Method for manufacturing exhaust gas purification catalyst device

By simultaneously performing the suction and blowing process in the coating liquid storage unit and the unit flow path, the coating liquid adhesion problem is solved, and high-quality catalyst coating coating and cost reduction are achieved.

CN119072356APending Publication Date: 2024-12-03CATALER CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202380034396.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-26
Filing Date
2023-04-10
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

When applying a high viscosity coating liquid to a honeycomb substrate using the attraction method, the coating liquid is prone to adhere to the inner wall of the storage tool, resulting in uneven coating and waste, increasing the manufacturing cost and quality problems of the exhaust purification catalyst device.

Method used

By simultaneously performing the suction and blowing process in the coating liquid storage unit and unit flow path, the introduction and adhesion of the coating liquid is controlled, ensuring that the coating liquid is applied to the substrate at a predetermined length, and the coating liquid is suppressed from being stored and treated. With the attachment of the inner wall.

Benefits of technology

High-quality catalyst coating coating is achieved, reducing the waste of coating liquid, reducing manufacturing costs, and ensuring the predetermined length and uniformity of the catalyst coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119072356A_ABST
    Figure CN119072356A_ABST
Patent Text Reader

Abstract

A method for manufacturing an exhaust gas purification catalyst device includes: (A) arranging a base material such that one open end of a plurality of unit flow paths faces upward and the other open end faces downward, and mounting a coating liquid storage jig having a storage wall on the upper end portion of the base material to form a coating liquid storage portion; (B) supplying a coating liquid for forming a catalyst coating layer to a coating liquid storage unit; (C) applying the coating liquid for forming the catalyst coating layer in the coating liquid storage part to the partition wall of the base material by making the pressure in the unit flow path lower than the pressure in the coating liquid storage part; (D) blowing compressed air from above to the inner side of the storage wall of the coating liquid storage jig; and (E) firing the base material coated with the coating liquid for forming the catalyst coating layer, and performing the step (C) and the step (D) at the same time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for manufacturing an exhaust gas purification catalyst device. Background Art

[0002] Exhaust gas discharged from an internal combustion engine such as an automobile engine is discharged into the atmosphere after being purified by an exhaust gas purification catalyst device provided in an exhaust system. The exhaust gas purification catalyst device has, for example, a structure including: a honeycomb substrate having a plurality of unit flow paths divided by partition walls, and a catalyst coating formed on at least one of the partition walls of the honeycomb substrate and the partition walls.

[0003] Such an exhaust gas purification catalyst device is produced, for example, by applying a coating liquid containing a raw material component of a catalyst coating layer onto the partition walls of a honeycomb substrate and then firing the coating liquid.

[0004] Here, it is known that a coating liquid is applied to the partition wall of the honeycomb substrate by placing the coating liquid on one end face of the honeycomb substrate and sucking it from the opposite end face (suction method). For example, Patent Document 1 describes that a frame-shaped storage fixture capable of storing the coating liquid is installed on the first end face of the honeycomb substrate, the coating liquid is stored on the first end face, and on this basis, the pressure on the second end face side opposite to the first end face is relatively lowered than the pressure on the first end face side, thereby generating a coating liquid flow from the first end face to the second end face, thereby applying the coating liquid to the partition wall of the honeycomb substrate.

[0005] However, in an exhaust gas purification catalyst device, sometimes catalyst coatings of different compositions are arranged on the upstream and downstream sides of a honeycomb substrate, respectively, to form a structure called "regional coating" to improve the exhaust gas purification capability. The catalyst coating of such a region coating structure can be manufactured, for example, by forming a first catalyst coating of a predetermined length from one end face of the substrate by an attraction method, and then forming a first catalyst coating of a predetermined length from the other end face of the substrate.

[0006] Prior art literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2018-015704 Summary of the invention

[0008] In the case where the coating liquid is applied to the honeycomb substrate by the suction method, if the coating liquid leaks out of the honeycomb substrate from the end of the suction side, part of the coating liquid will be wasted, and the manufacturing cost of the exhaust gas purification catalyst device will increase. In particular, when the catalyst coating layer contains a catalyst precious metal, since the price of the coating liquid is high, the increase in the manufacturing cost of the exhaust gas purification catalyst device caused by the waste of the coating liquid is large.

[0009] Therefore, in order to avoid such waste, the coating liquid used in the suction method is often adjusted to a relatively high viscosity.

[0010] Furthermore, when forming a catalyst coating layer having an area coating structure by a suction method, the coating liquid is adjusted to have a high viscosity in order to control the catalyst coating layer to a predetermined length.

