparent conductive layer 600;
[0058] forming a perovskite absorption layer 400 on the hole transport layer 500;
[0059] The electron transport layer 300 is formed on the perovskite absorption layer 400;
[0060] forming a hole blocking layer 200 on the electron transport layer 300;
[0061] The metal electrode 100 is formed on the hole blocking layer 200 .
[0062] Specifically, in some embodiments, the steps of forming the perovskite absorption layer include: spin coating a perovskite precursor solution; spin coating the perovskite precursor solution in two steps; adding a perovskite reaction solution during the second step of spin coating the precursor solution; and heating and annealing a thin film formed by a mixture of the perovskite precursor solution and the perovskite reaction solution after the spin coating is completed.
[0063] Specifically, in some embodiments, the transparent base plate includes glass; the material of the transparent conductive layer includes ITO or FTO; the material of the hole transport layer includes nickel oxide; the solute material of the perovskite precursor solution has a general formula of ABX3, wherein A is one or more of methylamine, methylamine, and cesium, B is lead or tin, and X is iodine or bromine; the material of the hole blocking layer includes PCB or SnO2; the material of the metal electrode includes gold, silver, copper or their alloys.
[0064] A specific implementation process is as follows:
[0065] A glass substrate having an ITO layer formed thereon, ie, ITO conductive glass, is provided.
[0066] The ITO conductive glass is pretreated, including: cleaning the ITO conductive glass: etching the numbers on the back of the ITO conductive glass in sequence with an etching knife, placing it in a culture dish, pouring deionized water and detergent, and wiping impurities on the surface of the ITO conductive glass with absorbent cotton. Put the cleaned ITO conductive glass into a polytetrafluoroethylene cleaning rack, put it in a beaker, cover it with plastic wrap and cover it tightly, pour detergent in sequence, and ultrasonicate it in an ultrasonic instrument with deionized water, anhydrous ethanol, acetone, and isopropanol for 20 minutes each. Blow dry the ITO conductive glass with an air gun, put the ITO conductive glass in a culture dish, and treat it in an ultraviolet ozone machine (UVO3) for 15 minutes. Preheat the ozone machine for 20 minutes before use.
[0067] Forming a hole transport layer. Disperse nickel oxide in ultrapure water at 10 mg / ml, filter after ultrasonication for 5 minutes, and spin-coat the treated ITO conductive glass at 4000 rpm for 30 seconds. Then heat and anneal at 100°C in air for 10 minutes to form a hole transport layer. After annealing, quickly transfer to a nitrogen glove box.
[0068] Forming a perovskite absorption layer. In a nitrogen glove box, the filtered 1.1M perovskite precursor solution was spin-coated on the upper surface of nickel oxide (i.e., the hole transport layer) at 1000 rpm / min for 10 seconds and 3000 rpm / min for 30 seconds, wherein 200 ul of anti-solvent chlorobenzene was injected when 15 seconds remained in the second step of the rotation process. After the spin coating was completed, it was immediately placed on a 115°C hot stage for annealing for 10 minutes. After the annealing was completed, the perovskite film was cooled to room temperature to obtain the annealed perovskite absorption layer film.
[0069] To form an electron transport layer, spin-coat a 0.02 g / ml PCBM chlorobenzene solution on the perovskite substrate, and drop the PCBM solution onto the perovskite absorption layer at 4000 rpm / min for 30 seconds. Figure 3 The linear laser shown in Figure 2 is used to apply the PCBM film to Figure 2 The laser scanning speed is 1mm / s and the scanning acceleration is 1mm / S 2 , laser power is 320mW. Scanning times are 3 times. Laser scanning area is 2.4*2.4cm 2 After linear laser preheating, annealing was performed on a hot plate at 70°C for 10 min.
[0070] The hole blocking layer is formed by spin coating BCP on the electron transport layer at 5000 rpm / min for 30 s.
[0071] The metal electrode is formed. The perovskite solar cell substrate formed with the electron transport layer and the hole blocking layer is transferred to the evaporation chamber and the vacuum is evacuated. When the vacuum reaches below the target vacuum, the Ag electrode is deposited, and the evaporation thickness is 100 nm. The perovskite solar cell is obtained.
[0072] In order to verify the improvement of the performance of the perovskite solar cell provided by the present invention, a comparative example is provided as follows: Comparative Example 1
[0073] The specific implementation process of the embodiment described above is different from that of the embodiment described above in that:
[0074] In the step of forming the electron transport layer, after spin coating the PCBM film, no linear laser preheating was used, and annealing was directly performed on a hot stage at 70° C. for 10 minutes.
[0075] The remaining steps are the same as the specific implementation process in the embodiment and will not be repeated here.
[0076] Comparative Example 2
[0077] The specific implementation process of the embodiment described above is different from that of the embodiment described above in that:
[0078] In the step of forming the electron transport layer, after spin coating the PCBM film, no linear laser preheating is used, and pulsed laser annealing is directly used for 10 minutes. The laser and other conditions used are the same as those in the embodiment, except that the laser is changed from continuous linear laser to pulsed laser, and the hot stage annealing after preheating is changed to direct pulsed laser annealing.
