Multilayer polyvinyl alcohol film and method for preparing the same
Multi-layer water-soluble films were prepared by simultaneous solution co-casting method, combining the first layer with a high anti-blocking agent and the second layer with a low anti-blocking agent, and using a bio-based resin and a PVOH homopolymer blend, the existing ones were solved The film has problems with adhesion, sealing and solubility, which achieves high barrier properties and good sealing properties.
Patent Information
- Application Number
- CN202380035556.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-05-03
- Filing Date
- 2023-05-03
- Publication Date
- 2024-12-03
AI Technical Summary
During storage and use, existing water-soluble polymer films are prone to problems such as adhesion, low sealing, poor solubility, etc., resulting in leaks or residues of contents, and chemical incompatibility leads to undesirable interactions.
Multi-layer water-soluble films are prepared by simultaneous solution co-casting method, including multi-layer structures of polyvinyl alcohol (PVOH) homopolymer and copolymer. The first layer contains a high anti-blocking agent and the second layer contains a low anti-blocking agent. And improve wet vapor permeability and sealing properties through a bio-based resin and PVOH homopolymer blend.
High barrier properties and good sealing properties are achieved, which reduces haze and friction coefficient, extends the service life of the film and reduces content residues.
Smart Images

Figure CN119072384A_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] The benefit of U.S. Provisional Patent Application No. 63 / 337,956, filed on May 3, 2022, is claimed under 35 U.S.C. §119(e), and the entire disclosure of which is incorporated herein by reference. Technical Field
[0003] The present disclosure relates generally to water-soluble films and related packages. More specifically, the present disclosure relates to multilayer water-soluble polyvinyl alcohol films and simultaneous casting methods for preparing such films. Background Art
[0004] Water-soluble polymer films are commonly used as packaging materials to simplify the dispensing, pouring, dissolving and dosing of materials to be delivered. The consumer can directly add the bagged composition to a mixing container such as a bucket, a sink or a washing machine. Advantageously, this provides accurate dosing, while eliminating the need for the consumer to measure the composition. Additionally, the water-soluble polymer film packaging can block the original strong chemical substance from the consumer's hand, thereby protecting the consumer from contacting with irritating chemicals. The bagged composition can also reduce the trouble of dispensing similar compositions from a container, such as pouring compositions from a bottle. In a word, soluble pre-measured polymer film bags provide convenience and safety for the use of consumers in various applications.
[0005] Some water-soluble polymer films used to make currently commercially available bags interact with other bags (i.e., stick), are visually unattractive due to having a high haze %, or do not exhibit sufficiently high sealing or solubility, for example, after storage. For example, a bag may exhibit a low haze %, but stick to other bags too easily. Alternatively, a bag may exhibit good solubility, but poor water sealing, such as commonly used water-soluble films, such as certain polyvinyl alcohol films. Films that exhibit poor water sealing may experience rupture of the bag or bag seal prematurely before use and release the contents. In another type of problem, a bag may exhibit good sealing, but poor solubility in cold water. For example, this reduced solubility may result in a large amount of residue remaining after the contents of the bag have been dispersed (e.g., greater than 50%). Additionally, chemical incompatibility between the film comprising the bag and one or more materials packaged therein may result in undesirable interactions or chemical reactions. For example, interaction of the film comprising the bag with the material enclosed therein may result in: degradation or failure of the film, resulting in leakage of the bag contents; degradation of the bag contents; generation of gaseous byproducts, which may result in bag rupture; or cross-linking of the film, which may result in cracking of the film during storage.
[0006] In some cases, modifying a water-soluble film to improve one property may have a negative impact on other properties. For example, anti-blocking agents may be incorporated into the film or applied to the film surface to improve the blocking properties of the film, but the addition of such anti-blocking agents generally increases the haze of the film. It would be advantageous to produce a water-soluble film that can provide a combination of beneficial chemical and / or physical properties that are generally opposed to each other.
[0007] Multilayer polyvinyl alcohol films have been prepared by melt coextrusion, for example, as described in U.S. Pat. No. 8,597,796 B2. For solution casting, a drying process has been described to remove the carrier solvent after the first casting step before casting the second layer to form a two-layer film, for example, as described in U.S. Patent Application Publication No. 2009 / 0196908 A1, U.S. Pat. Nos. 4,765,916 and 9,744,695 B2, and International (PCT) Publication No. WO 1998 / 021118 A1, the disclosures of which are hereby incorporated by reference. Existing literature also describes laminating two films or producing a multilayer configuration by sequential casting, for example, as described in U.S. Pat. No. 6,776,287, the disclosures of which are hereby incorporated by reference. Summary of the invention
[0008] One aspect of the present disclosure provides a water-soluble film including a plurality of layers in continuous contact with each other, wherein the film is prepared by a simultaneous solution co-casting method.
[0009] Another aspect of the present disclosure provides a multilayer water-soluble film, the multilayer water-soluble film comprising a first layer and a second layer, the first layer comprising a blend of polyvinyl alcohol (PVOH) homopolymer and PVOH copolymer, the second layer comprising a blend of PVOH homopolymer. The film according to this aspect can optionally provide both high barrier properties to moisture vapor transmission and good sealing properties.
[0010] Another aspect of the present disclosure provides a multilayer water-soluble film, wherein the amount of anti-blocking agent in a first layer of the film as a percentage of the total weight of the first layer is higher than the amount of anti-blocking agent in a second layer of the film as a percentage of the total weight of the second layer.
[0011] Another aspect of the present disclosure provides a multi-layer water-soluble film comprising a first layer comprising a bio-based resin and a second layer comprising a PVOH homopolymer, a PVOH copolymer, or a blend thereof.
[0012] Another aspect of the present disclosure provides a method for producing a multi-layer water-soluble film such as a bi-layer film by a simultaneous solution co-casting method.
[0013] For the compositions and methods described herein, it is considered that optional features are selected from various aspects, embodiments, claims and examples provided herein, and the features include but are not limited to components and their composition ranges. For example, the features of the embodiments and formulation methods described in Examples 1 to 7 can be combined with any of the additional features provided in the description and claims herein.
[0014] By reviewing the following detailed description, additional aspects and advantages will be apparent to those of ordinary skill in the art. Although the films and methods of the present disclosure are susceptible of embodiments in many forms, the following description includes specific embodiments, wherein it is understood that the present disclosure is illustrative and is not intended to limit the invention to the specific embodiments described herein. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] To further facilitate understanding of the present disclosure, eight drawings are attached hereto. The drawings herein are illustrative in nature and are not intended to be limiting.
[0016] Figure 1 and 2 is a graph of the coefficient of static friction (COF) versus % haze for the single and dual layer films described herein.
[0017] Figure 3 is a perspective view of a multi-slot die that can be used to prepare co-cast bi-layer films.
[0018] 4A and 4B show in side view Figure 3 FIG4B shows an enlarged view of the circled portion of FIG4A .
[0019] Figure 5 A schematic diagram showing the angle of the die relative to the casting surface is shown.
[0020] Figure 6 A perspective view of the coefficient of friction test fixture used in Example 2 is shown.
[0021] FIG. 7 shows an optical microscope cross-sectional view of the multilayer co-cast film 3C described in Example 3. As shown in FIG.
[0022] FIG. 8 shows an optical microscope cross-sectional view of the multilayer sequential cast film described in Example 3. DETAILED DESCRIPTION
[0023] One aspect of the present disclosure provides a kind of water-soluble film, and the water-soluble film comprises a plurality of layers that are in continuous contact with each other, wherein the film is prepared by a simultaneous solution co-casting method. The film (that is, multilayer water-soluble film) of this aspect comprises a plurality of layers, and the plurality of layers comprises a water-soluble resin, wherein each water-soluble resin independently comprises one or more polymers selected from polyvinyl alcohol homopolymer, polyvinyl alcohol copolymer and its combination. As described herein, each layer can further comprise one or more secondary components.
[0024] The multilayer water-soluble film of this aspect can comprise two layers.The first layer can comprise the first water-soluble resin, and the first water-soluble resin can comprise polyvinyl alcohol homopolymer, polyvinyl alcohol copolymer or its combination, and the second layer can comprise the second water-soluble resin, and the second water-soluble resin can comprise polyvinyl alcohol homopolymer, polyvinyl alcohol copolymer or its combination.Optionally, the second water-soluble resin can be different from the first water-soluble resin.In other options, the water-soluble film can contain the first layer and the second layer, and the first layer comprises water-soluble cellulose (for example, hydroxypropyl methylcellulose), and the second layer comprises polyvinyl alcohol resin, and the polyvinyl alcohol resin can be polyvinyl alcohol homopolymer, polyvinyl alcohol copolymer or its blend.
[0025] For the film in which the first water-soluble resin and / or the second water-soluble resin include a blend of a polyvinyl alcohol homopolymer and a polyvinyl alcohol copolymer, the amount of the polyvinyl alcohol homopolymer and the polyvinyl alcohol copolymer including the first water-soluble resin and / or the second water-soluble resin is not particularly limited. Optionally, based on the total weight of the first layer, the first water-soluble resin may include an amount of polyvinyl alcohol homopolymer in the following range: about 20wt.% to about 70wt.%, or about 25wt.% to about 60wt.%, or about 30wt.% to about 50wt.%, or about 35wt.% to about 45wt.%. Optionally, based on the total weight of the first layer, the first water-soluble resin may include an amount of polyvinyl alcohol copolymer in the following range: about 5wt.% to about 50wt.%, or about 10wt.% to about 40wt.%, or about 15wt.% to about 35wt.%, or about 20wt.% to about 30wt.%. Optionally, based on the total weight of the second layer, the second water-soluble resin may include a polyvinyl alcohol homopolymer in an amount ranging from about 20 wt.% to about 70 wt.%, or about 25 wt.% to about 60 wt.%, or about 30 wt.% to about 50 wt.%, or about 35 wt.% to about 45 wt.%. Optionally, based on the total weight of the second layer, the second water-soluble resin may include a polyvinyl alcohol copolymer in an amount ranging from about 5 wt.% to about 50 wt.%, or about 10 wt.% to about 40 wt.%, or about 15 wt.% to about 35 wt.%, or about 20 wt.% to about 30 wt.%. Optionally, the amount of the polyvinyl alcohol homopolymer comprising the first water-soluble resin is greater than or equal to the amount of the polyvinyl alcohol copolymer comprising the first water-soluble resin.
[0026] The multilayer water-soluble film of this aspect can have any suitable thickness.For example, the thickness of the water-soluble film can be in the range of about 15 microns to about 150 microns.Each layer including the water-soluble film can have any suitable thickness.For example, the thickness of each layer can be independently in the range of about 1 micron to about 100 microns.The relative thickness of the layer including the multilayer film is not particularly limited.For example, the first layer of the multilayer film of the present disclosure can be in the following ranges with respect to the thickness ratio of the second layer: about 1:200 to about 200:1, or about 1:100 to about 100:1, or about 1:20 to about 20:1, or about 1:5 to about 5:1, or about 1:2 to 2:1, or about 1:1.
[0027] Optionally, the multilayer water-soluble film according to the present disclosure may include one or more water-insoluble layers. The water-insoluble layer may include a backing layer or a peeling layer in contact with the multilayer water-soluble film, and may facilitate peeling the multilayer water-soluble film when the water-soluble film is wound into a roll. Suitable water-insoluble layers may include polymers including, but not limited to, polyethylene, polypropylene, polyethylene terephthalate, and combinations thereof.
[0028] Another aspect of the present disclosure provides a kind of multilayer water-soluble film, wherein the amount of one or more antiblocking agents in the first layer of the film accounts for the percentage of the total weight of the first layer higher than the amount of the antiblocking agent in the second layer of the film accounts for the percentage of the total weight of the second layer. Optionally, compared with the first layer, the second layer can be free of antiblocking agent, substantially free of antiblocking agent or have a lower concentration of antiblocking agent. Optionally, the first layer includes the glossy surface of the film, i.e. the surface in contact with air during drying. The film according to this aspect can be designed to simultaneously show a combination of low friction coefficient and low haze, for example, when the film is set to the outer surface of a multilayer film, the friction coefficient corresponding to the layer containing one or more antiblocking agents, and the haze value characteristics of the entire multilayer film thickness. For example, a film according to this aspect can exhibit a combination of haze (%) and static coefficient of friction ("COF") that is within a polygon defined by vertices (haze (%), static COF) of about (0.03, 13), about (59, 0.5), about (10, 0.1), and about (0.1, 0.1). Figure 1 A graph of this polygon is shown with dashed lines, and also shows the (Haze (%), Static COF) points for single-layer and dual-layer films according to the examples described herein. Optionally, a film according to this aspect can exhibit a combination of haze (%) and static coefficient of friction ("COF") that is within the polygon defined by vertices (Haze (%), Static COF) of about (0.03, 10), about (55, 0.5), about (10, 0.1), and about (0.1, 0.1). Figure 2 A diagram of this polygon shown in dotted lines is shown, and the (haze (%), static COF) points of the monolayer and bilayer films according to the examples described herein are also shown. The one or more antiblocking agents in the first layer can impart a low friction coefficient to this layer. However, since the multilayer film of this aspect can contain an antiblocking agent preferentially, primarily or only in one layer, the multilayer film can be designed to exhibit a lower haze than a film containing the same concentration of antiblocking agents in the cross section of the entire film. Therefore, the film utilizes the property that the friction coefficient is essentially a characteristic of the outer surface of the film, so that the entire film thickness does not need to contain an antiblocking agent to make the surface of the film have a low friction coefficient. Therefore, compared with a monolayer film with the same concentration of antiblocking agents, the multilayer film of this aspect can be designed to exhibit an equivalent friction coefficient but a reduced haze. Alternatively, compared with a monolayer film containing the same concentration of antiblocking agents, the multilayer film of this aspect can be designed to exhibit a superior, reduced friction coefficient and an equivalent haze.
[0029] Another aspect of the present disclosure provides a multilayer water-soluble film, the multilayer water-soluble film comprising a first layer and a second layer, the first layer containing a blend of a PVOH homopolymer and a PVOH copolymer, the second layer comprising a PVOH homopolymer or a blend of PVOH homopolymers. Due to the layer containing the PVOH copolymer, the film according to this aspect can provide a high barrier to moisture vapor transmission, and due to the PVOH homopolymer layer, the film can provide good sealing properties, that is, a high sealing strength when the first part of the film is heat-sealed to the second part of the film or a separate such film is sealed to each other. The first part and the second part can be sealed, wherein the surface of the layer including the blend of the PVOH homopolymer and the PVOH copolymer is sealed to the surface of the layer including the PVOH homopolymer or the blend of the PVOH homopolymer.
[0030] Another aspect of the present disclosure provides a multi-layer water-soluble film comprising a first layer comprising a bio-based resin and a second layer comprising a PVOH homopolymer, a PVOH copolymer, or a blend thereof.
[0031] Another aspect of the present disclosure provides a multi-layer water-soluble film comprising a top layer including a foam film.
[0032] The multi-layer water-soluble films according to the present disclosure may have no intermediate layers, such as adhesives, between the layers (eg, between the first and second layers of a bi-layer film).
[0033] Based on the MSTM 205 test method described herein, a water-soluble film having the same composition and thickness as the first layer of the multilayer film of the present disclosure may have a dissolution time of 300 seconds or less, or 200 seconds or less at 20°C.
[0034] The multi-layer water-soluble film according to the present disclosure can have a second layer including an outer surface, and based on the Seal Strength Test described herein, the water seal strength of the film when sealed to itself by sealing the first portion of the outer surface of the second layer to the second portion of the outer surface of the second layer can be in the following range: about 5N to about 18N, or about 10N to about 18N, or about 12N or greater.
[0035] The multi-layer water-soluble film according to the present disclosure may have a second layer including an outer surface, and the water seal strength of the film when sealed to itself by sealing the first portion of the outer surface of the second layer to the second portion of the outer surface of the second layer may be in the range of about 10N or greater, or about 12N or greater, or about 15N or greater based on the Seal Strength Test described herein, and the moisture vapor transmission rate of the film is about 100 g / m per 24 hours based on the Moisture Vapor Transmission Rate Test Method described herein. 2 or less, or about 50 g / m2 per 24 hours 2or less, or about 30 g / m2 per 24 hours 2 or smaller.
[0036] The present disclosure also provides a co-casting method for producing a multilayer water-soluble film, wherein the method includes simultaneously casting a plurality of resin solutions to form a multilayer solution composition of a layer including a plurality of resin solutions, and drying the multilayer solution composition to form a multilayer film. Compared with the multilayer film produced according to the sequential casting method, the multilayer film produced according to the co-casting method of the present disclosure can provide one or more favorable properties, wherein the multilayer film is constructed by: solution casting the second layer, applying heat to make the second layer at least partially dry to form a film, solution casting the first layer in contact with the second film, and drying the layer to form a multilayer film. Compared with the sequential casting method, the co-casting method of the present disclosure can be used to provide a multilayer film with fewer steps. In addition, advantageously, each layer of the multilayer film produced by the co-casting method of the present disclosure will experience the same heating history, while each layer of the multilayer film produced by the sequential casting method will experience different heating histories due to the multiple heating and drying steps including the sequential casting method, for example, wherein the first casting layer experiences a longer heating and drying time because it experiences excessive heating to dry the second casting layer. Without intending to be bound by theory, the simultaneous solution co-casting process according to the present disclosure allows for limited migration of adjacent layers into each other, thereby more effectively bonding the adjacent layers and minimizing the risk of cohesive failure in the multilayer film.