[0011] When applying a high-viscosity coating liquid by suction, the coating liquid may sometimes adhere to the inner wall of a storage jig mounted on the end face of the honeycomb substrate. If the coating liquid adheres to the inner wall of the storage jig, the coating amount on the partition wall of the honeycomb substrate is insufficient, or the coating cannot be applied to a predetermined length, which may result in poor quality of the exhaust gas purification catalyst device.

[0012] Furthermore, if the coating liquid attached to the inner wall of the storage jig falls onto the honeycomb substrate, a portion of the unit flow path is blocked, or the coating liquid adheres to the outer surface of the honeycomb substrate, which may still result in poor quality of the exhaust gas purification catalyst device.

[0013] The present invention has been made in view of the above circumstances. Therefore, an object of the present invention is to provide a method for stably manufacturing a high-quality exhaust gas purification catalyst device, which can suppress the adhesion of the coating liquid to the inner wall of a storage jig even when a high-viscosity coating liquid is applied to a substrate by a suction method.

[0014] The present invention is as follows.

[0015] [Scheme 1] A method for manufacturing an exhaust gas purification catalyst device, the exhaust gas purification catalyst device comprising:

[0016] a substrate having a plurality of unit flow paths partitioned by partition walls; and

[0017] a catalyst coating applied in or on the partition walls of the substrate, or both,

[0018] The manufacturing method comprises the following steps:

[0019] Step (A): arranging the substrate so that one opening end of the plurality of unit flow paths faces upward and the other opening ends face downward, and attaching a coating liquid storage jig having a storage wall extending upward from the outer periphery of the upper end of the substrate to the upper end portion of the substrate, thereby forming a coating liquid storage portion defined by the upper end surface of the substrate and the inner side of the storage wall of the coating liquid storage jig;

[0020] Step (B): supplying a coating liquid for forming a catalyst coating layer to the coating liquid storage portion;

[0021] Step (C): introducing the catalyst coating layer forming coating liquid of the coating liquid storage section into the unit flow path by making the pressure in the unit flow path lower than the pressure in the coating liquid storage section, and coating the catalyst coating layer forming coating liquid on the partition wall;

[0022] Step (D): blowing compressed air from above toward the inner side of the storage wall of the coating liquid storage jig; and

[0023] Step (E): calcining the substrate coated with the catalyst coating layer-forming coating liquid, and

[0024] At least a part of the step (C) and at least a part of the step (D) are performed simultaneously.

[0025] [Scheme 2] The method according to Scheme 1, after starting the step (C), starting the step (D).

[0026] <<Scheme 3>> The method according to Scheme 1 or 2, after completing step (D), completing step (C).

[0027] [Scheme 4] According to the method described in any one of Schemes 1 to 3, the storage wall of the coating liquid storage fixture has: a vertical portion extending upward approximately vertically from the outer periphery of the upper end portion of the substrate, and an inclined portion extending upward and outward from the upper end of the vertical portion.

[0028] [Scheme 5] According to the method described in Scheme 4, in the step (D), the compressed air is blown to the inner side of the vertical part of the storage wall.

[0029] [Scheme 6] According to the method described in Scheme 5, in the step (D), the angle between the blowing direction of the compressed air and the inner side surface of the vertical part of the storage wall is greater than 0.5° and less than 60°.

[0030] [Scheme 7] According to the method described in any one of schemes 1 to 6, in the step (D), the width of the blowing hole for blowing compressed air toward the inner side of the storage wall in a direction parallel to the radial direction of the substrate is greater than 0.05 mm and less than 1.00 mm.

[0031] [Scheme 8] According to the method described in any one of schemes 1 to 7, in the step (D), the pressure of the compressed air blown toward the inner side of the storage wall is greater than 0.05 MPa and less than 1.50 MPa at the compressed air outlet hole.

[0032] [Scheme 9] The method according to any one of schemes 1 to 8, wherein the catalyst coating layer-forming coating liquid is heated at 25° C. for 0.4 s.-1 The viscosity measured at a shear rate of 500 mPa·s or more and 10000 mPa·s or less.

[0033] [Scheme 10] According to the method according to any one of schemes 1 to 9, the coating liquid for forming a catalyst coating layer is applied to the partition wall in a predetermined range from the upper end of the substrate to the lower side.

[0034] <<Scheme 11>> The method according to any one of schemes 1 to 10, wherein at least after performing the steps (A) to (D), the substrate is turned upside down and the steps (A) to (E) are performed.

[0035] [Scheme 12] According to the method described in any one of Schemes 1 to 11, the substrate is a direct-flow type honeycomb substrate.

[0036] [Scheme 13] According to the method described in any one of Schemes 1 to 11, the substrate is a wall-flow honeycomb substrate.

