Preparation method of high-performance flexible piezoelectric film

By introducing propylene segments and carbon-carbon double bonds into the piezoelectric film and carrying out specific treatments, the problem of insufficient flexibility and performance of piezoelectric films in the prior art is solved, and the preparation of high-performance flexible piezoelectric films is realized. for wearable devices and ultrasonic transducers.

CN119072213APending Publication Date: 2024-12-03ZHEJIANG SCI-TECH UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410970036.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing piezoelectric films still have room for improvement in high performance requirements and flexibility, especially in the field of wearable devices, where piezoelectric and electromechanical coupling performance are insufficient.

Method used

The appropriate amount of propylene segments and carbon-carbon double bonds are introduced into the substrate polymer of the piezoelectric film, and the flexibility and electromechanical coupling performance of the film are improved through copolymerization, elimination reaction, annealing treatment and polarization treatment.

Benefits of technology

It significantly improves the electromechanical coupling performance and piezoelectric properties of piezoelectric films, realizes huge electrostrictive strain under low electric fields, is suitable for the preparation of ultrasonic transducers, and has the characteristics of lightness and high sensitivity, suitable for wearables equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004952884210000081
    Figure BDA0004952884210000081
Patent Text Reader

Abstract

The invention relates to the field of piezoelectric sensors, and discloses a preparation method of a high-performance flexible piezoelectric film. A proper amount of propylene chain segments and carbon-carbon double bonds are introduced into a base material polymer of the piezoelectric film. Wherein the flexibility of the polymer can be improved by introducing a proper amount of propylene chain segments, so that the piezoelectric film can be applied to wearable equipment. In addition, the compound also plays an important role in adjusting the structure and the performance of the polymer as a structural defect. A proper amount of carbon-carbon double bonds are introduced, and subsequent annealing treatment and polarization treatment are matched, so that the electromechanical coupling performance and piezoelectric performance of the piezoelectric film can be obviously improved, and huge electrostrictive strain under a low electric field is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of piezoelectric sensors, and in particular to a method for preparing a high-performance flexible piezoelectric film. Background Art

[0002] Piezoelectric materials refer to crystalline materials that will generate voltage between the two end surfaces when subjected to pressure, and can realize the mutual conversion between mechanical vibration (sound waves) and electrical energy. Therefore, piezoelectric materials are widely used in actuators and sensor elements. Piezoelectric materials mainly include inorganic piezoelectric materials, organic piezoelectric materials and composite materials. Among organic piezoelectric materials, polyvinylidene fluoride (PVDF) and its copolymers have become important ferroelectric polymers due to their excellent dielectric and electromechanical properties, chemical stability and processability. And their dielectric, ferroelectric and electromechanical properties can be adjusted by changing the chemical composition and processing conditions, which makes them suitable for various applications. Polyvinylidene fluoride PVDF is a typical semi-crystalline polymer, in which the β-type crystal molecular chain orientation is planar serrated, and the dipole moment comes from the electronegative fluorine (δ - ) and electropositive hydrogen (δ + ), perpendicular to the polymer chain. Therefore, the β phase provides the highest electroactive energy, exhibits a large spontaneous polarization, and shows high piezoelectricity. In order to increase the proportion of the β phase, vinylidene fluoride is usually copolymerized with trifluoroethylene (TrFE) with a larger size, and the steric effect is used to induce the P(VDF-TrFE) polymer to directly generate the β phase, and its piezoelectric properties are better than those of pure PVDF polymer. In order to further improve the electrostrictive strain, dielectric constant and high piezoelectric properties, additional CTFE or CFE monomer units are introduced into the well-organized VDF-TrFE chain, thereby increasing the dipole mobility and inducing unique relaxed ferroelectric properties.

[0003] However, for some fields with high performance requirements, the piezoelectricity and electromechanical coupling performance of existing piezoelectric films still need to be further improved. In addition, for the field of wearable devices, the flexibility of piezoelectric films also needs to be further improved. Therefore, the preparation of a high-performance flexible piezoelectric film is very important for the advancement of future wearable electronic devices. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a method for preparing a high-performance flexible piezoelectric film. The present invention introduces an appropriate amount of propylene segments and carbon-carbon double bonds into the substrate polymer of the piezoelectric film to improve the flexibility, piezoelectricity and electromechanical coupling performance of the piezoelectric film.

