Catalyst compositions and methods of making and using same

Through the chromium-free copper catalyst composition, the combination of aluminum oxide and copper compounds and cocatalysts is used to solve the threat of traditional catalysts to the environment and health, and the efficient catalytic performance and stability are achieved, suitable for hydrogenation or hydrogenation and hydrogenation reaction.

CN119072355APending Publication Date: 2024-12-03BASF CORPORATON
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380036023.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-25
Filing Date
2023-04-18
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The chromium-containing copper catalysts used in the prior art pose a threat to the environment and human health, and the use of REACH regulations limits its limitations.

Method used

The chromium-free copper catalyst composition is developed to form a catalyst with stable catalytic activity and high tolerance for hydrogenation or hydrogenation of carbonyl-containing organic compounds by combining alumina with copper compounds and cocatalysts.

Benefits of technology

Replaced with traditional copper-chromium catalysts, it reduces environmental pollution and health risks, improves the stability and selectivity of the catalyst, extends the service life of the catalyst, and shows excellent performance in multi-cycle tests.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119072355A_ABST
    Figure CN119072355A_ABST
Patent Text Reader

Abstract

Disclosed herein are chromium-free catalyst compositions having an alumina support and a copper compound on the alumina support. The catalyst composition may further include a co-catalyst. Further disclosed are methods of making such catalyst compositions and methods of using the same.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Priority declaration

[0002] This application claims the benefit of U.S. Provisional Patent Application No. 63 / 334,414, filed on April 25, 2022, under 35 U.S.C. §119(e), which is incorporated herein by reference. Technical Field

[0003] Embodiments of the present disclosure relate to chromium-free copper catalyst compositions and methods of making and using the same. Background Art

[0004] Some current commercial manufacturing processes for hydrogenation / hydrogenolysis of esters or carbonyl compounds to their corresponding alcohols use chromium-containing copper catalysts. Chromium-containing catalysts are considered hazardous chemicals for human health and environmental pollution under the Registration, Evaluation, Authorization and Restriction of Chemicals (REACH) regulations. Under such REACH regulations, the substance chromium (VI) trioxide (CrO 3 ) should not be put on the market and should not be used in the EU. Chromium-containing catalysts may potentially contain traces of Cr(6+) as an impurity. Summary of the invention

[0005] According to various embodiments, catalyst compositions are disclosed herein. In some embodiments, the catalyst composition comprises a support including alumina, a copper compound on the support, and a promoter, wherein the catalyst composition is free of chromium.

[0006] Further disclosed herein are methods of preparing the catalyst composition. In some embodiments, the methods include combining a copper-containing solution with alumina to form a combination, precipitating the combination with an alkaline solution to form a precipitate solution, filtering the precipitate solution to obtain a precipitate, and calcining the precipitate to form the catalyst composition.

[0007] In further embodiments, disclosed herein are methods for hydrogenating or hydrogenolyzing organic compounds containing carbonyl groups. According to embodiments, the methods may include contacting the organic compounds with a catalyst composition according to embodiments herein, wherein the catalyst composition does not contain chromium. BRIEF DESCRIPTION OF THE DRAWINGS

[0008] The present disclosure is illustrated by way of example, and not by way of limitation, in the figures of the accompanying drawings in which like references indicate similar elements.

[0009] Figure 1 is a graph showing incremental pore volume as a function of pore size for exemplary catalysts prepared in Examples 6-9 and calcined according to embodiments herein at 500° C. (Examples 6 and 8) and 750° C. (Examples 7-3 and 9).

[0010] Figure 2 is a graph showing cumulative pore area as a function of pore size for exemplary catalysts prepared in Examples 6-9 and calcined according to embodiments herein at 500° C. (Examples 6 and 8) and 750° C. (Examples 7-3 and 9).

[0011] Figure 3 is a graph showing incremental pore volume as a function of pore size for exemplary catalysts prepared in Examples 6-9 and calcined according to embodiments herein at 500° C. (Examples 6 and 8) and 750° C. (Examples 7-3 and 9).

[0012] Figure 4 is a graph showing cumulative pore area as a function of pore size for exemplary catalysts prepared in Examples 6-9 and calcined according to embodiments herein at 500° C. (Examples 6 and 8) and 750° C. (Examples 7-3 and 9).

[0013] Figure 5 is a graph showing x-ray diffraction (XRD) patterns of catalysts prepared in Examples 6-9 and calcined at 500° C. (Examples 6 and 8) and 750° C. (Examples 7-3 and 9) according to the embodiments herein.

[0014] Figure 6 is a graph showing XRD patterns of catalysts prepared using dried powder from Example 6, prepared in accordance with the embodiments herein, calcined at different temperatures, and prepared in Example 6 and Example 7-1 to Example 7-4.

[0015] Figure 7 is a graph showing the change in copper oxide crystallite size of the catalyst prepared in Example 7 according to embodiments herein as a function of calcination temperature.

[0016] Figure 8 The uncatalyzed Cu-Al 2 O 3 Plot of the performance of the catalyst (Example 1) compared to the CuCr Reference Example 1 in terms of fatty alcohol yield.

[0017] Fig. 9 It is shown that Mn promotes the Cu-Al 2 O 3 Plot of the performance of the catalyst (Example 2) compared to the CuCr Reference Example 1 in terms of fatty alcohol yield.

[0018] Fig.10 Figure 2 shows the Mn-promoted Cu-Al calcined at 500°C and 750°C, respectively. 2 O 3 Plot of the performance of the catalysts (Example 3 and Example 4) compared to the CuCr Reference Example 1 in terms of fatty alcohol yield.

[0019] Fig.11 The La-catalyzed Cu-Al 2 O 3 Plot of the performance of the catalysts (Example 5, Example 6 and Example 8) compared to the CuCr Reference Example 1 in terms of fatty alcohol yield.

[0020] Fig.12 Figure 2 shows the La-promoted Cu-Al calcined at 500°C and 750°C, respectively. 2 O 3 Plot of the performance of the catalysts (Example 6 and Example 7-3) compared to CuCr Reference Example 1 in terms of fatty alcohol yield.

[0021] Fig.13 is a graph showing a multi-cycle performance test of a CuCr reference catalyst composition (Example 1) according to embodiments herein.

[0022] Fig.14 is a graph showing a multi-cycle performance test of a catalyst composition (Example 6) according to an embodiment herein.

[0023] Fig.15A is a graph showing a comparison between the CuCr reference catalyst (Example 1) and the catalyst compositions of Examples 3 and 6 for the first cycle (fresh) of a multi-cycle performance test.

[0024] Fig. 15B is a graph showing a comparison between the CuCr reference catalyst (Example 1) and the catalyst compositions of Examples 3 and 6 for the second cycle (first reuse) of the multi-cycle performance test.

[0025] Fig. 15C is a graph showing a comparison of fatty alcohol yields between a CuCr reference catalyst (Example 1) and the catalyst compositions of Examples 3 and 6 for the third cycle (second reuse) of a multi-cycle performance test.

[0026] Fig.15D is a graph showing a comparison of fatty alcohol yields between a CuCr reference catalyst (Example 1) and the catalyst compositions of Examples 3 and 6 for the fourth cycle (third reuse) of a multi-cycle performance test.

[0027] Fig.15E is a graph showing a comparison of fatty alcohol yields between a CuCr reference catalyst (Example 1) and the catalyst compositions of Examples 3 and 6 for the fifth cycle (fourth reuse) of a multi-cycle performance test.

[0028] Fig.16is a graph showing a comparison between the CuCr reference catalyst (Example 1) and the catalyst composition of Example 6 for each cycle of repeated use in the hydrogenolysis of methyl esters to form fatty alcohols. DETAILED DESCRIPTION

[0029] In view of pollution and health hazards, it is desirable to replace chromium-containing copper catalysts with chromium-free catalysts. Therefore, embodiments of chromium-free copper catalysts are disclosed herein. The chromium-free promoted copper catalysts according to various embodiments herein can be used to replace the currently used copper-chromium (CuCr) catalysts that cause such environmental and health problems.

[0030] Catalyst composition

[0031] The catalyst composition according to the embodiments herein contains a carrier (e.g., alumina, pseudo-boehmite, gamma alumina, VERSAL TM V-250 alumina powder). The carrier is configured to carry metals (e.g., copper) and / or other promoters such as La, Mn, Ba, Zr, and Mg. The carrier formed by alumina powder can form a stable catalyst with a powder particle size distribution desired for the final catalyst. The powder catalyst composition with an appropriate particle size distribution leads to improved liquid product separation by filtration or centrifugation, and produces a more stable catalyst in the slurry phase process. Such a supported powder catalyst composition with an alumina powder carrier leads to providing greater tolerance to free organic acids present in the feed than the coprecipitated catalyst. In various embodiments, the catalyst composition contains copper and does not contain chromium. The catalyst composition according to one or more embodiments can also be in any suitable form, including but not limited to tablets and extrudates.

[0032] The catalyst composition may include one or more promoters. Adding a promoter to an alumina supported catalyst may improve further catalyst activity and stability through the additional interaction of the promoter with active metals and carriers. Suitable promoters include, but are not limited to, manganese (Mn), lanthanum (La), barium (Ba), calcium (Ca), magnesium (Mg), zirconium (Zr), strontium (Sr) and combinations thereof. Powdered catalysts with one or more promoters may exhibit higher product yields and higher stability to poisonings such as free acids and the like of impurities. After repeated use in the slurry phase hydrogenation process, the promoter Cu / alumina (Cu on alumina) catalyst may have stable catalytic activity. In certain embodiments, the promoter catalyst according to the embodiments herein has higher tolerance to chemical attack (such as raw materials containing organic acids), which will result in extended catalyst life.

[0033] According to at least one embodiment, shaped catalysts such as tablets exhibit favorable physical properties and stability in the presence of promoters such as Mn and La. In the presence of these promoters, shrinkage during calcination at higher temperatures is minimized. Such catalysts are particularly useful for hydrogenating organic compounds containing carbonyl groups such as aldehydes, esters, ketones, and carboxylic acids.