[0037] According to the present invention, there is provided a method for stably manufacturing a high-quality exhaust gas purification catalyst device, which can suppress adhesion of a coating liquid to the inner wall of a storage jig even when a coating liquid with a high viscosity is applied. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 It is a schematic cross-sectional view for explaining the steps in the method for manufacturing the exhaust gas purification catalyst device of the present invention.

[0039] Figure 2 This is a cross-sectional photograph of the honeycomb substrate after coating. Figure 2 (a) relates to Example 1, Figure 2 (b) Concerning Comparative Example 1, Figure 2 (c) relates to Comparative Example 2.

[0040] Figure 3 This is a table showing the steps and coating results in Examples and Comparative Examples. DETAILED DESCRIPTION

[0041] 《Method for manufacturing exhaust gas purification catalyst device》

[0042] In the method for manufacturing an exhaust gas purification catalyst device of the present invention, the exhaust gas purification catalyst device comprises:

[0043] a substrate having a plurality of unit flow paths partitioned by partition walls; and

[0044] The catalyst coating layer is coated in or on the partition walls of the substrate or both, and the manufacturing method comprises the following steps:

[0045] Step (A): arranging the substrate so that one opening end of the plurality of unit flow paths faces upward and the other opening ends face downward, attaching a coating liquid storage jig having a storage wall extending upward from the outer periphery of the upper end of the substrate to the upper end portion of the substrate, and forming a coating liquid storage portion defined by the upper end surface of the substrate and the inner side of the storage wall of the coating liquid storage jig (coating liquid storage portion forming step);

[0046] Step (B): supplying a coating liquid for forming a catalyst coating layer to the coating liquid storage portion (coating liquid supplying step);

[0047] Step (C): introducing the catalyst coating layer forming coating liquid of the coating liquid storage section into the unit flow path by making the pressure in the unit flow path lower than the pressure in the coating liquid storage section, and applying the catalyst coating layer forming coating liquid on the partition wall (suction step);

[0048] Step (D): blowing compressed air from above toward the inner side of the storage wall of the coating liquid storage jig (blowing step); and

[0049] Step (E): calcining the substrate coated with the catalyst coating layer-forming coating liquid (calcining step), and

[0050] At least a part of the step (C) and at least a part of the step (D) are performed simultaneously.

[0051] The method for manufacturing an exhaust gas purification catalyst device of the present invention is characterized in that when applying a high-viscosity coating liquid on a substrate by suction, at least a part of the (C) suction step and the (D) blowing step are performed simultaneously.

[0052] According to this method of the present invention, it is possible to suppress adhesion of the coating liquid to the inner wall of the storage jig and to apply the coating liquid to the base material in a desired length.

[0053] If the suction step (C) is performed first and the blowing step (D) is performed after the suction step is completed, the coating liquid can be prevented from adhering to the inner wall of the storage jig, but there is a tendency that the coating length of the coating liquid becomes longer than a predetermined value on the outer peripheral side of the honeycomb substrate. On the other hand, if the blowing step (D) is performed first and the suction step (C) is performed after the suction step is completed, the coating liquid stored in the storage jig is scattered, and it is sometimes difficult to apply a predetermined amount of the coating liquid.

[0054] Therefore, in the present invention, by simultaneously performing at least a part of the (C) suction step and the (D) blowing step, it is possible to simultaneously suppress adhesion of the coating liquid to the inner wall of the storage jig and apply the coating liquid to a desired length on the substrate.

[0055] Hereinafter, a method for manufacturing an exhaust gas purification catalyst device according to the present invention will be described with reference to the drawings. Figure 1 A typical example of the method for manufacturing the exhaust gas purification catalyst device of the present invention is shown in the form of a schematic cross-sectional view.

[0056] In the manufacturing method of the exhaust purification catalyst device of the present invention, the substrate (10) is arranged in a manner that the opening end of one side of the plurality of unit flow paths faces upward and the opening end of the other side faces downward. Then, a coating liquid storage jig is installed on the upper end portion of the substrate (10). The coating liquid storage jig has a storage wall (20) extending upward from the outer periphery of the upper end of the substrate (10). The storage wall (20) may have a vertical portion (20a) extending upward approximately vertically from the outer periphery of the upper end portion of the substrate (10), and an inclined portion (20b) extending upward and outward from the upper end of the vertical portion (20a). If the coating liquid storage jig is installed on the substrate (10), a coating liquid storage portion (20a) defined by the upper end surface of the substrate (10) and the inner side of the storage wall (20) of the coating liquid storage jig is formed. Figure 1 (a), (A) coating liquid storage portion forming step).

