Substrate, preparation method thereof, device and metal tunnel junction
By forming a modified layer of metal-carbon covalent bond on the substrate surface of the molecular device, the problem of instability of the molecular device environment is solved, the stability of the molecular tunnel junction and the thermal stability of the tunnel barrier are improved, and it is suitable for molecular electrons Applications of devices and plasmon components.
Patent Information
- Application Number
- CN202310650039.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-02
- Publication Date
- 2024-12-03
AI Technical Summary
Existing molecular devices are unstable in the surrounding environment, especially the self-assembled monolayer molecular film formed by metal-sulfur covalent bonds on the metal surface is prone to oxidation, resulting in instability of molecular tunnel junctions.
The substrate adopts metal-carbon covalent bonds and the preparation method thereof, by forming a modified layer on the substrate surface, the metal-carbon covalent bonds are formed by carbene compound and the metal substrate to improve the structural stability of the substrate, thereby improving the molecular devices and Environmental stability of metal tunnel junctions.
It realizes high stability of the substrate surface modification layer, improves the thermal stability of the tunnel barrier, and the excellent performance of carbene films in molecular tunnel junctions, which are suitable for the wide application of molecular electronic devices and plasmon components.
Smart Images

Figure CN119072207A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of molecular electronic devices and plasma devices, and in particular to a substrate and a preparation method thereof, a device, and a metal tunnel junction. Background Art
[0002] Since the discovery of molecular rectifiers, the preparation of low-energy multifunctional nanoelectronic devices through the synthesis and design of organic molecules is one of the most active frontier sciences. Studies have found that compared with inorganic dielectric materials (such as metal oxides), the easy synthesis and purification of organic compounds and the diversity of their own structures can greatly reduce the manufacturing cost of electronic devices. Therefore, in the past four decades, in addition to molecular diodes, other types of molecular electronic devices such as molecular switches, molecular transistors, molecular storage devices, molecular sensors and molecular thermoelectric devices have been reported in a series of reports. In addition, in the past decade, the plasmon phenomenon in molecular tunnel junctions has been studied, aiming to achieve the combination of nanoelectronics and nano-optics.
[0003] However, the above-mentioned molecular devices are restricted in their practical application and development. In particular, when they are used to prepare molecular tunnel junctions, the self-assembled monolayer molecular film (SAM) formed on the surface of the metal through the metal-sulfur covalent bond (MS) is relatively fragile in the surrounding environment and is easily oxidized. Summary of the invention
[0004] In order to overcome the problem of instability of molecular devices in the surrounding environment in the prior art, the present application provides a substrate and its preparation method, a device, and a metal tunnel junction, which improves the structural stability of the substrate by performing metal-carbon covalent bonds on the surface of the substrate, thereby improving the stability of the molecular device or the metal tunnel junction in the environment.
[0005] The first aspect of the present application provides a substrate, including a metal substrate and a modified layer covering the metal substrate, wherein the modified layer includes a carbene compound, and the carbene compound forms a metal-carbon covalent bond with the metal substrate. The metal-carbon covalent bond has excellent chemical stability, is not easily destroyed by reaction in the surrounding environment, and is not easily broken. The aforementioned carbene-modified metal surface, coating or substrate can be widely used in the preparation of various molecular devices, including, but not limited to, molecular electronic devices and molecular photonic devices, for example, molecular tunneling devices composed of molecular tunnel junctions.
[0006] In some embodiments, the carbene compound is a monomer. In other embodiments, the carbene compound is a polymer.
[0007] In some embodiments, the carbene compound is a derivative of a first compound, the first compound comprising a diaryldiazomethane.
[0008] In some embodiments, the diaryldiazomethane comprises a compound of Formula 1,
[0009]
[0010] In formula 1, R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , R 8 , R 9 and R 10 Each independently selected from hydrogen atom, substituted or unsubstituted C1-C20 alkyl, substituted or unsubstituted C1-C20 alkoxy, substituted or unsubstituted phenyl, substituted or unsubstituted heteroaryl, substituted substituents are independently selected from amino, diazo. Heteroaryl is a composite structure composed of aromatic ring and non-aromatic ring group, wherein aromatic ring includes but is not limited to benzene ring, thiophene ring, pyrrole ring, etc., and non-aromatic ring group includes but is not limited to oxygen, nitrogen, sulfur and other elements.
[0011] In some embodiments, heteroaryl includes phenoxy.
[0012] In some embodiments, the first compound includes but is not limited to bis(diaryldiazomethane). Bis(diaryldiazomethane) has a symmetrical structure. On the one hand, it can form a carbene compound with two carbene sites. Then, one molecule of the carbene compound can be anchored to the metal substrate based on two metal-carbon bonds, thereby improving the direct contact stability between the metal substrate and the modified layer. On the other hand, the aforementioned symmetrical structure is also conducive to improving the structural uniformity of the modified layer.
[0013] In some embodiments, the first compound includes, but is not limited to, 4,4'-(((1,3-phenylene-bis(diazomethylene))bis(4,1-phenylene))diphenylamine.