[0005] The specific technical solution of the present invention is: a method for preparing a high-performance flexible piezoelectric film, comprising the following steps:

[0006] Step 1: Add potassium persulfate and water into a reactor, seal the reactor and place it in a liquid nitrogen bath for vacuum degassing; introduce gaseous vinylidene fluoride (VDF), trifluoroethylene (TrFE), chlorofluoroethylene (CFE) and propylene into the reactor, and the gas will liquefy instantly when cooled to carry out copolymerization reaction; after the reaction, cool to room temperature, separate, wash and dry to obtain a tetrapolymer.

[0007] The present invention finds that the introduction of propylene segments into copolymers can increase the flexibility of the polymers, thereby facilitating the application of piezoelectric films in wearable devices. In addition, as structural defects, propylene segments also play an important role in adjusting the structure and properties of polymers.

[0008] Step 2: dissolving the tetrapolymer in an organic solvent and stirring to obtain a homogeneous solution.

[0009] Step 3: Pour the homogeneous solution into an oxygen-free environment reactor, add an organic base, and carry out an elimination reaction to remove hydrogen chloride from part of the chlorofluoroethylene chain segments in the tetrapolymer to form carbon-carbon double bonds.

[0010] The present invention finds that after introducing an appropriate amount of carbon-carbon double bonds into the quaternary copolymer, combined with subsequent annealing and polarization treatments, the electromechanical coupling performance and piezoelectric performance of the piezoelectric film can be significantly improved, and a huge electrostrictive strain under a low electric field can be achieved.

[0011] Step 4: After the reaction solution obtained in step 3 is cooled to room temperature, it is added to a mixed solution of ethanol and water, precipitated, washed, and dried to obtain a carbon-carbon double bond modified tetrapolymer.

[0012] Step 5: dissolving the carbon-carbon double bond modified tetrapolymer in an organic solvent and stirring to form a homogeneous solution, coating the homogeneous solution on a substrate, and drying to form a film.

[0013] Step 6: After soaking the film in water, peel it off from the substrate, and anneal the film to crystallize it and increase the size and content of the β-phase crystals; the annealing treatment includes: heating at 110-120°C for 8-24 hours, and then cooling to room temperature. Within this annealing temperature window, the quaternary copolymer film has a non-polar pure relaxation phase and exhibits a critical transition phenomenon, with a very small energy barrier between the non-polar (relaxation) and polar (ferroelectric) condensed chain states, which is conducive to the formation of the β phase.

[0014] Step 7: The annealed film is polarized to obtain a high-performance flexible piezoelectric film.

[0015] Preferably, in step 1, the molar ratio of vinylidene fluoride, trifluoroethylene, chlorofluoroethylene and propylene is in the range of 63-69: 24.5-33.5: 6.5-8.5: 4.5-5.5.

[0016] The present invention finds that the content of propylene monomer needs to be strictly controlled. If its content is too high, its side methyl structure will increase the interlamellar spacing, which is not conducive to the transformation of the polar phase; if its content is too low, it is not conducive to improving the flexibility of the film.

[0017] Preferably, in step 1, the copolymerization reaction temperature is 85-95° C. and the time is 4-8 hours.

[0018] Preferably, in step 2, the organic solvent is N,N-dimethylpropylene urea (DMPU), dimethyl sulfoxide (DMSO) or triethyl phosphate (TEP).

[0019] Preferably, in step three, the usage ratio of the organic base to the tetrapolymer is 0.5 g: 2-5 mL; and the time of the elimination reaction is 1-6 h.

[0020] The amount of organic base used and the elimination reaction time determine the double bond content. The present invention finds that if the amount of organic base used is too much or the reaction time is too long, the double bond content produced will increase, which will hinder the conversion of the product from a non-polar phase to a polar phase; if the amount of organic base used is too little or the reaction time is too short, the double bond content produced will decrease, and the remaining CFE will be more, which will expand the interchain spacing and is not conducive to the growth of the β phase.

[0021] Preferably, in step three, the organic base is triethylamine, diethylamine or tri-n-butylamine.

[0022] Preferably, in step 4, the volume ratio of ethanol to water is 2:3 to 3:2.