[0034] In some embodiments, the catalyst composition comprises about 35 wt % to about 70 wt % CuO, about 0 wt % to about 12 wt % BaO, about 0 wt % to about 12 wt % La 2 O 3 , about 0 wt% to about 15 wt% Mn 2 O 3 and about 20 wt % to about 40 wt % Al 2 O 3 The catalyst may have a crystalline phase of monoclinic copper (II) oxide (CuO), and one or more of the following crystalline phases: monoclinic lanthanum oxide carbonate (LaCO 3 ), lanthanum copper oxide (La 2 CuO 4 ), copper lanthanum oxide (CuLaO 3 ), copperaluminum oxide (CuAl 4 O 7 ), cubic copper aluminum oxide (CuAl 2 O 4 ), monoclinic lanthanum manganese oxide (LaMnO 3.13 ), Cubic copper manganese oxide (Cu 1.5 Mn 1.5 O 4 ), lanthanum copper oxide (La 2 CuO 4 ), cubic alumina (aluminum oxide) (Al 2 O 3 ) or alumina, etc. BET SA can be about 80m 2 / g to about 160m 2 / g, and the pore volume may be from about 0.25 ml / g to about 0.4 ml / g.

[0035] In embodiments where the catalyst composition is in the form of sub-units such as particles, granules, powders, spheres, extrudates, microplatelets, etc., the sub-units may have an average particle size distribution as follows: 10 From about 1 micron to about 3 microns, D 50 is about 10 microns to about 20 microns, and D 90 The bulk density may be about 0.25 g / ml to about 0.6 g / ml, and the CuO crystallite size may be about to

[0036] When the catalyst composition is in solid form such as a 1 / 8" tablet, the catalyst solid may have a crush strength of about 10 lbs to about 40 lbs. The bulk density may be about 1.0 g / ml to about 1.7 g / ml, and the BET SA may be about 20 m 2 / g to about 100m 2 / g, a pore volume of about 0.25 ml / g to about 0.4 ml / g, and an average pore diameter (as measured and calculated by 4V / A) of about to about

[0037] In the case of adding promoters (such as La and Ba), when the feed contains organic acids, the catalyst composition can have better stability to chemical attack such as repeated use. In addition, the catalyst composition according to the embodiments of the present invention can have stronger mechanical strength, especially after heat treatment at higher temperatures, and no or minimal shrinkage in the case of La promoter. Mn as a promoter also increases the catalyst hydrogenation and hydrogenolysis activity and selectivity to alcohol products.

[0038] According to various embodiments, the catalyst composition disclosed herein may include a carrier. The carrier may be composed of any suitable material. Suitable materials include, but are not limited to, alumina, pseudo-boehmite alumina, gamma alumina, VERSAL TM V-250 alumina powder, bayerite alumina, or a combination thereof.The catalyst composition can include the support material in an amount of about 10 wt % to about 50 wt %, about 15 wt % to about 45 wt %, or about 20 wt % to about 40 wt % based on the total weight of the catalyst composition.

[0039] According to various embodiments, the carrier has a bulk density of about 1 lbs / ft 3 About 60lbs / ft 3 , about 5lbs / ft 3 About 50lbs / ft 3, or about 10lbs / ft 3 About 40lbs / ft 3 , or any single value or sub-range within these ranges. In some embodiments, the carrier has a bulk density of about 1 lbs / ft 3 About 60lbs / ft 3 , about 5lbs / ft 3 About 50lbs / ft 3 , or about 10lbs / ft 3 About 40lbs / ft 3 , or any single value or sub-range within these ranges. According to some embodiments, the carrier has a surface area of ​​about 250 m 2 / g to about 400m 2 / g, about 275m 2 / g to about 375m 2 / g, or about 300m 2 / g to about 350m 2 / g.

[0040] In some embodiments, one or more metals or metal-containing compounds may be adsorbed onto the support. Suitable metals or metal-containing compounds include, but are not limited to, copper, copper oxide, copper-containing compounds, copper (I) oxide (cuprous oxide), copper (II) oxide (cupric oxide), or combinations thereof. The copper compound may include about to about In one or more embodiments, the catalyst composition may include monoclinic copper (II) oxide (CuO), and may further include one or more of the following crystalline phases: monoclinic lanthanum carbonate (LaCO 3 ); Orthorhombic lanthanum copper oxide (La 2 CuO 4 ); tetragonal copper lanthanum oxide (CuLaO 3 ); copper aluminum oxide (CuAl 4 O 7 ); Cubic copper aluminum oxide (CuAl 2 O 4 ); monoclinic lanthanum manganese oxide (LaMnO 3.13 ); Cubic copper manganese oxide (Cu 1.5 Mn 1.5 O 4 ); Orthorhombic lanthanum copper oxide (La 2 CuO 4 ); and / or cubic alumina (Al 2 O 3 ).

[0041] In some embodiments, the catalyst composition does not contain one or more of chromium, aluminum nitrate, acetate, chloride, or sodium aluminate. According to various embodiments, the catalyst composition according to embodiments herein may include a copper compound in an amount of about 25 wt % to about 80 wt %, about 35 wt % to about 70 wt %, or any single value or sub-range within these ranges, based on the total weight of the catalyst composition.

[0042] In at least one embodiment, the catalyst composition may include a promoter. Suitable promoters include, but are not limited to, lanthanum, manganese, barium, zirconium, calcium, magnesium, zinc, yttrium oxide, erbium oxide, cerium oxide, rare earth oxides, strontium, boron, nickel, platinum, silver, gold, palladium, ruthenium, or a combination thereof. In some embodiments, the catalyst composition contains one or more promoters in an amount of about 0wt% to about 20wt%, about 1wt% to about 15wt%, or about 5wt% to about 12wt%, or any single value or sub-range within these ranges. In some embodiments, the promoter includes barium oxide in an amount of about 0wt% to about 20wt%, or about 1wt% to about 15wt%, or about 5wt% to about 12wt% based on the total weight of the catalyst composition. In one or more embodiments, the promoter includes lanthanum oxide (LaO2) in an amount of about 0wt% to about 20wt%, or about 1wt% to about 17wt%, or about 5wt% to about 15wt% based on the total weight of the catalyst composition. 2 O 3 The co-catalyst may include manganese oxide (MnO) in an amount of about 0 wt % to about 20 wt %, or about 1 wt % to about 17 wt %, or about 5 wt % to about 15 wt %, based on the total weight of the catalyst composition. 2 O 3 ).

[0043] In one or more embodiments, the catalyst composition is in the form of a powder, a granule, an extrudate, a sphere, a solid, a tablet, a capsule, a slug, or a combination thereof. According to at least one embodiment, the catalyst composition comprises a D 10 , D from about 10 μm to about 20 μm 50 and D from about 30 μm to about 60 μm 90 In some embodiments, the catalyst composition is in powder form and comprises a loose bulk density of about 0.25 g / ml to about 0.6 g / m, or wherein the catalyst is in tablet form and comprises a bulk density greater than about 1.0 g / ml.

[0044] According to one or more embodiments, the catalyst composition has a stability against impurity poisoning of about 0.1% to about 0.5% organic acid or up to about 0.5% organic acid. In some embodiments, the catalyst composition has a stability of about 1 to about 10 reuses, about 1 to about 5 reuses, about 1 to about 4 reuses, about 2 to about 5 reuses when in a slurry phase when measured using a multi-cycle performance test for fatty alcohol production. In at least one embodiment, the catalyst composition has a fatty acid conversion of about 73% to about 99%, or at least about 73%, based on a reduction in % saponification (SAP) value.

[0045] The catalyst composition can be calcined. The calcined catalyst composition contains less moisture and / or impurities than the uncalcined catalyst composition. In some embodiments, the size of the catalyst composition before calcination is the same or approximately the same as the size of the catalyst composition after calcination.

[0046] The catalyst composition as described herein may have a BET surface area of ​​about 60 m 2 / g to about 200m 2 / g, about 70m 2 / g to about 180m 2 / g, or about 80m 2 / g to about 160m 2 / g, or any single value or sub-range within these ranges. In some embodiments, the catalyst composition is in the form of at least one of a sphere, a solid, a tablet, a capsule, or a small piece, and the thickness of the form is about 1 / 4 inch to about 1 / 16 inch, or about 1 / 8 inch, or any single thickness or sub-range within this range. The catalyst composition can be in any of the above forms, and the crush strength can be about 5lbs to about 40lbs, or any single value or sub-range within this range. In some embodiments, the catalyst composition has a bulk density of about 1.0g / ml to about 1.7g / ml, or any single value or sub-range within this range. In one or more embodiments, the catalyst composition as described herein has a BET surface area (SA) of about 20m 2 / g to about 100m 2 / g, or any single value or sub-range therein. The catalyst compositions described herein may include a pore volume of about 0.25 ml / g to about 0.4 ml / g, or any single value or sub-range therein. In some embodiments, the catalyst compositions described herein may have an average pore size of about to about Or any single value or sub-range within this range, as measured and calculated by 4 volume / area (V / A).

[0047] Method for preparing a chromium-free catalyst composition

[0048] The catalyst composition according to the embodiments of the present invention can be prepared using a metal or a metal-containing compound (e.g., CuO) and one or more promoters (e.g., an oxide promoter) on a support material (e.g., an alumina powder) Deposition-precipitation. Compared to conventional catalyst compositions, the resulting catalyst composition can have improved stability and higher activity and selectivity for hydrogenation and hydrogenolysis of organic compounds containing carbonyl groups. Previous copper catalysts containing alumina were prepared by coprecipitation using alumina salts such as aluminum nitrate, aluminum acetate, aluminum chloride, or sodium aluminate as alumina raw materials, and such compositions did not show the same level of stability, activity, or selectivity for hydrogenation and hydrogenolysis of organic compounds containing carbonyl groups compared to the catalyst composition according to the embodiments of the present invention.

[0049] Further disclosed herein are methods of preparing a chromium-free catalyst composition. In some embodiments, the catalyst composition is formed by deposition-precipitation, wherein an alumina powder is combined with an initial water heel and another metal to form a slurry that is deposited onto a support (e.g., alumina powder).

[0050] In one or more embodiments, the method of preparing the catalyst composition includes combining a copper-containing solution with alumina to form a combination. The combination can be a slurry, a suspension, a dispersion, a liquid, a mixture thereof, or any combination thereof. The copper-containing solution can include, but is not limited to, copper (II) nitrate (Cu(NO 3 ) 2 ), copper(I) chloride, copper(II) acetate, or a combination thereof. The alumina may be in the form of a powder, granules, extrudates, spheres, solids, tablets, caplets, nuggets, or a combination thereof. In some embodiments, the alumina may include pseudo-boehmite alumina, bayerite alumina, gamma alumina, or a combination thereof.

[0051] The method may further include precipitating the combination with an alkaline solution to form a precipitate solution. In certain embodiments, precipitating the combination includes merging the combination with an alkali. The alkali may include but is not limited to sodium hydroxide (NaOH), soda ash or a combination thereof. According to an embodiment, when precipitating the combination, the combination is maintained at a pH of about 6.5 to about 7.8.