[0014] In some embodiments, the thickness of the modified layer is 0nm to 4.3nm. Controlling the thickness of the modified layer within the above range is conducive to electron tunneling in the molecular tunnel junction, and generates a suitable tunneling current. In addition, the thickness of the modified layer can be regulated according to the length of the molecular chain of the carbene compound and / or the type of substituents connected to the main chain of the carbene compound. For example, the first compound has a terminal amino group, and after it forms a carbene compound, the terminal amino group still exists, so that the thickness of the modified layer can be adjusted according to the actual application needs.
[0015] In some embodiments, the roughness of the substrate is less than or equal to 0.51 nm. After the modified layer is formed on the surface of the metal substrate, the roughness of the substrate surface can be significantly reduced. Therefore, when the substrate of the present application is used to form a device, it can ensure good contact between the substrate and other structures, and it is not easy to generate interface defects.
[0016] In some embodiments, the material of the metal substrate includes metal elements of Group II, Group IV, Group VIII, Group I, or Group II, or an alloy composed of metal elements.
[0017] In some embodiments, the electrical conductivity of the material of the metal substrate is greater than 3×10 7 S / m, and / or, the standard electrode potential of the material of the metal substrate is greater than 0V.
[0018] In some embodiments, the material of the metal substrate has 3, 4, 5, or 6 electron shells, and the number of electrons in the outermost electron shell is 1.
[0019] In some embodiments, the material of the metal substrate includes a divalent metal or a trivalent metal.
[0020] In some embodiments, the material of the metal substrate includes, but is not limited to, at least one of gold, silver, copper, platinum, and aluminum.
[0021] In some embodiments, the substrate of the present application further includes a carrier, and the metal base is located on at least one side surface of the carrier.
[0022] In some embodiments, the material of the carrier includes but is not limited to at least one of silicon, glass, and quartz.
[0023] The second aspect of the present application provides a method for preparing a substrate, which is used to prepare the aforementioned substrate, including: step 1, preparing a first compound solution; step 2, providing a metal substrate and cleaning it; step 3, coating the first compound solution on the surface of the metal substrate to form a modification layer liquid film, and drying or blowing it to form a modification layer film; step 4, treating the modification layer film so that the first compound releases nitrogen to generate a carbene compound to form a modification layer, and the carbene compound forms a metal-carbon covalent bond with the metal atoms of the metal substrate.
[0024] In some embodiments, the concentration of the first compound solution is less than 5.00 mg / mL. The concentration of the first compound solution can be adjusted based on the specific application scenario of the substrate.
[0025] In some embodiments, the concentration of the first compound solution is 0.05 mg / mL to 1.00 mg / mL.
[0026] In some embodiments, in step 3, the coating method for forming the modification layer liquid film includes dipping coating and spraying coating.
[0027] In some embodiments, the coating method is dip coating, and the immersion time is 2s to 24h.
[0028] In some embodiments, in step 4, the method for treating the modified layer membrane comprises heat treatment, and the heat treatment temperature is 100° C. to 150° C., and the time is 15 min to 45 min.
[0029] In some embodiments, in step 4, the method of treating the modified layer film includes UV treatment, and the wavelength of the UV treatment is 200nm to 365nm.
[0030] In some embodiments, step 2 includes providing a carrier, depositing a metal substrate on at least one side of the carrier, and then performing a cleaning process. In some embodiments, the method of depositing the metal substrate includes but is not limited to physical vapor deposition or electrochemical deposition.
[0031] A third aspect of the present application provides a molecular device, comprising the aforementioned substrate.
[0032] In some embodiments, the molecular device includes a molecular electronic device or a molecular optical device.
[0033] In some embodiments, the molecular electronic device comprises a molecular tunneling device, wherein the current density Log J of the molecular tunneling device is from -2.26 A / cm 2 Reduced to -4.37A / cm 2 .
[0034] In some embodiments, a molecular optical device comprises an electroplasmonic device.
[0035] A fourth aspect of the present application provides a metal tunnel junction, comprising the aforementioned substrate and a metal electrode, wherein the metal electrode is covered with a modification layer.
[0036] In some embodiments, the metal electrode comprises liquid metal or solid metal.
[0037] In some embodiments, the material of the metal electrode includes, but is not limited to, gold, silver, copper, platinum, aluminum, mercury, indium, gallium, tin, or alloys thereof.
[0038] In some embodiments, the material of the metal electrode includes eutectic gallium-indium alloy (EGaIn).
[0039] The technical solution of this application can achieve the following beneficial effects:
[0040] The surface of the substrate of the present application is formed with a modified layer, which is formed by carbene compounds and metals based on metal-carbon covalent bonds, has excellent stability, and has no electrical degradation after storage under ambient conditions for more than 5 months. The thermal stability of the tunnel barrier is also improved, and heat treatment up to 200°C will not affect the electrical transmission at the metal-carbene interface. Finally, we also show that the carbene-based tunnel junction can be used as an electrically driven plasma light source. Therefore, based on the excellent performance of carbene films in molecular tunnel junctions, they can be widely used in molecular electronic devices and plasmonic devices. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] The present application is further explained and illustrated below in conjunction with the accompanying drawings. It should be understood that the following drawings are only for illustrative purposes and are not intended to limit the technical solutions of the present application.