[0057] Next, using an appropriate spray nozzle (30), the coating liquid (40) for forming a catalyst coating layer is supplied to the coating liquid storage portion formed in the coating liquid storage portion forming step (A) ( Figure 1 (b), (B) coating liquid supply step).

[0058] In addition, the following steps are performed simultaneously: Figure 1 (c), (C) suction process and (D) blowing process):

[0059] The catalyst coating layer forming coating liquid (40) supplied from the coating liquid storage section is introduced into the unit flow path by making the pressure in the unit flow path of the substrate (10) lower than the pressure in the coating liquid storage section, so as to apply the catalyst coating layer forming coating liquid (40) on the partition wall of the substrate (10); and

[0060] Using an appropriate compressed air supplier (50), compressed air (60) is blown from above toward the inner side of the storage wall (20) of the coating liquid storage jig.

[0061] Then, the substrate (10) coated with the coating liquid for forming a catalyst coating layer is fired (not shown, (E) firing step), thereby manufacturing an exhaust gas purification catalyst device.

[0062] Hereinafter, the substrate and the catalyst coating layer in the present invention will be described, and then each step of the method for manufacturing the exhaust gas purification catalyst device of the present invention will be described in sequence.

[0063] <Base Material>

[0064] The substrate applicable to the present invention is a substrate having a plurality of unit flow paths divided by partition walls, and may be a honeycomb substrate used in a conventional exhaust gas purification catalyst device. The partition walls of the substrate may have pores that connect adjacent exhaust flow paths in a fluid state.

[0065] The constituent material of the substrate may be, for example, a refractory inorganic oxide such as cordierite. The substrate may be a direct-flow type or a wall-flow type.

[0066] Typically, the substrate in the method for producing an exhaust gas purification catalyst device of the present invention may be, for example, a straight-flow type monolithic honeycomb substrate made of cordierite or a wall-flow type monolithic honeycomb substrate made of cordierite.

[0067] <Catalyst coating>

[0068] The catalyst coating layer formed by the method for producing an exhaust gas purification catalyst device of the present invention is formed on at least one of the partition walls of the substrate and the partition walls.

[0069] The catalyst coating layer contains at least inorganic oxide particles, and may further contain optional components such as catalyst noble metal particles and a binder.

[0070] The catalyst coating layer may be the same as the catalyst coating layer in the exhaust gas purification catalyst device of the prior art, or may be a new structure different therefrom.

[0071] According to the method of the present invention, it is easy to apply the coating liquid to the substrate in a desired length. Therefore, if the catalyst coating is a coating form called "area coating" extending from the open end of one side of the substrate to a predetermined length along the length direction of the substrate, the effect of the present invention can be advantageously manifested.

[0072] <(A) Coating Liquid Storage Section Forming Step>

[0073] In the coating liquid storage portion forming step, first, the substrate is arranged so that one opening end of the plurality of unit flow paths faces upward and the other opening end faces downward. The substrate may be arranged so that its longitudinal direction substantially coincides with the vertical direction.

[0074] Next, a coating liquid storage jig is attached to the upper end of the substrate to form a coating liquid storage portion.

[0075] The coating liquid storage jig may have a substantially cylindrical shape. At least one end of the tube may have a shape and size that surrounds the upper end of the substrate and prevents the coating liquid from leaking out of the gap between the outer end of the substrate and the inner side of the coating liquid storage jig.

[0076] When the coating liquid storage jig is mounted on the substrate, the upper portion of the tube (the portion other than the portion in contact with the upper end portion of the substrate) forms a storage wall extending upward from the outer circumference of the upper end of the substrate. Therefore, when the coating liquid storage jig is mounted on the substrate, a coating liquid storage portion defined by the upper end surface of the substrate and the inner side of the storage wall of the coating liquid storage jig is formed.

[0077] The storage wall of the coating liquid storage jig may include a vertical portion extending substantially vertically upward from the outer periphery of the upper end portion of the substrate, and an inclined portion extending outwardly and upwardly from the upper end of the vertical portion.

[0078] The lengths of the vertical portion and the inclined portion, and the total length of the storage wall can be appropriately set according to the amount of the coating liquid supplied to the coating liquid storage portion in the coating liquid supplying step (B).

[0079] As the constituent material of the coating liquid storage jig, a material that is easy to install and remove to the upper end of the substrate, has softness and flexibility to the extent that the substrate is not damaged during installation and removal, and to which the coating liquid is difficult to adhere can be used. As the constituent material of the coating liquid storage jig, for example, synthetic resins, particularly polyolefin resins, polyester resins, acrylic resins, polyurethane resins, ABS resins, polyimide resins, fluororesins, etc. can be cited.

