Polymer molded body provided with base
By designing the thermal bonding technology of the surface and base portion of the high-rigid and multi-layer structure on the polymer molded body, the problem of insufficient rigidity and scratch resistance of the polymer molded body is solved, and efficient solution in the field of food packaging is achieved plan.
Patent Information
- Application Number
- CN202380034273.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-21
- Filing Date
- 2023-04-21
- Publication Date
- 2024-12-03
AI Technical Summary
The prior art is difficult to improve the rigidity and scratch resistance of polymer molded bodies, especially in the field of food packaging. The thickness of the polymer molded bodies is prone to bending and other adverse conditions, and the thermally sensitive adhesive in the prior art is The composite layer and decorative film are difficult to effectively improve the rigidity and scratch resistance of the substrate.
By designing a polymer molded body with a base part and a thermally bonded surface part, ensuring that the surface part is more rigid than the base part and meeting a specific melting point relationship during thermal bonding, a multi-layer structure and specific polymerization are adopted. The composition, including a biaxially stretched sheet layer and a filler layer, improves the overall rigidity and scratch resistance of the molded body.
It achieves excellent rigidity and scratch resistance of polymer molded bodies, meets the needs of food packaging and other fields, and provides a lighter and superior mechanical characteristics solution.
Smart Images

Figure CN119072393A_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a polymer molded body comprising a base portion and a surface layer portion. [Background Technology]
[0002] In a wide range of technical fields, including automobiles, the replacement of metal materials with polymers is being considered. However, polymers are inferior in rigidity and scratch resistance to metal materials, so it is difficult to make such replacements in fields that require these properties. In particular, in the field of food packaging, it is necessary to reduce the thickness of the container, but after reducing the thickness, the container is easily bent, so it is difficult to put it into practical use.
[0003] However, it is a well-known technology to attach a film to the surface of a molded body to impart a function to it. For example, Patent Document 1 proposes a label for in-mold molding having a heat-sensitive adhesive layer on the back side of a biaxially stretched film. In addition, Patent Documents 2 and 3 propose a technology for attaching a decorative film to a resin molded body by thermoforming. Patent Document 4 also proposes a decorative laminated sheet, which includes a surface layer, a design layer, and an adhesive layer in sequence, wherein the adhesive layer contains a polymer having 85% by weight or more of propylene units.
[0004] [Prior art literature]
[0005] [Patent Document]
[0006] [Patent Document 1] Patent No. 3514867
[0007] [Patent Document 2] Patent No. 6943044
[0008] [Patent Document 3] Patent No. 6969176
[0009] [Patent Document 4] Japanese Patent Application Publication No. 2014-124940 [Summary of the invention]
[0010] [Problems to be Solved by the Invention]
[0011] The technology described in Patent Document 1 uses a heat-sensitive adhesive layer formed on the back side of a biaxially stretched film to adhere the biaxially stretched film to a substrate. The heat-sensitive adhesive layer uses a hot-melt resin and the like, and has low rigidity. Therefore, it is difficult to improve the rigidity and scratch resistance of the substrate by this technology. In addition, thermal bonding on the biaxially stretched film will cause partial melting of the biaxially stretched film, resulting in undesirable phenomena such as reduced rigidity. The technology specifically described in Patent Documents 2 and 3 uses polypropylene as a substrate and uses an unstretched polypropylene resin as a decorative film. Therefore, it is also difficult to improve the rigidity and scratch resistance of the substrate by this technology. Patent Document 4 does not specifically propose a polymer molded body in which a decorative laminate is actually thermally bonded to a base portion. In view of the above, the present invention is intended to provide a polymer molded body having excellent rigidity and scratch resistance.
[0012] [Solution to solve the problem]
[0013] The inventors have found that a molded body including a base portion and a specific surface layer portion thermally bonded to the base portion can solve the above-mentioned problems. Therefore, the above-mentioned problems can be solved by the present invention described below.
[0014] Form 1
[0015] A polymer molded body having a base portion and a surface layer portion thermally bonded to the base portion, which satisfies the following conditions:
[0016] 1) Gs>Gb
[0017] (Gs is the rigidity of the surface layer, and Gb is the rigidity of the base layer.)
[0018] 2) Tms<Tp
[0019] (Tms is the melting point of the bonding portion between the surface layer portion and the base portion, and Tp is the molding temperature during the thermal bonding.)
[0020] Form 2
[0021] The molded article according to aspect 1, wherein the base portion and the surface layer portion are composed of a polymer having the same repeating unit.