[0052] The method may further include filtering the precipitate solution to obtain a precipitate. The precipitate is a solid material collected by a filter. The precipitate may be in the form of subunits such as particles, aggregates, flakes, etc. In some embodiments, the method includes washing the precipitate and then drying the washed precipitate.

[0053] In one or more embodiments, the method further includes calcining the precipitate to form a catalyst composition. The calcining of the precipitate can be at a temperature of about 200°C to about 800°C, 300°C to about 700°C, about 400°C to about 600°C, or about 450°C to about 500°C for about 30 minutes to about 4 hours, about 1 hour to about 3 hours, about 1.5 hours to about 2.0 hours. The resulting catalyst composition may be free of chromium. In some embodiments, the catalyst composition also does not contain aluminum nitrate, acetate, chloride or sodium aluminate.

[0054] In some embodiments, the catalyst composition prepared may include about 40 wt% to about 70 wt%, or about 55 wt% to about 65 wt% copper (II) oxide (CuO) and about 30 wt% to about 60 wt%, or about 40 wt% to about 50 wt% alumina. The catalyst composition may have a loose bulk density of about 0.1 g / cc to about 0.5 g / cc, or about 0.2 g / cc to about 0.3 g / cc. In some embodiments, the catalyst composition may have a packed bulk density of about 0.2 g / cc to about 0.6 g / cc, or about 0.3 g / cc to about 0.4 g / cc. In some embodiments, the catalyst composition is a catalyst having a D of about 1 μm to about 10 μm. 10 , D from about 10 μm to about 20 μm 50 and D from about 30 μm to about 60 μm 90 The average particle size of the powder.

[0055] Methods of using chromium-free catalyst compositions

[0056] In some embodiments, the catalyst composition according to the embodiments herein (e.g., a CuO / alumina (CuO on alumina) powder catalyst of the catalytic promoter) can be used for the hydrogenation or hydrogenolysis of compounds containing carbonyl groups, especially methyl esters, dimethyl esters, wax esters, aldehydes, ketones and carboxylic acids. The method for hydrogenating or hydrogenolyzing organic compounds containing carbonyl groups may include contacting these organic compounds with the catalyst composition according to the embodiments herein. The catalyst composition may be chromium-free.

[0057] In some embodiments, these organic compounds include one or more of aldehydes, esters, ketones or carboxylic acids. These organic compounds may include one or more of fatty esters or methyl esters. In some embodiments, these organic compounds include methyl esters, which undergo hydrogenolysis to form one or more fatty alcohols. In one or more embodiments, these organic compounds include wax esters, which undergo hydrogenolysis to form one or more fatty alcohols.

[0058] Examples

[0059] These catalyst samples were characterized and evaluated for catalytic performance for fatty ester hydrogenolysis applications. The details of the catalyst preparation procedure are illustrated by the following examples.

[0060] Reference Example 1CuCr Catalyst

[0061] A commercial copper chromium catalyst was obtained.

[0062] Reference Example 2Cu-Al 2 O 3 catalyst

[0063] Preparation of Cu-Al using co-precipitation method 2 O 3 The Cu-Al catalyst was prepared by weighing out 1640 g of copper nitrate solution (15.48% Cu) and then diluting it to 2500 ml with deionized water. 2 O 3 The preparation method further comprises weighing 815.6 g of sodium aluminate (25% Al 2 O 3 ) and dilute the solution to 2500 ml with deionized water.

[0064] Fill 2500ml of deionized water in a 12-liter tank. The method then weighs out 318g of sodium carbonate powder and dissolves it in deionized water to 1500ml. Copper nitrate solution and sodium aluminate solution are added to 2500ml of deionized water at the same time. Copper nitrate solution and sodium aluminate solution are added at a rate of 33ml / min. Sodium carbonate (soda ash) solution is added to the mixture, keeping the pH of the slurry constant at about 7.4 (by adjusting the addition rate of the soda ash solution). Precipitation is carried out at room temperature. The resulting slurry is filtered to form a filter cake. The filter cake is washed three or more times with 3000ml of deionized water. The filter cake is dried overnight at 120°C. The dried CuAl powder is calcined at 700°C-800°C for 2 hours.

[0065] Reference Example 3Cu-Mn-Al 2 O 3

[0066] Preparation of Cu-Mn-Al using co-precipitation method 2 O 3 Catalyst Cu. Weigh out 984.6 g Cu(NO 3 ) 2 Solution. To this Cu(NO 3 ) 2 200.3 g Mn(NO 3 ) 2 The resulting mixture was diluted to 1 L with deionized water. The preparation method includes weighing 439 g Na 2 Al 2 O 4, which was diluted to 667 mL with deionized water. 1.33 L of deionized water feed was placed in a baffled impact tank with a stirring rate of 400 RPM. 267 g of Na 2 CO 3 And diluted to 1.33L with deionized water. CuMn solution was added at 16mL / min, while Al solution was added at 11mL / min. Sodium carbonate (soda ash) solution was added to the mixture, keeping the pH of the slurry constant at about 7.0 (by adjusting the addition rate of the soda ash solution at room temperature). The slurry was filtered to collect the filter cake solids. The filter cake was washed with deionized water and dried at 120°C overnight. The dried powder was calcined at 750°C for 4 hours. The resulting preparation has a chemical composition of 58% CuO-12% Mn 2 O 3 -30% Al 2 O 3 .

[0067] These reference catalysts are used to illustrate the superior performance of the catalysts of the present invention when applied to the hydrogenolysis of fatty esters. 2 O 3 and Cu-Mn-Al 2 O 3 Improvements in catalysts.

[0068] Examples of the present invention

[0069] Preparation of Catalyst Compositions According to Various Examples Described herein The following list of raw materials was used to prepare the inventive examples.

[0070] UOP V-250 Alumina Powder

[0071] NaOH 50% solution

[0072] Na 2 CO 3 Sodium carbonate

[0073] Cu(NO 3 ) 2 Copper Nitrate 17%

[0074] La(NO 3 ) 3

[0075] Mn(NO 3 ) 2

[0076] BaCO 3

[0077] Ba(NO 3 ) 2

[0078] Example 1 - Chromium-free copper catalyst composition

[0079] The following laboratory procedure was used to prepare the CuO / Al according to the examples described herein. 2 O 3 (CuO on Al 2 O 3 ) Catalyst composition:

[0080] 1) Weigh out 2100g Cu(NO 3 ) 2 Solution (Soln.) (16.16% Cu, from the factory), diluted to 2 liters with DI.

[0081] 2) Add DI water to 2 liters and set the mixing speed to 400 RPM.

[0082] 3) Weigh out 287g of V-250 UOP alumina powder and slowly add it to the feed. Keep stirring until the alumina powder is completely dispersed in the slurry.

[0083] 4) Weigh out 250 g of 50% NaOH, dissolve in DI, and dilute to 2.75 L. Weigh the solution before and after precipitation to get the amount of soda ash consumed.

[0084] 5) Maintain the slurry pH = 7.0 by adjusting the rate of addition of alkaline solution (room temperature)

[0085] 6) The precipitation is completed by adding copper nitrate and alkaline solution simultaneously within one hour

[0086] 7) Measure slurry particle size throughout the precipitation process

[0087] 8) Filter the slurry and wash the filter cake

[0088] 9) Dry the washed filter cake to form a powder

[0089] 10) The dried powder was calcined at 500°C for 2 hours to form the final catalyst powder.

[0090] The resulting calcined powder catalyst contained about 60% CuO, with the balance being alumina. Other characteristics of the catalyst included a loose apparent bulk density (ABD) of 0.27 g / cc and a packed ABD of 0.37 g / cc. The catalyst had the following particle size distribution: 10 =6.2 microns, D 50 = 16.7 μm, and D 90 =56.5 microns.

[0091] Example 2 - Target composition - 58% CuO - 12% M2 O 3 -30% Al 2 O 3 Chromium-free copper catalyst

[0092] The following laboratory procedure was used to prepare the Cu-Mn-Al according to the examples described herein. 2 O 3 (58% CuO-12% MnOX-30% Al 2 O 3 ), 34846-43-2 and 34846-47-3 catalyst compositions:

[0093] 1) Weigh out 1400g Cu(NO 3 ) 2 Solution (16.16% Cu, from factory),

[0094] 2) Weigh out 311g of manganese nitrate solution

[0095] 3) Mix solutions 1 and 2 and dilute to 1.33 liters with deionized (DI) water.

[0096] 4) Add 2 liters of water and set the mixing speed to 400 RPM.

[0097] 5) Weigh out 191 g of V-250 UOP alumina powder and slowly add it to the feed. Keep stirring until the alumina powder is completely dispersed in the slurry.

[0098] 6) Weigh out 750 g of soda ash and dissolve in 2.75 liters of DI water. Weigh the solution before and after precipitation to get the amount of soda ash consumed.

[0099] 7) Maintain the slurry pH = 7.0 by adjusting the rate of addition of alkaline solution (room temperature)

[0100] 8) The precipitation is completed by adding copper nitrate and alkaline solution simultaneously within one hour

[0101] 9) Measure slurry particle size throughout the precipitation process

[0102] 10) Filter the slurry and wash the filter cake

[0103] 11) Dry the washed filter cake to form a powder

[0104] 12) Calcine the dried powder at 500°C for 2 hours

[0105] The obtained dry powder has the following main characteristics: The particle size distribution of this catalyst is D 10 , 3.3 μm, D 50 , 12.7 μm, D 90, 126.9 microns; loose apparent bulk density (LABD) = 0.37 g / ml; and filled apparent bulk density (PABD) = 0.47 g / ml.

[0106] Example 3 - Target composition - 61% CuO - 6.5% Mn 2 O 3 -30% Al 2 O 3 Chromium-free copper catalyst

[0107] The following laboratory procedure was used to prepare 61% CuO-6.5% Mn according to the examples described herein. 2 O 3 -30% Al 2 O 3 Catalyst composition:

[0108] 1) Weigh out 1400g Cu(NO 3 ) 2 Solution (16.16% Cu, from factory),

[0109] 2) Weigh out 156g of manganese nitrate solution

[0110] 3) Mix solutions 1 and 2 and dilute to 1.33 L with DI water

[0111] 4) Add 2 liters of water and set the mixing speed to 400 RPM

[0112] 5) Weigh out 191g of V-250UOP alumina powder and slowly add it to the feed. Keep stirring until the alumina powder is completely dispersed in the slurry.