[0042] Figure 1 This is an exemplary structural schematic diagram of the second substrate surface (carbene-Au / Si) modified by the modification layer according to an embodiment of the present application.
[0043] Figure 2 This is another exemplary structural schematic diagram of the second substrate surface (carbene-Au / Si) modified by the modification layer according to an embodiment of the present application.
[0044] Figure 3 An atomic force microscope image of the first substrate surface (Au / Si) without modification by the modification layer.
[0045] Figure 4 This is an atomic force microscope image of the surface of the second substrate after being modified with the modification layer.
[0046] Figure 5 Au 4f X-ray photoelectron spectra of the first substrate surface and the second substrate surface.
[0047] Figure 6 C1s X-ray photoelectron spectra of the first substrate surface and the second substrate surface.
[0048] Figure 7 It is the N1s X-ray photoelectron spectrum diagram of the first substrate surface and the second substrate surface.
[0049] Figure 8 Enhanced Raman spectra of the first substrate surface and the second substrate surface.
[0050] Fig. 9 The figure is a relationship diagram between the thickness and concentration of the second substrate surface modification layer prepared with the first compound of different concentrations measured by angle-resolved photoelectron spectroscopy.
[0051] Fig.10Schematic diagram of Au-carbene / / EGaIn tunnel junction.
[0052] Fig.11 The Log J versus voltage curve of Au-carbene / / EGaIn tunnel junctions prepared with different monomer concentrations.
[0053] Fig.12 The Log J curve of Au-carbene / / EGaIn tunnel junction is plotted against the thickness of the modification layer.
[0054] Fig.13 The graph is a graph of Log J and voltage measured at different temperatures.
[0055] Fig.14 This is a graph of Log J versus temperature for Au-carbene / / EGaIn tunnel junction at +0.5V.
[0056] Fig.15 The surface enhanced Raman spectra of the metal base second substrate at 150°C and 200°C.
[0057] Fig.16 The scatter plot of Log J and time of Au-carbene / / EGaIn tunnel junction measured for 5 consecutive months.
[0058] Fig.17 Schematic diagram of Au-carbene / / EGaIn tunnel junction electroluminescence test.
[0059] Fig.18 Real-space image of the light emission from the Au-carbene / / EGaIn tunnel junction under an external bias voltage of 1.8 V.
[0060] Fig.19 Back-focal plane image of the light emission from the Au-carbene / / EGaIn junction under an external bias voltage of 1.8 V.
[0061] Fig. 20 Figure 2 shows the light emission spectra of the Au-carbene / / EGaIn tunnel junction under different external bias voltages.
[0062] Fig.21 The time trajectory diagram of the emission intensity of three points at different positions on the excitation surface. DETAILED DESCRIPTION
[0063] In order to make the purpose, technical scheme and advantages of the present application clearer, the technical scheme of the present application will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present application, rather than all the embodiments. The relevant embodiments described herein are illustrative and are used to provide a basic understanding of the present application. The embodiments of the present application should not be interpreted as limiting the present application.
[0064] For simplicity, only some numerical ranges are specifically disclosed herein. However, any lower limit can be combined with any upper limit to form an unspecified range; and any lower limit can be combined with other lower limits to form an unspecified range, and any upper limit can be combined with any other upper limit to form an unspecified range. In addition, each separately disclosed point or single value can itself be combined as a lower limit or upper limit with any other point or single value or with other lower limits or upper limits to form an unspecified range.
[0065] In the description herein, unless otherwise specified, “above” and “below” include the number.
[0066] Unless otherwise specified, the terms used in this application have the commonly known meanings generally understood by those skilled in the art. Unless otherwise specified, the numerical values of the various parameters mentioned in this application can be measured using various measurement methods commonly used in the art (for example, they can be tested according to the methods given in the examples of this application).
[0067] A list of items connected by the terms "at least one of," "at least one of," "at least one of," or other similar terms may mean any combination of the listed items. For example, if items A and B are listed, the phrase "at least one of A and B" means only A; only B; or A and B. In another example, if items A, B, and C are listed, the phrase "at least one of A, B, and C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may contain a single component or multiple components. Item B may contain a single component or multiple components. Item C may contain a single component or multiple components.
[0068] The present application is further described below in conjunction with specific implementations. It should be understood that these specific implementations are only used to illustrate the present application and are not used to limit the scope of the present application.
[0069] One or more embodiments of the present application provide a metal surface, coating or substrate based on carbene modification to achieve a wide range of applications of molecular devices. The surface, coating or substrate includes a metal substrate on at least one side surface and a modified layer covering the metal substrate, the modified layer includes a carbene compound, and the carbene compound and the metal substrate are formed based on a metal-carbon covalent bond. The surface, coating or substrate can be used for the preparation of a wide range of molecular electronic devices, including, but not limited to, molecular tunneling devices composed of molecular tunnel junctions.
[0070] In some embodiments, the carbene compound is a monomer. In other embodiments, the carbene compound is a polymer.
[0071] In some embodiments, the carbene compound is a derivative of a first compound comprising a diaryldiazomethane.