[0080] <(B) Coating Liquid Supplying Step>

[0081] In the coating liquid supplying step (B), the coating liquid for forming a catalyst coating layer is supplied to the coating liquid storage portion.

[0082] The coating liquid for forming the catalyst coating layer is a liquid composition containing the constituent components of the catalyst coating layer or their precursors. The coating liquid for forming the catalyst coating layer can be, for example, a slurry containing inorganic oxide particles and water, and can also contain optional components such as a precursor of catalyst noble metal particles, a binder or its precursor, and a thickener.

[0083] The viscosity of the coating liquid for forming a catalyst coating layer may be relatively high. For example, the viscosity of the coating liquid for forming a catalyst coating layer may be relatively high. -1 and 400s -1 The viscosities measured at the shear rates can be shown as follows.

[0084] Shear speed 0.4s -1The viscosity at the time of the above-mentioned reaction is 500 mPa·s or more, 1,000 mPa·s or more, 1,500 mPa·s or more, 2,000 mPa·s or more, 2,500 mPa·s or more, 3,000 mPa·s or more, or 3,500 mPa·s or more, and 10,000 mPa·s or less, 8,000 mPa·s or less, 7,000 mPa·s or less, 6,000 mPa·s or less, or 5,000 mPa·s or less.

[0085] Shear speed 400s -1 The viscosity at the time is: 50 mPa·s or more, 60 mPa·s or more, 80 mPa·s or more, 100 mPa·s or more, 120 mPa·s or more, or 140 mPa·s or more, and 500 mPa·s or less, 400 mPa·s or less, 300 mPa·s or less, or 200 mPa·s or less.

[0086] The amount of the catalyst coating layer forming coating liquid supplied to the coating liquid storage portion can be appropriately set according to the expected coating length of the catalyst coating layer. The catalyst coating layer forming coating liquid is preferably supplied to the entire upper end surface of the substrate with a thickness as uniform as possible. Therefore, the catalyst coating layer forming coating liquid can be supplied to the coating liquid storage portion using, for example, an appropriate spray nozzle.

[0087] In addition, it is also a preferred embodiment of the present invention that after the coating liquid for forming a catalyst coating layer is supplied to the coating liquid storage portion, the subsequent (C) suction step is started after a predetermined time has passed.

[0088] <(C) Suction process>

[0089] In the suction step (C), the pressure in the unit flow channel of the substrate is made lower than the pressure in the coating liquid storage section, so that the coating liquid for forming a catalyst coating layer in the coating liquid storage section is introduced into the unit flow channel, and the coating liquid for forming a catalyst coating layer is applied to the partition walls.

[0090] Here, the pressure difference between the coating liquid storage part and the unit flow path is used as a driving force to generate an airflow in the unit flow path, and the coating liquid for forming a catalyst coating layer is introduced into the unit flow path. However, if the viscosity and amount of the coating liquid for forming a catalyst coating layer supplied in the coating liquid supplying step (B) and the pressure difference are appropriately set, the coating liquid for forming a catalyst coating layer will be coated from the upper end of the substrate to the lower side by a desired length.

[0091] The degree of pressure difference can be set so that the wind speed on the upper end surface of the substrate is greater than 10 m / s, greater than 20 m / s, greater than 30 m / s or greater than 35 m / s, and less than 120 m / s, less than 100 m / s, less than 80 m / s, less than 60 m / s or less than 50 m / s.

[0092] From the perspective of effectively and efficiently introducing the coating liquid for forming the catalyst coating into the unit flow path, the implementation time of the (C) suction process can be more than 1.0 seconds, more than 1.5 seconds, more than 2.0 seconds, more than 2.5 seconds or more than 3.0 seconds, and can be less than 10 seconds, more than 8.0 seconds, more than 6.0 seconds, more than 5.0 seconds, more than 4.0 seconds or more than 3.0 seconds.

[0093] <(D) Blowing process>

[0094] In the blowing step (D), compressed air is blown from above to the inner side of the storage wall of the coating liquid storage jig. Thus, even if part of the catalyst coating layer forming coating liquid is attached to the inner side of the storage wall, it will be blown off and fall into the unit flow path, thereby achieving the coating of a predetermined amount of the catalyst coating layer forming coating liquid.

[0095] Compressed air can be blown to the inner side of the storage wall using an appropriate compressed air source. In order to effectively and reliably blow off the catalyst coating layer forming coating liquid attached to the inner side of the storage wall, the compressed air supplier can have an annular blowing hole from which the compressed air is ejected.