[0113] 6) Weigh out 750 g of soda ash and dissolve in 2.75 liters of DI water. Weigh the solution before and after precipitation to get the amount of soda ash consumed

[0114] 7) Maintain the slurry pH = 7.0 by adjusting the rate of addition of alkaline solution (room temperature)

[0115] 8) The precipitation is completed by adding copper nitrate and alkaline solution simultaneously within one hour

[0116] 9) Measure slurry particle size throughout the precipitation process

[0117] 10) Filter the slurry and wash the filter cake

[0118] 11) Dry the washed filter cake to form a powder

[0119] 12) Calcine the dried powder at 500°C for 2 hours

[0120] The dry powder had the following chemical composition: 61.5% CuO, 6.3% Mn 2 O 3 and 30.1% Al 2 O 3 The particle size distribution of this catalyst is: D 10 , 4.3 μm, D 50 , 29.0 μm and D 90 , 128.5 microns. The final calcined catalyst had the following properties: LABD - 0.28 g / ml, PABD = 0.36 g / ml and BET = 127 m 2 / g.

[0121] Tablets were prepared from the dried powder. These tablets had a size of 3 mm x 3 mm tablets and were made by adding 2%-3% graphite to the powder, calcining the powder at 500°C. The tablets were finally calcined at 750°C for 4h. The tablet properties were as follows:

[0122] Side crushing strength (lbs): 45

[0123] BET surface area (m 2 / g):48

[0124] Average bed density (g / mL): 1.5

[0125] N 2 Pore ​​volume (cm 3 / g): 0.14

[0126] Average pore size (nm): 128.2

[0127] Cu dispersion (%): 1.7

[0128] Example 4 - Chromium-free copper catalyst composition

[0129] The procedure for precipitation and drying was the same as in Example 3. The final calcination was at 750°C for 2 hours. The resulting dry powder had the same chemical composition as in Example 3: 61.5% CuO, 6.3% Mn 2 O 3 and 30.1% Al 2 O 3 The particle size distribution of the catalyst is: 10 , 4.3 μm, D 50 , 29.0 μm and D 90 , 128.5 microns.

[0130] Example 5 - Chromium-free copper catalyst composition - Cu-La-Al 2 O 3 (low La)

[0131] The following laboratory procedure was used to prepare the Cu-La-Al 2 O 3 (Low La). Catalyst compositions according to embodiments described herein:

[0132] 1) Weigh out 1400g Cu(NO 3 ) 2 Solution (16.16% Cu, from factory),

[0133] 2) Weigh out 53g of lanthanum nitrate solution (22% La solution)

[0134] 3) Mix solutions 1 and 2 and dilute to 1.33 liters with DI water.

[0135] 4) Add 2 liters of water and set the mixing speed to 400 RPM.

[0136] 5) Weigh out 191 g of V-250 UOP alumina powder and slowly add it to the feed. Keep stirring until the alumina powder is completely dispersed in the slurry.

[0137] 6) Weigh 750 g of soda ash and dissolve in 2.75 liters of DI water. Weigh the solution before and after precipitation to get the amount of soda ash consumed.

[0138] 7) Maintain the slurry pH = 7.0 by adjusting the rate of addition of alkaline solution (room temperature)

[0139] 8) The precipitation is completed by adding copper nitrate and alkaline solution simultaneously within one hour

[0140] 9) Measure slurry particle size throughout the precipitation process

[0141] 10) Filter the slurry and wash the filter cake

[0142] 11) Dry the washed filter cake to form a powder

[0143] 12) Calcine the dried powder at 500°C for 2 hours

[0144] The analysis results showed that the catalyst had the following composition: 66.3% CuO-3.2% La 2 O 3 -30.5% Al 2 O 3 .

[0145] Tablets were prepared from the dry powder. These tablets had a size of 3 mm x 3 mm and were made by adding 2%-3% graphite to the dry powder, calcining the dry powder at 500°C. The tablets were finally calcined at 750°C for 4h. The tablets obtained had the following properties: side crushing strength (lbs): 29, BET surface area (m 2 / g): 52, average bed density (g / mL): 1.42, and N 2 Pore ​​volume (cm 3 / g):0.16.

[0146] Example 6 - Chromium-free copper catalyst composition - Cu-La-Al 2 O 3 (Chinese)

[0147] The following laboratory procedure was used to prepare the Cu-La-Al 2 O 3 (La in). Catalyst compositions according to embodiments described herein:

[0148] 1) Weigh out 1400g Cu(NO 3 ) 2 Solution (16.16% Cu, from factory),

[0149] 2) Weigh out 106g of lanthanum nitrate solution (22% La solution)

[0150] 3) Mix solutions 1 and 2 and dilute to 1.33 liters with DI water.

[0151] 4) Add 2 liters of water and set the mixing speed to 400 RPM.

[0152] 5) Weigh out 191 g of V-250 UOP alumina powder and slowly add it to the feed. Keep stirring until the alumina powder is completely dispersed in the slurry.

[0153] 6) Weigh out 750 g of soda ash and dissolve in 2.75 liters of DI water. Weigh the solution before and after precipitation to get the amount of soda ash consumed.

[0154] 7) Maintain the slurry pH = 7.0 by adjusting the rate of addition of alkaline solution (room temperature)

[0155] 8) The precipitation is completed by adding copper nitrate and alkaline solution simultaneously within one hour

[0156] 9) Measure slurry particle size throughout the precipitation process

[0157] 10) Filter the slurry and wash the filter cake

[0158] 11) Dry the washed filter cake to form a powder

[0159] 12) Calcine the dried powder at 500°C for 2 hours

[0160] The analysis results showed that the obtained catalyst had the following composition: 63.3% CuO-6.3% La 2 O 3 -29.4% Al 2 O 3 .

[0161] Tablets were prepared from the dry powder. Each tablet had a size of 3 mm x 3 mm and was made by adding 2%-3% graphite to the dry powder and calcining the dry powder at 500°C. The tablets were finally calcined at 750°C for 4h. Each tablet had the following properties: side crushing strength (lbs): 27, BET surface area (m 2 / g): 48, and average bed density (g / mL): 1.45.

[0162] The pore size and distribution and surface area and distribution of Examples 6 to 9 were analyzed by nitrogen. The two groups of samples were calcined at different temperatures of 500°C and 750°C. The higher temperature calcination produced lower surface area and larger pore size, and the pore area also shifted to larger pore size. When the calcination temperature increased from 500°C to 750°C, the pore volume decreased from 0.36 ml / g to 0.30 ml / g. This resulted in a larger average pore size, from To 155 to

[0163] Example 7 - Chromium-free copper catalyst composition - Cu-La-Al 2 O 3 (Medium La, calcined at 750℃ for 4 hours)

[0164] The chromium-free copper catalyst composition (Cu-La-Al) was prepared using the same precipitation and drying method as described in Example 6. 2 O 3 , in La). The dried powder from Example 6 was calcined for 4 hours at different temperatures: 600°C, 700°C, 750°C and 800°C. This process produced the following catalysts:

[0165] Example 7-1, 600°C

[0166] Example 7-2, 700°C

[0167] Example 7-3, 750°C

[0168] Example 7-4, 800°C

[0169] The catalytic performance of these catalysts was tested and analyzed by XRD.

[0170] Example 8 - Chromium-free copper catalyst composition - Cu-La-Al 2 O 3 (Gao La)

[0171] The following laboratory procedure was used to prepare the Cu-La-Al 2 O 3 (High La) Catalyst Composition:

[0172] 1) Weigh out 1400g Cu(NO 3 ) 2 Solution (16.16% Cu, from factory),

[0173] 2) Weigh out 212g of lanthanum nitrate solution (22% La solution)

[0174] 3) Mix solutions 1 and 2 and dilute to 1.33 liters with DI water.

[0175] 4) Add 2 liters of water and set the mixing speed to 400 RPM.

[0176] 5) Weigh out 191 g of V-250 UOP alumina powder and slowly add it to the feed. Keep stirring until the alumina powder is completely dispersed in the slurry.

[0177] 6) Weigh out 750 g of soda ash and dissolve in 2.75 liters of DI water. Weigh the solution before and after precipitation to get the amount of soda ash consumed.

[0178] 7) Maintain the slurry pH = 7.0 by adjusting the rate of addition of alkaline solution (room temperature)

[0179] 8) The precipitation is completed by adding copper nitrate and alkaline solution simultaneously within one hour

[0180] 9) Measure slurry particle size throughout the precipitation process

[0181] 10) Filter the slurry and wash the filter cake

[0182] 11) Dry the washed filter cake to form a powder

[0183] 12) Calcine the dried powder at 500°C for 2 hours

[0184] The analysis results showed that the catalyst had the following composition: 58.7% CuO, 11.9% La 2 O 3 and 28.4% Al 2 O 3 .

[0185] Example 9 - Chromium-free copper catalyst composition - Cu-La-Al 2 O3 (Gao La)

[0186] A chromium-free copper catalyst composition was prepared using the method described in Example 8. The resulting dry powder was calcined at 750°C for 2 hours. The analysis results showed that this catalyst had the same composition as Example 8: 58.7% CuO, 11.9% La 2 O 3 and 28.4% Al 2 O 3 .

[0187] The pore size and distribution and surface area and distribution of Examples 6 to 9 were analyzed by nitrogen. The two groups of samples were calcined at different temperatures of 500°C and 750°C. The pore area of ​​the sample calcined at 750°C increased from about to Move to about The data are summarized in Table 1.

[0188] Table 1 - Properties of Chromium-free Catalysts of Examples 6 to 9

[0189]

[0190] Incremental and Cumulative Pore Volume vs. Pore Size for Selected Catalysts from Examples 6, 7, 8, and 9

[0191] Figure 1 is a graph showing incremental pore volume as a function of pore size for exemplary catalysts prepared in Examples 6-9 and calcined according to embodiments herein at 500° C. (Examples 6 and 8) and 750° C. (Examples 7-3 and 8), respectively. Figure 2 is a graph showing the cumulative pore area as a function of pore size for exemplary catalyst samples prepared in Examples 6-9 and calcined according to embodiments herein at 500° C. (Examples 6 and 8) and 750° C. (Examples 7-3 and 8), respectively.

[0192] Figure 3 is a graph showing incremental pore volume as a function of pore size for exemplary catalysts prepared in Examples 6-9 and calcined according to embodiments herein at 500° C. (Examples 6 and 8) and 750° C. (Examples 7-3 and 8), respectively. Figure 4 is a graph showing the cumulative pore area as a function of pore size for exemplary catalysts prepared in Examples 6-9 and calcined at 500° C. (Examples 6 and 8) and 750° C. (Examples 7-3 and 8) according to the embodiments herein, respectively. With the addition of more La, the total pore volume remains unchanged, although the higher calcination temperature reduces the pore volume, and the pore size is relatively larger.