[0072] In some embodiments, the diaryldiazomethane comprises a compound of Formula 1,
[0073]
[0074] In formula 1, R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , R 8 , R 9 and R 10 Each independently selected from hydrogen atom, substituted or unsubstituted C1-C20 alkyl, substituted or unsubstituted C1-C20 alkoxy, substituted or unsubstituted phenyl, substituted or unsubstituted heteroaryl, substituted substituents are independently selected from amino, diazo. Heteroaryl is a composite structure composed of aromatic ring and non-aromatic ring group, wherein aromatic ring includes but is not limited to benzene ring, thiophene ring, pyrrole ring, etc., and non-aromatic ring group includes but is not limited to oxygen, nitrogen, sulfur and other elements.
[0075] In some embodiments, heteroaryl includes phenoxy.
[0076] In some embodiments, the first compound includes but is not limited to bis(diaryldiazomethane). Bis(diaryldiazomethane) has a symmetrical structure. On the one hand, it can form a carbene compound with two carbene sites. Then, a molecule of carbene compound can be anchored to the metal substrate based on two metal-carbon bonds, thereby improving the direct contact stability between the metal substrate and the modified layer. On the other hand, the aforementioned symmetrical structure is also conducive to improving the structural uniformity of the modified layer.
[0077] In some embodiments, the first compound includes, but is not limited to, 4,4'-(((1,3-phenylene-bis(diazomethylene))bis(4,1-phenylene))diphenylamine.
[0078] In some embodiments, the thickness of the modified layer is 0 nm to 4.3 nm. Exemplarily, the thickness of the modified layer is 0.01 nm, 0.05 nm, 0.1 nm, 0.15 nm, 0.2 nm, 0.25 nm, 0.3 nm, 0.35 nm, 0.4 nm, 0.45 nm, 0.5 nm, 0.55 nm, 0.6 nm, 0.65 nm, 0.7 nm, 0.75 nm, 0.8 nm, 0.85 nm, 0.9 nm, 0.95 nm, 1 nm, 1.1 nm, 1.2 nm, 1.3 nm, 1.4 nm, 1.5 nm. , 1.6nm, 1.7nm, 1.8nm, 1.9nm, 2nm, 2.1nm, 2.2nm, 2.3nm, 2.4nm, 2.5nm, 2.6nm, 2.7nm, 2.8nm, 2.9nm, 3nm, 3.1nm, 3.2nm, 3.3nm, 3.4nm, 3.5nm, 3.6nm, 3.7nm, 3.8nm, 3.9nm, 4nm, 4.1nm, 4.2nm, 4.3nm or a range consisting of any two of the above values.
[0079] It is understandable that if the thickness of the modified layer is too low, the degree of metal surface modification is limited, the conductivity of the metal substrate is little affected, the electron tunneling current is too high to form a molecular tunnel junction, and if the thickness of the modified layer is too high, the metal conductivity is too weak, resulting in too small electron tunneling current in the molecular tunnel junction. Within the above range, it is conducive to electron tunneling in the molecular tunnel junction. Because of the presence of the terminal amino group of the first compound, the thickness of the modified layer can be adjusted according to the needs of practical applications. In addition, the thickness of the modified layer can be regulated according to the length of the molecular chain of the carbene compound and / or the type of substituents connected to the main chain of the carbene compound. For example, the presence of the terminal amino group of the first compound, after it forms a carbene compound, the terminal amino group still exists, so that the thickness of the modified layer can be adjusted according to the needs of practical applications.
[0080] In some embodiments, the material of the metal substrate includes metal elements of Group II, Group IV, Group VIII, Group I, or Group II, or an alloy composed of metal elements.
[0081] In some embodiments, the electrical conductivity of the material of the metal substrate is greater than 3×10 7 S / m, and / or, the standard electrode potential of the material of the metal substrate is greater than 0V.
[0082] In some embodiments, the material of the metal substrate has 3, 4, 5, or 6 electron shells, and the number of electrons in the outermost electron shell is 1.
[0083] In some embodiments, the material of the metal substrate includes a divalent metal or a trivalent metal.
[0084] In some embodiments, the material of the metal substrate includes but is not limited to at least one of gold, silver, copper, platinum, and aluminum.
[0085] In some embodiments, the substrate of the present application further includes a carrier, and the metal base is located on at least one side surface of the carrier.
[0086] In some embodiments, the material of the carrier includes but is not limited to at least one of silicon, glass, and quartz.
[0087] One or more embodiments of the present application further provide a method for preparing a substrate, which is used to prepare the substrate of the aforementioned embodiment, comprising:
[0088] Step 1, preparing a first compound solution;
[0089] Step 2, providing a metal substrate and performing a cleaning process;
[0090] Step 3, coating the first compound solution on the surface of the metal substrate to form a modification layer liquid film, and drying or blowing to form a modification layer film;
[0091] Step 4, treating the modified layer film so that the first compound releases nitrogen to generate a carbene compound to form a modified layer, and the carbene compound forms a metal-carbon covalent bond with the metal atoms of the metal substrate.