[0022] Form 3
[0023] The molded article according to aspect 1 or 2, wherein the surface layer portion has a multilayer structure.
[0024] Form 4
[0025] The molded article according to aspect 3, wherein the surface layer portion has a multilayer structure comprising a biaxially stretched sheet layer L having a melting point of Tml and a biaxially stretched sheet layer H having a melting point of Tmh, and
[0026] Tmh>Tml,
[0027] The biaxially stretched sheet layer L forms the bonding surface.
[0028] Form 5
[0029] The molded article according to aspect 4, wherein the layer H is composed of
[0030] Polypropylene resin (A) or
[0031] The invention comprises a resin composition comprising a polypropylene resin (A) and a plate-like inorganic filler (B), wherein the weight ratio of component (B) / [component (A)+component (B)] is greater than 0 weight % and less than 60 weight %.
[0032] Form 6
[0033] The molded article according to aspect 5, wherein
[0034] The polypropylene resin (A) comprises a polypropylene resin consisting of a component (A1) and an optional component (A2),
[0035] The component (A1) is 100 to 50% by weight of a propylene (co)polymer, and the (co)polymer contains 0 to 10% by weight of comonomer-derived units selected from C2 to C10-alpha olefins (but excluding C3-alpha olefins);
[0036] Component (A2) is 0 to 50% by weight of an ethylene-α-olefin copolymer, and the copolymer contains 10 to 90% by weight of ethylene-derived units;
[0037] The MFR (230°C, load 2.16 kg) of the polypropylene resin (A) is 1 to 15 g / 10 minutes.
[0038] Form 7
[0039] The molded article according to any one of aspects 4 to 6, wherein the outermost surface of the surface layer portion includes a top layer other than the biaxially stretched sheet layers L and H.
[0040] Form 8
[0041] The molded article according to any one of aspects 4 to 7, wherein the ratio of the total thickness of the layer L to the thickness of the surface layer portion is 1 to 50%.
[0042] Form 9
[0043] The molded article according to any one of aspects 4 to 8, wherein the surface layer portion has alternate layers in which the layer L and the layer H are alternately laminated.
[0044] Form 10
[0045] The molded article according to any one of aspects 1 to 9, wherein the surface layer portion has a thickness of 30 μm or more.
[0046] Form 11
[0047] In the molded article according to any one of aspects 1 to 10, the thickness of the base portion is 5 to 250 times the thickness of the surface layer portion.
[0048] Form 12
[0049] The method for producing a molded article according to any one of aspects 1 to 11, wherein the method comprises:
[0050] Step 1 of preparing the surface layer portion, and
[0051] Step 2 of forming the base portion by thermoforming the base portion raw material and thermally bonding the surface layer portion to the surface thereof.
[0052] Form 13
[0053] The manufacturing method according to aspect 12, wherein the step 2 comprises:
[0054] the step of arranging the surface layer portion in a mold cavity, and
[0055] The step of forming the base portion by injection molding the base portion material in the cavity and thermally bonding the surface layer portion on the surface of the base portion.
[0056] [Effects of the invention]
[0057] According to the present invention, a polymer molded body having excellent rigidity and scratch resistance can be provided. [Drawings]
[0058] Figure 1 is a schematic diagram of one embodiment of a polymer molding.
[0059] Figure 2 FIG. 1 is a schematic diagram of another embodiment of a polymer molded article.
[0060] Figure 3A It is a schematic diagram of one embodiment of the surface layer portion.
[0061] Figure 3B is a schematic diagram of another embodiment of the surface layer portion.
[0062] Figure 4 It is a schematic diagram of an embodiment of a method for manufacturing a surface layer portion.
[0063] Figure 5It is a schematic diagram schematically showing another embodiment of the method for manufacturing a surface layer portion.
[0064] Figure 6 This is a schematic diagram schematically showing one embodiment of a method for producing a polymer molded article.
[0065] Figure 7 It is an explanatory diagram of a slice for measuring the residual rate R. [Specific implementation method]
[0066] The present invention is described in detail below. In the present invention, "X to Y" include their end values, i.e., X and Y. In the present invention, sheet and film have the same meaning, but a film-like component with a thickness of 150 μm or more is sometimes referred to as a sheet, and a film-like component with a thickness of less than 150 μm is sometimes referred to as a film. In addition, sheets and films are sometimes collectively referred to as "sheet-like components".