[0037] The simultaneous solution co-casting method of the present disclosure can be used to produce textured films. Specifically, the inserts of the multi-slot die described herein can be used to produce striations in the top layer of a multilayer film during simultaneous solution co-casting.
[0038] Another aspect of the present disclosure provides a kind of water-soluble unit dose product.Unit dose product can include bag, and the bag includes outer wall, and the outer wall has outer surface and inner surface that limit inner bag volume, wherein the outer wall includes the multilayer water-soluble film of the present disclosure. Optionally, inner bag volume can contain composition.Multilayer film of unit dose product including this aspect can be selected, to provide the product with useful property derived from the property of component film layer.For example, multilayer film can be designed to include the first layer that provides high barrier property to moisture vapor permeability and the second layer that shows high sealing strength when sealed to itself, for example.Such multilayer film can be used for constructing water-soluble unit dose product, for example, by sealing the first part of the second layer to the second part of the second layer to form the bag that can contain composition.It is expected that the product constructed by such multilayer film shows low sealing failure risk (that is, low premature rupture risk), while also preventing moisture from reaching the composition contained therein.
[0039] Another aspect of the present disclosure provides a water-soluble unit dose product including a plurality of compartments, wherein the unit dose product includes one or more multilayer films of the present disclosure. The unit dose product may include a first sealed compartment and a second sealed compartment. The second compartment may be in a substantially overlapping relationship with the first sealed compartment, so that the second sealed compartment and the first sealed compartment share the partition wall in the bag. The unit dose product including the first and second sealed compartments may further include a third sealed compartment. The third sealed compartment may be in a substantially overlapping relationship with the first sealed compartment, so that the third sealed compartment and the first sealed compartment share the partition wall in the bag. The film of the first compartment may be a multilayer film of the present disclosure. The film of the second compartment may be a multilayer film of the present disclosure. The film of the partition wall may be a multilayer film of the present disclosure. The film of the first and second compartments may be a multilayer film of the present disclosure. The film of the first and second compartments and the partition wall may be a multilayer film of the present disclosure.
[0040] A unit dose article comprising a plurality of compartments may be prepared according to a method comprising the following steps, wherein the unit dose article comprises one or more multilayer films of the present disclosure: (a) forming a first compartment comprising a first film; (b) forming a groove in part or all of the enclosed first compartment formed in step (a) to generate a second molded compartment comprising a second film superimposed on the first compartment; (c) filling and enclosing the second compartment with a third film; (d) sealing the first film, the second film, and the third film; and (e) cutting the film to produce a multi-compartment bag. The groove formed in step (b) may be achieved by applying a vacuum to the compartment prepared in step (a). The first water-soluble film may be a multilayer film of the present disclosure. The second water-soluble film may be a multilayer film of the present disclosure. The third water-soluble film may be a multilayer film of the present disclosure. The first and second water-soluble films may be multilayer films of the present disclosure. The first and third water-soluble films may be multilayer films of the present disclosure. The first, second, and third water-soluble films may be multilayer films of the present disclosure.
[0041] The different compartments of a multi-compartment article can be prepared together in a side-by-side or concentric manner, wherein the article comprises one or more multilayer films of the present disclosure, wherein the resulting cojoined bags may or may not be separated by cutting. Alternatively, the compartments may be prepared separately.
[0042] Another method for producing a unit dose product comprising multiple compartments may include the following, wherein the unit dose product comprises one or more multilayer films of the present disclosure: (a) deforming a first water-soluble film in a mold to produce an open cavity; (b) filling the open cavity formed by the first water-soluble film with a composition; (c) deforming a third water-soluble film in a mold to produce at least one open cavity; (d) filling at least one open cavity in the third film with a composition (e.g., the composition is the same or different from the composition of step (b)); (e) closing one or more open filled cavities of step (d) with a second water-soluble film; (f) optionally sealing the second water-soluble film and the third water-soluble film by solvent sealing to produce a closed intermediate; (g) closing the open filled cavity of step (b) with the closed intermediate of step (f); and (h) optionally sealing the first water-soluble film and the second water-soluble film of the closed intermediate of step (g) by solvent sealing to produce a water-soluble unit dose product. This method can be used to provide, for example, a unit dose product with overlapping composition compartments, such as one or more compartments overlapping relative to another compartment. Any one of the sealing steps can include solvent sealing, and at least one of the sealing steps can include solvent sealing. Each of the first and second water-soluble films has a first side and a second side, and the first side of the first water-soluble film can be sealed to the second side of the second water-soluble film to produce a first compartment between the first water-soluble film and the second water-soluble film, and the first side of the second water-soluble film can be sealed to the second side of the third water-soluble film to produce at least a second compartment between the second water-soluble film and the third water-soluble film, and the second compartment can be located above the first compartment. The first water-soluble film and the third water-soluble film can be the same before thermoforming, i.e., physically and chemically the same, wherein the term "same" means making specification changes within a standard process. Optionally, the sealing of the first water-soluble film and the second water-soluble film can include, for example, a step of wetting the second water-soluble film with a sealing solution as described herein by a contact wetting method. Additionally or alternatively, the sealing of the second water-soluble film and the third water-soluble film optionally may include a step of wetting the second water-soluble film with a sealing solution as described herein, for example, by a contact wetting method. The first water-soluble film may be a multilayer film of the present disclosure. The second water-soluble film may be a multilayer film of the present disclosure. The third water-soluble film may be a multilayer film of the present disclosure. The first and second water-soluble films may be multilayer films of the present disclosure. The first and third water-soluble films may be multilayer films of the present disclosure. The first, second and third water-soluble films may be multilayer films of the present disclosure.
[0043] The water-soluble unit dose articles comprising a plurality of compartments including compartments having overlapping configurations may optionally contain fabric and home care compositions in one or more compartments. Fabric and home care compositions include fabric treatments, treatments for hard surfaces and any other surface in the fabric and home care field, air care agents, car care agents, dishwashing agents, fabric conditioners and softeners, laundry detergents, laundry and rinse additives and / or care agents, hard surface cleaners and / or treatments, and other cleaning agents for consumer or institutional use.
[0044] Fabric and home care products are optionally used or consumed in the form in which they are sold and are used to treat fabrics, hard surfaces and any other surface in the field of fabric and home care, and include: air care agents, including air fresheners and fragrance delivery systems; car care agents; dishwashing agents; fabric conditioners (including softeners and / or fresheners); laundry detergents; laundry and rinse additives and / or care agents; hard surface cleaners and / or treatments, including floor and toilet bowl cleaners; and other cleaning agents for fabric or household uses.
[0045] Cleaning and / or treatment compositions include, but are not limited to, products for treating fabrics, hard surfaces and any other surface in the field of fabric and home care, including: air care agents, including air fresheners and fragrance delivery systems; car care agents; dishwashing agents; fabric conditioners (including softeners and / or fresheners); laundry detergents; laundry and rinse additives and / or care agents; hard surface cleaners and / or treatments, including floor and toilet bowl cleaners; granular or powdered general purpose or "heavy duty" detergents, especially detergents; liquid, gel or paste-form general purpose detergents, especially the so-called heavy duty liquid types; liquid delicate fabric detergents; hand dishwashing agents or light duty dishwashing agents, especially high foaming types; machine dishwashing agents, including various tablet, granular, liquid and rinse aid types for fabric and household use; car or carpet shampoos; bathroom cleaners, including toilet bowl cleaners; and cleaning aids, such as bleach additives and "stain bars" or pre-treatment types; substrate-loaded products, such as sheets with added desiccant.
[0046] Unless otherwise specified, fabric and / or hard surface cleaning and / or treatment compositions include all-purpose or "heavy duty" detergents, particularly detergents, in granular or powder form; all-purpose detergents in liquid, gel or paste form, particularly so-called heavy duty liquid types; liquid delicate fabric detergents; hand dishwashing detergents or light duty dishwashing detergents, particularly high foaming types; machine dishwashing detergents, including various tablet, granular, liquid and rinse aid types for home and institutional use; liquid detergents and disinfectants; car or carpet shampoos; bathroom cleaners, including toilet bowl cleaners; fabric conditioning products, including softeners and / or fresheners, which may be in liquid, solid and / or dryer sheet form; and cleaning aids, such as bleach additives and "stain bars" or pre-treatment types; substrate-loaded products, such as dryer sheets. All such products, where applicable, may be in standard, concentrated or even highly concentrated form, even though to some extent such products may be non-aqueous in some respects.
[0047] Optionally, the multilayer water-soluble film according to the present disclosure may include one or more active ingredients. One or more active ingredients may be present in the entire film or one or more layers thereof, deposited on one or both surfaces of the film, or both. Suitable active ingredients include, but are not limited to, cleaning agents; detergents; superabsorbents; water softeners; stain removers; fabric softeners; color protectants; enzymes; fragrances; deodorants; polishing agents; disinfectants; peroxides and other bleaching agents, including, but not limited to, hypochlorites, hydroxides, chloramines, chloramines, chloramides, and chlorimides; and personal care / hygiene products, including, but not limited to, shampoos, skin cleansers, exfoliants, and tooth cleaners. Suitable active ingredients may also include ingredients that can inhibit or suppress crosslinking, such as sodium acetate.
[0048] The multilayer water-soluble film according to the present disclosure can be designed to reduce or eliminate harmful interactions between the content of the unit dose product (such as a bag) and the product. The multilayer water-soluble film according to the present disclosure can be prepared so that one layer of the film is enriched with components relative to one or more other layers of the film. The unit dose product including one or more compartments can be constructed by such a film so that the inner surface of the compartment of the unit dose product (i.e., the surface arranged adjacent to or in direct contact with the content of the compartment) includes a film layer enriched with components. For example, a multilayer water-soluble film can be constructed in which one layer of the film is enriched with low molecular weight polyols, such as one or more of the following: glycerol, diglycerol, sorbitol, ethylene glycol, diethylene glycol, triethylene glycol, dipropylene glycol, tetraethylene glycol, propylene glycol, polyethylene glycol up to 400MW, neopentyl glycol, trimethylolpropane, polyether polyols, sorbitol, methylpropylene glycol, 2-methyl-1,3-propanediol Or its combination.Unit dose article can be constructed by this type of film so that the film layer enriched with low molecular weight polyol forms the inner surface of one or more compartments of unit dose article.In this type of configuration, the polyol in the inner film surface can be used for example to crosslink with the material in the bag contents, and the material, for example, includes but is not limited to aldehyde (for example, glutaraldehyde), acid and polyacid (for example, citric acid) or sodium borate.This type of crosslinking can advantageously improve the rigidity of the packaging film.This use of low molecular weight polyol can be considered as a kind of sacrificial use, for example, so that polyol is used for crosslinking rather than its typical film layer plasticizing use.This type of crosslinking can also alleviate the undesirable chain disconnection of polymer film, which may occur in the film for packaging oxidative bleaching agent.
[0049] All percentages, parts and ratios referred to herein are based on the total dry weight of the film compositions of the present disclosure or the total weight of the content compositions, as applicable, and unless otherwise specified, all measurements are made at about 25° C. All such weights as they pertain to listed ingredients are based on the active level, and, therefore, do not include carriers or by-products that may be included in commercially available materials, unless otherwise specified.
[0050] All ranges set forth herein include all possible subsets of ranges and any combination of such subset ranges.By default, ranges include the end values, unless otherwise stated.In the case of providing a range of values, it is to be understood that each intermediate value between the upper and lower limits of the range and any other stated value or intermediate value within the stated range are encompassed within the disclosure.The upper and lower limits of these smaller ranges can be independently included within a smaller range, and are also encompassed within the disclosure, subject to any clearly excluded limits within the stated range.In the case where the stated range includes one or two limits in the limits, it is also contemplated that the scope excluding any one or two limits in those included limits is a part of the disclosure.
[0051] It is expressly contemplated that, for any numerical value recited herein, for example as a parameter of or part of a range relating to the subject matter, alternatives forming part of the description are functionally equivalent ranges surrounding the specific numerical value (e.g., for a dimension disclosed as "40 mm," an alternative embodiment contemplated is "approximately 40 mm").
[0052] As used herein, the terms bag and bag should be considered interchangeable. The terms bag and bag can be used to refer to a container prepared using a film and a fully sealed container preferably having a material sealed therein, such as in the form of a measured dose delivery system. The sealed bag can be prepared by any suitable method, including such processes and features as heat sealing, solvent welding, and adhesive sealing (e.g., using a water-soluble adhesive).
[0053] As used herein and unless otherwise specified, the terms "wt. %" and "wt %" are intended to refer to the composition of the identified element in the "dry" (non-water) part by weight of the entire film (including residual moisture in the film) (when applicable, as describing the film) or the part by weight of the entire composition or coating, whichever may depend on the context.
[0054] As used herein and unless otherwise specified, the term "PHR" ("phr") is intended to refer to the composition of the identified elements per hundred parts of a water-soluble polymer resin (whether PVOH or other polymer resin unless otherwise specified) in a water-soluble film or solution used to prepare a film.
[0055] The method of forming a container by a film is known in the art. The film can be used to form a container (bag) by any suitable method, the method comprising vertical forming, filling and sealing (VFFS) or thermoforming. The film can be sealed by any suitable method, the method comprising solvent sealing or heat sealing of a film layer, such as around the periphery of the container. For example, the bag can be used to dose the material to be delivered into a large amount of water.
[0056] Unless otherwise stated, the films, bags, and related methods of use are contemplated to include embodiments comprising any combination of one or more of the additional optional elements, features, and steps further described below.
[0057] The water-soluble bag may contain (enclosed) compositions. Compositions may be selected from liquids, solids or combinations thereof. As used herein, "liquids" include free-flowing liquids, as well as pastes, gels, foams and mousses. Gases (e.g., suspended bubbles) or solids (e.g., particles) may be contained in liquids. As used herein, "solids" include but are not limited to powders, agglomerates and mixtures thereof. Non-limiting examples of solids include particles, microcapsules, beads, strips and pearlescent balls.
[0058] For each layer of the multilayer film of the present disclosure, the water-soluble resin comprising the layer may include one or more polyvinyl alcohol (PVOH) homopolymers, one or more polyvinyl alcohol copolymers, or a combination thereof. As used herein, the term "homopolymer" generally includes polymers having a single type of monomer repeating unit (e.g., a polymer chain consisting of a single monomer repeating unit or substantially consisting of a single monomer repeating unit). For the specific case of PVOH, the term "homopolymer" (or "PVOH homopolymer") may include copolymers consisting of a distribution of vinyl alcohol monomer units and vinyl acetate monomer units, depending on the degree of hydrolysis (e.g., a polymer chain consisting of vinyl alcohol and vinyl acetate monomer units or substantially consisting of vinyl alcohol and vinyl acetate monomer units). In the limiting case of 100% hydrolysis, the PVOH homopolymer may include a true homopolymer having only vinyl alcohol units.
[0059] For each layer of the multilayer film of the present disclosure, the water-soluble resin including the layer may include one or more bio-based resins. Suitable bio-based resins include, but are not limited to, cellulose ethers, cellulose esters, cellulose amides, gelatin, methylcellulose, carboxymethylcellulose and salts thereof, dextrin, ethylcellulose, hydroxyethylcellulose, hydroxypropylmethylcellulose, maltodextrin, starch, modified starch, guar gum, acacia gum, gum arabic, xanthan gum, pullulan, carrageenan, iota carrageenan, kappa carrageenan, pea protein, chitosan, chitosan derivatives, alginate and salts thereof and one or more combinations of any of the foregoing items. Bio-based resins particularly suitable for incorporation into the multilayer film according to the present disclosure are cellulose polymers and modified celluloses, including, but not limited to, hydroxypropylmethylcellulose, hydroxyethylcellulose, ethylcellulose, methylcellulose, carboxymethylcellulose and salts thereof and combinations thereof. Suitable bio-based resins may also include synthetic polymers derived from bio-sourced monomers, such as polylactic acid and polyethylene derived from bio-sourced ethylene. The bio-based resin may be selected from the water-soluble resin type.
[0060] Optionally, the multilayer film may comprise a first layer and at least a second layer, wherein the first layer comprises a first polyvinyl alcohol resin, wherein the first polyvinyl alcohol resin comprises a polyvinyl alcohol homopolymer, a polyvinyl alcohol copolymer, or a combination thereof, and the at least second layer comprises a second polyvinyl alcohol resin, wherein the second polyvinyl alcohol resin comprises a polyvinyl alcohol homopolymer, a polyvinyl alcohol copolymer, or a combination thereof, wherein the second polyvinyl alcohol resin is different from the first polyvinyl alcohol resin.