[0092] In some embodiments, the concentration of the first compound solution is less than 5.00 mg / mL. Exemplarily, the concentration of the first compound solution is 0.01 mg / mL, 0.02 mg / mL, 0.05 mg / mL, 0.07 mg / mL, 0.08 mg / mL, 1 mg / mL, 1.1 mg / mL, 1.2 mg / mL, 1.3 mg / mL, 1.4 mg / mL, 1.5 mg / mL, 1.6 mg / mL, 1.7 mg / mL, 1.8 mg / mL, 1.9 mg / mL, 2.0 mg / mL, 2.1 mg / mL, 2.2 mg / mL, 2.3 mg / mL, 2.4 mg / mL, 2.5 mg / mL, 2.6 mg / mL, 2.7 The range of any two values of the above. The concentration of the first compound solution can be adjusted based on the specific application scenario of the substrate. For example, for the molecular tunnel junction formed using the substrate of the present application, the concentration of the first compound solution is adjusted so that the modified layer has a suitable thickness so that the molecular tunnel junction can generate a tunneling current, and the size of the tunneling current can be further adjusted.
[0093] In some embodiments, the concentration of the first compound solution is 0.05 mg / mL to 1.00 mg / mL. Exemplarily, the concentration of the first compound solution is 0.05 mg / mL, 0.1 mg / mL, 0.15 mg / mL, 0.2 mg / mL, 0.25 mg / mL, 0.3 mg / mL, 0.35 mg / mL, 0.4 mg / mL, 0.45 mg / mL, 0.5 mg / mL, 0.55 mg / mL, 0.6 mg / mL, 0.65 mg / mL, 0.7 mg / mL, 0.75 mg / mL, 0.8 mg / mL, 0.85 mg / mL, 0.9 mg / mL, 0.95 mg / mL, 1.00 mg / mL or a range consisting of any two of the above values.
[0094] In some embodiments, in step 3, the coating method for forming the modification layer liquid film includes but is not limited to dipping and spraying. Any method that can form the modification layer liquid film is acceptable, and this application does not impose any specific limitation.
[0095] In some embodiments, the coating method is dip coating, and the soaking time is 2s to 24h. Exemplary, the soaking time is 2s, 30s, 1min, 5min, 10min, 20min, 30min, 40min, 50min, 1h, 2h, 5h, 8h, 10h, 12h, 15h, 16h, 18h, 20h, 24h or the scope of any two of the above numerical values. It is understandable that the soaking time is relevant to the required modification layer thickness and the concentration of the first compound solution, and the soaking time can be adjusted based on the specific circumstances.
[0096] In some embodiments, in step 4, the method for treating the modified layer film includes heat treatment, the temperature of the heat treatment is 100°C to 150°C, and exemplarily, the temperature of the heat treatment is 100°C, 105°C, 110°C, 115°C, 120°C, 125°C, 130°C, 135°C, 140°C, 145°C, 150°C or a range consisting of any two of the above values; the time is 15min to 45min, and exemplarily, the time is 15min, 20min, 25min, 30min, 35min, 40min, 45min or a range consisting of any two of the above values. It can be understood that when the first compound is the same, the temperature of the heat treatment is negatively correlated with the heat treatment time, and the temperature and time can be adjusted according to actual needs. The speed at which the modified layer liquid film forms the modified layer is uniform, and the quality of the formed film is high, without obvious defects such as pinholes. In addition, the temperature and time of the heat treatment are also related to the specific structure of the first compound.
[0097] In some embodiments, in step 4, the method for treating the modified layer film includes UV treatment, and the wavelength of the UV treatment is 200nm to 365nm. In some embodiments, step 2 includes providing a carrier, depositing a metal substrate on at least one side surface of the carrier, and then performing a cleaning process. In some embodiments, the method of depositing the metal substrate includes but is not limited to physical vapor deposition or electrochemical deposition.
[0098] In a specific example of the present application, the preparation method of the substrate of the present application includes: depositing a metal substrate on a carrier; then using a polar organic solvent (e.g., acetone) to ultrasonically clean the metal substrate to remove organic impurities and particles adsorbed on the surface; then, using an inert gas (e.g., nitrogen) for drying, and after drying, performing an oxygen plasma treatment for 5 to 10 minutes to enhance the wettability of the surface of the metal substrate; then, dissolving the first compound monomer in a solvent (e.g., dichloromethane (DCM)) under light-proof conditions to prepare a solution with a concentration of less than 5.00 mg / mL; then, placing the carrier / metal substrate in the aforementioned solution for 2s to 24h to form a modified layer liquid film, drying or blowing to remove excess solution to form a modified layer film, and placing the carrier / metal substrate / modified layer film at 100 to 150 ℃ The modified layer is formed for 15 to 45 minutes, and a stable metal-carbon covalent bond is formed between the metal substrate and the modified layer; after cooling to room temperature, the surface of the substrate is thoroughly rinsed with a solvent and dried with an inert gas.
[0099] Hereinafter, in order to further explain the technical concept of the present application in detail, gold is used as a metal substrate and 4,4'-(((1,3-phenylene-bis(diazomethylene))bis(4,1-phenylene))diphenylamine is used as a first compound to prepare a substrate for detailed explanation.