[0193] XRD Analysis of Selected Catalysts from Examples 6, 7, 8 and 9

[0194] XRD analysis of the catalyst of the present invention (calcined from 500°C to 800°C) was performed to identify the crystallite phase and crystallite size.

[0195] XRD analysis was performed according to the procedure described herein. An Empyrean diffraction system with a copper anode tube was operated at generator settings of 45 kV and 40 mA to produce a wavelength of Cu K α1 Radiation, which is used to generate XRD analysis data. The optical path consists of a 0.04 rad primary Soller slit, a 15 mm beam mask, a 1° divergence slit, a 2° anti-scattering slit, a sample, a monochromator, a 0.02 rad secondary Soller slit and an X'Celerator position sensitive detector.

[0196] The sample was ground into a fine powder using a mortar and pestle and then backfilled into a circular base sample holder. The sample holder was loaded onto a sample rotator during data collection to improve particle counting statistics. Data collection from the circular base covered the range from 15° to 90° 2θ using a continuous scan with a step size of 0.017° 2θ and a step time of 400 s. A graphite monochromator was used to strip unwanted radiation, including Cu K β radiation.

[0197] Panalytical HighScore version 4.5 software and ICDD PDF version 4+2020 powder diffraction file database were used for phase identification analysis. Highstore was also used for characteristic curve fitting to determine d-spacing, FWHM, and peak positions, which were used to calculate crystallite size estimates using the Scherrer equation.

[0198] Details of the XRD patterns and crystallite sizes of samples from each example are shown in Figure 5 And summarize as follows:

[0199] Example 6 - Possible candidate phases include monoclinic copper (II) oxide (CuO) and monoclinic lanthanum carbonate (La 2 CO 5 ).

[0200] Example 7 - Possible candidate phases include monoclinic copper (II) oxide (CuO), tetragonal copper lanthanum oxide (CuLaO 3 ) and orthorhombic lanthanum copper oxide (La 2 CuO 4 ), and there may also be cubic copper aluminum oxide (CuAl 2 O 4 ).

[0201] Example 8 - Possible candidate phases include monoclinic copper (II) oxide (CuO), monoclinic lanthanum carbonate (La2 CO 5 ) and possibly cubic spinel manganese oxide (Mn 2 O 3 ).

[0202] Example 9 - Possible candidate phases include monoclinic copper (II) oxide (CuO), orthorhombic lanthanum copper oxide (La 2 CuO 4 ) and possible formation of cubic copper aluminum oxide (CuAl 2 O 4 ).

[0203] Figure 5 is a graph showing x-ray diffraction (XRD) patterns of catalysts prepared in Examples 6-9 and calcined at 500° C. (Example 6 and Example 8) and 750° C. (Example 7-3 and Example 8), respectively, according to the embodiments herein.

[0204] As the calcination temperature increases, La 2 CO 5 Transformed into tetragonal copper lanthanum oxide (CuLaO 3 ) or orthorhombic lanthanum copper oxide (La 2 CuO 4 ; and part of CuO is converted into tetragonal copper lanthanum oxide (CuLaO 3 ) and orthorhombic lanthanum copper oxide (La 2 CuO 4 ) and possibly cubic copper aluminum oxide (CuAl 2 O 4 ).

[0205] The microcrystalline phase identification results of each of these samples were compared with the reference XRD index card (Table 2-6). Table 2-6 provides 2θ, d-spacing, I (relative intensity), hkl (crystal plane). By comparing the XRD diffraction pattern with 2θ and relative intensity, the microcrystalline phase characteristics of each chromium-free copper catalyst sample were identified.

[0206] Table 2 - Microcrystalline phase characteristics of CuO 00-048-1548

[0207]

[0208] Table 3 - CuAl 2 O 4 Microcrystalline phase characteristics of 04-002-5874

[0209]

[0210] Table 4-La 2 CO 5 Microcrystalline phase characteristics of 00-023-0322

[0211]

[0212] Table 5 - CuLaO 3 ,04-022-5441 microcrystalline phase characteristics

[0213]

[0214] Table 6-La 2 CuO 4 Microcrystalline phase characteristics of 00-038-0709

[0215]

[0216] Example 10 - Chromium-free copper catalyst composition - Cu-Mn-La-Al 2 O 3 (500℃)

[0217] Target 58% CuO-3% Mn 2 O 3 -9% La 2 O 3 -30% Al 2 O 3

[0218] The following laboratory procedure was used to prepare the Cu-Mn-La-Al according to the examples described herein. 2 O 3 (36084-4A (500°C) (target 58% CuO-3% Mn 2 O 3 -9% La 2 O 3 -30% Al 2 O 3 ) Catalyst composition:

[0219] 1) Weigh out 930g Cu(NO 3 ) 2 Solution (16.16% Cu, from factory),

[0220] 2) Weigh out 53g of manganese nitrate solution

[0221] 3) Weigh out 115.5g of lanthanum nitrate solution (22% La solution)

[0222] 4) Mix solutions 1, 2 and 3 and dilute to 1.0 liter with DI water.

[0223] 5) Add 1.33 liters of water and set the mixing speed to 400 RPM.

[0224] 6) Weigh out 142g of V-250 UOP alumina powder and slowly add it to the feed. Keep stirring until the alumina powder is completely dispersed in the slurry.

[0225] 7) Weigh 500 g of soda ash and dissolve in 1.33 liters of DI water. Weigh the solution before and after precipitation to get the amount of soda ash consumed.

[0226] 8) Maintain the slurry pH = 7.0 by adjusting the rate of addition of alkaline solution (room temperature)

[0227] 9) The precipitation is completed by adding copper nitrate and alkaline solution simultaneously within one hour

[0228] 10) Measure slurry particle size during the entire precipitation process

[0229] 11) Filter the slurry and wash the filter cake

[0230] 12) Dry the washed filter cake to form a powder

[0231] 13) Calcine the dried powder sample at 500°C for 2 hours

[0232] Example 11 - with target composition (750°C) 58% CuO-3% Mn 2 O 3 -9% La 2 O 3 -30% Al 2 O 3 Chromium-free copper catalyst

[0233] The chromium-free copper catalyst composition (Cu-Mn-La-Al 2 O 3 , 750℃, target 58% CuO-3% MnO-9% La 2 O 3 -30% Al 2 O 3 The obtained dry powder was calcined at 750°C for 2 hours. The catalyst composition had the following particle size distribution (micrometers): D 10 5.76μm, D 50 18.7 μm and D 90 38.3μm.

[0234] Example 12 - with target composition - Cu-Mn-La-Al 2 O 3 (500℃)58%CuO-6%Mn 2 O 3 -6% La 2 O3 -30% Al 2 O 3 Chromium-free copper catalyst

[0235] The following laboratory procedure was used to prepare the Cu-Mn-La-Al according to the examples described herein. 2 O 3 (500℃)Target 58% CuO-6% Mn 2 O 3 -6% La 2 O 3 -30% Al 2 O 3 Catalyst composition:

[0236] 1) Weigh out 930g Cu(NO 3 ) 2 Solution (16.16% Cu, from factory),

[0237] 2) Weigh out 105g of manganese nitrate solution

[0238] 3) Weigh out 77g of lanthanum nitrate solution (22% La solution)

[0239] 4) Mix solutions 1 and 2 and dilute to 1.0 liter with DI water.

[0240] 5) Add 1.33 liters of water and set the mixing speed to 400 RPM.

[0241] 6) Weigh out 142g of V-250 UOP alumina powder and slowly add it to the feed. Keep stirring until the alumina powder is completely dispersed in the slurry.

[0242] 7) Weigh out 500 g of soda ash, dissolve in DI, and dilute to 1.33 L. Weigh the solution before and after precipitation to get the amount of soda ash consumed.

[0243] 8) Maintain the slurry pH = 7.0-7.5 by adjusting the rate of addition of alkaline solution (room temperature)

[0244] 9) The precipitation is completed by adding copper nitrate and alkaline solution simultaneously within one hour

[0245] 10) Measure slurry particle size during the entire precipitation process

[0246] 11) Filter the slurry and wash the filter cake

[0247] 12) Dry the washed filter cake to form a powder

[0248] 13) Calcine the dried powder at 500°C for 2 hours

[0249] Example 13 - with target composition (750°C) 58% CuO-6% Mn 2 O 3 -6% La 2 O 3 -30% Al 2 O 3 Chromium-free copper catalyst

[0250] The chromium-free copper catalyst composition (Cu-Mn-La-Al 2 O 3 (750℃) Target 58% CuO-6% Mn 2 O 3 -6% La 2 O 3 -30% Al 2 O 3 The obtained dry powder was calcined at 750°C for 2 hours. The catalyst composition had the following particle size distribution (micrometers): D 10 6.4μm, D 50 21 μm and D 90 41.5μm.

[0251] Example 14 - with target composition - (500°C) 58% CuO - 9% Mn 2 O 3 -3% La 2 O 3 -30% Al 2 O 3 Chromium-free copper catalyst

[0252] The following laboratory procedure was used to prepare the Cu-Mn-La-Al according to the examples described herein. 2 O 3 36084-12A (500°C) Target 58% CuO-9% Mn 2 O 3 -3% La 2 O 3 -30% Al 2 O 3 Catalyst composition:

[0253] 1) Weigh out 930g Cu(NO 3 ) 2 Solution (16.16% Cu, from factory),

[0254] 2) Weigh out 157g of manganese nitrate solution

[0255] 3) Weigh out 39g of lanthanum nitrate solution (22% La solution)

[0256] 4) Mix solutions 1 and 2 and dilute to 1.0 liter with DI water.

[0257] 5) Add 1.33 liters of water and set the mixing speed to 400 RPM.

[0258] 6) Weigh out 142g of V-250 UOP alumina powder and slowly add it to the feed. Keep stirring until the alumina powder is completely dispersed in the slurry.

[0259] 7) Weigh out 500 g of soda ash, dissolve in DI, and dilute to 1.33 L. Weigh the solution before and after precipitation to get the amount of soda ash consumed.