[0061] Polyvinyl alcohol is a synthetic resin that is typically prepared by alcoholysis (commonly referred to as hydrolysis or saponification) of polyvinyl acetate. Fully hydrolyzed PVOH is a strongly hydrogen-bonded, highly crystalline polymer that is soluble only in hot water (i.e., water above about 140°F (about 60°C)), with nearly all acetate groups converted to alcohol groups. If a sufficient number of acetate groups are allowed to remain after the hydrolysis of polyvinyl acetate, i.e., PVOH homopolymer is partially hydrolyzed, the polymer is more weakly hydrogen-bonded, less crystalline, and is generally soluble in cold water (i.e., water below about 50°F (about 10°C)). Thus, the partially hydrolyzed polymer is a vinyl alcohol-vinyl acetate copolymer, but is often referred to as a PVOH homopolymer.
[0062] The viscosity (μ) of the PVOH homopolymer or copolymer is determined by measuring a freshly prepared PVOH solution using a Brookfield LV type viscometer with a UL adapter, as described in the British Standard ENISO 15023-2:2006 Annex E Brookfield Test method. International convention specifies the viscosity of a 4% aqueous solution of polyvinyl alcohol at 20°C. Unless otherwise specified, all viscosities specified in this disclosure in centipoise (cPs) should be understood to refer to the viscosity of a 4% aqueous solution of polyvinyl alcohol at 20°C. Similarly, when a resin is described as having (or not having) a specific viscosity, unless otherwise specified, it is meant that the specified viscosity is the average viscosity of the resin, which may inherently have a corresponding molecular weight distribution.
[0063] It is well known in the art that the viscosity of PVOH is related to the weight average molecular weight of the PVOH resin, and viscosity is generally used as a substitute for the weight average molecular weight. The viscosity of the PVOH resin can be from about 1.0 cPs to about 50.0 cPs, from about 1.0 cPs to about 40.0 cPs, or from about 1.0 cPs to about 30.0 cPs, such as about 4 cPs, 8 cPs, 15 cPs, 18 cPs, 23 cPs, or 26 cPs. The viscosity of PVOH can be from about 1.0 cPs to about 30.0 cPs, for example, about 1 cPs, 1.5 cPs, 2 cPs, 2.5 cPs, 3 cPs, 3.5 cPs, 4 cPs, 4.5 cPs, 5 cPs, 5.5 cPs, 6 cPs, 6.5 cPs, 7 cPs, 7.5 cPs, 8 cPs, 8.5 cPs, 9 cPs, 9.5 cPs, 10 cPs, 1 The viscosity of the PVOH resin may be about 21-26 cPs. The viscosity of the PVOH resin may be about 5 cPs to about 14 cPs.
[0064] The first water-soluble resin and the second water-soluble resin may each have a weight average molecular weight, and the weight average molecular weight of the first water-soluble resin may be greater than the weight average molecular weight of the second water-soluble resin. Alternatively, the first water-soluble resin and the second water-soluble resin may each have a number average molecular weight, and the number average molecular weight of the first water-soluble resin may be greater than the number average molecular weight of the second water-soluble resin.
[0065] As used herein, the degree of hydrolysis of a polyvinyl alcohol homopolymer or copolymer is expressed as the molar percentage of vinyl acetate units converted into vinyl alcohol units. The degree of hydrolysis (DH) of the polyvinyl alcohol homopolymer or copolymer comprising the first or second water-soluble resin may be independently at least about 70%, 80%, 84% or 85% and up to about 99% or 99.9%, for example, between about 70% and about 99.9%, between about 75% and about 95%, between about 85% and about 88%, between about 88% and about 90%, between about 84% and about 89%, between about 85% and about 99.7%, between about 85% and about 99.9%, between about 86% and about 88%, between about 89% and about 81%, between about 80% and about 81%, between about 82% and about 83%, between about 84% and about 85%, between about 86% and about 83%, between about 85 ... The degree of hydrolysis is in the range of about 95%, about 87% to about 98%, about 89% to about 99%, or about 90% to about 99%, such as about 75%, 76%, 77%, 78%, 79%, 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98% or 99%. Although the degree of hydrolysis is specifically a measure of the amount of acetate removed from the polyvinyl acetate polymer (e.g., by hydrolysis or saponification), it is most commonly used to understand the amount of acetate remaining on the PVOH polymer or copolymer. The acetate groups form the amorphous or non-crystalline regions of the PVOH copolymer. Therefore, it can be approximately stated that the higher the DH, the higher the crystallinity of the PVOH copolymer or the blend of PVOH copolymers. When a PVOH resin is described as having (or not having) a particular DH, it is intended that the specified DH is the average DH of the PVOH resin, unless otherwise specified.
[0066] The first water-soluble resin and the second water-soluble resin may independently include a PVOH homopolymer, a PVOH copolymer, or a blend thereof, and a hydrolysis degree of the first water-soluble resin may be greater than or equal to a hydrolysis degree of the second water-soluble resin.
[0067] The water-soluble resin of any layer of the multilayer film of the present disclosure can include PVOH copolymer, and the copolymer can be anion-modified polyvinyl alcohol, i.e., a PVOH copolymer comprising a partial or complete hydrolysis of anionic monomer units. Anion-modified polyvinyl alcohol can be a PVOH terpolymer, comprising vinyl alcohol monomer units, vinyl acetate monomer units (i.e., when not completely hydrolyzed) and a single type of anionic monomer units (e.g., wherein the single type of monomer units can include an equivalent acid form, salt form and optionally ester form of anionic monomer units). Optionally, the first water-soluble resin can include anion-modified polyvinyl alcohol. Optionally, the second water-soluble resin can include anion-modified polyvinyl alcohol. The general classification of anionic monomer units that can be used for PVOH copolymers includes vinyl polymerization units corresponding to monocarboxylic acid vinyl monomers, their esters and anhydrides, dicarboxylic acid monomers with polymerizable double bonds, their esters and anhydrides, and any of the alkali metal salts of the foregoing. Examples of suitable anionic monomer units include vinyl polymerized units derived from vinyl anionic monomers including, but not limited to, vinyl acetic acid, maleic acid, monoalkyl maleates, dialkyl maleates, maleic anhydride, fumaric acid, monoalkyl fumarate, dialkyl fumarate, itaconic acid, monoalkyl itaconate, dialkyl itaconate, itaconic anhydride, citraconic acid, monoalkyl citraconic acid, dialkyl citraconic acid, citraconic anhydride, mesaconic acid, monoalkyl mesaconic acid, dialkyl mesaconic acid, glutaconic acid, monoalkyl glutaconate, dialkyl glutaconate, glutaconic anhydride, alkyl acrylate, methyl acrylate, vinyl sulfonic acid, alkali metal salts of the foregoing, esters of the foregoing, and combinations of the foregoing. The anionic monomer units may be derived from monomers selected from the group consisting of vinylacetic acid, alkyl acrylates, maleic acid, monoalkyl maleates, dialkyl maleates, monomethyl maleates, dimethyl maleates, maleic anhydride, fumaric acid, monoalkyl fumarate, dialkyl fumarate, monomethyl fumarate, dimethyl fumarate, itaconic acid, monomethyl itaconate, dimethyl itaconate, itaconic anhydride, citraconic acid, monoalkyl citraconic acid, dialkyl citraconic acid, citraconic anhydride, mesaconic acid, monoalkyl mesaconic acid, dialkyl mesaconic acid, pentane Gluconic acid, monoalkyl glutaconate, dialkyl glutaconate, glutconic anhydride, vinyl sulfonic acid, alkyl sulfonic acid, vinyl sulfonic acid, 2-acrylamido-1-methylpropanesulfonic acid, 2-acrylamido-2-methylpropanesulfonic acid (AMPS), 2-methacrylamido-2-methylpropanesulfonic acid, 2-sulfoethyl acrylate, hydrolyzed N-vinyl pyrrolidone, alkali metal salts of the foregoing, esters of the foregoing, and combinations of the foregoing (e.g., multiple types of anionic monomer units or equivalent forms of the same anionic monomer unit).
[0068] When the water-soluble resin includes a PVOH copolymer, the degree of modification of the PVOH copolymer is not particularly limited. For example, the amount of the degree of modification of the PVOH copolymer can be in the following range: about 0.5 mol.% to about 10 mol.%, or about 1 mol.% to about 10 mol.%, about 1 mol.% to about 8 mol.%, about 1 mol.% to about 5 mol%, about 2 mol.% to about 6 mol.%, about 3 mol.% to about 5 mol.%, or about 1 mol.% to about 3 mol.% (e.g., at least about 1.0 mol.%, 1.5 mol.%, 1.8 mol.%, 2.0 mol.%, 2.5 mol.%, 3.0 mol.%, 3.5 mol.% or 4.0 mol.% and at most about 3.0 mol.%, 4.0 mol.%, 4.5 mol.%, 5.0 mol.%, 6.0 mol.%, 8.0 mol.% or 10 mol.%).
[0069] It is understood in the art that the PVOH copolymer (e.g., maleate-modified PVOH) with a pendant carboxyl group can form a lactone ring between adjacent pendant carboxyls and an alcohol group, thereby reducing the water solubility of the PVOH copolymer resin. In the presence of a strong base, the lactone ring can be opened in a process of several weeks under relatively warm (environment) and high humidity conditions (e.g., by the lactone ring opening reaction to form corresponding pendant carboxyls and an alcohol group, while water solubility improves). Therefore, it is believed that due to the chemical interaction between the alkaline composition in the film and the bag during storage, such PVOH copolymer films can become more soluble. Maleate-modified PVOH can be substantially free of lactone rings, so that every maleate monomer unit of modified PVOH has about 2 pendant carboxylate groups. The maleate-modified PVOH may include from about 1.5 pendant carboxylate groups to 2 pendant carboxylate groups per maleate monomer unit, or from about 1.2 pendant carboxylate groups to about 2 pendant carboxylate groups per maleate monomer unit, or from about 1 pendant carboxylate groups to about 2 pendant carboxylate groups per maleate monomer unit, such as about 2 pendant carboxylate groups per maleate monomer unit, or about 1.9 pendant carboxylate groups per maleate monomer unit, or about 1.8 pendant carboxylate groups per maleate monomer unit, or about 1.7 pendant carboxylate groups per maleate monomer unit, or about 1.6 pendant carboxylate groups per maleate monomer unit, or about 1.5 pendant carboxylate groups per maleate monomer unit, or about 1.2 pendant carboxylate groups per maleate monomer unit, or about 1 pendant carboxylate group per maleate monomer unit.
[0070] Each layer of the multilayer film of the present disclosure may further include one or more water-soluble polymers, including but not limited to: polyvinyl alcohol; water-soluble acrylate copolymers; polyethylene imine; pullulan; water-soluble natural polymers, including but not limited to guar gum, gum Acacia, xanthan gum, carrageenan and starch; water-soluble polymer modified starch; copolymers of the foregoing; or a combination of any of the foregoing. Other water-soluble polymers may include polyalkylene oxides, polyacrylamide, cellulose, cellulose ethers, cellulose esters, cellulose amides, polyvinyl acetates, polycarboxylates and salts thereof, polyamino acids, polyamides, gelatin, methylcellulose, carboxymethylcellulose and salts thereof, dextrin, ethylcellulose, hydroxyethylcellulose, hydroxypropyl methylcellulose, maltodextrin, polymethacrylates or a combination of any of the foregoing. Such water-soluble polymers are commercially available from various sources.
[0071] For each layer of the multilayer film, the water-soluble resin comprising the layer may further include a second PVOH resin. The second PVOH resin may include a PVOH homopolymer, a PVOH copolymer, or a combination thereof. The second PVOH may include a PVOH copolymer including anionic monomer units as described above. The second PVOH may include anionic monomer units selected from the following groups: AMPS, hydrolyzed N-vinyl pyrrolidone (NVP), maleic anhydride, monomethyl maleate, its alkali metal salts, and combinations thereof. The second PVOH may include anionic monomer units selected from the following groups: maleic acid monoesters, maleic anhydride, its alkali metal salts, and combinations thereof.
[0072] In addition to the water-soluble resin, each layer of the multilayer film may optionally contain one or more additional agents in an amount suitable for its intended purpose, including but not limited to plasticizers, surfactants, lubricants, release agents, fillers, extenders, cross-linking agents, anti-blocking agents, detackifiers, defoaming agents, nanoparticles (such as nanoclays of the layered silicate type), bleaching agents, antioxidants, aversive agents (such as bittering agents, pungency agents), other functional ingredients, and combinations of the foregoing.
[0073] Each layer of the multilayer film can independently include any suitable plasticizer.Plasticizer is liquid, solid or semisolid, which is added to a material (usually a resin or elastomer) to make the material softer, more flexible (by reducing the glass transition temperature of the polymer) or easier to process.In addition or alternatively, the polymer can be internally plasticized by chemically modified polymers or monomers.The water-soluble film described herein may include one or more plasticizers.Plasticizers may include glycerol, diglycerol, sorbitol, ethylene glycol, diethylene glycol, triethylene glycol, dipropylene glycol, tetraethylene glycol, propylene glycol, polypropylene glycol, polyethylene glycol of up to 400Da molecular weight, hexylene glycol, neopentyl glycol, trimethylolpropane, polyether polyol, polyether diol, polyether triol, xylitol, 2-methyl-1,3-propanediol Ethanolamine, glycerol propylene oxide polymer (e.g., Voranol available from The Dow Chemical Company) TM ) or mixtures thereof. Lower levels (e.g., 1 wt.% to 10 wt.%) of low molecular weight polar plasticizers, such as glycerol and / or trimethylolpropane, may be included as a means of maintaining flexibility and the ability to be converted into articles using standard equipment.
[0074] When the layer of the multilayer film includes a plasticizer, the following range of plasticizer can be provided, based on the total weight of the water-soluble resin in the layer: about 1wt.% to about 45wt.%, or about 5wt.% to about 35wt.%, or about 7.5wt.% to about 30wt.%, or about 8wt.% to about 20wt.%, or about 8wt% to about 12wt%, such as about 1wt.%, 5wt.%, 7.5wt.%, 9wt%, 10wt.%, 15wt.%, 17.5wt% or 25wt.%. The amount of the plasticizer can also be characterized in units of phr, and each layer can include the following amount of plasticizer: about 2phr to about 75phr, about 3phr to about 60phr, about 3phr to about 50phr, about 4phr to about 40phr or about 2phr to about 20phr.
[0075] Without intending to be bound by theory, it is believed that a plasticizer can be selected to balance the maintenance of flexible film and active chemicals migrate into the film matrix. Further, without intending to be bound by theory, it is believed that as the film plasticizes, the ability of active chemicals to migrate into the film increases. Without intending to be bound by theory, it is believed that the closer the glass transition temperature of the film is to the low end of the operating temperature range, the higher the resistance of the film to chemical migration into the film. Therefore, the type and amount of plasticizer can be selected to provide a film with a glass transition temperature close to the low end of the operating temperature range. As used herein, "operating temperature range" refers to the temperature to which the film is exposed during the life cycle of the film (e.g., the storage of the film and the use of the film by consumers). In general, the operating temperature range is not limited, and can generally be in the range of about 0°C to about 40°C or about 5-10°C to about 38-40°C.
[0076] Each layer may optionally contain other adjuvants and treatment agents in an amount suitable for its intended purpose, including but not limited to surfactants, lubricants, mold release agents, fillers, extenders, cross-linking agents, anti-blocking agents, detackifiers, anti-foaming agents (defoamers), nanoparticles (such as layered silicate nanoclays (e.g., sodium montmorillonite)), bleaching agents (e.g., sodium metabisulfite, sodium bisulfate (SBS) or others), aversive agents (such as bittering agents (e.g., denatonium salts, such as denatonium benzoate, denatonium sugar and denatonium chloride; sucrose octaacetate; quinine; flavonoids, such as quercetin and naringenin; and quasinoids, such as quasin and strychnine) and pungent agents (e.g., capsaicin, piperine, allyl isothiocyanate and resinferatoxin) and other functional ingredients. For example, each layer may contain fillers, surfactants, anti-blocking agents, or combinations of the foregoing.