[0100] The applicant first deposited 5 nm of Cr on a silicon substrate as an adhesion layer, and then deposited 100 nm of Au on the surface of the adhesion layer facing away from the silicon substrate to form a first substrate as a blank control sample. In addition, the applicant immersed the first substrate in a DCM solution of 4,4'-(((1,3-phenylene-bis(diazomethylene))bis(4,1-phenylene))diphenylamine at different concentrations (e.g., 0.05 mg / L-1.00 mg / mL) for 2 seconds to 24 hours, and then heated at 100 to 150 °C for 24 hours. ℃ The modified layer is formed by heating for 15 to 45 minutes, at which time bis(diaryldiazomethane) releases N 2 The generated bisdiarylcarbene is spontaneously anchored to the Au surface by forming Au-C bonds (see Figure 1 ), forming a molecular tunnel junction. After cooling, the surface was rinsed with a large amount of DCM to remove any physically adsorbed and unreacted molecules, forming a second substrate as an experimental sample. As the concentration of the DCM solution of 4,4'-(((1,3-phenylene-bis(diazomethylene))bis(4,1-phenylene))diphenylamine increases, the terminal amino group can form more CN covalent bonds with carbene, thereby polymerizing and cross-linking on the gold surface, resulting in an increase in the thickness of the gold surface modification layer.
[0101] See also Figure 3 Hehe Figure 4Since the raw materials and the forming methods of the metal substrates of the first substrate and the second substrate are the same, the sizes of the gold particles in the metal substrates of the two substrates are basically the same. Figure 3 The surface of the metal base of the first substrate has no modified layer and its surface roughness is R q1 =1.15nm; see Figure 4 After the metal base of the second substrate is modified by the modification layer, its surface flatness is significantly improved, and the surface roughness is R q2 =0.51nm.
[0102] In order to better prove that the carbene compound and gold form a molecular tunnel junction based on the Au-C bond, the applicant also conducted X-ray photoelectron spectroscopy (XPS) tests on the first substrate surface and the second substrate surface respectively. Figures 5 to 7 , the XPS graph of Au 4f on the first substrate surface has an obvious double peak in the range of 83eV to 90eV, the N1s peak on the first substrate surface is not obvious, and the peak signal of the XPS graph of C1s on the first substrate surface is much lower; while the double peak signal of Au 4f on the second substrate surface is significantly reduced, the surface gold atoms are covered by other materials, the XPS graph of N1s on the second substrate surface has an obvious single peak in the range of 397eV to 401eV, and the XPS graph of C1s on the second substrate surface has obvious multiple peaks in the range of 281eV to 292eV. Furthermore, the π-π vibration peak of 291.6eV and the CO peak of 285.9eV confirm the existence of double bonds and carbon-oxygen bonds in the dicarbene molecular structure on the Au surface. Finally, see Figure 8 , surface enhanced Raman spectroscopy (SERS) at 416 cm -1 The absorption peak of the Au-C bond was detected at , thereby confirming that a metal-carbon covalent bond was formed on the surface of the second substrate.
[0103] When the concentration of the first compound increased from 0.05 mg / mL to 1 mg / mL, in order to test the thickness of the modified layer, the applicant conducted an angle-resolved X-ray photoelectron spectroscopy test on the second substrate at each concentration, see Fig. 9 As the concentration increases, the thickness of the modified layer gradually increases. The thickness of the modified layer prepared at a concentration of 1 mg / mL is 4.3 nm, indicating that the thickness of the modified layer can be regulated. The reason is combined with Figure 2 It can be seen that carbene can be embedded in the terminal amino group of the first compound to form a polymerized cross-linked structure, thereby increasing the thickness of the modified layer.
[0104] In addition, if Fig.10As shown in , the applicant prepared an Au-carbene / / EGaIn tunnel junction to study the electron transport between the metal substrate and the modified layer in the substrate of the present application, wherein EGaIn represents a liquid metal composed of 75% Ga and 25% In, and “ / / ” represents the van der Waals contact between carbene and EGaIn. EGaIn is used as a top electrode to provide soft contact with organic molecules, with high tunnel junction yield and good reproducibility. Fig.11 The Log J versus voltage curves of Au-carbene / / EGaIn tunnel junctions prepared using different monomer concentrations from 0.05 mg / mL to 1.00 mg / mL are shown, J (A / cm 2 ) represents the current density. As the concentration increases, the thickness of the carbene film (modification layer) will also increase, but a systematic decrease in the measured current density is observed. This is because organic compounds are composed of covalent bonds, and the charge flow is slow, resulting in weak conductivity. Therefore, as the thickness of the modification layer increases, its conductivity decreases, resulting in a decrease in the tested current density. Fig.12 The curve showing the relationship between Ln J and the thickness of the modified layer.
[0105] Due to the larger dissociation energy of Au-C bonds (~67 kcal / mol) compared to Au-S bonds (~45 kcal / mol), carbene films immobilized on Au surfaces exhibit excellent thermal stability up to 200 °C. Here, see Fig.13 In order to study the thermal stability of carbene films, the Au-carbene surface was heated to different temperatures of 25°C, 75°C, 100°C, 125°C, 150°C, 175°C, 200°C, 225°C, 250°C, 275°C, and 300°C, and maintained at each temperature for 10 minutes, then naturally cooled to room temperature, and the relationship between log J and voltage was measured using an EGaIn top electrode. For further information, see Fig.14 The applicant further measured the relationship between Log J and temperature at a voltage of 0.5 V. The current density dropped rapidly by two orders of magnitude from 200°C to 250°C, indicating that changes occurred between the carbene film and gold in this temperature range. Fig.15 The SERS results show that the Au-C covalent bond breaks in this temperature range.