[0096] The width of the blowing hole of the compressed air supplier in a direction parallel to the radial direction of the substrate (preferably the width of a circular ring) can be greater than 0.05 mm, greater than 0.07 mm, greater than 0.10 mm, greater than 0.30 mm, greater than 0.40 mm or greater than 0.50 mm, and can be less than 1.00 mm, less than 0.80 mm, less than 0.70 mm or less than 0.60 mm.

[0097] From the viewpoint of making the attached coating liquid for forming a catalyst coating layer fall into the unit flow path reliably, compressed air may be blown toward the inner side of the vertical portion of the storage wall. In this case, the angle between the blowing direction of the compressed air and the inner side surface of the vertical portion of the storage wall may be 0.5° or more, 1.0° or more, 5.0° or more, 10° or more, 15° or more, 20° or more, or 25° or more, and may be 60° or less, 50° or less, 45° or less, 40° or less, or 35° or less.

[0098] The pressure of the compressed air blown toward the inner side of the storage wall can be above 0.05 MPa, above 0.10 MPa, above 0.30 MPa, above 0.50 MPa, above 0.75 MPa or above 1.00 MPa in the compressed air outlet hole, and can be below 1.50 MPa, below 1.25 MPa, below 1.00 MPa or below 0.80 MPa.

[0099] <(E) Firing step>

[0100] In the calcining step (E), the substrate coated with the coating liquid for forming a catalyst coating layer is calcined.

[0101] (E) The calcination in the calcination step can be performed by a known method or a method in which a person skilled in the art appropriately modifies the method according to the composition of the coating liquid for forming a catalyst coating layer to be used.

[0102] <Implementation Methods of (C) Suction Step and (D) Blowing Step>

[0103] In the method for manufacturing an exhaust gas purification catalyst device of the present invention, it is characterized in that at least a part of the above-mentioned (C) suction step and at least a part of the above-mentioned (D) blowing step are performed simultaneously.

[0104] In one embodiment of the present invention, the blowing step (D) is started after the suction step (C) is started. In this case, the time from the start of the suction step (C) to the start of the blowing step (D) may be 0.1 seconds or more, 0.2 seconds or more, 0.3 seconds or more, 0.4 seconds or more, or 0.5 seconds or more, and may be 1.0 seconds or less, 0.8 seconds or less, 0.7 seconds or less, 0.6 seconds or less, or 0.5 seconds or less.

[0105] In one embodiment of the present invention, the suction step (C) is terminated after the blowing step (D) is terminated. In this case, the time from the end of the blowing step (D) to the end of the suction step (C) may be 0.1 seconds or more, 0.2 seconds or more, 0.3 seconds or more, 0.4 seconds or more, or 0.5 seconds or more, and may be 1.0 seconds or less, 0.8 seconds or less, 0.7 seconds or less, 0.6 seconds or less, or 0.5 seconds or less.

[0106] In one embodiment of the present invention, the (D) blowing step is started after the (C) suction step is started, and the (C) suction step is ended after the (D) blowing step is ended.

[0107] <Application Mode of the Method for Manufacturing the Exhaust Gas Purification Catalyst Device of the Present Invention>

[0108] According to the method of the present invention, it is easy to apply the coating liquid for forming the catalyst coating layer to the substrate in a desired length. Therefore, the coating liquid for forming the catalyst coating layer can be applied from the upper end of the substrate to the lower end within a predetermined range. Thus, a coating form called "area coating" in which the catalyst coating layer extends from the opening end of one side of the substrate to a predetermined length along the length direction of the substrate can be easily and accurately realized.

[0109] It is also possible to carry out at least (A) the step of forming the coating liquid storage portion, (B) the step of supplying the coating liquid for forming the catalyst coating layer, (C) the step of sucking, and (D) the step of blowing, and then,

[0110] Turn the substrate upside down.

[0111] (A) a coating liquid storage portion forming step, (B) a coating liquid supplying step for forming a catalyst coating layer, (C) a suction step, (D) a blowing step, and (E) a calcining step are performed.

[0112] At this time, (A) the coating liquid storage portion forming step, (B) the coating liquid supplying step for forming the catalyst coating layer, (C) the suction step, (D) the blowing step and (E) the calcining step may be performed, and then,

[0113] Turn the substrate upside down.

[0114] The (A) coating liquid storage portion forming step, (B) catalyst coating layer forming coating liquid supplying step, (C) suction step, (D) blowing step and (E) calcining step are performed again.

[0115] According to such an embodiment, if the substrate is of a straight-flow type, a "zone coating" catalyst coating can be obtained in which the composition of the catalyst coating is different on the upstream side and the downstream side of the substrate in the exhaust gas flow.

[0116] In addition, if the substrate is a wall flow type, the catalyst coating layer can be formed on both the inlet side unit and the outlet side unit of the substrate.