[0077] The surfactant used in the water-soluble film is well known in the art. Optionally, a surfactant is included to help the resin solution disperse when casting. Suitable surfactants can include nonionic, cationic, anionic and zwitterionic surfactants. The surfactants suitable for each layer of the multilayer film can include but are not limited to polyoxyethylene polyoxypropylene glycol, alcohol ethoxylate, alkylphenol ethoxylate, tertiary acetylenic glycol, alkanolamide, polyoxyethylene amine, quaternary ammonium salt, quaternized polyoxyethylene amine, amine oxide, N-alkyl betaine and sulfobetaine. The surfactant that is suitable for each layer of multilayer film can also include but is not limited to dialkyl sulfosuccinate, lactic acid ester of glycerol and propylene glycol, lactic acid ester, sodium alkyl sulfate, polysorbate 20, polysorbate 60, polysorbate 65, polysorbate 80, alkyl polyethylene glycol ether, lecithin, acetylated fatty acid ester of glycerol and propylene glycol, sodium lauryl sulfate, acetylated ester of fatty acid, myristyl dimethylamine oxide, trimethyl tallow alkyl ammonium chloride, quaternary ammonium compound, its salt and the combination of any item in the foregoing. Surfactant is too little sometimes may cause hole on film, and surfactant is too much may cause excessive surfactant to exist on the surface of film and produce greasy feeling or oily feeling. Therefore, for example, surfactant can be optionally included in water-soluble film with following amount: less than about 2phr, for example, less than about 1phr or less than about 0.8phr.
[0078] One secondary component contemplated for use is a defoamer. Defoamers can help foam bubbles coalesce. Defoamers suitable for use in a layer of a multilayer film according to the present disclosure include, but are not limited to, hydrophobic silica, such as finely divided silicon dioxide or fumed silica, including Foam available from Emerald Performance Materials. Defoamers, including Foam 327. Foam UVD、Foam 163. Foam 269. Foam 338. Foam 290. Foam 332. Foam 349. Foam 550 and Foam 339, which are proprietary non-mineral oil defoamers. For example, the layers of the multilayer film disclosed herein include Foam 338. Optionally, the defoaming agent may be used in an amount of 0.5 phr or less, or 0.5 phr to 0.01 phr, for example, 0.3 phr, 0.2 phr, 0.1 phr, 0.05 phr, 0.04 phr, 0.03 phr, 0.02 phr or 0.01 phr.
[0079] Suitable fillers, extenders and detackifiers include, but are not limited to, starch, modified starch, cross-linked polyvinyl pyrrolidone, cross-linked cellulose, microcrystalline cellulose, silicon dioxide, metal oxides, calcium carbonate, talc, mica, stearic acid and its metal salts (e.g., magnesium stearate). Preferred materials are starch, modified starch and silicon dioxide, such as high amylose starch, amorphous silicon dioxide, hydroxyethylated starch or a combination thereof.
[0080] The aversive agent may be incorporated into each layer of the multilayer film or may be applied as a coating to the multilayer film. The aversive agent may be added in an amount that causes an aversive response (e.g., bitter taste), diluted from its commercial form or otherwise mixed with a solvent for mixing with other water-soluble film components or applied as a coating to a water-soluble film. Such solvents may be selected from water, low molecular weight alcohols (methanol, ethanol, etc.), or plasticizers disclosed herein.
[0081] Antiblocking agents (e.g., silicon dioxide and / or stearic acid) may optionally be present in any layer of the multilayer film of the present disclosure in an amount of at least 0.1 phr, or at least 0.5 phr, or at least 1 phr, or in the range of about 0.1 phr to 8.0 phr, or about 0.1 phr to about 5.0 phr, or about 0.4 phr to 3.0 phr, or about 0.5 phr to about 2.0 phr, or about 0.5 phr to about 1.5 phr, or 0.1 phr to 1.2 phr, or 0.1 phr to 2.7 phr, for example, 2.0 phr, 2.8 phr, 3.6 phr, 5.0 phr, or 7.2 phr. The amount of antiblocking agents in any layer of the multilayer film of the present disclosure may also be expressed as a percentage of the total weight of the layer. The first layer of the multilayer water-soluble film according to the present disclosure may include an anti-blocking agent in an amount ranging from about 2% to about 10%, or from about 3% to about 8%, or from about 3.5% to about 6.5%, or from about 4% to about 6%, based on the total weight of the first layer. Optionally, the second layer of the film according to the present disclosure may be substantially free of anti-blocking agents or free of anti-blocking agents.
[0082] Suitable median particle sizes for the antiblocking agent include median sizes in the range of about 3 or about 4 microns to about 11 microns, or about 4 to about 8 microns, or about 5 to about 6 microns, such as 5 microns, 6 microns, 7 microns, or 8 microns. Suitable silica is an untreated synthetic amorphous silica designed for use in aqueous systems.
[0083] The multilayer film described herein can have any suitable thickness. For example, the thickness of the multilayer film can be in the following range: about 15 microns (μm) to about 150 μm, or about 25 μm to about 100 μm, or about 30 μm to about 70 μm, or about 40 μm to about 60 μm. For example, the thickness of the water-soluble film can be about 40 μm, 45 μm, 50 μm, 51 μm, 60 μm, 76 μm or 88 μm. The thickness of the multilayer film can be in the following range: about 25 μm to about 100 μm, or about 40 μm to about 100 μm, or about 30 μm to about 70 μm. In addition, each layer of the multilayer film can have any suitable thickness. For example, the thickness of each layer of the water-soluble film can be in the following range: about 1 micron to about 100 microns, or about 5 μm to about 90 μm, or about 10 μm to about 80 μm, or about 20 μm to about 70 μm, or about 30 μm to about 50 μm, such as about 1 μm, 2 μm, 3 μm, 5 μm, 10 μm, 20 μm, 30 μm, 40 μm, 45 μm, 50 μm, 51 μm, 60 μm, 76 μm or 88 μm. The thickness of the first layer can be in the range of about 1 μm to about 5 μm, and the thickness of the second layer can be in the range of about 40 μm to about 75 μm. The relative thickness of the layer comprising the multilayer film is not particularly limited. For example, the thickness ratio of the first layer to the second layer of the multilayer film of the present disclosure can be in the range of about 1:200 to about 200:1, or about 1:100 to 100:1, or about 1:20 to about 20:1, or about 1:5 to about 5:1, or about 1:2 to 2:1, or about 1:1.
[0084] The multilayer film produced by the simultaneous solution co-casting method according to the present disclosure may include a layer including a foam film, i.e., a film layer including multiple macroscopic voids and / or microscopic voids. The top layer of the simultaneous co-cast multilayer film may be a foam film layer. The simultaneous co-cast multilayer film may be a double-layer film, the top layer of which includes a foam film. The foam film layer may be produced by casting a layer of foamed resin solution (i.e., a resin solution in which air or another gas is already entrained) and drying the foamed resin solution layer to provide a film layer containing multiple macroscopic voids and / or microscopic voids. The foamed resin solution may be formed by fully mixing the resin solution to entrain air. Alternatively, during the simultaneous solution co-casting method, the foamed resin solution may be formed by online mixing. For example, the resin solution may be mixed in an online mixing device placed downstream of a storage tank containing the resin solution and upstream of a casting surface on which the resin solution layer is cast, so that when the solution is fed to the casting surface, air or another gas is entrained in the resin solution. Optionally, in-line mixing may also include mixing the resin solution with a separate gas feed to entrain the gas in the resin solution.
[0085] The multilayer film may include a layer including a foam film. The foam layer may be cast on an already formed film (a film prepared by any method), and this may be referred to as overcasting. The foam layer may be cast on a film just formed by the same method, and this may be referred to as sequential casting. The top layer of the multilayer film may be a foam film layer. The sequentially cast multilayer film may be a double-layer film, the top layer of which includes a foam film layer, i.e., a layer in which the foam film layer is cast on a lower substrate layer. The sequential casting method for forming a double-layer film having a layer of foam film may include: casting a layer of a second resin solution onto a casting surface by any suitable means to form a second (bottom) resin solution layer; at least partially drying the second resin solution layer; directly casting a first (top) resin solution onto the at least partially dried second resin solution layer, wherein the first resin solution is a foam resin solution; and drying the resulting multilayer composition to form a multilayer film. The resin solution may be cast according to a solution casting method known in the art. The lower substrate layer may be a film prepared by any method, such as a cast film or a blown film. The second resin solution may be cast using a die such as a slot die; and the first resin solution may be cast using any suitable method (eg, a doctor blade apparatus), or may be cast.
[0086] The top layer and bottom layer of the double-layer film including the top layer as the foam film layer can independently include PVOH homopolymer, PVOH copolymer or its blend. Optionally, the foam film layer can include an anion-modified PVOH copolymer. Optionally, the bottom layer can include an anion-modified PVOH copolymer. Optionally, both the foam film layer and the bottom layer can include an anion-modified PVOH copolymer, wherein the foam film layer and the bottom layer can optionally include the same anion-modified PVOH copolymer.
[0087] Casting a layer of a foamed resin solution (i.e., a resin solution in which air or another gas has been entrained) can provide a foamed film layer containing macrovoids and / or microvoids after drying. The foamed film layer can be characterized by the entrained gas fraction, i.e., the percentage by which the volume of the foamed film layer is increased relative to the volume of the same film prepared from the same amount of the same resin solution that has not been foamed (i.e., not fully mixed to entrain air or another gas). The entrained gas fraction of the foamed film layer of the water-soluble film according to the present disclosure can be at least about 5 vol%, or at least about 10 vol%, or at least about 20 vol%, or at least about 30 vol%, based on the volume of the second layer.
[0088] The water-soluble film according to the present disclosure may include a first layer and a second layer, wherein the first layer includes a methacrylate-modified PVOH copolymer, a plasticizer, an antiblocking agent, and a surfactant, and the second layer includes a blend of a maleate-modified PVOH copolymer and a monomethyl maleate-modified PVOH copolymer, wherein the first layer and the second layer are present in the following ratio based on the total weight of the water-soluble film: about 1:200 to about 1:1, or about 1:100 to about 1:3, or about 1:20 to about 1:5. The film according to this aspect may exhibit a haze % of less than about 50, as determined by the haze test described herein, and the static friction coefficient between the first portion and the second portion of the outer surface of the first layer is less than about 2, as determined by the friction coefficient test described herein.
[0089] The water-soluble film according to the present disclosure may include a first layer and a second layer, wherein the first layer includes a blend of a PVOH copolymer modified with monomethyl maleate and a PVOH homopolymer, and the second layer includes a blend of a polyvinyl alcohol homopolymer, wherein the first layer and the second layer are present in the following ratios, respectively, based on the total weight of the water-soluble film: from about 1:200 to about 1:1, or from about 1:100 to about 1:3, or from about 1:20 to about 1:5. The film according to this aspect may exhibit less than 25 g H2O / m 2 / day Moisture Vapor Transmission Rate as measured by the Moisture Vapor Transmission Rate Test Method described herein; and a heat seal strength of at least 15N as measured by the Seal Strength Test described herein.
[0090] Further provided herein is a water-soluble unit dose product comprising a package comprising an outer wall having an outer surface and an inner surface defining an inner bag volume, the outer wall comprising a multilayer water-soluble film as disclosed herein and optionally a composition contained in the inner bag volume.
[0091] The composition contained in the inner bag volume can be a fabric or home care composition, such as one of the compositions described above in conjunction with the multi-compartment article. The water-soluble unit dose article can include a non-home care composition. The non-home care composition can be selected from agricultural compositions, aviation compositions, food and nutrient compositions, industrial compositions, livestock compositions, marine compositions, medical compositions, trade compositions, military and paramilitary compositions, office compositions, recreational and park compositions, pet compositions, pools and / or water treatment compositions, and combinations thereof. The non-home care composition can be a pool and / or water treatment composition.
[0092] The water-soluble unit dose preparation may include a home care composition. The home care composition may be selected from light duty liquid detergent compositions, heavy duty liquid detergent compositions, hard surface cleaning compositions, laundry detergent gels, bleaching compositions, laundry additives, fabric enhancer compositions, shampoos, body washes, other personal care compositions, and combinations thereof, optionally liquid laundry detergent compositions.
[0093] In another aspect of the present disclosure, the home care composition may be selected from the group having laundry and automatic dishwashing detergent compositions, including liquid laundry detergent compositions.
[0094] In another aspect of the present disclosure, the home care composition can be selected from non-laundry and non-automatic dishwashing compositions, for example selected from the group consisting of light-duty liquid detergent compositions, heavy-duty liquid detergent compositions, hard surface cleaning compositions, bleaching compositions, shampoos, body washes, other personal care compositions, and other compositions that are non-laundry and non-automatic dishwashing compositions or mixtures of any of the foregoing.
[0095] The term 'liquid laundry detergent composition' refers to any laundry detergent composition comprising a liquid capable of wetting and treating fabrics, and includes but is not limited to liquids, gels, pastes, dispersions, etc. Liquid compositions may contain solids or gases in appropriately finely divided form, but liquid compositions exclude generally non-fluid forms such as tablets or granules.
[0096] Liquid detergent compositions can be used in hand fabric washing operations, or can be used in automatic machine fabric washing operations.
[0097] In other aspects, the household care composition can be an automatic dishwashing detergent composition comprising ingredients selected from the group consisting of surfactants, builders, sulfonated / carboxylated polymers, silicone foam suppressors, silicates, metal and / or glass care agents, enzymes, bleaches, bleach activators, bleach catalysts, alkalinity sources, fragrances, dyes, solvents, fillers, and mixtures thereof.
[0098] The home care composition may include one or more acids for adjusting the pH of the solution to an acidic pH. The home care composition may include one or more acids, including but not limited to glycolic acid, citric acid, acetic acid, hydrochloric acid, levulinic acid, gluconic acid, and the like. The pH of the home care composition may be less than or equal to 3. The pH of the home care composition may be less than or equal to 2.5. The pH of the home care composition may be less than or equal to 2. The pH of the home care composition may be less than or equal to 1.5.
[0099] The water-soluble unit dose preparation may include the following concentration range of acid, oxidant, base or combination thereof: 50 wt% to 100 wt%, or 60 wt% to 100 wt%, or 70 wt% to 100 wt%, or 80 wt% to 100 wt%, or 90 wt% to 100 wt%, based on the total weight of the composition contained in the water-soluble unit dose preparation. The concentration of acid, oxidant, base or combination thereof in the non-home care composition of the water-soluble unit dose preparation is in the following range: 50 wt% to 100 wt%, or 60 wt% to 100 wt%, or 70 wt% to 100 wt%, or 80 wt% to 100 wt%, or 90 wt% to 100 wt%, based on the total weight of the non-home care composition.
[0100] Optionally, after exposure to TCCA, SBS or calcium hypochlorite compositions in an atmosphere of 38°C and 80% RH for 6 or 8 weeks, the water-soluble unit dose preparations of the present disclosure are characterized by a disintegration time of no more than 300 seconds in 23°C water according to MSTM 205. The disintegration time can be controlled by selecting the film thickness, and the resistance of the film to such harsh chemicals can be mitigated, for example, by including an antioxidant.
[0101] After exposure to TCCA, SBS or calcium hypochlorite compositions in an atmosphere of 38°C and 80% RH for 6 or 8 weeks, the surface area of the residue of the water-soluble unit dose product after testing in 23°C water according to MSTM 205 can be less than about 50% of the surface area of the water-soluble unit dose before testing according to MSTM 205.
[0102] The water-soluble unit dose product can be provided in any size suitable for fitting through the neck of a push-on spray bottle (e.g., a spray bottle having a screw cap neck with a diameter of about 28 mm). The length of the water-soluble unit dose product can optionally be about 250 mm or less, or in the following range: about 5 mm to about 250 mm, about 10 mm to about 250 mm, about 25 mm to about 250 mm, about 50 mm to about 225 mm, about 100 mm to about 225 mm, about 150 to about 225 mm, about 175 mm to about 225 mm, or about 200 mm. The width of the water-soluble unit metering product can optionally be about 50 mm or less, or in the following range: about 2 mm to about 50 mm, about 5 mm to about 45 mm, about 10 mm to about 40 mm, about 15 mm to about 35 mm, or about 20 mm to about 30 mm. The length of the water-soluble unit dose article can be from about 175 mm to about 225 mm or about 200 mm, and its width can be from about 20 mm to about 30 mm or about 25 mm. In embodiments where the water-soluble unit dose article is provided to fit through the neck of a snap-on spray bottle, the water-soluble unit dose article optionally comprises a home care composition having a pH of less than or equal to 2.
[0103] The water-soluble unit dose article can be heat-sealed or solution-sealed by any suitable method and apparatus (such as methods and apparatus well known in the art). For example, the water-soluble unit dose article can be heat-sealed on three sides. For example, the water-soluble film can be folded onto itself and sealed with a heat pulse sealer on the edge opposite to the fold and along one of the two remaining opening edges to provide a bag of desired size. Liquid compositions (e.g., home care compositions) can be filled into the bag using injection systems such as pumps or syringes. Optionally, the water-soluble film can be stretched on a cavity of a specified size, and heat and vacuum can be applied to form the film into the shape of the cavity. Then, the cavity can be filled with the desired composition (e.g., home care compositions). Then, the filled bag can be sealed with a second film. The second film can be pulled to the top of the cavity, and the side of the second film facing the filled bag can be moistened to perform solution sealing. Pressure can be applied, and the filled bag is bonded to the second film around the forming cavity to form an encapsulated composition in the water-soluble unit dose article. Solution sealing can be achieved using a Mespack-Cloud sampler, etc.