[0067] 1. Polymer moldings
[0068] The polymer molded body in this embodiment comprises a base portion and a surface portion thermally bonded to the base portion. That is, the base portion and the surface portion are welded. The base portion refers to the portion that forms the matrix of the polymer molded body. The surface portion is formed on the base portion and imparts functions to the molded body. Such functions may include improving rigidity or improving scratch resistance.
[0069] (1) Base part and surface part
[0070] The base part and the surface part satisfy the relationship of Gs>Gb. Gs is the rigidity of the surface part, and Gb is the rigidity of the base part. The rigidity is measured according to a well-known method. For example, the rigidity is preferably the bending modulus measured by a bending test (JIS K6921-2), or the tensile modulus measured by a tensile test (JIS K7161). The surface part can be a single-layer structure or a multi-layer structure. If the surface part has a multi-layer structure, Gs means the rigidity of all layers as a whole. The same is true for the base part. The base part and the surface part of the polymer molded body have unchanged properties before and after bonding. Therefore, the rigidity of the surface part and the base part before bonding can be used as Gs and Gb, respectively. In addition, as described later, the base part can be thermally bonded to the surface part by injection molding such as insert molding. At this time, the rigidity of the base part that is not thermally bonded to the surface part but is thermally molded alone can be used as Gb.
[0071] The polymer molded product preferably has a rigidity of 1400 MPa or more, more preferably 1500 MPa or more, further preferably 1600 MPa or more, further preferably 1800 MPa or more, and particularly preferably 2000 MPa or more in any direction at 23°C. In addition, the polymer molded product preferably has a rigidity of 300 MPa or more, more preferably 500 MPa or more in any direction at 100°C. There is no upper limit on the rigidity of the polymer molded product, but it should be 5000 MPa or less in any direction at 23°C and 2000 MPa or less at 100°C.
[0072] Gs and Gb are set to ensure that this rigidity can be achieved. In one embodiment, Gs and Gb should meet the following requirements in any direction.
[0073] At 23°C, the lower limit of Gs is preferably 2000 MPa or more, more preferably 2200 MPa or more, and further preferably 2500 MPa or more. The upper limit of Gs is preferably 7000 MPa or less, and more preferably 6000 MPa or less. At 100°C, the lower limit of Gs is preferably 500 MPa or more, and more preferably 1000 MPa or more; the upper limit is preferably 3000 MPa or less, and more preferably 2000 MPa or less.
[0074] At 23°C, the lower limit of Gb is preferably 1000 MPa or more, more preferably 1500 MPa or more; the upper limit is preferably 5000 MPa or less, more preferably 3000 MPa or less. At 100°C, the lower limit of Gb is preferably 200 MPa or more, more preferably 300 MPa or more; the upper limit is preferably 2000 MPa or less, more preferably 1500 MPa or less.
[0075] The base part and the surface part satisfy the relationship of Tms<Tp. Tms is the melting point of the joining part between the surface part and the base part, and Tp is the molding temperature during thermal bonding. After satisfying the relationship of Tms<Tp, the surface part and the base part can be thermally bonded. When the surface part has a multi-layer structure, Tms is the melting point of the representative layer of the joining part between the surface part and the base part. The representative layer refers to, in one embodiment, the layer with the highest melting point among multiple layers or the layer with the highest weight ratio among multiple layers. The melting point is measured by a well-known thermal analysis method. For example, it is preferred to use DSC to measure the melting point. At this time, it is preferably measured under the condition of a heating rate of 10℃ / minute from 30℃ to 230℃. As with the aforementioned rigidity, the melting point of the surface part before bonding can be used as Tms.
[0076] The state of the surface part may change before and after thermal bonding. The residual rate is used as an indicator of the degree to which the surface part maintains its original state. The residual rate will be explained in detail later.
[0077] Tp is the molding temperature during thermal bonding. When the base portion and the surface portion are thermally bonded by press molding or vacuum molding, Tp is the temperature of the base portion during molding. In addition, when the base portion and the surface portion are thermally bonded by injection molding, that is, when the two are thermally bonded by insert molding, Tp is the temperature of the molten polymer of the base portion ejected from the molding machine nozzle. Tp can be measured using a thermocouple or infrared rays.
[0078] There is no limit to the thickness of the surface layer, but if it is too thin, it is easy to have insufficient rigidity and impact resistance, and if it is too thick, it will cause manufacturing difficulties. Based on the above viewpoints, the lower limit of the thickness is preferably 30 μm or more, more preferably 80 μm or more, and more preferably 100 μm or more. The upper limit of the thickness is preferably 500 μm or less, more preferably 400 μm or less, and further preferably 300 μm or less.