[0117] Example

[0118] 《Example 1》

[0119] In Example 1, according to Figure 1 In the methods shown in (a) to (c), a coating liquid is applied on a honeycomb substrate.

[0120] First, a cylindrical straight-flow type cordierite honeycomb substrate (10) having a diameter of 100 mm and a length of 70 mm was arranged so that its axial direction was vertical.

[0121] A coating liquid storage jig made of polyethylene is installed on the upper side of the honeycomb substrate (10). The coating liquid storage jig has a substantially cylindrical shape, is in close contact with the upper side of the honeycomb substrate (10) at the lower part, and has a storage wall extending upward from the outer periphery of the upper end of the honeycomb substrate (10) at the upper part. The storage wall of the coating liquid storage jig has a vertical portion 20a extending upward approximately vertically from the outer periphery of the upper end of the honeycomb substrate 10, and an inclined portion 20b extending upward from the upper end of the vertical portion 20a ( Figure 1 (a)).

[0122] Next, a predetermined amount of the coating liquid (40) for forming a catalyst coating layer is supplied to a coating liquid storage portion formed by the upper end surface of the honeycomb substrate (10) and the storage wall of the coating liquid storage jig using a spray nozzle (30) disposed above the honeycomb substrate (10) ( Figure 1 (b)). The coating liquid (40) for forming a catalyst coating layer contains inorganic oxide particles. The viscosity of the coating liquid (40) is measured at 25°C at 0.4 s / min using a cone and plate viscometer. -1 The viscosity was 4,000 mPa·s at a shear rate of 400 s -1 The viscosity measured at a shear rate of 150 mPa·s.

[0123] Next, the spray nozzle (30) is removed from above the honeycomb substrate (10), and a compressed air supply device (50) is arranged instead. The compressed air supply device (50) can blow compressed air in a circular ring shape with a width of 0.5 mm from above at an angle of 30 degrees relative to the vertical direction to the inner side of the storage wall of the coating liquid storage fixture.

[0124] Thereafter, suction was performed from the lower end face of the honeycomb substrate (10) for 3.0 seconds. The suction was performed at a wind speed of 40 m / s on the upper end face of the honeycomb substrate (10). In addition, during the period of 2.0 seconds from 0.5 seconds after the start of the suction to 2.5 seconds after the start of the suction, the compressed air supply device (50) was used to blow 0.10 MPa of compressed air to perform air blowing ( Figure 1 (c)).

[0125] Through the above operation, the coating liquid for forming a catalyst coating layer was applied to the honeycomb substrate. The cross section of the coated honeycomb substrate cut in the radial direction was observed to investigate the uniformity of the coating length. Figure 2 (a) is a photograph showing a cross section of the honeycomb substrate of Example 1 after coating.

[0126] In the coating of the catalyst coating layer forming coating liquid in Example 1, no adhesion of the coating liquid to the coating liquid storage jig was observed, and the total amount of the catalyst coating layer forming coating liquid supplied to the coating liquid storage portion was coated on the honeycomb substrate. Figure 2 As shown in (a), the coating length is longest near the periphery of the substrate, and decreases temporarily and then increases slightly as it approaches the center. The difference between the longest and shortest portions of the coating length is 11.0 mm.

[0127] Comparative Example 1

[0128] In Comparative Example 1, after supplying the coating liquid for forming a catalyst coating to the coating liquid storage portion above the honeycomb substrate, suction was performed for 3.0 seconds and blowing was performed for 2.0 seconds in sequence. Except for this, the coating liquid for forming a catalyst coating was applied to the honeycomb substrate in the same manner as in Example 1 and evaluated.

[0129] Figure 2 (b) is a photograph showing a cross section of the honeycomb substrate of Comparative Example 1 after coating.

[0130] In the coating of the catalyst coating layer forming coating liquid in Comparative Example 1, no adhesion of the coating liquid to the coating liquid storage jig was observed, and the total amount of the catalyst coating layer forming coating liquid supplied to the coating liquid storage portion was coated on the honeycomb substrate. However, the difference between the longest and shortest portions of the coating length of the obtained catalyst coating layer was 16.0 mm.

[0131] Comparative Example 2

[0132] In Comparative Example 2, after supplying the coating liquid for forming a catalyst coating to the coating liquid storage portion above the honeycomb substrate, suction for 3.0 seconds, blowing for 2.0 seconds and suction for 3.0 seconds were performed in sequence. Otherwise, the coating liquid for forming a catalyst coating was applied to the honeycomb substrate in the same manner as in Example 1 and evaluated.