[0104] Further provided herein is a method for dosing a bulk water composition, the method comprising the steps of contacting a water-soluble unit dose product as described herein with bulk water, thereby dissolving at least a portion of the water-soluble film and releasing the composition into the bulk water.
[0105] In general, the bulk water can be any bulk water in which the non-home care composition is to be provided. For example, the bulk water can be a pool or spa. In general, the temperature of the bulk water can be any temperature sufficient to dissolve or disintegrate at least a portion of the water-soluble film. The temperature of the bulk water can be at least about 10°C, for example, in the range of about 10°C to about 100°C, about 10°C to about 70°C, about 10°C to about 60°C, about 20°C to about 50°C, or about 20°C to about 40°C. In general, the bulk water can be characterized by any pH value. For example, the pH of the bulk water can be in the range of about 4 to about 10, about 5 to about 9, or about 6 to about 7.
[0106] Method for preparing membrane
[0107] Methods for producing PVOH films by solution casting are well known in the art. Typically, PVOH polymers and secondary additives are dissolved in a solvent (usually water) to form a resin solution, and the solution is metered onto a casting surface and allowed to substantially dry or forced dry with heated air to form a cast film. The resulting cast film is removed from the casting surface and optionally wound onto a roll. The process can be performed in batches and is more efficient when performed as a continuous process.
[0108] When forming continuous film web, conventional practice is to meter the solution of resin and secondary component to moving casting surface, such as continuously moving metal cylinder or belt, then make solvent be removed substantially from liquid, thus form self-supporting casting film, and then peel off gained casting film from casting surface.Solution can be optionally metered or coated on carrier film, release liner or removable backing, thus after removing solvent, gained casting film or coating can be separated (for example, immediately separated after drying or at a later time point (for example before use) separation) with carrier film, release liner or removable backing, or remain attached to carrier film, release liner or removable backing.Film or coating prepared on carrier film, release liner or removable backing can be self-supporting or non-self-supporting.Such carrier film, release liner and removable backing can be prepared by various materials known in the art, such as polyethylene, polyethylene oxide, polyethylene terephthalate, polyolefin, oriented polypropylene, polytetrafluoroethylene, polyvinyl chloride and cross-linked polyvinyl alcohol.
[0109] In general, the casting surface can be any suitable substrate known to those skilled in the art for producing polymer films. The substrate can be a casting roll or drum, a casting belt or a combination thereof. As used herein, the substrate is used to produce a polymer film with one or more polymer resins or polymer resin solutions. The substrate includes a substrate surface, and the substrate surface can be coated with a peel coating. The polymer resin solution can be cast onto the substrate while the substrate moves (e.g., rotates). The substrate can include stainless steel, and optionally can have a stainless steel surface. The substrate can include stainless steel, and the stainless steel is optionally plated, such as chrome plating, nickel plating, zinc plating or a combination thereof.
[0110] According to the multilayer film disclosed herein, a solvent belt casting system can be used to produce. The system can include a tank for mixing and / or storing a variety of water-soluble resin solutions, each of which has an optional secondary additive for use with a belt casting machine, and the belt casting machine has at least a first and a second rotating cylinder, and the casting surface around the at least first and second rotating cylinders is tensioned to travel with the rotation of the cylinder. The multi-groove mold can be used to cast one or more resin solutions from the tank at the same time to form a multilayer solution composition on the casting surface. When the multilayer solution composition travels on the casting surface with a thin sheet, the drying chamber of at least a part of the casting surface under the closed mold is used to remove the solvent from the multilayer solution composition. In addition, a release coating can be applied to the casting surface to provide one or more advantages for the film and / or method. For example, the release coating can greatly reduce or eliminate bubbles in the multilayer film produced, or the release coating can improve the ease of releasing the produced film from the casting surface. A roll coater release coating applicator connected to a portion of the release coating supply and the belt can transfer the fluid release coating to the casting surface before the resin solution is applied to the belt. Suitable solvent tape casting systems and related materials are further described in U.S. Patent Application Publication Nos. 2006 / 0081176A1 and 2007 / 0085234A1, the disclosures of which are incorporated herein by reference in their entireties.
[0111] In general, the release coating may include one or more surfactants and an optional carrier, such as water. The release coating may include one or more surfactants, such as one or more surfactants selected from fluorinated surfactants, non-fluorinated anionic surfactants or non-fluorinated zwitterionic surfactants, salts thereof or any combination thereof. The anionic or zwitterionic surfactant may be non-fluorinated and include C6-C 30 Phosphate, C6-C 30 Phosphate diester, C6-C 30 Carboxylic acid ester, C6-C 30 Dicarboxylic acid esters, C6-C 30 Sulfate, C6-C 30 The stripping coating may include a non-fluorinated zwitterionic surfactant or a salt thereof. The stripping coating may include a non-fluorinated anionic surfactant or a salt thereof. The non-fluorinated anionic surfactant may include a C6-C 30 Phosphate or C8-C 16 Phosphate, C6-C 60 Phosphate diester, C 16 -C 32 Phosphate diester, C6-C 30 Carboxylic acid ester, C6-C 30 Dicarboxylic acid esters, C6-C 30Sulfate, C6-C 30 Disulfate or its salt. Non-fluorinated anionic surfactants may include C6-C 30 Phosphate or C6-C 18 Phosphate, C6-C 60 Phosphate diester, C 18 -C 32 Phosphate diester or its salt. The anionic surfactant may include one or more of the following: C6-based fluoroaliphatic ammonium phosphate; tridecyl alcohol ethoxy phosphate POE-12; tridecyl alcohol ethoxy phosphate POE-3; laureth-11 carboxylic acid; crypto-anionic surfactant-laureth-6 carboxylic acid; or sodium laureth sulfate POE-4.
[0112] As used herein, the term "non-fluorinated" refers to surfactants having less than 0.01 wt % fluorine based on the total molecular weight of the compound, or less than 0.001 wt % fluorine based on the total molecular weight of the compound, or less than 0.0001 wt % fluorine based on the total molecular weight of the compound.
[0113] The stripping coating can include a fluorosurfactant, such as a compound containing a perfluoroalkyl group. The fluorosurfactant can include a solution of a ZONYL FSP surfactant (EI du Pont de Nemours and Company). The range of surfactants in the stripping coating is considered to be about 0.05% by weight to about 5.0% by weight. The amount of surfactant required to provide sufficient wetting can vary depending on the film coated on the band. Other products may require higher concentrations to improve stripping performance. Before the surfactant solution reaches the critical micelle concentration (CMC), the higher the concentration of the surfactant, the more efficient the hard surface spreading wetting will be. This concentration represents a threshold value, and beyond the threshold value, other surfactants will not produce any further efficiency in terms of spreading wetting. However, increasing the concentration to more than the CMC may improve the wetting performed by the polymer solution, and improve the stripping performance of some film formulations.
[0114] The release coating can be applied to the surface of the substrate and optionally subsequently dried before the polymer resin or polymer resin solution is cast onto the surface-coated substrate. Before the release coating on the substrate surface is dried, the pH of the release coating when applied to the surface of the substrate can be from about 1 to about 5. When the surfactant includes a non-fluorinated anionic surfactant, a non-fluorinated zwitterionic surfactant, a salt thereof, and a combination thereof, before the release coating on the substrate surface is dried, the pH of the release coating when applied to the surface of the substrate can be from about 1 to about 8, or a pH of about 1 to about 5. For example, the pH of the release coating when applied to the surface of the substrate can be about 1, about 1.5, about 2, about 2.5, about 3, about 3.5, about 4, about 5, about 6, about 7, or about 8. The pH of the release coating when applied to the surface of the substrate can be from about 1 to about 7, or from about 1 to about 6, or from about 1 to about 4, or from about 1 to about 3, or from about 2 to about 7, or from about 2 to about 6, or from about 2 to about 5, or from about 2 to about 4, or from about 2 to about 3, or from about 3 to about 7, or from about 3 to about 5, or from about 1.5 to about 3.5, or from about 4 to about 7, before drying the release coating on the surface of the substrate.
[0115] In general, based on the total weight of the peeling coating, the surfactant concentration of the peeling coating can be in the range of about 0.001wt% to about 100wt%. Before the peeling coating on the substrate surface is dried, the surfactant concentration of the peeling coating can be in the range of about 0.001wt% to about 20wt%. For example, before the peeling coating on the substrate surface is dried, the surfactant concentration of the peeling coating can be in the following range: about 0.001wt% to about 10wt%, or about 0.01wt% to about 5wt%, or about 0.01wt% to about 4wt%, or about 0.01wt% to about 3wt%, or about 0.01wt% to about 2wt%, or about 0.05wt% to about 2wt%, or about 0.1wt% to about 2wt%, or about 0.5wt% to about 2wt%. Before the peeling coating on the substrate surface is dried, based on the total weight of the peeling coating, the surfactant concentration of the peeling coating can be in the range of about 0.01wt% to about 4.00wt%. Before the peeling coating on the substrate surface is dried, the surfactant concentration of the peeling coating can be in the range of about 0.05wt% to about 2.00wt% based on the total weight of the peeling coating. After the peeling coating on the substrate surface is dried, the surfactant concentration of the peeling coating can be in the range of about 2.5wt% to about 100wt% based on the total weight of the peeling coating. For example, after the peeling coating on the substrate surface is dried, the surfactant concentration of the peeling coating can be in the range of about 3wt% to about 100wt%, or about 4wt% to about 90wt%, or about 4wt% to about 80wt%, or about 4wt% to about 70wt%, or about 4wt% to about 50wt%, or about 4wt% to about 30wt%, or about 4wt% to about 20wt%, or about 4.7wt% to about 100wt%, or about 5wt% to about 90wt%. After the peeling coating on the substrate surface is dried, the surfactant concentration of the peeling coating can be in the range of about 4.7wt% to about 100wt% based on the total weight of the peeling coating. For example, the release coating can include an amount of ZONYL surfactant in the range of about 0.05 wt % to about 5.0 wt %, based on the total weight of the release coating.
[0116] In general, the hydrophilicity-lipophilicity balance of the release coating as described herein can be in the range of about 1 to about 30. The hydrophilicity-lipophilicity balance of the release coating can be in the range of about 1 to about 20, or about 1 to about 18, or about 1 to about 17, or about 1 to about 16, or about 1 to about 15, or about 2 to about 17, or about 3 to about 17, or about 4 to about 15, or about 5 to about 12, or about 8 to about 12. The hydrophilicity-lipophilicity balance of the release coating can be in the range of about 1 to about 20. The hydrophilicity-lipophilicity balance of the release coating can be in the range of about 3 to about 17.
[0117] In general, the thickness of the peeling coating on the surface of the substrate is from about 0.1 nm to about 100 nm. On the surface of the substrate, the thickness of the peeling coating can be from about 0.1 nm to about 80 nm, or from about 0.1 nm to about 60 nm, or from about 0.1 nm to about 40 nm, or from about 0.1 nm to about 40 nm, or from about 0.1 nm to about 20 nm, or from about 0.1 nm to about 10 nm, or from about 1 nm to about 10 nm, or from about 1 nm to about 5 nm. On the surface of the substrate, the thickness of the peeling coating can be from about 0.1 nm to about 40 nm. On the surface of the substrate, the thickness of the peeling coating can be from about 0.1 nm to about 10 nm.
[0118] The amount of water in the metered resin solution of polyvinyl alcohol, additional resins and / or secondary components for film casting can be optionally selected so that when the solution is heated to the casting temperature, the solution has the highest solid level below the viscosity inflection point. Methods for determining the amount of solids at the viscosity inflection point are known in the art. In general, the metered resin solution can include about 60% to 85% water, or about 60% to 75% water, to provide a suitable solution for casting. The viscosity of each resin solution at 175°F (about 80°C) can be, for example, at least about 5,000 cPs, or at least about 6,000 cPs, or at least about 7,000 cPs, or at least about 8,000 cPs, or at least about 9,000 cPs. The viscosity of each resin solution at 175°F (about 80°C) can be, for example, no more than about 15,000 cPs, or no more than about 14,000 cPs, or no more than about 13,000 cPs, or no more than about 12,000 cPs, or no more than about 11,000 cPs.
[0119] The resin concentration of the resin solution is not particularly limited. Based on the total weight of the corresponding resin solution, the resin concentration of the first and second resin solutions can be independently in the following ranges: from about 1wt.% to about 50wt.%, or from about 5wt.% to about 45wt.%, or from about 10wt.% to about 40wt.%, or from about 20wt.% to about 35wt.%. The resin concentration of the first resin solution can be in the range of about 1wt.% to about 50wt.%. The resin concentration of the second resin solution can be in the range of about 5wt.% to about 37wt.%.
[0120] The resin solution may be cast at any suitable temperature such that the temperature of the film during drying is optionally in the range of about 50°C to about 105°C. Without intending to be bound by theory, it is believed that as the temperature of the resin solution and the film is significantly reduced to below about 50°C, the amount of time required to dry the film is undesirably increased, and the length of the drying chamber required to completely dry the cast solution is undesirably increased. Further, without intending to be bound by theory, it is believed that as the temperature of the solution and the film is significantly increased to above about 105°C, the solvent may be rapidly boiled out of the film, which results in defects such as holes or bubbles in the finished film on the film surface and / or promotes undesirable reactions between adjacent PVOH backbones, resulting in reduced film solubility.
[0121] In continuous or semi-continuous casting process, the moving casting surface can have any desired linear speed, for example, in the range of about 5 meters per minute to about 50 meters per minute. Linear speed may sometimes affect the property of the resulting film, such as physical property, thickness, residual moisture content and film quality. In general, assuming that the delivery rate of the solution remains constant, as the linear speed decreases, the thickness of the resulting film will increase, and as the linear speed increases, the thickness of the resulting film will reduce. In general, as the linear speed increases, the residence time of the film in the drying machine of fixed size is shortened, thus it is necessary to increase the drying temperature, which may cause drying defects or have viscosity at a sufficiently high temperature. On the contrary, as the linear speed decreases, the residence time of the film in the drying machine increases.
[0122] Method for preparing co-cast multilayer film
[0123] In order to prepare a co-cast multilayer film, under conditions suitable for achieving no flutter, uniform, multilayer film, two or more resin solutions as described herein are fed into a multi-groove mold simultaneously. Before being fed into the mold, the resin solution can be filtered to remove particles greater than 25 microns. Initially, the second (e.g., bottom) resin solution is cast through the bottom groove of the multi-groove mold to form a second solution layer on the substrate. Before the second solution layer is dried, the first (e.g., top) resin solution is cast through the first upper groove of the multi-groove mold to form a first solution layer in contact with the second solution layer. The resulting multilayer solution composition can be conveyed on the substrate by one or more furnaces, and the one or more furnaces are operated at a temperature sufficient to affect the drying of the multilayer solution composition and the formation of the multilayer film, and the multilayer film is optionally a self-supporting multilayer film. The drying temperature is not particularly limited. For example, the multilayer solution composition can be dried by exposure to a temperature in the following range: about 70°C to about 180°C, or about 80°C to about 160°C, or about 90°C to about 150°C, or about 100°C to about 150°C, or about 100°C to about 140°C. In addition, the drying time is not particularly limited. For example, drying the multilayer solution composition can be carried out in the following time range: about 1 minute to about 60 minutes, or about 1 minute to about 30 minutes, or about 1 minute to about 20 minutes, or about 5 minutes to about 20 minutes, or about 5 minutes to about 15 minutes, or about 10 minutes to about 15 minutes. After leaving the furnace, the film can be cooled by conveying the substrate on one or more cooling rollers. The cooling time is not particularly limited; for example, the cooling can be carried out in the following time range: about 1 second to about 30 minutes, or about 1 second to about 20 minutes, or about 30 seconds to about 10 minutes, or about 1 minute to about 5 minutes. Then, the film can be pulled under tension to peel it from the substrate and convey it to a winding roller.
[0124] Figure 3 is a perspective view of a multi-slot die 1 that can be used to prepare the co-cast multilayer film of the present disclosure. FIG. 4 shows a side view of Figure 3The multi-slot die 1 comprises a wedge-shaped central die body 10 which separates an upper die body 20 and a lower die body 40 so that two feed slots 32 and 52 are formed. The resin solution is fed into the die through an upper injection port 36 and a lower injection port 56. The upper offset shims 26a-d and the lower offset shims 46a-d are thin sheet materials that are inserted into the offset blocks 24a-d and 44a-d, respectively, to control the degree of "overbite" 62, or how far the upper die lip 28 protrudes forward than the lower die lip 48. These shims are important for controlling the pressure distribution relative to the machine or downweb direction, where the die lips 28 and 48 are positioned adjacent to a casting surface such as a belt. The upper body shims 30 and the lower body shims 50 are thin sheet materials that act as spacers between the central die body 10 and the top die body 20 and the lower die body 40, respectively. These shims 30 and 50 set the spacing or die gap between the two bodies and therefore set the height 34 and 54 of the feed slots 32 and 52 through which each solution flows. Proper die gap setting is important for maintaining uniformity of the width of each web flowing through. Improper die gap setting may result in uneven thickness of the film in the transverse direction. The side view shown in FIG4A also indicates the upper 26a and lower 46a offset shims and the upper 30 and lower 50 body shims. FIG4B (an enlarged view of a portion of FIG4A ) shows the level of "overbite" 62, which can be controlled by adjusting the upper offset shims 26a-d and the lower offset shims 46a-d. Figure 5 A schematic side view of the die 1 relative to the casting surface 70 is shown to illustrate the die angle ∠XYZ. The die angle is the casting surface ( Figure 5 The plane defined by the bottom groove of the mold through which the resin solution passes ( Figure 5 The angle between them is represented by XY.