[0260] 8) Maintain the slurry pH = 7.0 by adjusting the rate of addition of alkaline solution (room temperature)

[0261] 9) The precipitation is completed by adding copper nitrate and alkaline solution simultaneously within one hour

[0262] 10) Measure slurry particle size during the entire precipitation process

[0263] 11) Filter the slurry and wash the filter cake

[0264] 12) Dry the washed filter cake to form a powder

[0265] 13) Calcinate the dried powder at 500°C for 2 hours Sample 36084-12A (500°C)

[0266] Example 15 - Target composition (750°C) 58% CuO-9% MnO-3% La 2 O 3 -30% Al 2 O 3 Chromium-free copper catalyst

[0267] The chromium-free copper catalyst composition (Cu-Mn-La-Al 2 O 3 , 750°C, target 58% CuO-9% Mn 2 O 3 -3% La 2 O 3 -30% Al 2 O 3 The obtained dry powder was calcined at 750°C for 2 hours. The catalyst composition had the following particle size distribution (micrometers): D 10 8.54μm, D 50 19.5 μm and D 90 35.1μm.

[0268] Further analysis of the CuO crystallite size of the catalysts prepared in various examples showed that the CuO crystallite size was about to about The results are summarized in Table 7. Using the dried powder from Example 6, the powder was calcined at different temperatures. X-ray diffraction (XRD) analysis showed that the crystalline phase changed with increasing temperature. The data showed that La was in the form of lanthanum carbonate at low temperatures, and it was converted to orthorhombic lanthanum copper oxide (LaCO) at 700°C. 2 CuO 4 ), and then partially converted into tetragonal copper lanthanum oxide (CuLaO) at 750 °C. 3 ), and finally, in addition to the phase at 750°C, cubic copper aluminum oxide (CuAl 2 O 4 )’s new phase.

[0269] The XRD pattern is shown in Figure 6 middle. Figure 6 is a graph showing XRD patterns of catalysts prepared using dried powder from Example 6 and Examples 7-1 to 7-4 prepared according to the embodiments herein and calcined at different temperatures. Analysis of CuO crystallite size shows that the CuO size increases with calcination temperature, from becomes The results are summarized in Table 7. Figure 7 The effect of calcination temperature on the CuO crystallite size is also shown.

[0270] Table 7 - Analysis of CuO crystallite size changes with calcination temperature

[0271]

[0272] Example 16 - Catalyst Performance Evaluation

[0273] Testing Procedure : The catalytic activity and selectivity of the catalyst compositions prepared in the above examples according to the embodiments herein were evaluated by slurry phase hydrogenolysis of methyl esters to fatty alcohols. Catalyst performance evaluations were conducted for both methyl ester hydrogenolysis and wax ester hydrogenolysis in a one liter autoclave.

[0274] Procedure for Hydrogenolysis Testing of Methyl Esters (Including Reuse Testing)

[0275] Catalyst performance testing in a system equipped with baffles and Disperimax TM For each experiment, 396 g of fatty acid methyl ester (approximately 75 wt % C 12 / 25% C 14 -C 18) and a catalyst powder having a concentration of 0.8 wt%. 2 Pressure purge 2-3 times to remove air, then heat at 250 psig H 2 After 2-3 pressure purges, stir at 2000 RPM and 150 psig H 2 The autoclave was heated to 280°C. Once the temperature stabilized at 280°C, stirring was stopped and H 2 The pressure was increased to 2500 psig. Agitation was then resumed at 2000 RPM; this was designated as time 0. Approximately 5-10 cc product samples were collected once an hour for a total of 5 hours.

[0276] To evaluate catalyst deactivation, the experiment can be repeated multiple times using the same catalyst. In this case, after sampling is complete, the reactor is cooled and depressurized, and the entire liquid content of the autoclave is drained through a 1.2 μm sintered disk that allows the catalyst to remain in the reactor. Fresh feed is then added to the autoclave, and the experiment is repeated in its entirety.

[0277] Each sample was analyzed via gas chromatography, whereby fatty alcohols, wax esters and hydrocarbon byproducts were quantified. The gas chromatograph used for analysis was an Agilent 7890 equipped with a flame ionization detector (FID) and a Quadrex capillary column, 75 μm x 320 μm x 0.25 μm. The column flow rate was kept constant at 4.7 cc / min at a split ratio of 100:1. After sample injection (1 μl), the oven was heated from 100°C to 200°C at 5°C / min and maintained at 200°C for 55 min.

[0278] Procedure for Hydrogenolysis of Wax Esters

[0279] Reaction conditions: pressure: 4350psi; temperature: 300℃; stirring: 1500rpm; feed: C 16 -C 18 Fatty acids (27% C 16 Acid, 72% C 18 Acid); Feed: 454g C 12 -C 14 Fatty alcohols; 6-hour run (55 g fatty acid injected every hour for hour 0, hour 1, hour 2, hour 3)

[0280] program:

[0281] 1. Load the catalyst (0.75 wt% catalyst loading) by opening the top screw of the reactor top cover. Load 454 g of C 12 -C 14Fatty alcohol.

[0282] 2. Use N 2 The autoclave system was purged several times to remove air and then purged several times with hydrogen.

[0283] 3. Start stirring at 1500 rpm and start increasing the furnace temperature, and install the jacket on the autoclave. The typical heating rate is 3°C / min.

[0284] 4. When the temperature reaches 300°C, begin pressurizing the autoclave to 4350 psi with hydrogen. Inject 55 g of C 16 -C 18 This will start time "0". At hour 1, a 5 ml liquid sample is collected through a port with a glass frit at the tip inside the autoclave. An additional 55 g C 16 -C 18 Fatty acids. At the 2nd and 3rd hour, this sampling and fatty acid injection will continue. After 3HOS, the experiment will continue to 6 hours without further injection of fatty acids. The by-products of each sample (6 samples in total) will be analyzed in GC.

[0285] 5. Calculate the SAP value of each sample by wet titration. Calculate the conversion of fatty acids based on the % SAP value reduction.

[0286] 6. Conversion rate, % = (SAP value in the obtained feed mixture - SAP value in the product) * 100 / SAP value in the obtained feed mixture

[0287] CuCr reference catalyst and CuMnAl according to the examples herein 2 O 3 and CuLaAl 2 O 3 Catalyst composition in multiple cycles Comparison of catalyst performance in the ring test

[0288] Comparison with CuCr Reference Catalyst (Example 1)

[0289] Fatty alcohol yield curve ( Figure 8 ) shows that when using the Cu-Al of the present invention prepared by the deposition-precipitation method using V-250 UOP alumina in Example 1 according to the embodiments herein, 2 O 3 The catalyst composition of the present invention has a lower alcohol yield than the CuCr reference catalyst within six (6) hours of reaction time. This is promoted by using Mn, La and other metals or metal oxides to promote the Cu-Al 2 O 3 Catalyst development.

[0290] Example 2 Mn-catalyzed CuMn-Al 2 O 3 Comparison of V250 and CuCr Reference Catalyst (Example 1)

[0291] In the case of adding Mn to Cu-Al using the precipitation-deposition method 2 O 3 In the case of Example 2, the catalyst has significantly better alcohol yield than not only the catalyst of Example 1, but also the CuCr reference catalyst ( Fig. 9 ).

[0292] Example 3 and Example 4 Comparison of Reference Catalysts

[0293] The Mn-promoted Cu / alumina catalysts from Examples 3 and 4 (calcined at different temperatures) were tested against Reference Example 1 (CuCr). Both catalysts outperformed the commercially available CuCr reference catalyst ( Fig.10 ).

[0294] Example 5, Example 6 and Example 8La 2 O 3 Catalytically promoted Cu-Al 2 O 3 Performance of catalysts compared to CuCr reference

[0295] At three different La loadings, all catalysts from Examples 5, 6, and 8 had better alcohol yields than the CuCr reference catalyst over the entire reaction time ( Fig.11 ). These results demonstrate that the catalysts according to the embodiments described herein can outperform the commercial CuCr reference catalyst. These examples show that La is a promoter for Cu / alumina catalysts.

[0296] Example 7 Comparison with CuCr Reference

[0297] Two new Cr-free candidate catalysts, Example 7Cu / La / Al 2 O 3 , which are similar to Example 6, but calcined at a higher temperature of 750°C, their performance is comparable to the reference CuCr catalyst after a reaction time of 3 hours. Fatty alcohol yield curve ( Fig.12 ) show that the catalyst composition from Example 7 provides higher alcohol yields than the CuCr reference catalyst when equilibrium is approached at a reaction time of about 5 hours.

[0298] Example 17 - Catalyst Stability Testing by Multi-Cycle Performance Testing

[0299] The catalyst stability as measured by the multi-cycle performance test is evaluated. In order to simulate the life or service life of the catalyst according to the embodiments of this article, the multi-cycle performance test provides useful results. Under standard laboratory test conditions, two samples (Example 6 and Example 3) and the reference catalyst (Example 1) are tested for repeated use. The only difference is that after each activity test, the catalyst is kept in the reactor to be further tested with fresh feed.

[0300] The results are shown in Fig.13 and Fig.14 middle. Fig.13 is a graph showing multi-cycle performance testing of catalyst compositions according to examples herein. Fig.14 is a graph showing multi-cycle performance testing of catalyst compositions according to examples herein.

[0301] As described above, the catalyst compositions according to the embodiments herein have higher activity than the CuCr catalyst currently used in commercial processes. In the slurry phase process for fatty alcohol production, the residence time of the catalyst in the system is much longer than the conventional reaction time of 5 hours. CuCr Reference Example 1, Example 6 (CuLa-Al 2 O 3 ) and Example 3 (CuMn-Al 2 O 3 The fatty alcohol yields of the repeated use test of Figure 15A-15E The test conditions are the same as the standard conditions.

[0302] Fig.15A is a graph showing a comparison between a commercial catalyst and the catalyst compositions of Examples 3 and 6 for the first cycle (fresh) of a multi-cycle performance test. Fig. 15B is a graph showing a comparison between the commercial catalyst and the catalyst compositions of Examples 3 and 6 for the second cycle (first reuse) of the multi-cycle performance test. Fig. 15C is a graph showing a comparison of fatty alcohol yields between commercial catalysts and the catalyst compositions of Examples 3 and 6 for the third cycle (second reuse) of the multi-cycle performance test. Fig.15D is a graph showing a comparison of fatty alcohol yields between commercial catalysts and the catalyst compositions of Examples 3 and 6 for the fourth cycle (third reuse) of a multi-cycle performance test. Fig.15E is a graph showing a comparison of fatty alcohol yields between commercial catalysts and the catalyst compositions of Examples 3 and 6 for the fifth cycle (fourth reuse) of the multi-cycle performance test. Fig.16 is a graph showing a comparison between a commercial catalyst and the catalyst composition of Example 6 for each cycle of repeated use in the hydrogenolysis of methyl esters to form fatty alcohols.