[0023] Preferably, in step 5, the film is prepared by a spin coating method, a solution casting method, a drop coating method or a blade coating method, etc. Preferably, the coating blade coating method is used.

[0024] Preferably, in step five, the drying conditions are: 50-70° C., 8-12 h.

[0025] Preferably, in step six, the soaking time is 2 to 6 hours.

[0026] Preferably, in step seven, the polarization electric field is 40 to 100 MV / m, the polarization temperature is room temperature, and the polarization time is 15 to 30 min.

[0027] Compared with the prior art, the beneficial effects of the present invention are:

[0028] (1) The present invention introduces an appropriate amount of propylene segments into the piezoelectric film polymer, which can increase the flexibility of the polymer, thereby facilitating the application of the piezoelectric film in wearable devices. In addition, as a structural defect, it also plays an important role in adjusting the structure and performance of the polymer.

[0029] (2) The present invention introduces an appropriate amount of carbon-carbon double bonds into the quaternary copolymer, and combined with subsequent annealing and polarization treatments, can significantly improve the electromechanical coupling performance and piezoelectric performance of the piezoelectric film, and achieve huge electrostrictive strain under low electric fields.

[0030] (3) The piezoelectric film of the present invention has the characteristics of being thin, light, small in area and highly sensitive, so that it can be directly used in the preparation of ultrasonic transducers without the need for an elastic substrate.

[0031] (4) The method of the present invention has a simple production process, is environmentally friendly and can meet the requirements of mass production in actual production processes. DETAILED DESCRIPTION

[0032] The present invention is further described below in conjunction with embodiments. It should be pointed out that the described embodiments are only part of the embodiments of the present application, rather than all the embodiments, and other similar schemes are within the protection scope of the present invention.

[0033] Comparative Example 1

[0034] Step 1: Add 0.15g potassium persulfate (K2S2O8) and 100mL deionized water to a 300ml stainless steel container. The container is sealed and placed in a -140℃ liquid nitrogen bath, and then degassed by a vacuum pump. Gaseous vinylidene fluoride (VDF), trifluoroethylene (TrFE), and chlorofluoroethylene (CFE) are pumped into the container and liquefied instantly at liquid nitrogen temperature. The feed molar ratio of the monomers is 63:25:7, which is controlled by the pumping time of each gas, and the reaction is carried out at 90℃ for 6 hours. After the reaction is completed, the container is cooled to room temperature and the excess gas is carefully removed. The separated polymer is repeatedly washed with deionized water and methanol and dried in vacuo at 50℃.

[0035] Step 2: Take 0.5 g of P(VDF-TrFE-CFE) terpolymer powder, dissolve it in 15 ml of dimethyl sulfoxide (DMSO), and stir it magnetically overnight (24 h) to obtain a homogeneous solution.

[0036] Step 3: Take a double-necked round-bottom flask, treat it to be anhydrous and oxygen-free and place it in a 50°C oil bath, pour the homogeneous solution into the round-bottom flask, then add 2 ml of tri-n-butylamine dropwise, and stir the reaction at 600 rpm for 1 hour.

[0037] Step 4: After the reaction is completed, the reaction system is slowly cooled to room temperature and added to a mixed solution of ethanol and water with a volume ratio of 3:2 for the first washing, mainly to remove chloride salts, ammonium salts, etc. Then the washed precipitate is redissolved in 10ml N,N-dimethylpropylene urea (DMPU) and washed twice. Then the reaction product is placed in a vacuum oven at 45°C and dried for about 24 hours to finally obtain a modified polymer solid.

[0038] Step 5: Take 0.3 g of the modified polymer obtained in step 4 and dissolve it in 5 ml of N,N-dimethylpropylene urea (DMPU), and stir for a certain period of time to obtain a homogeneous sample solution. Step 6: Use a dropper to absorb an appropriate amount of the homogeneous sample solution and drop it on the quartz glass substrate of the doctor blade coater for coating. The coating speed of the doctor blade is 200 cm / min, and a thin film with a wet film thickness of 500 μm is formed on the substrate, and then vacuum dried at a temperature of 60°C for 8 hours.