[0079] The remaining steps are the same as the specific implementation process in the embodiment and will not be repeated here.
[0080] The PCBM films processed during the preparation of the above three perovskite solar cells were photographed by scanning electron microscope. Figure 5 , Figure 6 , Figure 7 By comparison, it can be found that the PCBM film ( Figure 5 ), the surface particle flatness is significantly better than that of comparative example 1 ( Figure 6 ) and Comparative Example 2 ( Figure 7 ). Figure 6 and Figure 7 There is obvious particle agglomeration in the sample, and there are holes between the agglomerates. Figure 5 This indicates that the method of the embodiment of the present invention can effectively improve the particle agglomeration and hole phenomenon of the PCBM film.
[0081] The photoelectric performance of the perovskite solar cells obtained in the specific implementation process of the above embodiment, comparative example 1, and comparative example 2 is tested to obtain the following Table 1, Table 2, and Figure 8 :
[0082] From the contents shown in Table 1 and Table 2, refer to Figure 8 It can be seen from the line graph comparison that the method of the embodiment of the present invention, which first performs continuous linear laser preheating and then hot stage annealing, has significantly higher open circuit voltage, photoelectric conversion efficiency, fill factor, and short circuit current than Comparative Example 1 and Comparative Example 2. The conductivity is also significantly improved. Therefore, the method of the embodiment of the present invention can effectively improve the performance of perovskite solar cells.
[0083] Table 1 Comparison of photoelectric conversion performance of perovskite solar cells
[0084]
[0085] Table 2 Comparison of conductivity of perovskite solar cells
[0086]
[0087] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.
Claims
1. A method for preparing a perovskite solar cell, characterized in that: The following steps are involved: forming an electron transport layer; The step of forming an electron transport layer comprises: Forming a PCBM film; Scanning the PCBM film with a continuous laser to preheat it; The PCBM film is heated and annealed to form the electron transport layer.
2. The method for preparing a perovskite solar cell according to claim 1, characterized in that: The continuous laser is a continuous linear laser; The area of the spot projected by the continuous laser on the PCBM film is smaller than the area of the PCBM film; The linear laser scans and moves back and forth on the surface of the PCBM film so that the laser scanning path covers the entire surface of the PCBM film; Heating annealing uses hot stage annealing.
3. The method for preparing a perovskite solar cell according to claim 2, characterized in that: The number of reciprocating motions of the linear laser is 1 to 10 times.
4. The method for preparing a perovskite solar cell according to claim 2, characterized in that: The scanning movement speed of the linear laser is 1 mm / s-20 mm / s.
5. The method for preparing a perovskite solar cell according to claim 2, characterized in that: The scanning movement acceleration of the linear laser is 1 mm / S 2 -20mm / S 2 .
6. The method for preparing a perovskite solar cell according to claim 2, characterized in that: The power of the laser emitting the linear laser is 50 mW-700 mW.
7. The method for preparing a perovskite solar cell according to any one of claims 1 to 6, characterized in that: In the step of using continuous laser to scan the PCBM film for preheating, a linear laser scanner is used for scanning; The linear laser scanner comprises: A carrier, suitable for carrying a solar cell substrate to be scanned; the solar cell substrate is at least formed with the PCBM film; A laser emitter, adapted to emit the linear laser; A bracket, mounted on the carrier and connected to the laser emitter; The support comprises: A horizontal guide rail, used for adjusting the horizontal position of the laser transmitter; A vertical guide rail is used to adjust the vertical distance between the laser emitter and the solar cell substrate.
8. The method for preparing a perovskite solar cell according to claim 1, characterized in that: The following steps are also included: Provide transparent bottom plate; forming a transparent conductive layer on the transparent substrate; Alternatively, a transparent substrate having a transparent conductive layer formed thereon is provided; then, forming a hole transport layer on the transparent conductive layer; forming a perovskite absorption layer on the hole transport layer; The electron transport layer is formed on the perovskite absorption layer; forming a hole blocking layer on the electron transport layer; A metal electrode is formed on the hole blocking layer.
9. The method for preparing a perovskite solar cell according to claim 8, characterized in that: The steps of forming the perovskite absorption layer include: The perovskite precursor solution was spin-coated in two steps; The perovskite reaction solution is added during the second step of spin coating the precursor solution; After the spin coating is completed, the film formed by the mixture of the perovskite precursor solution and the perovskite reaction solution is heated and annealed.
10. The method for preparing a perovskite solar cell according to claim 9, characterized in that: The transparent bottom plate comprises glass; The material of the transparent conductive layer includes ITO or FTO; The material of the hole transport layer includes nickel oxide; The general formula of the solute material of the perovskite precursor solution is ABX3, wherein A is one or more of methylamine, methylamine, and cesium, B is lead or tin, and X is iodine or bromine; The material of the hole blocking layer includes PCB or SnO2; The material of the metal electrode includes gold, silver, copper or alloys thereof.
Citation Information
Cited By
Method for regulating and controlling crystallization of perovskite thin film based on surface laser annealing and preparation method of perovskite photovoltaic module
CN120265089A