[0303] like Figure 15A-15E As shown, each catalyst loses some activity after each use (test). This can be most easily seen by comparing the fatty alcohol yields at constant time, which decrease for all three catalysts when the samples are reused multiple times. If the reaction is allowed to proceed for a long enough time, an equilibrium fatty alcohol yield can be achieved during each cycle, but for multiple cycles, a constant time of five (5) hours is used instead. Without being bound by any particular theory, it is believed that the loss of activity from cycle to cycle can be attributed to poisoning caused by catalyst Cu crystallite size growth and feed impurities.

[0304] Compared with the CuCr reference catalyst (Example 1), both Example 6 and Example 3 have better fatty alcohol yields as fresh catalysts. Further reuse tests show that Example 6 (CuLa-Al 2 O 3 ) catalyst had the same or better activity than the CuCr reference catalyst (Example 1) until 2 reuses and then began to show lower fatty alcohol yields due to deactivation. Example 3 (CuMn-Al 2 O 3 ) sample deactivated more rapidly than the CuCr reference catalyst (Example 1) immediately after reuse, which was most clearly seen in the first reuse test results, and continued to function at a lower activity in all subsequent tests.

[0305] Further analysis of the product distribution of the CuCr reference catalyst (Example 1) and Example 6 samples showed that the lower fatty alcohol yield was due to the formation of a higher concentration of fat-fatty esters. This suggests that fat-fatty esters are intermediates in the hydrogenolysis of methyl esters. It may be formed by transesterification of methyl esters with the produced fatty alcohols. A catalyst with good activity can minimize the formation of this intermediate and promote complete hydrogenolysis.

[0306] Example 18 - Comparison of wax ester hydrogenolysis performance

[0307] Using the procedure described below for catalyst performance comparison, the liquid product during the reaction was collected for SAP (saponification) value analysis. The SAP value is the hydrolysis of the ester with KOH (or NaOH) to form the potassium or sodium salt of the alcohol and the corresponding acid. The higher the SAP value, the higher the ester content. In this case, the higher the SAP value, the lower the conversion of the ester, and therefore the lower the catalyst activity.

[0308] The wax ester hydrogenolysis performance of the catalysts according to the examples herein was compared with a commercially available CuCr catalyst. In these tests, the hydrogenolysis product was withdrawn every hour for analysis and then fresh fatty acid was injected as feed for the first four hours.

[0309] After the fourth injection, as the reaction time continued, the residual wax esters decreased, and due to the approach to equilibrium, the ester conversion rate decreased. The catalyst according to the embodiments of this article (e.g., Example 6, calcined at 500°C) began to have a higher wax ester conversion rate than the CuCr reference catalyst at the second hour of the test. The total wax ester conversion rate after 6 hours is summarized in Table 8. Under the same test conditions, the catalyst composition according to the embodiments of this article has a higher wax ester conversion rate than the commercial CuCr reference catalyst, 76.63% vs. 72.95%. In general, the catalyst of the present invention has significantly higher activity and alcohol yield.

[0310] Table 8 - Comparison of the activity of the catalysts of the invention with commercial CuCr reference

[0311] catalyst Total conversion rate, % CuCr Reference (Example 1) 72.95 Example 6 76.63

[0312] Example 19 - Separation and Filtration Properties

[0313] Catalyst Filtration Properties: Used catalyst separation experiments (both centrifugation and filtration) were conducted to compare the filterability of the catalysts. 2 O 3 -Al 2 O 3 The catalyst has considerable separation properties.

[0314] Procedure for centrifugation: It is a qualitative assessment of sedimentation and separation by centrifugation at 11,000 rpm for 5 minutes, taking pictures for visual comparison. First, the spent catalyst slurry (0.8 wt% catalyst loading) containing liquid product and unreacted fatty acid methyl esters was centrifuged for 5 minutes. Then, the top 35 mL of liquid was collected and photos were taken to see if there were any particles floating. The separation efficiency was qualitatively measured based on the color of the collected liquid and the fine particles floating therein. The centrifugation test showed that both the catalyst of the present invention and CuCr had clear liquid products.

[0315] Procedure for filtration: Draw 12 ml of used catalyst slurry (mixed thoroughly) into a syringe. Insert a syringe filter (0.45 μm) at the tip of the syringe. Press the syringe to allow filtrate to flow out of the syringe filter while starting a timer. If no filtrate comes out under maximum hand pressure, replace the filter and stop the timer. When 12 mL of slurry has been filtered out, stop the timer. This test qualitatively estimates the ease of filtration (number of filters required and time required to make the same amount of filtrate) using a 0.45 μm filter.

[0316] Another measure of the success of the new catalyst is the separation / filtration of the catalyst solid-liquid products after the reaction. Two tests were performed for comparison. The liquid products were collected by (a) centrifugation and (b) syringe filtration. Example 6 was compared with the CuCr reference catalyst (Example 1). All liquid products collected by centrifuge or syringe filter were clear, which is a good indication of catalyst particle integrity and chemical stability after the reaction (these results are only from fresh tests).

[0317] In order to give Example 6, the CuMn-Al catalyst was deposited 2 O 3 The coprecipitated catalyst CuMn-Al with CuCr reference catalyst (Example 1) and reference example 3 2 O 3 For quantitative comparison of the filterability of the catalysts, one method is to quantify the time and number of syringe filters used to collect the same amount of liquid product (12 ml). Example 6 catalyst (73-2) has a filtration time comparable to CuCr (about 40 seconds), CuCr reference catalyst (Example 1), and both catalysts require one syringe filter to collect 12 ml of liquid product. Under the same filtration test conditions, Example 3 requires 2 syringe filters to collect the same amount of liquid product, and requires about twice as long (80 seconds) to collect 12 ml of liquid product.

[0318] Example 20 - Particle size analysis of spent catalyst after repeated use testing

[0319] Used Reference Example 3CuMn-Al 2 O 3 and Example 6CuLa-Al 2 O 3 The particle size distribution (PSD) of the catalyst was similar to that of the fresh catalyst. The catalyst particle size was not broken into smaller sizes less than 0.1 μm. These results further confirm the stability of the catalyst composition according to the examples herein.

[0320] Example 21 - Catalyst particle size stability test

[0321] The used Example 7 gave an acceptable particle size distribution with no fines < 0.5 μm. Example 7 had good performance and a stable PSD. This is superior to conventional coprecipitated CuMn-Al 2 O 3 The catalyst has the advantages of, and more importantly, has better catalytic performance than the CuCr reference catalyst (Example 1).

[0322] Example 22 - Tablet Preparation, Properties and Catalytic Performance

[0323] The powder from Example 6 was formed into tablets by compaction. The tablets had the following properties: Packed bulk density: 1.43 g / ml; Crush strength: 30.0 lbs; BET surface area: 95.8 m 2 / g.

[0324] This sample was tested in fixed bed liquid phase butyraldehyde to butanol under the following test conditions:

[0325] Reaction conditions

[0326] Pressure: 700psi;

[0327] Temperature: 150℃-180℃;

[0328] Feed: C 4 aldehyde

[0329] LHSV: 0.75-1.5h -1

[0330] Run time: 150 hours

[0331] Catalyst: 30cc

[0332] H 2 / Feed (mole): 5-7

[0333] This sample was tested in fixed bed liquid phase butyraldehyde to butanol under the following test conditions:

[0334] The catalyst (30 cc) was loaded in the reactor along with an equal volume of inert materials.

[0335] The catalyst was activated with 3% hydrogen in nitrogen at 190 °C overnight with a total gas flow rate of 1000-1500 h -1 GHSV, then slowly increase the hydrogen concentration (25%, 50%, 75% and 100%) every 2-3 hours, and keep it at 100% hydrogen concentration at 190°C for 1 hour. The temperature was raised to 210°C and 100% hydrogen was passed at this temperature for another hour to complete the activation of the catalyst.

[0336] The reactor was cooled to its reaction temperature. The reaction system was pressurized to 700 psi. Liquid flow was started and hydrogen was adjusted to its required flow rate.

[0337] Liquid samples were collected every 24 hours and analyzed off-line in a GC.

[0338] nC 4 Aldehyde conversion rate (%) = (input nC 4 Aldehyde-leaving nC 4 Aldehyde) / entry nC 4 Aldehyde*100

[0339] n-Butanol selectivity (%) = (n-butanol leaving – n-butanol entering) / (nC entering 4 Aldehyde – leaving nC 4 Aldehyde)*100.

[0340] At reaction temperature: 150°C, LHSV: 1hr -1 and running time: 122 hours, butyraldehyde conversion was 99.06%, and butanol selectivity was 93.34%.

[0341] References throughout this specification to, for example, "one embodiment," "certain embodiments," "one or more embodiments," or "an embodiment" mean that a particular feature, structure, material, or characteristic described in conjunction with that embodiment is included in at least one embodiment of the present invention. Thus, phrases such as "in one or more embodiments," "certain embodiments," "in one embodiment," or "in an embodiment" appearing in different places throughout this specification do not necessarily refer to the same embodiment of the present invention. Furthermore, these particular features, structures, materials, or characteristics may be combined in any suitable manner in one or more embodiments.

[0342] As used herein, the singular forms "a," "an," and "the" include plural referents unless the context clearly dictates otherwise. Thus, for example, reference to "a robotic arm" includes a single robotic arm as well as more than one robotic arm.

[0343] As used herein, the term "about" in conjunction with a measured amount refers to the standard variation of the measured amount as would be expected by one of ordinary skill in the art in making the measurements and exercising a level of care commensurate with the objective of the measurement and the precision of the measuring equipment. In certain embodiments, the term "about" includes ±10% of the listed number, such that "about 10" would include from 9 to 11.

[0344] The term "at least about" in conjunction with the measured amount refers to the standard variation of the measured amount, as expected by a person of ordinary skill in the art when making the measurement and implementing a level of caution commensurate with the measurement target and the precision of the measuring equipment and any amount above the measured amount. In certain embodiments, the term "at least about" includes the listed number minus 10% and any higher amount, so that "at least about 10" will include 9 and any number greater than 9. This term can also be expressed as "about 10 or greater". Similarly, the term "less than about" typically includes the listed number plus 10% and any smaller amount, so that "less than about 10" will include 11 and any number less than 11. This term can also be expressed as "about 10 or less".

[0345] Unless otherwise indicated, all parts and percentages are by weight. If not otherwise indicated, weight percentages (wt. %) are based on the overall composition without any volatiles, ie, on a dry solids basis.