[0133] Figure 2 (c) is a photograph showing a cross section of the honeycomb substrate of Comparative Example 2 after coating.

[0134] In the coating of the coating liquid for forming the catalyst coating layer in Comparative Example 2, no adhesion of the coating liquid to the coating liquid storage jig was observed. However, a portion of the coating liquid for forming the catalyst coating layer supplied to the coating liquid storage portion flowed out from the lower end surface of the honeycomb substrate. In addition, the difference between the longest and shortest portions of the coating length of the obtained catalyst coating layer was 16.5 mm.

[0135] The above results are summarized in Table 1 ( Figure 3 ).

[0136] Description of Reference Numerals

[0137] 10Honeycomb substrate

[0138] 20 Storage Wall

[0139] 20a vertical part

[0140] 20b inclined portion

[0141] 30 spray nozzles

[0142] 40 Coating liquid for forming catalyst coating

[0143] 50 Compressed air supply

[0144] 60 Compressed air

Claims

1. A method for manufacturing an exhaust gas purification catalyst device, the exhaust gas purification catalyst device comprising: a substrate having a plurality of unit flow paths partitioned by partition walls; and a catalyst coating applied in or on the partition walls of the substrate, or both, The manufacturing method comprises the following steps: Step (A): arranging the substrate so that one opening end of the plurality of unit flow paths faces upward and the other opening ends face downward, and attaching a coating liquid storage jig having a storage wall extending upward from the outer periphery of the upper end of the substrate to the upper end portion of the substrate, thereby forming a coating liquid storage portion defined by the upper end surface of the substrate and the inner side of the storage wall of the coating liquid storage jig; Step (B): supplying a coating liquid for forming a catalyst coating layer to the coating liquid storage portion; Step (C): introducing the catalyst coating layer forming coating liquid of the coating liquid storage section into the unit flow path by making the pressure in the unit flow path lower than the pressure in the coating liquid storage section, and coating the catalyst coating layer forming coating liquid on the partition wall; Step (D): blowing compressed air from above toward the inner side of the storage wall of the coating liquid storage jig; as well as Step (E): calcining the substrate coated with the catalyst coating layer-forming coating liquid, and At least a part of the step (C) and at least a part of the step (D) are performed simultaneously. 2 . The method according to claim 1 , wherein the step (D) is started after the step (C) is started.

3. The method according to claim 1, wherein the step (C) is terminated after the step (D) is terminated. 4 . The method according to claim 2 , wherein the step (C) is terminated after the step (D) is terminated.

5. The method according to claim 1, wherein the storage wall of the coating liquid storage jig has a vertical portion extending upward substantially vertically from the outer periphery of the upper end of the substrate, and an inclined portion extending upward and outward from the upper end of the vertical portion. 6 . The method according to claim 5 , wherein in the step (D), the compressed air is blown to the inside of the vertical portion of the storage wall. 7 . The method according to claim 6 , wherein in the step (D), an angle between a blowing direction of the compressed air and an inner side surface of the vertical portion of the storage wall is 0.5° or more and 60° or less.

8. The method according to any one of claims 1 to 7, wherein in the step (D), the width of the blowout hole for blowing compressed air toward the inside of the storage wall in a direction parallel to the radial direction of the substrate is 0.05 mm to 1.00 mm.

9. The method according to any one of claims 1 to 7, wherein in the step (D), the pressure of the compressed air blown toward the inner side of the storage wall is 0.05 MPa or more and 1.50 MPa or less at the compressed air outlet hole.

10. The method according to any one of claims 1 to 7, wherein the catalyst coating layer-forming coating liquid is heated at 25°C for 0.4 seconds. -1 The viscosity measured at a shear rate of 500 mPa·s or more and 10000 mPa·s or less. 11 . The method according to claim 1 , wherein the catalyst coating layer-forming coating liquid is applied to the partition walls in a predetermined range from an upper end of the substrate downward. 12 . The method according to claim 1 , wherein after at least performing the steps (A) to (D), the substrate is turned upside down and the steps (A) to (E) are performed. 13 . The method according to claim 1 , wherein the substrate is a direct-flow type honeycomb substrate.

14. The method according to any one of claims 1 to 7, wherein the substrate is a wall-flow honeycomb substrate.

Citation Information

Patent Citations

  • Manufacturing method for exhaust gas purification device

    CN111836686A

  • Method for producing exhaust-gas-purifying catalyst

    CN112203764A

  • Slurry supplying nozzle and production apparatus and production method of exhaust gas purifying catalyst using the same

    JP2015039672A

  • Method for producing exhaust gas purification catalyst

    JP2018069113A

  • Method for producing exhaust gas purification catalyst

    JP2018153718A