[0079] The thickness of the base portion can be appropriately adjusted depending on the application, but from the viewpoint of ease of production, the thickness is preferably 5 to 250 times, more preferably 10 to 100 times, the thickness of the surface layer portion.
[0080] In one embodiment, the thickness of the polymer molded article is preferably 0.1 to 5 mm, more preferably 1 to 4 mm, and even more preferably 1.5 to 3.5 mm. The thickness in the present invention is defined as the average value of the part.
[0081] In general, the bonding strength between the surface layer and the base of the thermal bond is difficult to quantify, but in one embodiment, the peel strength can be used as an indicator. The peel strength is preferably 7N / 15mm, more preferably 10N / 15mm, and more preferably 100N / 15mm or more. The peel strength can be obtained by a 180-degree peel test at 23°C using a short strip test piece with a width of 15mm. There is no upper limit to the peel strength, but it is preferably less than 200N / 15mm. In one embodiment, the distance between the clamps is 50mm, the moving speed of the clamps is 300mm / minute, the tensile length is 100mm, and the average test force of the stable interval of 50mm when the material is destroyed is used as the test value.
[0082] The base part and the surface part can be composed of any polymer. However, considering the affinity between the two, the base part and the surface part are preferably composed of the same polymer, and more preferably composed of a polymer having the same repeating unit. Such polymers include polyolefins, engineering plastics and super engineering plastics. Polyolefins include polypropylene and polyethylene. Engineering plastics include polyesters such as PET. Super engineering plastics include PES resins or PEEK resins.
[0083] (2) Preferred first embodiment
[0084] The surface layer is preferably composed of a stretched sheet member. The stretching may be uniaxial stretching or multiaxial stretching, preferably biaxial stretching. At this time, the surface layer preferably has a multilayer structure, and the multilayer structure has a biaxial stretching sheet L with a melting point of Tml and a biaxial stretching sheet H with a melting point of Tmh. However, Tmh>Tml. The biaxial stretching sheet L is preferably connected to the base portion.
[0085] This embodiment is as Figure 1 As shown. In the figure, 1 is the surface layer, 10 is the base layer, and 100 is the polymer molded body. In the figure, H is the biaxially stretched sheet H, and L is the biaxially stretched sheet L. The surface layer preferably has an alternating layer of biaxially stretched sheet H and biaxially stretched sheet L alternately laminated. In this case, layer L is preferably the bonding surface with the base portion. The layers of the surface layer 1 are mutually fused and integrated. This can be confirmed by cross-sectional observation using a polarizing microscope as described in International Publication No. 2020 / 075755.
[0086] 1) Surface part
[0087] [Multi-layer structure]
[0088] At least a part of all the layers of the surface layer 1 may be composed of a co-extruded layer obtained by alternately laminating a biaxially stretched sheet layer H and a biaxially stretched sheet layer L obtained by co-extrusion molding. The manufacturing method will be described in detail later.
[0089] The total number of layers of the surface layer portion 1 is preferably 2 to 50. The total number of layers within this range shows excellent moldability. In an embodiment in which the surface layer portion 1 includes a coextruded layer, the thickness of the coextruded layer is preferably 0.04 to 0.50 mm. In addition, the total number of layers of the coextruded layer is preferably 1 to 6, and more preferably 1 to 3.
[0090] The total thickness (total thickness) of the biaxially stretched sheet L in the thickness of the surface part 1 is not particularly limited, but from the viewpoint of easy manufacturability and cost, the thickness is preferably 2 to 120 μm, more preferably 5 to 60 μm, and further preferably 10 to 30 μm. The thickness of each layer can be the same or different. If the proportion of the total thickness of the layer L in the thickness of the surface part (the total thickness of the layer L / the thickness of the surface part) is too small, the weldability between the layers of the multilayer sheet will be insufficient; if the proportion is too large, the rigidity of the multilayer sheet will be insufficient. From the perspective of weldability and rigidity balance, the total thickness of the layer L / the thickness of the surface part is preferably 1 to 50%. Appropriate adjustments can be made to make the thickness of each layer reach the ratio. The thickness of each layer of the biaxially stretched sheet H is preferably 20 to 300 μm. The thickness of each layer of the biaxially stretched sheet L is preferably 2 to 40 μm. However, as described later, the surface layer portion 1 is sometimes formed by preparing a plurality of multilayer sheets including a biaxially stretched sheet layer L, placing the biaxially stretched sheet layers L in contact with each other, and heating and welding them. At this time, the thickness of each layer of the biaxially stretched sheet layer L in the surface layer portion 1 is 4 to 80 μm.