[0106] In addition to thermal stability, the applicant also studied the storage life of the Au-carbene surface in ambient environment. Fig.16 , for the same sample, the Au-carbene surface exhibited excellent storage life with no electrical degradation observed over 150 days.
[0107] In addition, see Fig.17, the applicants used Au-carbene / / EGaIn tunnel junctions to achieve the excitation of electrically driven plasmons, which has potential applications in molecular optoelectronic circuits. To study the Au-carbene / / EGaIn tunnel junctions that induce surface plasmon excitation via tunneling electrons, the applicants used a semi-transparent Au film (50 nm thickness) as the bottom electrode. The Au-carbene / / EGaIn tunnel junction was formed directly on top of an inverted optical microscope to record the backside light emission (see Fig.18 ). By applying a constant bias (above 1.5V) to the Au-carbene / / EGaIn tunnel junction, the tunneling electrons excite surface plasmons on the bottom Au electrode through an inelastic tunneling process. The excited surface plasmons have the opportunity to further couple to photons through leakage radiation and local scattering, so that we can see light emission from these junctions in the far field. This plasmon excitation mechanism can be applied to different types of tunnel junctions. Since the electrical contact to EGaIn is much smaller than its geometrical contact, tunneling always occurs through the shortest path, so we observe local emission points. In addition, Fig.19 is a back focal plane image, where a ring feature is observed at k = 1.01 as direct evidence showing the excitation of surface plasmons propagating along the Au surface. Fig. 20 The light emission spectrum measured when different external bias voltages are applied is shown. It can be seen that the plasma peak moves toward the blue direction as the voltage increases. This shows that the surface plasmon light source absorption peak is affected by the external applied voltage and the wavelength of the light source is adjustable. Fig.21 Shown are the time traces of the emission intensity at three points at different locations on the excitation surface.
[0108] One or more embodiments of the present application also provide a molecular device, including the aforementioned substrate.
[0109] The molecular device has the advantages of good stability and long life, and the substrate surface contains substituents (for example, amino groups), which are easy to be functionalized later to change the surface structure of the substrate and thus achieve diversification of device performance.
[0110] In some embodiments, the molecular device includes a molecular electronic device or a molecular optical device.
[0111] In some embodiments, the molecular electronic device includes a molecular tunneling device, wherein the current density LogJ of the molecular tunneling device is from -2.26 A / cm at 0.5 V to 2 Reduced to -4.37A / cm 2 .
[0112] In some embodiments, the molecular optical device comprises an electroplasmonic device.
[0113] One or more embodiments of the present application further provide a metal tunnel junction, comprising the aforementioned substrate and a metal electrode, wherein the metal electrode is covered with a modification layer.
[0114] In some embodiments, the metal electrode comprises liquid metal or solid metal.
[0115] In some embodiments, the material of the metal electrode includes, but is not limited to, gold, silver, copper, platinum, aluminum, mercury, indium, gallium, tin, or alloys thereof.
[0116] In some embodiments, the material of the metal electrode includes eutectic gallium-indium alloy (EGaIn).
[0117] Test Method
[0118] 1. Characterization of carbene film (second substrate surface)
[0119] The surface roughness of the carbene-modified Au surface was measured by atomic force microscopy (AFM, Bruker Dimension Icon) with a measurement area of 1 × 1 μm 2 . XPS spectra were collected using an ESCALAB 250Xi from ThermoScientific at 10-9 mbar using a monochromatic Al Kα source (hv = 1486.6 eV). The pass energy for the full spectrum was 100 eV, and the high-resolution spectra were acquired at a pass energy of 30 eV. The X-ray spot size was 500 μm for a normal escape angle of 90°. For thickness measurements, the X-ray spot size was 200 μm with escape angles of 15°, 30°, 45°, 60°, 75°, and 90°. Raman spectra were recorded on a confocal Raman microspectrometer (WITec alpha300 R) using 633 nm laser excitation, a laser power of 0.5 mW, and a laser spot diameter of 1 μm. The integration time was 20 s, and each Raman spectrum was accumulated 5 times.
[0120] 2. Electrical measurement
[0121] For all current densities J(A / cm 2 ) measurements, we used a freshly prepared EGaIn conical tip as the top electrode. A source meter (Lakeshore Keithly 4200) was used to apply voltage to the bottom electrode while EGaIn was grounded. For each Au-carbene / / EGaIn tunnel junction, we recorded 20 J (A / cm 2) curve scans, and statistical analysis was performed based on the data collected from more than 20 nodes. Finally, the value of |J| for each measurement was plotted as a histogram, and we fitted it with a Gaussian function to obtain the logarithmic mean and logarithmic standard deviation. For thermal stability measurements, the second substrate Au-carbene surface was heated to different temperatures of 25°C, 75°C, 100°C, 125°C, 150°C, 175°C, 200°C, 225°C, 250°C, 275°C, and 300°C. For each temperature, the Au-carbene surface was kept at the corresponding temperature for 10 minutes and then naturally cooled to room temperature, and J (A / cm 2 For the storage stability experiments, we measured the same Au-carbene surface continuously for 150 days, during which time the sample was stored in ambient environment.