[0039] Step 7: Take out the dried film, soak it in deionized water for 4 hours, and then carefully peel it off from the glass substrate. Place the peeled film on a homemade frame, and then put it into a vacuum drying oven and anneal it at 120°C for 24 hours.

[0040] Step 8: Finally, the annealed film is polarized with the polarization electric field controlled at 60MV / m, the polarization time at 30min, and the polarization temperature at room temperature to obtain a piezoelectric film, which is then subjected to performance testing.

[0041] Comparative Example 2

[0042] Step 1: Add 0.15g potassium persulfate (K2S2O8) and 100mL deionized water into a 300ml stainless steel container. The container is sealed and placed in a liquid nitrogen bath (-140°C), and then degassed by a vacuum pump. Gaseous vinylidene fluoride (VDF), trifluoroethylene (TrFE), chlorofluoroethylene (CFE), and propylene monomers are pumped into the container and liquefied instantly at liquid nitrogen temperature. The feed molar ratio of the monomers is 63:25:7:5, which is controlled by the pumping time of each gas, and the reaction is carried out at 90°C for 6 hours. After the reaction is completed, the container is cooled to room temperature and the excess gas is carefully removed. The separated polymer is repeatedly washed with deionized water and methanol and dried in vacuo at 50°C.

[0043] Step 2: Take 0.3 g of the modified polymer obtained in step 1 and dissolve it in 5 ml of N,N-dimethylpropylene urea (DMPU), and stir for a certain period of time to obtain a homogeneous sample solution.

[0044] Step 3: Use a dropper to absorb an appropriate amount of homogeneous sample solution and drop it on the quartz glass substrate of the doctor blade coater for coating. The coating speed of the doctor blade is 200 cm / min. A thin film with a wet film thickness of 500 μm is formed on the substrate, and then vacuum dried at a temperature of 60°C for 8 hours.

[0045] Step 4: Take out the dried film, soak it in deionized water for 4 hours, and then carefully peel it off from the glass substrate. Place the peeled film on a homemade frame, and then put it into a vacuum drying oven and anneal it at 120°C for 24 hours.

[0046] Step 5: Finally, the annealed film is polarized with the polarization electric field controlled at 60MV / m, the polarization time at 30min, and the polarization temperature at room temperature to obtain a piezoelectric film, which is then subjected to performance testing.

[0047] Example 1

[0048] Step 1: Add 0.15g potassium persulfate (K2S2O8) and 100mL deionized water into a 300ml stainless steel container. The container is sealed and placed in a liquid nitrogen bath (-140°C), and then degassed by a vacuum pump. Gaseous vinylidene fluoride (VDF), trifluoroethylene (TrFE), chlorofluoroethylene (CFE), and propylene monomers are pumped into the container and liquefied instantly at liquid nitrogen temperature. The feed molar ratio of the monomers is 63:25:7:5, which is controlled by the pumping time of each gas, and the reaction is carried out at 90°C for 6 hours. After the reaction is completed, the container is cooled to room temperature and the excess gas is carefully removed. The separated polymer is repeatedly washed with deionized water and methanol and dried in vacuo at 50°C.

[0049] Step 2: Take 0.5 g of P (VDF-TrFE-CFE-P) tetrapolymer powder, dissolve it in 15 ml of dimethyl sulfoxide (DMSO), and stir it magnetically overnight (24 h) to obtain a homogeneous solution.

[0050] Step 3: Take a double-necked round-bottom flask, treat it to be anhydrous and oxygen-free and place it in a 50°C oil bath, pour the homogeneous solution into the round-bottom flask, then add 2 ml of tri-n-butylamine dropwise, and stir the reaction at 600 rpm for 1 hour.

[0051] Step 4: After the reaction is completed, the reaction system is slowly cooled to room temperature and added to a mixed solution of ethanol and water with a volume ratio of 3:2 for the first washing, mainly to remove chloride salts, ammonium salts, etc. Then the washed precipitate is redissolved in 10ml N,N-dimethylpropylene urea (DMPU) and washed twice. Then the reaction product is placed in a vacuum oven at 45°C and dried for about 24 hours to finally obtain a modified polymer solid.

[0052] Step 5: Take 0.3 g of the modified polymer obtained in step 4 and dissolve it in 5 ml of N,N-dimethylpropylene urea (DMPU), and stir for a certain period of time to obtain a homogeneous sample solution.