[0091] Tmh-Tml is not limited, but is preferably 1°C or more, more preferably 10°C or more, and further preferably 25°C or more. In addition, Tmh-Tml is preferably 60°C or less. If the melting points of Tmh and Tml are too low, the rigidity and heat resistance of the surface layer portion 1 may be insufficient. From this viewpoint, Tml is preferably 160°C or more, more preferably 165°C or more, and Tml is preferably 100°C or more, more preferably 120°C or more, and further preferably 130°C or more. These melting points can be measured using DSC at a temperature increase rate of 10°C / min from 30°C to 230°C.
[0092] Functional groups can be imparted to the layer constituting the surface layer 1. Preferably, functional groups are imparted to the outermost layer constituting the surface layer 1. As the functional group, an oxygen-containing functional group is preferred. As the oxygen-containing functional group, carboxyl group, carboxylate group, acid anhydride group, hydroxyl group, aldehyde group or epoxy group can be cited. These functional groups can improve the adhesion between the surface layer 1 and other materials.
[0093] [Top]
[0094] The outermost surface of the surface layer 1 may have a top layer other than the biaxially stretched sheets L and H. Figure 2As shown. In the figure, T is the top layer. For example, the purpose of setting the top layer is to impart design, etc. The top layer is preferably a coating film used in vehicle body spraying. Such coating films include epoxy coating films, polyurethane coating films or polyester coating films. As needed, a lower coating film (primer coating film), a middle coating film or an upper coating film (transparent coating film) may also be provided. When a multilayer sheet is used as a sheet for painting (brushing sheet), the surface to be sprayed preferably has a functional group.
[0095] [Polymer constituting the biaxially stretched sheet layer H]
[0096] From the viewpoint of providing the surface layer with excellent rigidity and scratch resistance, the biaxially stretched sheet H is preferably composed of a polypropylene resin (A). The polypropylene resin (A) is composed of 100 to 50% by weight of a component (A1) and 0 to 50% by weight of any component (A2). If the component (A2) exceeds 0% by weight, the component (A) may be a polymer obtained by polymerizing the component (A1) and then polymerizing the component (A2) under the condition in which the component exists, i.e., a heterophasic copolymer (HECO), or a mixture of the component (A1) and the component (A2) prepared by separate polymerization. However, from the viewpoint of obtaining the component (A) through fewer manufacturing steps, the component (A) is preferably HECO.
[0097] Component (A1) is a propylene (co)polymer containing 0 to 10 wt% of comonomer-derived units, which are selected from C2 to C10 α-olefins (but excluding C3 α-olefins). The comonomer selected from C2 to C10-α-olefins naturally does not include C3-α-olefins. In the case of containing comonomers, ethylene is preferred from the viewpoint of economy. If the amount of the comonomer-derived units exceeds the upper limit, the rigidity of the surface portion may be reduced. From this viewpoint, component (A1) preferably does not contain comonomer-derived units, that is, a propylene homopolymer. Alternatively, if component (A1) contains comonomer-derived units, the amount thereof is preferably greater than 0 wt% and less than 1 wt%.
[0098] In the polypropylene resin, the content of component (A1) is 50 to 100 weight %. If the content of component (A1) is too small, the polypropylene resin may become difficult to manufacture or the rigidity of the surface layer may be reduced. Therefore, the content of component (A1) is preferably 60 to 100 weight %, more preferably 70 to 100 weight %.
[0099] The MFR (230°C, load 2.16 kg) of the polypropylene resin (A) is 1 to 15 g / 10 minutes. If the MFR exceeds the upper limit, the preparation of the raw material of the surface layer, i.e., the biaxially stretched polypropylene sheet component, becomes difficult; if it is lower than the lower limit, the production capacity of the polypropylene resin (A) is reduced. From this point of view, the lower limit of the MFR is preferably 2 g / 10 minutes or more, more preferably 3 g / 10 minutes or more; the upper limit is preferably 10 g / 10 minutes or less, more preferably 8 g / 10 minutes or less.
[0100] The optional component (A2) is an ethylene-α-olefin copolymer containing 10 to 90% by weight of ethylene-derived units. If the ethylene-derived units are below the lower limit or above the upper limit, the cold impact resistance will be reduced. From this point of view, the content of ethylene-derived units is preferably 15 to 85% by weight, more preferably 20 to 80% by weight. The α-olefin is not limited as long as it is not ethylene, and is preferably propylene, 1-butene, 1-hexene or 1-octene, more preferably propylene, 1-butene, and further preferably propylene.