[0125] The process conditions can be adjusted as needed, including but not limited to the resin solution temperature and viscosity, die temperature, the spacing between the top body gasket and the bottom body gasket, the spacing between the top bias gasket and the bottom bias gasket, the mold angle, the mold gap, the line pressure and the line speed to optimize the formation of the first and second solution layers and the multi-layer solution composition.
[0126] Method for preparing sequential cast multilayer film
[0127] Methods for preparing sequential cast multilayer films are known in the art. In general, the second resin solution can be cast onto a substrate to form a second resin solution layer, the second resin solution can be at least partially dried, and the first resin solution can be directly cast onto the at least partially dried second resin solution layer. The resulting multilayer composition can be transported on the substrate by one or more furnaces, which are operated at a temperature sufficient to affect the drying of the multilayer composition and the formation of the multilayer film, and the multilayer film is optionally a self-supporting multilayer film.
[0128] The first and second resin solutions can be cast by any suitable means. For example, the second resin solution can be cast using a die (such as a slot die), and the first resin solution layer can be cast using a doctor blade device or other suitable means.
[0129] Optionally, the first resin solution in the sequential casting process can be a foamed resin solution, such that the resulting multilayer film includes a top layer that is a foamed film layer.
[0130] Dissolution, disintegration and residue % test (MSTM 205)
[0131] Films may be characterized by or tested for dissolution time and disintegration time according to MonoSol Test Method 205 (MSTM 205), a method known in the art. See, e.g., U.S. Pat. No. 7,022,656.
[0132] Equipment and Materials:
[0133] 600mL beaker
[0134] Magnetic stirrer (Labline model 1250 or equivalent)
[0135] Magnetic stirring bar (5cm)
[0136] Thermometer (0 to 100℃±1℃)
[0137] Stainless steel template (3.8cm×3.2cm)
[0138] Timer (0-300 seconds, accurate to the nearest second)
[0139] Polaroid 35mm slide mount (or equivalent)
[0140] Monoso 35mm Slide Mount Holder (or equivalent)
[0141] Distilled water
[0142] For each film to be tested, three test specimens were cut from the film sample (i.e., 3.8 cm x 3.2 cm specimens). If cut from a film web, the specimens should be cut from areas of the web that are evenly spaced in the cross-direction of the web. Each test specimen was then analyzed using the following procedure.
[0143] Each specimen was locked into an individual 35 mm slide mount.
[0144] Fill the beaker with 500 mL of distilled water. Measure the water temperature with a thermometer and, if necessary, heat or cool the water to maintain a temperature of 20°C (about 68°F).
[0145] Mark the height of the water column. Place the magnetic stirrer on the holder base. Place the beaker on the magnetic stirrer, add a magnetic stir bar to the beaker, turn on the stirrer, and adjust the stirring speed until a vortex of approximately one fifth of the height of the water column is formed. Mark the vortex depth.
[0146] Secure the 35 mm slide mount in the alligator clip of the 35 mm slide mount holder so that the long end of the slide mount is parallel to the water surface. The depth adjuster of the holder should be set so that when dropped, the end of the clamp will be 0.6 cm below the water surface. One of the short sides of the slide mount should be against the side of the beaker, while the other short side is positioned just above the center of the stir bar so that the film surface is perpendicular to the water flow.
[0147] In one motion, the fixed slide is dropped and clamped into the water, and a timer is started. Disintegration occurs when the film breaks. When all visible film is released from the slide mount, the slide is raised from the water while continuing to monitor the solution for undissolved film fragments. Dissolution occurs when all film fragments are no longer visible and the solution becomes clear.
[0148] After 300 seconds, if any film residue remained in the frame, the percentage of surface area of remaining film was estimated by visual inspection.
[0149] Results should include the following: complete sample identification; individual and average disintegration and dissolution times; and the water temperature in which the samples were tested.
[0150] The film disintegration time (I) and film dissolution time (S) can be corrected to a standard or reference film thickness using the exponential algorithms shown below in Equation 1 and Equation 2, respectively.
[0151] I 校正的 =I 测得的 ×(reference thickness / measured thickness) 1.93 [1]
[0152] S 校正的 =S 测得的 ×(reference thickness / measured thickness) 1.83 [2]
[0153] Friction coefficient test
[0154] The coefficient of friction method measures the friction of two materials rubbing against each other; it measures the force required to move one material relative to another. Both the force to start the sled (static friction) and the force to keep the sled moving (dynamic friction) are measured by a load cell using ASTM D1894 "Friction Test of Plastic Film and Sheeting".
[0155] The method uses Model 2810-005 Coefficient of Friction Test Fixture or equivalent, represented by the diagram in Figure 6 In, and Model #5543 Tester or equivalent.
[0156] The test apparatus includes a friction fixture 110, a friction sled 112 located on the friction fixture, and a film sample 114 fixed to the friction sled. The sled 112 is connected to an upper handle 118 by a pull rope 120, which engages a pulley 122 fixed to the friction fixture 110. A lower coupling 124 secures the test fixture to On a testing machine (not shown).
[0157] according to Method Blue Hill Procedure: "System: Search the data from the start value to the end value on a specified channel for a maximum; determine the first data point that rises and falls as a percentage of the maximum value, and designate this point as the first peak; determine the coefficient of static friction using the equation: Static Friction = First Peak / Sled Weight; calculate the average load for the area from the first peak to the end value using the equation: Average Load = Energy / Change in Extension; and determine the coefficient of kinetic friction using the equation: Kinetic Friction = Average Load / Sled Weight."
[0158] The test specimen shall consist of a sample having the following dimensions: a sled that is 5 inches by 5 inches square (12.7 cm by 12.7 cm square) and a surface that is 5 inches by 8 inches rectangular (12.7 cm by 20.3 cm) to form the test area. The thickness of the film may be 3.0 ± 0.10 mils (or 76.2 ± 2.5 μm), although it is believed that film thickness will not affect the static COF. For example, the sample may be cut using an appropriately sized razor blade and template. Where applicable, the sample should be cut into the long dimension parallel to the machine direction of the cast film. Likewise, where applicable, the orientation of the 5 inch by 5 inch sample should be noted and oriented in the test so that the direction in which the sled is pulled is parallel to the machine direction of the film sample.
[0159] Before testing, the test specimens should be conditioned at 75°F ± 5°F (approximately 24°C ± 3°C) and 35% ± 5% relative humidity for no less than 8 hours, and the test should be performed under the same temperature and relative humidity conditions.
[0160] COF equipment installation procedure
[0161] 1. From Remove the clevis pin from the lower jaw on the Model 2810-005 Coefficient of Friction Test Fixture and discard it.
[0162] 2. Remove the clevis pin from the upper jaw and discard it.
[0163] 3. Place the lower connection of the friction fixture On the base adapter of the Tester Model #5543.
[0164] 4. Secure it with the clevis pin.
[0165] 5. Slide the loop on one end of the draw cord onto the upper clevis pin and replace the locking clip.
[0166] 6. Calibrate the #5543 testing machine.
[0167] 7. Put the loop on the other end of the pull rope onto the friction skid hook.
[0168] 8. Make sure the pulley can rotate freely.
[0169] 9. Move the sled until the draw rope has no more slack and is oriented in the groove around the pulley.
[0170] 10. Positioning Move the crosshead (upper end) of the Model 2810-005 Coefficient of Friction Test Fixture so that there is enough travel to pull the friction sled along the full 50 mm of the test without feeding the sled into the pulleys.
[0171] 11. Keep the rope taut while the crosshead moves.
[0172] 12. Using the JOG controls on the Instron #5543 control panel, set the extension limit so that the far end of the friction sled does not exceed the back plane of the friction fixture (the plane that is perpendicular to the axis of motion and farthest from the pulley). Press the GL button to set the travel limit. This prevents the friction sled from colliding with the pulley during testing and ensures that the coefficient of friction is correctly measured for the sample of interest.
[0173] 13. The test fixture is now ready for testing.
[0174] Sample placement procedure
[0175] 1. Place the surface sample in the aluminum friction fixture in the proper orientation.
[0176] 2. Pull the surface sample tightly over the edge of the aluminum surface and tape the sample to the bottom side of the friction fixture.
[0177] 3. It is important to tape along the end of the friction clamp farthest from the coupling to avoid skid binding to the surface.
[0178] 4. Make sure the material is taut, but not stretched.
[0179] 5. Wrap the rubbing sled with the 5 x 5 inch sample so that the machine direction of the film is parallel to the direction the sled will be pulled.
[0180] 6. Tape the leading edge overlap to the top of the sled, ensuring that no excess material will bond to the surface sample.
[0181] 7. Tape the other edge of the sample to the friction sled to ensure that the sample is taut on the contact surface being measured.
[0182] 8. Make sure there is no tape between the surface of concern on the sled and the friction fixture.
[0183] 9. The friction surface and the sample on the friction sled should be stretched taut with no wrinkles or bulges; these wrinkles or bulges will cause errors in measuring COF.
[0184] 10. Inspect the skid to ensure that no foreign matter is contacting the surface being tested.
[0185] 11. Attach the sled to the draw cord and place the sled very gently and softly on the friction table to prevent any unnatural bonding between the two samples and start the test immediately.
[0186] 12. Ensure that when fully extended, the sled is completely over the sample placed on the friction grips and does not touch the tape or hang over the edge of the friction grips.
[0187] Conducting COF testing
[0188] 1. Test no less than three specimens according to the required orientation (for example air side - air side or belt side - belt side).
[0189] 2. For a combination of air side to tape side testing, the air side of the membrane shall be oriented with the membrane sample placed on the aluminum test surface and the tape side for testing shall consist of the material wrapped around the sled.
[0190] 3. When handling membrane samples, make sure to wear powder-free moisture-barrier gloves; powder or moisture may compromise the accuracy of the test.
[0191] 4. Cut the sample as described above, for example using a template.
[0192] 5. Place the friction sled wrapped in the first specimen at the end of the friction fixture farthest from the pulley.
[0193] 6. Make sure the draw cord is tight.
[0194] 7. Open the Coefficient of Friction test titled “COF.im ptf” from the Tests screen.
[0195] 8. Click the Start button on the screen to begin the test.
[0196] 9. After the sample test run is complete, click "OK" and return the friction sled to the starting position and replace the film sample on the friction sled and fixture. Repeat the test.
[0197] Moisture Vapor Transmission Rate (MVTR) Test
[0198] The multilayer water-soluble film according to the present disclosure can be characterized by the amount of moisture that permeates the film or its layers. The permeation of moisture through one or more layers can be measured and described by the moisture vapor transmission rate (MVTR). MVTR is expressed as the mass of water permeated per unit area per day (g H2O / m 2 / day) to measure.
[0199] MVTR is measured using ASTM F-1249. Prior to testing, the samples are conditioned at 23°C and 35% RH for at least 8 hours and no more than 48 hours, such as about 24 hours. Measurements are made at about 38°C and 50% RH with the coating exposed to a water source.
[0200] The MVTR of the multilayer water-soluble film can be about 100 g H2O / m 2 / day or less, or about 50g H2O / m 2 / day or less, or about 30g H2O / m 2 / day or less, or about 20g H2O / m 2 / day or less, or about 10g H2O / m 2 / day or less, such as about 18g H2O / m 2 / day or less, about 16g H2O / m 2 / day or less, about 15g H2O / m 2 / day or less, about 14g H2O / m 2 / day or less, about 12H2O / m 2 / day or less, about 10g H2O / m 2 / day or less, about 8g H2O / m 2 / day or less, about 7gH2O / m 2 / day or less, about 5g H2O / m 2 / day or less, about 3g H2O / m 2 / day or less, about 2.5g H2O / m 2 / day or less, about 1g H2O / m 2 / day or less, or about 0.5 g H2O / m 2 / day or less. The MVTR of the water-soluble film can be in the following range: about 0.05 g H2O / m 2 / day to about 20 g H2O / m 2 / day, about 0.05g H2O / m 2 / day to about 18 g H2O / m 2 / day, about 0.10gH2O / m 2 / day to about 16 g H2O / m 2 / day, about 0.15g H2O / m 2 / day to about 14 g H2O / m 2 / day, about 0.50g H2O / m 2 / day to about 12 g H2O / m 2 / day, about 0.75g H2O / m 2 / day to about 10 g H2O / m 2 / day, about 10g H2O / m 2 / day to about 20 g H2O / m 2 / day, about 12g H2O / m 2 / day to about 18 g H2O / m 2 / day, about 14g H2O / m 2 / day to about 16 g H2O / m 2 / day, about 0.05gH2O / m 2 / day to about 10 g H2O / m 2 / day, about 1g H2O / m 2 / day to about 8 g H2O / m 2 / day, about 2g H2O / m 2 / day to about 6gH2O / m 2 / day, or about 3g H2O / m 2 / day to about 5g H2O / m 2 / day, for example, about 0.05 g H2O / m 2 / day, about 0.1g H2O / m 2 / day, about 0.5g H2O / m 2 / day, about 1g H2O / m 2 / day, about 1.5g H2O / m 2 / day, about 2g H2O / m 2 / day, about 2.5g H2O / m 2 / day, about 3g H2O / m 2 / day, about 3.5g H2O / m 2 / day, about 4g H2O / m 2 / day, about 4.5g H2O / m 2 / day, about 5g H2O / m 2 / day, about 5.5g H2O / m 2 / day, about 6g H2O / m 2 / day, about 6.5g H2O / m 2 / day, about 7g H2O / m 2 / day, about 7.5gH2O / m 2 / day, about 8g H2O / m 2 / day, about 8.5g H2O / m 2 / day, about 9g H2O / m 2 / day, about 9.5g H2O / m 2 / day, about 10gH2O / m 2 / day, about 10.5g H2O / m 2 / day, about 11g H2O / m 2 / day, about 11.5g H2O / m 2 / day, about 12g H2O / m 2 / day, about 12.5g H2O / m 2 / day, about 13g H2O / m 2 / day, about 13.5g H2O / m 2 / day, about 14g H2O / m 2 / day, about 14.5g H2O / m 2 / day, about 15g H2O / m 2 / day, about 15.5g H2O / m 2 / day, about 16g H2O / m 2 / day, about 16.5g H2O / m 2 / day, about 17gH2O / m 2 / day, about 17.5g H2O / m 2 / day, about 18g H2O / m 2 / day, about 18.5g H2O / m 2 / day, about 19g H2O / m 2 / day, about 19.5g H2O / m 2 / day, or about 20 g H2O / m 2 / sky.
[0201] Without intending to be bound by theory, it is believed that MVTR may be variable with film layer thickness. That is, as film layer thickness increases, MVTR may decrease, and as film layer thickness decreases, MVTR may increase.
[0202] Haze test
[0203] Haze is measured using a BYK Haze-Gard I benchtop haze meter according to ASTM D1003. Prior to testing, the test items are conditioned at 23°C and 35% RH for at least 8 hours and no more than 48 hours, such as about 24 hours. Measurements are made at 23°C and 35% RH.
[0204] Seal strength test
[0205] The seal strength test measures the seal strength between two sealed film surfaces. The sealed film surfaces can be surfaces of two different films sealed to each other, or surfaces of two films of the same composition, or the sealed film surfaces can be surfaces of a single film sealed to itself.
[0206] Film data was collected using an INSTRON tensile testing device (5544 model tensile tester or equivalent). The films can be sealed to each other by any suitable means, including heat sealing or water sealing methods known in the art. For example, an ESIPROOF proofing device or equivalent with an anilox roller 140 / 10 can be used to seal two film sheets with water. Alternatively, two film sheets can be heat sealed. Therefore, the seal strength of the seal between the two sealed film surfaces can be characterized as water seal strength or heat seal strength. At least three test samples are tested in the machine direction (MD) (if applicable) of each measurement, and each test sample is cut with a reliable cutting tool to ensure dimensional stability and reproducibility. Tests are performed in a standard laboratory atmosphere at 23°C ± 2.0°C and 35% ± 5% relative humidity.