[0053] Step 6: Use a dropper to absorb an appropriate amount of the modified homogeneous sample solution and drop it on the quartz glass substrate of the doctor blade coater for coating. The coating speed of the doctor blade is 200 cm / min. A thin film with a wet film thickness of 500 μm is formed on the substrate, and then vacuum dried at a temperature of 60°C for 8 hours.

[0054] Step 7: Take out the dried film, soak it in deionized water for 4 hours, and then carefully peel it off from the glass substrate. Place the peeled film on a homemade frame, and then put it into a vacuum drying oven and anneal it at 120°C for 24 hours.

[0055] Step 8: Finally, the annealed film is polarized with the polarization electric field controlled at 60MV / m, the polarization time at 30min, and the polarization temperature at room temperature to obtain a piezoelectric film, which is then subjected to performance testing.

[0056] Example 2

[0057] Step 1: Add 0.15g potassium persulfate (K2S2O8) and 100mL deionized water to a 300ml stainless steel container. The container is sealed and placed in a liquid nitrogen bath (-140°C), and then degassed by a vacuum pump. Gaseous vinylidene fluoride (VDF), trifluoroethylene (TrFE), chlorofluoroethylene (CFE) and propylene monomers are pumped into the container and liquefied instantly at liquid nitrogen temperature. The feed molar ratio of the monomers is 63:25:7:5, which is controlled by the pumping time of each gas, and the reaction is carried out at 90°C for 6 hours. After the reaction is completed, the container is cooled to room temperature and the excess gas is carefully removed. The separated polymer is repeatedly washed with deionized water and methanol and dried in vacuo at 50°C.

[0058] Step 2: Take 0.5 g of P (VDF-TrFE-CFE-P) tetrapolymer powder, dissolve it in 15 ml of dimethyl sulfoxide (DMSO), and stir it magnetically overnight (24 h) to obtain a homogeneous solution.

[0059] Step 3: Take a double-necked round-bottom flask, treat it to be anhydrous and oxygen-free and place it in a 50°C oil bath, pour the homogeneous solution into the round-bottom flask, then add 2 ml of tri-n-butylamine dropwise, and stir the reaction at 600 rpm for 2 hours.

[0060] Step 4: After the reaction is completed, the reaction system is slowly cooled to room temperature and added to a mixed solution of ethanol and water with a volume ratio of 3:2 for the first washing, mainly to remove chloride salts, ammonium salts, etc. Then the washed precipitate is redissolved in 10ml N,N-dimethylpropylene urea (DMPU) and washed twice. Then the reaction product is placed in a vacuum oven at 45°C and dried for about 24 hours to finally obtain a modified polymer solid.

[0061] Step 5: Take 0.3g of the modified polymer obtained in step 4 and dissolve it in 5ml of N,N-dimethylpropylene urea (DMPU), and stir for a certain period of time to obtain a homogeneous sample solution. Step 6: Use a dropper to absorb an appropriate amount of the modified sample solution and drop it on the quartz glass substrate of the doctor blade coater for coating. The coating speed of the doctor blade is 200cm / min, and a thin film with a wet film thickness of 500μm is formed on the substrate, and then vacuum dried at a temperature of 60℃ for 8h.

[0062] Step 7: Take out the dried film, soak it in deionized water for 4 hours, and then carefully peel it off from the glass substrate. Place the peeled film on a homemade frame, and then put it into a vacuum drying oven and anneal it at 120°C for 24 hours.

[0063] Step 8: Finally, the annealed film is polarized with the polarization electric field controlled at 60MV / m, the polarization time at 30min, and the polarization temperature at room temperature to obtain a piezoelectric film, which is then subjected to performance testing.

[0064] Example 3

[0065] Step 1: Add 0.15g potassium persulfate (K2S2O8) and 100mL deionized water into a 300ml stainless steel container. The container is sealed and placed in a liquid nitrogen bath (-140°C), and then degassed by a vacuum pump. Gaseous vinylidene fluoride (VDF), trifluoroethylene (TrFE), chlorofluoroethylene (CFE), and propylene monomers are pumped into the container and liquefied instantly at liquid nitrogen temperature. The feed molar ratio of the monomers is 63:25:7:5, which is controlled by the pumping time of each gas, and the reaction is carried out at 90°C for 6 hours. After the reaction is completed, the container is cooled to room temperature and the excess gas is carefully removed. The separated polymer is repeatedly washed with deionized water and methanol and dried in vacuo at 50°C.