[0101] In the polypropylene resin (A), the content of component (A2) is 0 to 50% by weight. If the content of component (A2) is too much, the production capacity of the polypropylene resin (A) will decrease. Therefore, the content of component (A2) is preferably 0 to 40% by weight, and more preferably 0 to 30% by weight.
[0102] Furthermore, the polypropylene resin (A) may be a propylene random copolymer (RACO) containing 0 to 5 wt% of comonomer-derived units selected from C2 to C10 α-olefins (but excluding C3 α-olefins).
[0103] Biaxially stretched sheet H can also be made of the resin composition containing nucleator. Nucleator refers to the additive (transparent nucleator) for improving transparency by controlling the size of the crystalline component in the resin to be smaller. Therefore, containing nucleator can promote the transparency of biaxially stretched sheet H. From the viewpoint of economy, if the polymer forming biaxially stretched sheet H is 100 weight parts, the amount of nucleator is preferably below 0.5 weight part, more preferably below 0.2 weight part, further preferably below 0.1 weight part. Nucleator is not particularly limited, and can use the commonly used nucleator in this field, preferably selected from nonesol nucleator, sorbitol nucleator, phosphate nucleator, triaminobenzene derivative nucleator, carboxylic acid metal salt nucleator and xylitol nucleator.
[0104] [Polymer constituting the biaxially stretched sheet layer L]
[0105] The biaxially stretched sheet L is preferably formed by a propylene random copolymer (RACO) or a resin composition containing the RACO, wherein the RACO contains at least one comonomer of less than 10% by weight, and these comonomers are selected from C2 to C10-α olefins (but excluding C3-α olefins). If the comonomer content of RACO is too little, the weldability with the substrate or the weldability with other layers when the surface layer is formed by multiple layers may be insufficient; and if the content is too much, the rigidity of the multilayer sheet may be reduced. From this point of view, the comonomer content is preferably greater than 0% by weight and less than 4.5% by weight. The comonomer is preferably ethylene (C2-α olefin). The MFR (230°C, load 2.16kg) of the polymer or resin composition constituting the biaxially stretched sheet L is not limited, but is preferably 1 to 15g / 10 minutes, more preferably 2 to 10g / 10 minutes, and further preferably 3 to 8g / 10 minutes.
[0106] Biaxially stretched sheet L can be made of the resin combination containing nucleator, and can also be made of the resin combination or polymer that do not contain nucleator.When containing nucleator, from the viewpoint of economy, if the polymer that forms biaxially stretched sheet L is 100 weight parts, then the amount of nucleator is preferably below 1 weight part.
[0107] [additive]
[0108] The resin composition constituting the layer may contain antioxidants, chlorine absorbers, heat stabilizers, light stabilizers, ultraviolet absorbers, internal lubricants, external lubricants, antiblocking agents, antistatic agents, antifogging agents, flame retardants, dispersants, copper inhibitors, neutralizers, plasticizers, crosslinking agents, peroxides, oil extensions and other organic and inorganic pigments and other conventional additives commonly used in polyolefins. The amount of each additive added may be a known amount. In addition, within the scope of not impairing the effect of the present invention, synthetic resins or synthetic rubbers other than polypropylene may also be contained. The synthetic resin or synthetic rubber may be one kind, or may be two or more kinds.
[0109] 2) Base part
[0110] The base portion is composed of the aforementioned polymer, but is preferably composed of the same polymer as the surface layer portion, more preferably composed of a polymer having the same repeating unit, and more preferably composed of a polypropylene-based resin.
[0111] (3) Preferred Second Embodiment
[0112] In this embodiment, the biaxially stretched sheet H contains a polypropylene resin (A) and a plate-like inorganic filler (B), and is composed of a resin composition in which the weight ratio of component (B) / [component (A)+component (B)] is greater than 0 wt% and less than 60 wt%.
[0113] [Multi-layer structure]
[0114] The surface layer part in the present embodiment preferably has a multilayer structure of alternate lamination of biaxially stretched sheet layer H and biaxially stretched sheet layer L. Hereinafter, in the present embodiment, biaxially stretched sheet layer H is also referred to as "filler layer F", and biaxially stretched sheet layer L is also referred to as "surface layer N". Since each layer is welded, the surface layer part is integrated.