[0207] Samples for measuring water seal strength can be prepared as follows. Test specimens are prepared by cutting four 100mm×300mm film sheets with a size of 300mm in the machine direction (MD). For two sheets, the four corners of one sheet are taped to one surface. Another sheet is covered on the top of the sheet that has been taped, so that the appropriate surfaces are in contact. On top of the other sheet that has been taped, the remaining sheets are placed on top so that the two surfaces to be sealed are in contact with each other. One 100mm end of each top sheet is taped to fix it to the bottom sheet. Use a 140 / 10 anilox roller to pass the loose end of each top sheet through the ESIPROOF proofing roller. Apply 0.5mL of water to the blade. Pull the roller at a constant speed (75mm / sec) to coat the upper film and fix it to the lower sheet. Allow the film to weld for 10-15 minutes. Using a strip punch or sample cutter, cut 25.4 mm wide samples in the transverse direction (TD).
[0208] Transfer the water-sealed or heat-sealed samples to the INSTRON testing machine for testing while minimizing environmental exposure. For seal strength testing, there is a distance of 0.50" (1.27 cm) between the rubber grips, all four of which are flat and square. Cut three (or more) 1" wide (2.54 cm) samples in the machine direction (MD). Place the unsealed flap of the sample in the grip of the testing machine, taking care to ensure that the sample is aligned with and parallel to the grip, and that the sample is not pulled too tight in the jaws of the testing machine. The load is balanced and the test is started according to the equipment manufacturer's instructions. At the end of the test, the tension (in N) required to tear or separate the layers is recorded as the seal strength.
[0209] Examples
[0210] The following examples are provided for illustration and are not intended to limit the scope of the invention.
[0211] To prepare the co-cast two-layer film, the two resin solutions were simultaneously fed into a multi-slot die through a supply line maintained at 160°F to 180°F (about 70°C to 80°C) under conditions suitable for achieving a flutter-free, uniform, multilayer film. Processing conditions were selected to achieve a 13-inch to 16-inch (33-cm to 40-cm) wide, 45 μm to 80 μm thick multilayer film. The co-cast multilayer film was conveyed from the die exit on a stainless steel belt at 4 to 13 feet per minute (fpm) (2 to 6.6 cm / sec) through a 100-foot (30 m) heated tunnel, the belt was peeled off under tension, and wound on a roll.
[0212] Resin solutions for preparing cast films, sequentially cast bilayer films, or co-cast bilayer films were prepared according to the formulations described in the examples below. The resin content of the solution was typically between 12 wt.% and 37 wt.%, although films can be cast from solutions with resin contents as low as about 5.0 wt.%. Prior to casting, the solution was mixed overnight with a ribbon blender at 175°F to 185°F (about 80°C to 85°C) to ensure complete dissolution of the resin.
[0213] Example 1: Co-cast bi-layer membranes with high bio-based content
[0214] A two-layer film including a PVOH-based film layer and a film layer with high bio-based content was prepared according to the above co-cast multilayer film preparation procedure. Table 1 shows the composition of the dried top and bottom film layers. The top layer included hydroxypropyl methylcellulose (HPMC; Shin-Etsu Chemical Co., Tokyo, Japan) and auxiliary components, including plasticizers and defoamers. Resin solutions for the bottom layer (PVOH) and top layer (HPMC) were prepared according to the stoichiometry listed in Table 1 and diluted to 24.0 wt.% PVOH and 12.0 wt.% HPMC, respectively. During co-casting, the PVOH and HPMC resin solutions were maintained at about 75°F and 145°F (about 24°C and 63°C), respectively, and the die was maintained at about 180°F (about 80°C). The line speed during co-casting ranged from 3 fpm to 6 fpm (about 1.5 cm / sec to 3 cm / sec).
[0215] Table 1
[0216] Components Layer weight % Top floor Hydroxypropyl methylcellulose (HPMC) 59.0 Auxiliary components + water 41.0 Bottom Layer Acrylate modified PVOH 60.1 Plasticizers 25.9 Fumed Silica 2.2 Surfactants 3.4 Defoaming agent 0.4 Auxiliary components 2.0 water 6.0
[0217] Surprisingly, it was found that the two-layer film of Example 1 can be formed into a bag by thermoforming. Films comprising HPMC or other cellulose as the primary or sole film-forming resin are generally too brittle to be successfully thermoformed. Thus, the simultaneous solution co-casting procedure according to the present disclosure can provide films with high bio-based content that exhibit advantageous physical properties, such as thermoformability, that are generally not obtainable with bio-based films.
[0218] Example 2: Dual-layer film with low haze and low COF
[0219] Single-layer PVOH films 2A-2C containing different amounts of silica (an anti-blocking agent) were prepared using a standard solution casting method according to the formulations listed in Table 2. Increasing the amount of silica in the film is expected to reduce the coefficient of friction (COF) between the film and other surfaces, but also reduce transparency, i.e., increase the degree of haze. A double-layer film 2D was prepared by sequentially casting a bottom layer of Film 2B composition (no silica) and a top layer of Film 2C composition (high silica), wherein the bottom layer was dried before casting the top layer. The haze % and gloss-gloss friction coefficient of each single-layer film and double-layer film were evaluated by the test methods described herein; Table 2 also contains these results.
[0220] Compared to Film 2A, as expected due to the absence of silica, Film 2B exhibited lower haze but higher COF, and as expected due to the high silica loading, Film 2C exhibited lower COF but higher haze. However, at approximately the same total silica loading, Bilayer Film 2D exhibited a low COF comparable to the 2x silica film and a haze comparable to the control Film 2A. Thus, the bilayer film exhibits the advantageous properties of both layers, a combination that previously could have existed only in separate films with offsetting disadvantages.
[0221] Table 2
[0222]
[0223] Example 3: Co-cast bi-layer films with low haze and low COF
[0224] Single-layer PVOH films 3A and 3B were prepared using a standard solution casting method according to the formulations listed in Table 3. A double-layer film 3C was prepared by a simultaneous solution co-casting method, the double-layer film comprising a top layer of the 3A composition and a bottom layer of the 3B composition. To prepare the double-layer film, an aqueous resin solution was prepared, the stoichiometry of which corresponded to the stoichiometry of the 3A and 3B compositions, but was diluted to PVOH concentrations of 31.5 wt% and 28.7 wt%, respectively. The resin solutions were fed simultaneously into a multi-slot die and co-cast onto a continuously moving metal belt, with the 3B solution fed through the bottom die slot and the 3A solution fed through the top die slot. During casting, the resin solution was maintained at 180°F (about 80°C) and was filtered through a medium to remove particles larger than 25 μm as the solution was fed into the multi-slot die. The main gasket spacing of the top and bottom slots was 0.01 inches (0.254 mm). The top offset shim spacing was 0.005 inches (0.127 mm), and the bottom offset shim spacing was 0.01 inches (0.254 mm). During casting, the die angle was adjusted between 48.5°-50.1°, and the die-belt gap was adjusted between 0.025 inches and 0.040 inches (0.635 mm and 1.016 mm). The line speed range was 6 fpm to 10 fpm (about 3 cm / sec to 5 cm / sec). During casting, the top and bottom die slots were maintained at about 140°F to 180°F (about 60°C to 80°C). The co-cast two-layer film was conveyed from the die outlet through a heating tunnel, where the heating zones were maintained at about 310°F and about 230°F (about 155°C and 110°C) to dry the co-cast film.
[0225] Table 3
[0226]
[0227]
[0228] Table 3 shows that the simultaneously co-cast bilayer film exhibits the advantageous attributes of both component layers, namely low coefficient of friction and low haze, without the offset disadvantages.
[0229] FIG. 7 shows optical microscope images of a cross section of a co-cast bilayer film 3C obtained by cutting the film along the machine direction (MD, shown in the left image) or along the transverse direction (TD, shown in the right image), respectively. Figure 6The images in are shown in the same orientation as the film was cast; that is, the bottom film layer in each image is the layer of the co-cast film that was in direct contact with the casting belt. FIG7 indicates that the component layers of the co-cast film are highly integrated and minimal layer mixing occurs during the simultaneous solution co-casting process. A cross-sectional image of a bilayer film having the same bottom and top layer compositions as film 3C prepared by a sequential casting process is shown in FIG8 , where the bottom layer is solution cast and dried, and the top layer is solution cast onto the dried bottom layer film. As shown in FIG7 , the left and right images show cross sections taken in MD and TD, respectively.
[0230] A bilayer film of similar composition to bilayer film 3C was prepared by a simultaneous solution co-casting method to demonstrate that very thin film layers can be obtained by the disclosed co-casting method. As shown in Table 4, bilayer film 3F was prepared by simultaneously co-casting the bottom layer of composition 3D and the top layer of composition 3E. As with film 3C, the top layer of film 3F contained silica, and the bottom layer did not contain silica. The flow rate of the resin solution through the multi-groove die was controlled to provide a dry film thickness of 70 microns and 1 micron for the bottom film layer and the top film layer, respectively. Table 4 contains coefficient of friction and haze data for bilayer films and monolayer films of compositions having the top layer and bottom layer of the bilayer film. Despite having a very thin top layer containing silica, film 3F embodies a favorable combination of low coefficient of friction and low haze. The results shown in Table 4 demonstrate that very thin top film layers can be obtained by simultaneous co-casting.
[0231] Table 4
[0232]
[0233]
[0234] Example 4: Double-layer film with high moisture barrier and high seal strength
[0235] A two-layer film 4C was prepared by a simultaneous solution co-casting process, comprising a top layer of 4A composition and a bottom layer of 4B composition listed in Table 5. To prepare the two-layer film, an aqueous resin solution was prepared, the stoichiometry of which corresponds to the stoichiometry of the dry film formulations 4A and 4B, diluted to 30.7 wt% and 36.6 wt% PVOH concentrations, respectively, for casting. The resin solutions were simultaneously fed into a multi-slot die and co-cast onto a continuously moving metal belt, with the 4B solution fed through the bottom die slot and the 4A solution fed through the top die slot. During casting, the resin solution was maintained at 180°F (about 80°C) and was filtered through a media to remove particles larger than 25 μm as the solution was fed into the multi-slot die. The body shim spacing for the top and bottom slots was 0.015". The top offset shim spacing was 0.002 inches (0.05 mm), and the bottom offset shim spacing was 0.01 inches (0.254 mm). During casting, the die angle was adjusted between 48° and 60°, and the die-belt gap was set to 0.025 inches (0.635 mm). The line speed range was 2 fpm to 6 fpm (about 1 cm / sec to 3 cm / sec). During casting, the top and bottom die slots were maintained at about 140°F to 180°F (about 60°C to 80°C). The co-cast two-layer film was conveyed from the die outlet through a heating tunnel, where the heating zones were maintained at about 310°F and about 230°F (about 155°C and 110°C) to dry the co-cast film. The heat seal strength of the two-layer film 4C was 13.7N.
[0236] Table 5
[0237]
[0238]
[0239] Example 5: Double-layer film with high moisture barrier and high seal strength
[0240] Single layer PVOH films having the dry film compositions 5A and 5B in Table 6 were prepared using a standard solution casting process. Sequentially cast dual layer film 5C included a 78 μm bottom layer of the 5B composition and an 11 μm top layer of the 5A composition. As shown in Table 6, film 5A exhibited high heat seal strength and also exhibited high moisture vapor transmission rate, while film 5B provided a high barrier to moisture vapor transmission but exhibited poor seal strength. However, dual layer film 5C exhibited the advantageous properties of the two component films: the heat seal strength was nearly as high as that of the single layer film 5A, and the moisture vapor transmission rate was nearly as low as that of the single layer film 5B, without offsetting the disadvantages.
[0241] Table 6
[0242]
[0243]
[0244] Example 6: Sequentially cast two-layer film with foam film layer
[0245] A double-layer film including a foam film layer as the first (i.e., top) layer was prepared by a sequential casting method. A second resin solution including water, 36wt.% anion-modified PVOH resin, plasticizer, other additives and defoamer was prepared by mixing using a belt blender. A first resin solution including water, 36wt.% anion-modified PVOH resin, plasticizer, other additives and no defoamer was prepared by mixing using a belt blender. Mixing the first resin solution provided a foam resin solution having a volume ratio of approximately 30% of the volume of the resin solution before mixing. Mixing the second resin solution did not significantly increase its volume. The increase in the volume of the first resin solution was attributed to entrainment of air through foam formation. The first foam resin solution was stable; however, pumping the foam resin solution was more difficult than pumping the second (i.e., non-foam) resin solution.
[0246] The lower film layer of the two-layer film (in this case, the bottom film layer) is produced by casting the second resin solution through the bottom groove of the mold onto the substrate and partially drying the bottom film layer by applying heat. The top film layer of the two-layer film is produced by casting the first (foamed) resin solution directly onto the partially dried bottom film layer using a doctor blade device, and the resulting multilayer composition is dried to provide a two-layer film.
[0247] The two-layer film is stable because the bottom layer (non-foam) and top layer (foam) do not easily delaminate from each other.
[0248] Example 7: Simultaneous co-casting of two-layer films with foam film layers
[0249] The first and second resin solutions described in Example 6 are prepared, and the first resin solution is mixed using a belt blender as described in Example 6 to form a foamed resin solution. Then, the second resin solution and the first (foamed) resin solution are fed to a multi-groove die simultaneously. The second resin solution is fed through the lower die slot, and the first (foamed) resin solution is fed through the upper die slot, so that the second resin solution is cast onto a continuously moving substrate (the travel rate is referred to as "line speed"), and the first resin solution is directly cast onto the second resin solution to form a two-layer solution composition. During co-casting, the die is maintained at 75°C-85°C (167°F-185°F). The resulting two-layer solution composition is then passed through an oven to dry the film and form a two-layer film.
[0250] During the simultaneous co-casting, some parameters such as line speed were changed to try to achieve the best casting conditions. Under some casting conditions, the top resin solution layer does not seem to be completely stable. Specifically, as the line speed increases, the top resin solution layer seems to be dehumidified from the bottom resin solution layer. Therefore, the line speed can be controlled (that is, by reducing the speed as required) to provide a stable multilayer film structure. In addition, as described in Example 6, the foamed resin solution is more difficult to be pumped from its storage tank to the casting equipment than the non-foamed resin solution. Therefore, a higher pumping pressure can be used for the foamed resin solution relative to the pressure of the non-foamed resin solution. Consider mixing the top resin solution online to form a foamed resin solution, thereby providing a more consistent casting result.
[0251] The foregoing description has been given only for clearness of understanding, and no unnecessary limitations should be understood therefrom, since modifications within the scope of the invention may be obvious to one skilled in the art.
[0252] All patents, publications, and references cited herein are hereby incorporated by reference in their entirety. In the event of a conflict between the present disclosure and the incorporated patents, publications, and references, the present disclosure shall control.
Claims
1. A water-soluble film comprising a first layer and a second layer in contact with each other, wherein the first layer comprises a first water-soluble resin, the first water-soluble resin comprises a polyvinyl alcohol homopolymer, a polyvinyl alcohol copolymer or a blend thereof, and the second layer comprises a second water-soluble resin, the second water-soluble resin comprises a polyvinyl alcohol homopolymer, a polyvinyl alcohol copolymer or a blend thereof; and The water-soluble film is obtained by simultaneously solution casting a first resin solution including the first water-soluble resin and a second resin solution including the second water-soluble resin.
2. The water-soluble film according to claim 1, wherein the second layer comprises an outer surface; and wherein the water seal strength of the film when sealed to itself through the first portion of the second layer outer surface sealed to the second portion of the second layer outer surface is about 10N or greater, or about 12N or greater, or about 15N or greater based on the Seal Strength Test, and the moisture vapor transmission rate of the film is about 100 g / m per 24 hours based on the Moisture Vapor Transmission Rate Test Method 2 or less, or about 50 g / m2 per 24 hours 2 or less, or about 30 g / m2 per 24 hours 2 or smaller.
3. The water-soluble film according to claim 1, wherein the first layer comprises an anti-blocking agent, and the amount of the anti-blocking agent in the first layer as a percentage of the total weight of the first layer is greater than the amount of the anti-blocking agent in the second layer as a percentage of the total weight of the second layer; wherein the first layer has a first surface that forms an outer surface of the film; and Wherein the combination of Haze (%) and Static Coefficient of Friction ("COF") is within the polygon defined by vertices (Haze (%), Static COF) of about (0.03, 13), about (59, 0.5), about (10, 0.1), and about (0.1, 0.1), or within the polygon defined by vertices (Haze (%), Static COF) of about (0.03, 10), about (55, 0.5), about (10, 0.1), and about (0.1, 0.1).
4. The water-soluble film of claim 3, wherein the first layer comprises an anti-blocking agent in an amount of about 2 wt% to about 10 wt% of the first layer.
5. The water-soluble film of claim 4, wherein the first layer comprises an anti-blocking agent in an amount of about 3.5 wt% to about 6.5 wt% of the first layer.
6. The water-soluble film according to any one of claims 3 to 5, wherein the second layer is substantially free of anti-blocking agents.
7. The water-soluble film according to any one of the preceding claims, wherein the weight average molecular weight of the first water-soluble resin is greater than or equal to the weight average molecular weight of the second water-soluble resin.