[0066] Step 2: Take 0.5 g of P (VDF-TrFE-CFE-P) tetrapolymer powder, dissolve it in 15 ml of dimethyl sulfoxide (DMSO), and stir it magnetically overnight (24 h) to obtain a homogeneous solution.

[0067] Step 3: Take a double-necked round-bottom flask, treat it to be anhydrous and oxygen-free and place it in a 50°C oil bath, pour the homogeneous solution into the round-bottom flask, then add 2 ml of tri-n-butylamine dropwise, and stir the reaction at 600 rpm for 4 hours.

[0068] Step 4: After the reaction is completed, the reaction system is slowly cooled to room temperature and added to a mixed solution of ethanol and water with a volume ratio of 3:2 for the first washing, mainly to remove chloride salts, ammonium salts, etc. Then the washed precipitate is redissolved in 10ml N,N-dimethylpropylene urea (DMPU) and washed twice. Then the reaction product is placed in a vacuum oven at 45°C and dried for about 24 hours to finally obtain a modified polymer solid.

[0069] Step 5: Take 0.3 g of the modified polymer obtained in step 4 and dissolve it in 5 ml of N,N-dimethylpropylene urea (DMPU), and stir for a certain period of time to obtain a homogeneous sample solution.

[0070] Step 6: Use a dropper to absorb an appropriate amount of the modified homogeneous sample solution and drop it on the quartz glass substrate of the doctor blade coater for coating. The coating speed of the doctor blade is 200 cm / min. A film with a wet film thickness of 500 μm is formed on the substrate, and then vacuum dried at a temperature of 60°C for 8 hours. The thickness of the film after drying can be calculated based on the concentration of the sample solution.

[0071] Step 7: Take out the dried film, soak it in deionized water for 4 hours, and then carefully peel it off from the glass substrate. Place the peeled film on a homemade frame, and then put it into a vacuum drying oven and anneal it at 120°C for 24 hours.

[0072] Step 8: Finally, the annealed film is polarized with the polarization electric field controlled at 60MV / m, the polarization time at 30min, and the polarization temperature at room temperature to obtain a piezoelectric film, which is then subjected to performance testing.

[0073] Example 4

[0074] Step 1: Add 0.15g potassium persulfate (K2S2O8) and 100mL deionized water into a 300ml stainless steel container. The container is sealed and placed in a liquid nitrogen bath (-140°C), and then degassed by a vacuum pump. Gaseous vinylidene fluoride (VDF), trifluoroethylene (TrFE), chlorofluoroethylene (CFE), and propylene monomers are pumped into the container and liquefied instantly at liquid nitrogen temperature. The feed molar ratio of the monomers is 63:25:7:5, which is controlled by the pumping time of each gas, and the reaction is carried out at 90°C for 6 hours. After the reaction is completed, the container is cooled to room temperature and the excess gas is carefully removed. The separated polymer is repeatedly washed with deionized water and methanol and dried in vacuo at 50°C.

[0075] Step 2: Take 0.5 g of P (VDF-TrFE-CFE-P) tetrapolymer powder, dissolve it in 15 ml of dimethyl sulfoxide (DMSO), and stir it magnetically overnight (24 h) to obtain a homogeneous solution.

[0076] Step 3: Take a double-necked round-bottom flask, treat it to be anhydrous and oxygen-free and place it in a 50°C oil bath, pour the homogeneous solution into the round-bottom flask, then add 2 ml of tri-n-butylamine dropwise, and stir the reaction at 600 rpm for 6 hours.

[0077] Step 4: After the reaction is completed, the reaction system is slowly cooled to room temperature and added to a mixed solution of ethanol and water with a volume ratio of 3:2 for the first washing, mainly to remove chloride salts, ammonium salts, etc. Then the washed precipitate is redissolved in 10ml N,N-dimethylpropylene urea (DMPU) and washed twice. Then the reaction product is placed in a vacuum oven at 45°C and dried for about 24 hours to finally obtain a modified polymer solid.