[0115] This embodiment is as Figure 1 In the figure, 1 is the surface layer, 10 is the base layer, F and N are the filler layer F and the surface layer N, which are respectively equivalent to the biaxially stretched sheet layer H and the biaxially stretched sheet layer L in the first embodiment.
[0116] As described later, the filler layer F in the surface layer portion is derived from the biaxially stretched polypropylene sheet member used for this layer, and the surface layer N is derived from the biaxially stretched polypropylene sheet member used for this layer. Each layer can be composed of an independent sheet member. For details of the surface layer portion, see Figure 3A In the figure, 1' is a precursor described later. The layers of the precursor 1' are welded to form a surface layer portion 1.
[0117] At least a portion of all the layers may be composed of coextruded layers formed by alternately laminating filler layers F and surface layers N obtained by coextrusion molding. Figure 3B As shown. In the figure, C represents a coextruded layer, such as C[N / F], which is a coextruded layer having two layers, a surface layer N and a filler layer F. There are three pieces of C[N / F / N] precursors 1' between C[F / N] and C[N / F], forming the surface layer part 1. The thickness of each C can be the same or different. In addition, the thickness of the layers constituting each C can be the same or different.
[0118] The total number of layers in the surface layer portion is 2 to 50. The total number of layers within this range exhibits excellent moldability. Figure 3B In the embodiment, the total number of layers in the surface layer portion is 11 layers. In addition, in the embodiment including the coextruded layer, the thickness of the coextruded layer is preferably 0.04 to 0.50 mm. In addition, the total number of coextruded layers is preferably 2 to 6 sheets, more preferably 2 to 5 sheets, further preferably 2 to 4 sheets, and particularly preferably 2 to 3 sheets. The thickness of the coextruded layer refers to the thickness of the entire C ( Figure 3B In the Figure 3B In the case of , the total number of co-extruded layers is 5.
[0119] If the ratio DF / DN of the total thickness (total thickness) DF of the filler layer F and the total thickness (total thickness) DN of the surface layer N is too small, the rigidity of the surface part will be insufficient; if it is too large, the weldability between the surface part and the base part and between the layers of the surface part will be insufficient. From the balance between weldability and rigidity, the ratio is preferably 1 to 30, more preferably 1 to 25, and further preferably 4 to 15. The thickness of each layer can be the same or different. And the thickness of each layer can be appropriately adjusted so that the ratio is within the range. The thickness of one layer of the filler layer F is preferably 50μm to 200μm. The thickness of one layer of the surface layer N is preferably 5μm to 40μmm.
[0120] The melting point TmF of the filler layer F and the melting point TmN of the surface layer N satisfy the relationship of TmF>TmN. That is, Tmh in the first embodiment is equivalent to TmF, and Tml is equivalent to TmN. TmF-TmN is not limited, but is preferably above 1°C, more preferably above 10°C, and further preferably above 25°C. In addition, TmF-TmN is preferably below 60°C. If these melting points are too low, the rigidity and heat resistance of the multilayer sheet become insufficient. From this point of view, TmF is preferably above 160°C, more preferably above 165°C; TmN is preferably above 100°C, more preferably above 120°C, and further preferably above 130°C. These melting points can be measured using DSC at a heating rate of 10°C / min from 30°C to 230°C.
[0121] [Resin composition constituting filler layer F]
[0122] The filler layer F is formed of a resin composition containing a polypropylene resin (A) and an inorganic filler (B). The polypropylene resin (A) is as described above.
[0123] The purpose of adding the inorganic filler (B) is mainly to improve the rigidity of the material. From the viewpoint of the substance, examples of the inorganic filler include the following.
[0124] Natural silicic acid or silicates such as talc, kaolin, clay, pyrophyllite, selenite, wollastonite, and mica; synthetic silicic acid or silicates such as hydrated calcium silicate, hydrated aluminum silicate, hydrated silicic acid, and anhydrous silicic acid; carbonates such as precipitated calcium carbonate, heavy calcium carbonate, and magnesium carbonate; hydroxides such as aluminum hydroxide and magnesium hydroxide; oxides such as zinc oxide and magnesium oxide.
[0125] In addition, as the inorganic filler, from the viewpoint of shape, for example, the following materials can be mentioned.