[0346] The foregoing description discloses example embodiments of the present disclosure. Modifications to the above disclosed components, devices, and methods that fall within the scope of the present disclosure will be apparent to those of ordinary skill in the art. Therefore, although the present disclosure has been disclosed in conjunction with example embodiments, it should be understood that other embodiments may fall within the scope of the present disclosure as defined by the following claims.

Claims

1. A catalyst composition comprising: a support comprising alumina; a copper compound on the support; and Co-catalyst, The catalyst composition contains no chromium.

2. The catalyst composition according to claim 1, wherein The carrier includes powders, granules, extrudates, spheres, solids, tablets, caplets, nuggets, or combinations thereof.

3. The catalyst composition according to claim 1 or 2, wherein The alumina includes pseudo-boehmite alumina, bayerite alumina or gamma alumina.

4. A catalyst composition as claimed in any preceding claim, wherein The catalyst composition does not contain aluminum nitrate, acetate, chloride or sodium aluminate.

5. A catalyst composition as claimed in any preceding claim, wherein The carrier includes approximately 1 lbs / ft 3 About 60lbs / ft 3 , about 5lbs / ft 3 About 50lbs / ft 3 , or about 10lbs / ft 3 About 40lbs / ft 3 The bulk density.

6. A catalyst composition as claimed in any preceding claim, wherein The catalyst is in powder form and comprises a loose bulk density of about 0.25 g / ml to about 0.6 g / m, or wherein the catalyst is in tablet form and comprises a bulk density greater than about 1.0 g / ml.

7. A catalyst composition as claimed in any preceding claim, wherein The carrier includes about 250m 2 / g to about 400m 2 / g, about 275m 2 / g to about 375m 2 / g, or about 300m 2 / g to about 350m 2 / g of surface area.

8. A catalyst composition as claimed in any preceding claim, wherein The catalyst composition comprises D 10 , D from about 10 μm to about 20 μm 50 and D from about 30 μm to about 60 μm 90 The average particle size of the powder.

9. The catalyst composition of any preceding claim having a stability against impurity poisoning of from about 0.1% to about 0.5% organic acid or up to about 0.5% organic acid.

10. The catalyst composition of any preceding claim having a stability of from about 1 reuse to about 10 reuses, from about 1 reuse to about 5 reuses, from about 1 reuse to about 4 reuses, from about 2 reuses to about 5 reuses when in a slurry phase when measured using a Multi-Cycle Performance Test for Fatty Alcohol Production.

11. The catalyst composition of any preceding claim having a fatty acid conversion based on a reduction in % saponification (SAP) value of from about 73% to about 99%, or at least about 73%.

12. A catalyst composition as claimed in any preceding claim, wherein The catalyst composition is in the form of one or more of a powder, a granule, an extrudate, a sphere, a solid, a tablet, a caplet, a nugget, or a combination thereof, or Wherein, the catalyst composition comprises D of about 1 μm to about 10 μm 10 , D from about 10 μm to about 20 μm 50 and D from about 30 μm to about 60 μm 90 The average particle size of the powder.

13. A catalyst composition as claimed in any preceding claim, wherein The catalyst composition is calcined.

14. A catalyst composition as claimed in any preceding claim, wherein The size of the catalyst composition before calcination is the same or approximately the same as the size of the catalyst composition after calcination.

15. A catalyst composition as claimed in any preceding claim, wherein The copper compound includes one or more of copper (I) oxide (cuprous oxide) or copper (II) oxide (cupric oxide).

16. A catalyst composition as claimed in any preceding claim, wherein The copper compound is comprised of about to about The crystallite size of copper(II) oxide.

17. A catalyst composition as claimed in any preceding claim, wherein The promoter includes one or more oxides of lanthanum, manganese, barium, zirconium, calcium, magnesium, zinc, yttrium, erbium, cerium, rare earth metals, strontium, boron, nickel, platinum, silver, gold, palladium, ruthenium or a combination thereof.

18. A catalyst composition as claimed in any preceding claim, wherein The copper compound is copper (II) oxide (CuO) in an amount of about 25 wt % to about 80 wt %, or about 35 wt % to about 70 wt %, based on the total weight of the catalyst composition.

19. A catalyst composition as claimed in any preceding claim, wherein The co-catalyst includes barium oxide in an amount of about 0 wt % to about 20 wt %, or about 1 wt % to about 15 wt %, or about 5 wt % to about 12 wt %, based on the total weight of the catalyst composition.

20. A catalyst composition as claimed in any preceding claim, wherein The co-catalyst includes lanthanum oxide (La2O3) in an amount of about 0 wt% to about 20 wt%, or about 1 wt% to about 17 wt%, or about 5 wt% to about 15 wt%, based on the total weight of the catalyst composition.

21. A catalyst composition as claimed in any preceding claim, wherein The co-catalyst includes manganese oxide (Mn2O3) in an amount of about 0 wt% to about 20 wt%, or about 1 wt% to about 17 wt%, or about 5 wt% to about 15 wt%, based on the total weight of the catalyst composition.

22. The catalyst composition of any preceding claim, comprising alumina in an amount from about 10 wt% to about 50 wt%, from about 15 wt% to about 45 wt%, or from about 20 wt% to about 40 wt%, based on the total weight of the catalyst composition.

23. A catalyst composition as claimed in any preceding claim, wherein The copper compound includes monoclinic copper (II) oxide (CuO), and further includes one or more of the following crystalline phases: Monoclinic lanthanum oxide carbonate (LaCO3); Orthorhombic lanthanum copper oxide (La2CuO4); Tetragonal copper lanthanum oxide (CuLaO3); Copper aluminum oxide (CuAl4O7); Cubic copper aluminum oxide (CuAl2O4); Monoclinic lanthanum manganese oxide (LaMnO 3.13 ); Cubic copper manganese oxide (Cu 1.5 Mn 1.5 O4); Orthorhombic lanthanum copper oxide (La2CuO4); or Cubic Alumina (Al2O3).

24. A catalyst composition as claimed in any preceding claim comprising about 60 m 2 / g to about 200m 2 / g, about 70m 2 / g to about 180m 2 / g, or about 80m 2 / g to about 160m 2 / g of BET surface area.

25. A catalyst composition as claimed in any preceding claim, wherein The catalyst composition is in the form of at least one of a sphere, a solid, a tablet, a caplet, or a pellet having a thickness of about 1 / 4 inch to about 1 / 16 inch, or about 1 / 8 inch.

26. The catalyst composition of claim 25, comprising a crush strength of about 5 lbs to about 40 lbs.

27. The catalyst composition of claim 25 or 26, comprising a bulk density of about 1.0 g / ml to about 1.7 g / ml.

28. The catalyst composition of any one of claims 25 to 27, comprising 20 m 2 / g to about 100m 2 / g of BETSA.

29. The catalyst composition of any one of claims 25 to 28, comprising a pore volume of about 0.25 ml / g to about 0.4 ml / g.

30. The catalyst composition of any one of claims 25 to 29, comprising about to about The average pore size.

31. A method for preparing a catalyst composition, the method comprising: combining the copper-containing solution with alumina to form a combination; precipitating the combination with an alkaline solution to form a precipitate solution; filtering the precipitate solution to obtain a precipitate; The precipitate is calcined to form the catalyst composition.

32. The method of claim 31, wherein: The copper-containing solution comprises at least one of copper (II) nitrate (Cu(NO3)2), copper (I) chloride or copper (II) acetate.

33. The method of claim 31 or 32, wherein: The catalyst composition contains no chromium.

34. The method of any one of claims 31 to 33, wherein: The alumina is in the form of powder, granules, extrudates, spheres, solids, tablets, caplets, chunks, or combinations thereof.

35. The method of any one of claims 31 to 34, wherein: The alumina includes pseudo-boehmite alumina, bayerite alumina or gamma alumina.

36. The method of any one of claims 31 to 35, wherein: The catalyst composition does not contain aluminum nitrate, acetate, chloride or sodium aluminate.

37. The method of any one of claims 31 to 36, wherein: The combination is a slurry.

38. The method of claim 37, wherein: The alumina is a powder dispersed in the slurry.

39. The method of any one of claims 31 to 38, wherein: Precipitating the combination includes combining the combination with a base.

40. The method of claim 39, comprising maintaining the combination at a pH of about 6.5 to about 7.8 while precipitating the combination.

41. The method of claim 39, wherein: The base includes sodium hydroxide (NaOH), soda ash, or a combination thereof.

42. The method of any one of claims 31 to 41, further comprising washing the precipitate.

43. The method of claim 42, further comprising drying the washed precipitate.

44. The method of any one of claims 31 to 43, wherein: The precipitate is calcined at a temperature of about 200°C to about 800°C, 300°C to about 700°C, about 400°C to about 600°C, or about 450°C to about 500°C for about 30 minutes to about 4 hours, about 1 hour to about 3 hours, about 1.5 hours to about 2.0 hours.

45. The method of any one of claims 31 to 44, wherein: The catalyst composition comprises about 40 wt % to about 70 wt %, or about 55 wt % to about 65 wt % copper (II) oxide (CuO) and about 30 wt % to about 60 wt %, or about 40 wt % to about 50 wt % alumina.

46. ​​The method of any one of claims 31 to 45, wherein: The catalyst composition includes about 0.1 g / cc to about 0.5 g / cc, or about 0.2 g / cc to about 0.3 g / cc of bulk ABD.

47. The method of any one of claims 31 to 46, wherein: The catalyst composition includes about 0.2 g / cc to about 0.6 g / cc, or about 0.3 g / cc to about 0.4 g / cc of packed ABD.

48. The method of any one of claims 31 to 47, wherein: The catalyst composition comprises D 10 , D from about 10 μm to about 20 μm 50 and D from about 30 μm to about 60 μm 90 The average particle size of the powder.

49. A process for hydrogenating or hydrogenolyzing an organic compound containing a carbonyl group, the process comprising: bringing these organic compounds into contact with a catalyst composition according to any one of claims 1 to 30, The catalyst composition contains no chromium.

50. The method of claim 50, wherein: These organic compounds include one or more of aldehydes, esters, ketones or carboxylic acids.

51. The method of claim 50, wherein: These organic compounds include one or more of aliphatic esters or methyl esters.

52. The method of claim 50, wherein: These organic compounds include methyl esters which undergo hydrogenolysis to form one or more fatty alcohols.

53. The method of claim 50, wherein: These organic compounds include wax esters which undergo hydrogenolysis to form one or more fatty alcohols.