[0078] Step 5: Take 0.3g of the modified polymer obtained in step 3 and dissolve it in 5ml of N,N-dimethylpropylene urea (DMPU), and stir for a certain period of time to obtain a homogeneous sample solution. Step 6: Use a dropper to absorb an appropriate amount of the modified homogeneous sample solution and drop it on the quartz glass substrate of the doctor blade coater for coating. The coating speed of the doctor blade is 200cm / min, and a thin film with a wet film thickness of 500μm is formed on the substrate, and then vacuum dried at a temperature of 60℃ for 8h.

[0079] Step 7: Take out the dried film, soak it in deionized water for 4 hours, and then carefully peel it off from the glass substrate. Place the peeled film on a homemade frame, and then put it into a vacuum drying oven and anneal it at 120°C for 24 hours.

[0080] Step 8: Finally, the annealed film is polarized with the polarization electric field controlled at 60MV / m, the polarization time at 30min, and the polarization temperature at room temperature to obtain a piezoelectric film, which is then subjected to performance testing.

[0081] Example 5

[0082] Step 1: Add 0.15g potassium persulfate (K2S2O8) and 100mL deionized water into a 300ml stainless steel container. The container is sealed and placed in a liquid nitrogen bath (-140°C), and then degassed by a vacuum pump. Gaseous vinylidene fluoride (VDF), trifluoroethylene (TrFE), chlorofluoroethylene (CFE), and propylene monomers are pumped into the container and liquefied instantly at liquid nitrogen temperature. The feed molar ratio of the monomers is 63:25:7:5, which is controlled by the pumping time of each gas, and the reaction is carried out at 90°C for 6 hours. After the reaction is completed, the container is cooled to room temperature and the excess gas is carefully removed. The separated polymer is repeatedly washed with deionized water and methanol and dried in vacuo at 50°C.

[0083] Step 2: Take 0.5 g of P (VDF-TrFE-CFE-P) tetrapolymer powder, dissolve it in 15 ml of dimethyl sulfoxide (DMSO), and stir it magnetically overnight (24 h) to obtain a homogeneous solution.

[0084] Step 3: Take a double-necked round-bottom flask, treat it to be anhydrous and oxygen-free and place it in a 50°C oil bath, pour the homogeneous solution into the round-bottom flask, then add 2 ml of tri-n-butylamine dropwise, and stir the reaction at 600 rpm for 9 hours.

[0085] Step 4: After the reaction is completed, the reaction system is slowly cooled to room temperature and added to a mixed solution of ethanol and water with a volume ratio of 3:2 for the first washing, mainly to remove chloride salts, ammonium salts, etc. Then the washed precipitate is redissolved in 10ml N,N-dimethylpropylene urea (DMPU) and washed twice. Then the reaction product is placed in a vacuum oven at 45°C and dried for about 24 hours to finally obtain a modified polymer solid.

[0086] Step 5: Take 0.3g of the modified polymer obtained in step 3 and dissolve it in 5ml of N,N-dimethylpropylene urea (DMPU), and stir for a certain period of time to obtain a homogeneous sample solution. Step 6: Use a dropper to absorb an appropriate amount of the modified homogeneous sample solution and drop it on the quartz glass substrate of the doctor blade coater for coating. The coating speed of the doctor blade is 200cm / min, and a thin film with a wet film thickness of 500μm is formed on the substrate, and then vacuum dried at a temperature of 60℃ for 8h.

[0087] Step 7: Take out the dried film, soak it in deionized water for 4 hours, and then carefully peel it off from the glass substrate. Place the peeled film on a homemade frame, and then put it into a vacuum drying oven and anneal it at 120°C for 24 hours.

[0088] Step 8: Finally, the annealed film is polarized with the polarization electric field controlled at 60MV / m, the polarization time at 30min, and the polarization temperature at room temperature to obtain a piezoelectric film, which is then subjected to performance testing.

[0089] Performance Testing

[0090] The electromechanical coupling coefficient, piezoelectric coefficient and elongation at break of the piezoelectric films obtained in the above examples and comparative examples are shown in the following table:

[0091]

[0092] From the data in the above table, we can see that:

[0093] From the elongation at break data of Comparative Example 1 and Example 1, it is found that the elongation at break of the film is greatly increased after the propylene segment is introduced into the copolymer, indicating that the tetrapolymer can increase the flexibility of the film.