[0122] 3. Optical performance characterization
[0123] Light emission experiments were performed using an inverted optical microscope (Nikon Eclipse Ti-E) and an Andor electron multiplying charge coupled device (EMCCD, iXon Ultra 897). Plasma excitation / light emission was driven by a DC voltage using a Keithley 6430 source meter. Optical properties were tested on the back of these Au-carbene / / EGaIn tunnel junctions from a semi-transparent Au (50nm) bottom electrode using a 100x oil objective (NA=1.30), with an electromagnetic gain of 300 times and an integration time of 120s. The same device was installed in a liquid nitrogen cooled spectrometer (Horiba, IHR550) for emission spectroscopy characterization.
[0124] Although some exemplary embodiments of the present application have been illustrated and described, the present application is not limited to the disclosed embodiments. On the contrary, those skilled in the art will recognize that some modifications and changes may be made to the described embodiments without departing from the spirit and scope of the present application as described in the appended claims.
Claims
1. A substrate, characterized in that: The invention comprises a metal substrate and a modification layer covering the metal substrate. The modification layer comprises a carbene compound. The carbene compound forms a metal-carbon covalent bond with the metal substrate.
2. The substrate according to claim 1, characterized in that The carbene compound is a derivative of a first compound, and the first compound includes diaryldiazomethane; Preferably, the diaryldiazomethane comprises a compound of formula 1, In Formula 1, R1, R2, R3, R4, R5, R6, R7, R8, R9 and R 10 Each independently selected from a hydrogen atom, a substituted or unsubstituted C1-C20 alkyl group, a substituted or unsubstituted C1-C20 alkoxy group, a substituted or unsubstituted phenyl group, a substituted or unsubstituted heteroaryl group, and the substituted substituents are each independently selected from an amino group and a diazo group; Preferably, the heteroaryl group includes a phenoxy group; Preferably, the first compound comprises bis(diaryldiazomethane); Preferably, the first compound includes 4,4′-(((1,3-phenylene-bis(diazomethylene))bis(4,1-phenylene))diphenylamine.
3. The substrate according to claim 1, characterized in that The thickness of the modified layer is 0 nm to 4.3 nm.
4. The substrate according to claim 1, characterized in that The roughness of the substrate is less than or equal to 0.51 nm.
5. The substrate according to claim 1, characterized in that The material of the metal substrate includes metal elements of the Шth main group, the Ⅳth main group, the Ⅷth main group, the Ⅰth sub-group, and the Ⅱth sub-group, or an alloy composed of the metal elements; preferably, the metal atoms include at least one of gold, silver, copper, platinum, and aluminum.
6. The substrate according to any one of claims 1 to 5, characterized in that It also includes a carrier plate, wherein the metal substrate is located on at least one side surface of the carrier plate; Preferably, the material of the carrier includes silicon, glass, or quartz.
7. A method for preparing a substrate, characterized in that: A method for preparing a substrate according to any one of claims 1 to 6, comprising: Step 1, preparing a first compound solution; Step 2, providing a metal substrate and performing a cleaning process; Step 3, coating the first compound solution on the surface of the metal substrate to form a modification layer liquid film, and drying in the air or by blowing to form a modification layer film; Step 4, treating the modified layer film so that the first compound releases nitrogen to generate a carbene compound to form a modified layer, wherein the carbene compound forms a metal-carbon covalent bond with the metal atoms of the metal substrate.
8. The preparation method according to claim 7, characterized in that: The concentration of the first compound solution is less than 5.00 mg / mL; Preferably, the concentration of the first compound solution is 0.05 mg / mL to 1.00 mg / mL.
9. The preparation method according to claim 7, characterized in that: In step 3, the coating method for forming the modification layer liquid film includes dipping and spraying; preferably, the coating method is dipping, and the immersion time is 2s to 24h; Preferably, in step 4, the method for treating the modified layer membrane comprises heat treatment, the heat treatment temperature is 100° C. to 150° C., and the time is 15 min to 45 min; Preferably, in step 4, the method for treating the modified layer film comprises UV treatment, and the wavelength of the UV treatment is 200nm to 365nm.
10. A molecular device, characterized in that: A substrate comprising any one of claims 1 to 6.
11. The device according to claim 10, characterized in that The molecular devices include molecular electronic devices and molecular optical devices; Preferably, the molecular electronic device comprises a molecular tunneling device, wherein the current density Log J of the molecular tunneling device is from -2.26 A / cm 2 Reduced to -4.37A / cm 2 ; Preferably, the molecular optical device comprises an electroplasmonic device.
12. A metal tunnel junction, characterized in that: The invention comprises the substrate according to any one of claims 1 to 6 and a metal electrode, wherein the metal electrode covers the modified layer.
13. The metal tunnel junction according to claim 12, characterized in that: The metal electrode includes liquid metal or solid metal.