8. The water-soluble film according to any one of the preceding claims, wherein the degree of hydrolysis of the first water-soluble resin is greater than or equal to the degree of hydrolysis of the second water-soluble resin.
9. The water-soluble film according to any one of the preceding claims, wherein the first water-soluble resin comprises a polyvinyl alcohol copolymer.
10. The water-soluble film according to any one of the preceding claims, wherein the second water-soluble resin comprises a polyvinyl alcohol copolymer.
11. The water-soluble film according to any one of the preceding claims, wherein the first water-soluble resin comprises a blend of a polyvinyl alcohol homopolymer and a polyvinyl alcohol copolymer. 12 . The water-soluble film according to claim 9 , wherein the polyvinyl alcohol copolymer including the first water-soluble resin includes anion-modified polyvinyl alcohol. 13 . The water-soluble film according to claim 12 , wherein the anionic group content of the polyvinyl alcohol copolymer including the first water-soluble resin is about 0.5 mol % to about 10 mol % based on the total amount of the polyvinyl alcohol copolymer of the first water-soluble resin.
14. The water-soluble film according to any one of the preceding claims, wherein the second water-soluble resin comprises a blend of a polyvinyl alcohol homopolymer and a polyvinyl alcohol copolymer. 15 . The water-soluble film according to claim 10 , wherein the polyvinyl alcohol copolymer including the second water-soluble resin includes anion-modified polyvinyl alcohol. 16 . The water-soluble film according to claim 15 , wherein the anionic group content of the polyvinyl alcohol copolymer including the second water-soluble resin is about 0.5 mol % to about 10 mol % based on the total amount of the polyvinyl alcohol copolymer of the second water-soluble resin. 17 . The water-soluble film according to claim 11 , wherein an amount of the polyvinyl alcohol homopolymer comprising the first water-soluble resin is greater than or equal to an amount of the polyvinyl alcohol copolymer comprising the first water-soluble resin. 18 . The water-soluble film of claim 17 , wherein the first water-soluble resin includes the polyvinyl alcohol homopolymer in an amount ranging from about 35 wt % to about 45 wt % based on the total weight of the first layer.
19. The water-soluble film according to claim 17 or claim 18, wherein the first water-soluble resin comprises the polyvinyl alcohol copolymer in an amount ranging from about 20 wt% to about 30 wt% based on the total weight of the first layer.
20. The water-soluble film according to any one of claims 11 to 16, wherein the first water-soluble resin comprises a higher amount of a polyvinyl alcohol copolymer than a polyvinyl alcohol homopolymer. 21 . The water-soluble film of claim 20 , wherein the second water-soluble resin includes the polyvinyl alcohol homopolymer in an amount ranging from about 35 wt % to about 45 wt % based on the total weight of the second layer.
22. The water-soluble film according to claim 20 or claim 21, wherein the second water-soluble resin comprises the polyvinyl alcohol copolymer in an amount ranging from about 20 wt% to about 30 wt% based on the total weight of the second layer.
23. The water-soluble film according to claim 13 or claim 16, wherein the anion-modified polyvinyl alcohol comprising the first water-soluble resin and / or the second water-soluble resin comprises anionic monomer units derived from monomers selected from the group consisting of vinylacetic acid, alkyl acrylates, maleic acid, monoalkyl maleates, dialkyl maleates, monomethyl maleates, dimethyl maleates, maleic anhydride, fumaric acid, monoalkyl fumarate, dialkyl fumarate, monomethyl fumarate, dimethyl fumarate, fumaric anhydride, itaconic acid, itaconic acid monomethyl ester, dimethyl itaconate, itaconic anhydride, citraconic acid, monoalkyl citraconic acid esters, dialkyl citraconic acid esters, citraconic anhydride, mesaconic acid, monoalkyl mesaconic acid esters, dialkyl mesaconic acid esters, mesaconic anhydride, glutaconic acid, monoalkyl glutaconic acid esters, dialkyl glutaconic acid esters, glutaconic anhydride, vinyl sulfonic acid, alkyl sulfonic acid, vinyl sulfonic acid, 2-acrylamido-1-methylpropanesulfonic acid, 2-acrylamido-2-methylpropanesulfonic acid, 2-methacrylamido-2-methylpropanesulfonic acid, 2-sulfoethyl acrylate, alkali metal salts thereof, esters thereof, and combinations thereof.
24. The water-soluble film according to claim 23, wherein the anionic monomer unit is derived from a monomer selected from the group consisting of maleic acid, monoalkyl maleate, dialkyl maleate, maleic anhydride, alkali metal salts thereof, esters thereof, and combinations thereof.
25. The water-soluble film according to claim 24, wherein the anionic monomer unit is derived from a monomer selected from the group consisting of maleic acid, monomethyl maleate, dimethyl maleate, maleic anhydride, alkali metal salts thereof, esters thereof, and combinations thereof.
26. The water-soluble film according to any one of the preceding claims, wherein the first water-soluble resin comprises a polyvinyl alcohol copolymer having a degree of hydrolysis in the range of about 80% to about 99%.
27. The water-soluble film according to any one of the preceding claims, wherein the second water-soluble resin comprises a polyvinyl alcohol copolymer having a degree of hydrolysis in the range of about 80% to about 99%.
28. The water-soluble film of any one of the preceding claims, wherein the first water-soluble resin comprises a polyvinyl alcohol homopolymer having a degree of hydrolysis in the range of about 80% to about 99%.
29. The water-soluble film of any one of the preceding claims, wherein the second water-soluble resin comprises a polyvinyl alcohol homopolymer having a degree of hydrolysis in the range of about 80% to about 99%.
30. A water-soluble film comprising a first layer and a second layer in contact with each other, wherein the first layer comprises a first water-soluble resin, the first water-soluble resin comprises a bio-based polymer, and the second layer comprises a second water-soluble resin, the second water-soluble resin comprises a polyvinyl alcohol (PVOH) homopolymer, a polyvinyl alcohol copolymer, or a blend thereof; and, The water-soluble film is obtained by simultaneously solution casting the first layer and the second layer.
31. The water-soluble film of claim 30, wherein the first water-soluble resin comprises a cellulosic polymer.
32. The water-soluble film according to claim 31, wherein the first water-soluble resin comprises hydroxypropyl methylcellulose.
33. The water-soluble film of any preceding claim, wherein the first layer further comprises a plasticizer.
34. The water-soluble film of any preceding claim, wherein the second layer further comprises a plasticizer.
35. The water-soluble film according to claim 33 or claim 34, wherein the plasticizer comprising the first layer and / or the plasticizer comprising the second layer is independently selected from the following group: glycerol, trimethylolpropane, sorbitol, propylene glycol, dipropylene glycol, polypropylene glycol, diglycerol, 2-methyl-1,3-propanediol and combinations thereof.
36. The water-soluble film of any preceding claim, wherein the first layer further comprises a surfactant.
37. The water-soluble film of any preceding claim, wherein the second layer further comprises a surfactant.
38. The water-soluble film according to claim 36 or claim 37, wherein the surfactant comprising the first layer and / or the surfactant comprising the second layer is independently selected from the following group: polyoxyethylene polyoxypropylene glycol, alcohol ethoxylate, alkylphenol ethoxylate, tertiary acetylene glycol, alkanolamide, polyoxyethylene amine, quaternary ammonium salt, quaternized polyoxyethylene amine, amine oxide, N-alkyl betaine, sulfobetaine and mixtures thereof.
39. The water-soluble film of any preceding claim, wherein the film has a thickness in the range of about 40 microns to about 100 microns.
40. The water-soluble film of claim 39, wherein the thickness of the first layer and the thickness of the second layer are independently in the range of about 1 micron to about 99 microns.
41. The water-soluble film of claim 40, wherein the thickness of the first layer and the thickness of the second layer are independently in the range of about 30 microns to about 70 microns.
42. The water-soluble film of claim 41, wherein the thickness of the first layer and the thickness of the second layer are independently in the range of about 20 microns to about 50 microns.
43. The water-soluble film of any one of claims 1 to 38, wherein the thickness of the first layer is in the range of about 1 micron to about 5 microns.
44. The water-soluble film of any one of claims 1 to 38 or claim 43, wherein the thickness of the second layer is in the range of about 40 microns to about 75 microns.
45. The water-soluble film according to any one of the preceding claims, wherein a film having the same composition and thickness as the first layer has a dissolution time of 300 seconds or less in water at a temperature of 20°C or less based on the MSTM-205 dissolution test method.
46. The water-soluble film according to any one of the preceding claims, wherein a film having the same composition and thickness as the first layer has a dissolution time of 200 seconds or less in water at a temperature of 20°C or less based on the MSTM-205 dissolution test method.
47. A water-soluble film according to any of the preceding claims, wherein the second layer has an outer surface, and wherein the water seal strength of the film when sealed to itself by sealing a first portion of the second layer outer surface to a second portion of the second layer outer surface is in the range of about 5N to about 18N, or is about 12N or greater based on a seal strength test.
48. The water-soluble film of any of the preceding claims, wherein the water seal strength of the film when sealed to itself by the first portion of the second layer sealed to the second portion of the second layer is in the range of about 10N to about 18N based on the Seal Strength Test.
49. The water-soluble film of any one of the preceding claims, wherein the film has a moisture vapor transmission rate of about 100 g / m per 24 hours based on the Moisture Vapor Transmission Rate test method. 2 or less, or about 50 g / m2 per 24 hours 2 or less, or about 30 g / m2 per 24 hours 2 or smaller.
50. The water-soluble film of any preceding claim, wherein the first layer and the second layer are in continuous contact with each other.
51. The water-soluble film of any preceding claim, wherein the first layer and the second layer are integrally connected.
52. The water-soluble film of any preceding claim, wherein the first layer and the second layer are bonded to each other without a separate intermediate layer between the films.
53. A water-soluble unit dose article comprising an outer wall comprising a water-soluble film according to any one of the preceding claims, wherein the outer wall comprises an outer surface and an inner surface; wherein the outer surface of the outer wall comprises the first layer of the water-soluble film, and the inner surface of the outer wall comprises the second layer of the water-soluble film; wherein said inner surface of said outer wall defines an inner bag volume; and Optionally, the inner bag volume contains a composition.
54. The water-soluble unit dose article of claim 53, wherein said article comprises a composition contained within said inner bag volume, wherein said composition is a cleaning and / or household care composition.
55. The water-soluble unit dose article of claim 53, wherein said article comprises a composition contained within said inner bag volume, wherein said composition is a non-home care composition.
56. A method for preparing a multilayer water-soluble film, the method comprising the steps of: (a) simultaneously casting at least a first water-soluble resin solution and a second water-soluble resin solution onto a surface of a substrate, wherein the second water-soluble resin solution is cast in contact with the substrate, and the first water-soluble resin solution is cast in contact with the second water-soluble resin solution, to form a multilayer structure comprising a second solution layer and a first solution layer, the second solution layer comprising the second water-soluble resin in contact with the substrate, and the first solution layer comprising the first water-soluble resin in contact with the second solution layer; (b) drying the multilayer structure to form a multilayer water-soluble film comprising at least a first layer and a second layer; as well as (c) optionally peeling the multi-layer water-soluble film from the surface of the substrate.
57. The method of claim 56, wherein the first water-soluble resin solution is an aqueous solution.
58. A method according to claim 56 or claim 57, wherein the second water-soluble resin solution is an aqueous solution.
59. The method according to any one of claims 56 to 58, wherein the first water-soluble resin solution has a water-soluble resin concentration of about 1 wt.% to 50 wt.%.
60. The method of any one of claims 56 to 59, wherein the second water-soluble resin solution has a water-soluble resin concentration of about 5 wt.% to 37 wt.%.
61. The method of any one of claims 56 to 60, wherein the surface of the substrate is metal or a coated metal.
62. The method of any one of claims 56 to 61, wherein the surface of the substrate is selected from the group consisting of stainless steel, chrome-plated steel, nickel-plated steel, galvanized steel, and combinations thereof.
63. The method of claim 62, wherein the surface of the substrate is stainless steel.
64. The method of any one of claims 56 to 63, wherein the substrate is a casting roll, a casting drum, a casting belt, or a combination thereof.
65. The method of claim 64, wherein the substrate is a casting tape.
66. The method of any one of claims 56 to 65, wherein the surface of the substrate is coated with a release coating prior to the co-casting step.
67. The method of claim 66, wherein the release coating is selected from the group consisting of non-fluorinated anionic surfactants, non-fluorinated zwitterionic surfactants, salts thereof, and combinations thereof.
68. The method of any one of claims 56 to 67, wherein the drying comprises exposing the multilayer structure to an elevated temperature environment, optionally at a temperature in the range of about 82°C to about 160°C.
69. The method of claim 68, wherein the temperature is in the range of about 100°C to about 150°C.
70. The method of any one of claims 56 to 69, wherein the drying is performed for about 60 seconds to about 20 minutes.
71. The method of any one of claims 56 to 70, wherein each of the first water-soluble resin solution and the second water-soluble resin solution has a viscosity at 175°F in a range from about 5,000 cPs to about 15,000 cPs.
72. The method according to any one of claims 56 to 71, further comprising (d) peeling the water-soluble film from the surface of the substrate.
73. The method of any one of claims 56 to 72, further comprising cooling the water-soluble film prior to said peeling the water-soluble film from the surface of the substrate.
74. The method of claim 73, wherein the cooling is performed for about 1 second to about 20 minutes.
75. The method of any one of claims 56 to 74, wherein the simultaneous casting comprises simultaneously passing the first water-soluble resin solution through a first slot of a multi-slot die and passing the second water-soluble resin solution through a second slot of the multi-slot die, and Wherein the mold angle (∠XYZ) is in the range of about 40° to about 90°, or about 45° to about 75°, or about 45° to about 55°, or about 46° to about 50°.
76. The method of claim 75, wherein the mold comprises a die lip, and wherein a distance (X1) between the die lip and the surface of the substrate is in a range of about 0.038 cm to about 0.127 cm or about 0.064 cm to about 0.0762 cm.
77. A multi-layer water-soluble film prepared by the method according to any one of claims 56 to 76.
78. The water-soluble film of claim 77, wherein each layer of the film comprises a resin selected from the group consisting of polyvinyl alcohol homopolymers, polyvinyl alcohol copolymers, and combinations thereof.
79. A water-soluble film comprising a first layer and a second layer in contact with each other, wherein the first layer comprises a first water-soluble resin comprising a methacrylate-modified polyvinyl alcohol copolymer, and the second layer comprises a second water-soluble resin comprising a blend of a maleate-modified polyvinyl alcohol copolymer and a monomethyl maleate-modified polyvinyl alcohol copolymer; wherein the first layer and the second layer are present in a ratio of about 1:200 to about 1:1, or about 1:100 to about 1:3, or about 1:20 to about 1:5, respectively, based on the total weight of the water-soluble film; wherein the first layer comprises a first surface forming an outer surface of the membrane; wherein the film exhibits a haze % of less than about 50, as determined by a Haze Test; wherein the coefficient of static friction (COF) between a first portion of the outer surface of the film and a second portion of the outer surface of the film is less than about 2, as determined by a Coefficient of Friction Test; and The first layer comprises a plasticizer, an anti-blocking agent and a surfactant, and the second layer comprises a plasticizer and a surfactant.
80. A water-soluble film comprising a first layer and a second layer in contact with each other, wherein the first layer comprises a first water-soluble resin comprising a blend of a polyvinyl alcohol copolymer modified with monomethyl maleate and a polyvinyl alcohol homopolymer, and the second layer comprises a blend of polyvinyl alcohol homopolymers; wherein the first layer and the second layer are present in a ratio of about 1:200 to about 1:1, or about 1:100 to about 1:3, or about 1:20 to about 1:5, respectively, based on the total weight of the water-soluble film; wherein the film exhibits less than 25 g H2O / m 2 MVTR per day, as measured by the Moisture Vapor Transmission Rate test; and wherein the film exhibits a heat seal strength of at least 15N as measured by the Seal Strength Test.
81. A water-soluble film comprising a first layer and a second layer in contact with each other, wherein the first layer comprises a first water-soluble resin, the first water-soluble resin comprises (a) a polyvinyl alcohol homopolymer, a polyvinyl alcohol copolymer or a mixture thereof, and (b) hydroxypropyl methylcellulose, and the second layer comprises a polyvinyl alcohol copolymer; and Wherein, based on the total weight of the water-soluble film, the first layer and the second layer are respectively present in a ratio of about 1:200 to about 1:1, or about 1:100 to about 1:3, or about 1:20 to about 1:
5.
82. The water-soluble film according to claim 81, wherein the polyvinyl alcohol copolymer of the second layer is an acrylate-modified polyvinyl alcohol copolymer.
83. The water-soluble film of claim 1, wherein the first layer comprises a foam film layer having an entrained gas fraction of at least about 5 vol%, or at least about 10 vol%, or at least about 20 vol%, or at least about 30 vol%, based on the volume of the first layer.
84. The method of claim 56, wherein the first layer comprises a foam film layer.