[0094] From the k of Comparative Example 2 and other embodiments 33 and d 33 The data shows that compared with the existing technology, the high-performance piezoelectric film prepared by introducing carbon-carbon double bonds can significantly improve the electromechanical coupling performance and piezoelectric performance, and achieve huge electrostrictive strain under low electric fields. From the reaction time and data results, it can be seen that there is an optimal carbon-carbon double bond introduction content of about 2% (reaction time of about 6h). In addition, its piezoelectric sensor is very thin and light, with a small area, higher sensitivity, and high flexibility, which enables it to be better used in wearable electronic devices and other fields.

[0095] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing a high-performance flexible piezoelectric film, characterized in that The steps include: Step 1: adding potassium persulfate and water into a reactor, sealing the reactor and placing it in a liquid nitrogen bath for vacuum degassing; introducing gaseous vinylidene fluoride, trifluoroethylene, chlorofluoroethylene and propylene into the reactor, the gas is instantly liquefied when cooled, and heating is performed for copolymerization reaction; cooling to room temperature after the reaction, separating, washing and drying to obtain a tetrapolymer; Step 2: dissolving the quaternary copolymer in an organic solvent and stirring to obtain a homogeneous solution; Step 3: pouring the homogeneous solution into an oxygen-free environment reactor, adding an organic base, and performing an elimination reaction to remove hydrogen chloride from part of the chlorofluoroethylene segments in the tetrapolymer to form carbon-carbon double bonds; Step 4: After the reaction solution obtained in step 3 is cooled to room temperature, it is added to a mixed solution of ethanol and water, precipitated, washed, and dried to obtain a carbon-carbon double bond modified tetrapolymer; Step 5: dissolving the carbon-carbon double bond modified tetrapolymer in an organic solvent and stirring to obtain a homogeneous solution, coating the homogeneous solution on a substrate, and drying to form a film; Step 6: After soaking the film in water, peel it off from the substrate, and anneal the film to crystallize the film and increase the size and content of the β-phase crystals; the annealing treatment includes: heating at 110-120° C. for 8-24 hours, and then cooling to room temperature; Step 7: The annealed film is polarized to obtain a high-performance flexible piezoelectric film.

2. The preparation method according to claim 1, characterized in that: In step 1, the molar ratio of vinylidene fluoride, trifluoroethylene, chlorofluoroethylene and propylene is 63-69: 22.5-33.5: 6.5-8.5: 3.5-5.

5.

3. The preparation method according to claim 1 or 2, characterized in that: In step 1, the copolymerization reaction temperature is 85-95° C. and the reaction time is 4-8 hours.

4. The preparation method according to claim 1, characterized in that: In step 2, the organic solvent is N,N-dimethylpropylene urea (DMPU), dimethyl sulfoxide or triethyl phosphate.

5. The preparation method according to claim 1, characterized in that: In step three, The usage ratio of the organic base to the tetrapolymer is 0.5 g: 1 to 5 mL; The elimination reaction time is 1 to 6 hours.

6. The preparation method according to claim 1 or 5, characterized in that: In step 3, the organic base is triethylamine, diethylamine or tri-n-butylamine.

7. The preparation method according to claim 1, characterized in that: In step 4, the volume ratio of ethanol to water is 2:3 to 3:

2.

8. The preparation method according to claim 1, characterized in that: In step five, The film is prepared by a spin coating method, a solution casting method, a drop coating method or a blade coating method; The drying conditions are: 50-70° C., 8-12 h.

9. The preparation method according to claim 1, characterized in that: In step six, the soaking time is 2 to 6 hours.

10. The preparation method according to claim 1, characterized in that: In step seven, the polarization electric field is 40 to 100 MV / m, the polarization temperature is room temperature, and the polarization time is 15 to 30 minutes.

Citation Information

Cited By

  • Grafted ferroelectric polymer film with high piezoelectric coefficient and preparation method thereof

    CN121159905A

  • A ferroelectric polymer thin film with high piezoelectric coefficient and a preparation method thereof

    CN121159905B