[0126] Powdered filling materials such as synthetic silicates or silicates such as hydrated calcium silicate, hydrated aluminum silicate, hydrated silicic acid, anhydrous silicic acid, etc.; plate-like filling materials such as talc, kaolin, clay, and mica; whisker-like filling materials such as basic magnesium sulfate whiskers, calcium titanate whiskers, aluminum borate whiskers, sepiolite, PMF (Processed Mineral Filler), xonotlite, potassium titanate, and silicate apatite; balloon-like filling materials such as glass balloons and fly ash balloons; fibrous filling materials such as glass fibers.
[0127] As the inorganic filler, one kind can be used, or two or more kinds can be used in combination. In order to improve the dispersibility of these fillers, the surface treatment of the inorganic filler can also be carried out as needed. The inorganic filler used in the present invention is not limited, but from the viewpoint of improving rigidity and impact resistance by promoting the orientation of polypropylene crystals in the filler layer F along the direction of the sheet surface, it is preferably a plate-like inorganic filler. Conventional materials such as talc, kaolin, clay, and mica can be used for the plate-like inorganic filler, but considering the affinity with polypropylene resins and the convenience and economy of purchasing raw materials, talc and mica are preferably used, and talc is further preferably used. The volume average particle size of the plate-like inorganic filler is preferably 1 to 10 μm, and more preferably 2 to 7 μm. If the volume average particle size is lower than the lower limit, the rigidity of the filler layer F may be reduced. If the volume average particle size is higher than the upper limit, it is easy to break during stretching, making it difficult to prepare a biaxially stretched sheet-like component as a multilayer sheet raw material. The volume average particle size can be measured by a laser diffraction method (based on JIS R1629) as a 50% diameter in a cumulative fraction on a volume basis.
[0128] [Weight ratio of components (A) and (B)]
[0129] The weight ratio of the components (A) and (B) in the filler layer F is as follows.
[0130] Component (B) / [Component (A) + Component (B)] = more than 0% by weight, 60% by weight or less
[0131] If the amount of component (B) is small, the rigidity of the multilayer sheet is insufficient, and if the amount of component (B) is large, it is difficult to produce the multilayer sheet. From this viewpoint, the weight ratio is preferably 5 to 55% by weight, more preferably 10 to 55% by weight, and further preferably 20 to 55% by weight.
[0132] [Polymer or resin composition constituting the surface layer N]
[0133] The surface layer N is formed by a resin composition containing component (A), i.e., a polypropylene resin, and any of the above-mentioned components (B). The component (A) here should be selected to satisfy the relationship between TmF and TmN. It is preferred to select a propylene homopolymer (HOMO) or a propylene random copolymer (RACO) containing less than 5% by weight of at least one comonomer, wherein these comonomers are selected from C2 to C10-α olefins (but excluding C3-α olefins); or they are selected from a combination of these HOMOs and RACOs. If the amount of the comonomer-derived unit is too small, the weldability between the base portion and the filler layer F may be insufficient; if the amount is too large, the rigidity of the multilayer sheet may be reduced. From this point of view, the amount of the comonomer-derived unit is preferably greater than 0% by weight and less than 10% by weight. The comonomer is preferably ethylene (C2-α olefin).
[0134] The MFR (230°C, load 2.16 kg) of the polymer or resin composition constituting the surface layer N is preferably 1 to 15 g / 10 minutes, more preferably 2 to 10 g / 10 minutes, and further preferably 3 to 8 g / 10 minutes. If the MFR is too small, the production capacity of the polypropylene resin as a raw material will be reduced; if it is too large, it may break during biaxial stretching, resulting in the inability to stably produce a multilayer sheet as a raw material for the surface layer.
[0135] [Weight ratio of components (A) and (B)]
[0136] The weight ratio of the components (A) and (B) in the surface layer N is as follows.
[0137] Component (B) / [Component (A)+Component (B)]=0-10% by weight
[0138] In particular, in the manufacture of multilayer sheets, when a process of preparing a raw material sheet by coextrusion is included, if the amount of component (B) in the raw material sheet N" (equivalent to the surface layer N of the multilayer sheet) is large, the strength of the raw material sheet may be reduced, so the weight ratio is preferably 8 weight % or less. The weight ratio is more preferably 5 weight % or less, further preferably 1 weight % or less, particularly preferably 0.5 weight % or less, and most preferably 0 weight %. In addition, the weight ratio in the surface layer N is smaller than the weight ratio in the filler layer F.
[0139] The filler layer F and the surface layer N may contain the aforementioned nucleating agent or additive.
[0140] (4) Survival rate
[0141] As mentioned above, the residual rate is an indicator of the degree to which the surface layer portion maintains its original state before and after thermal bonding. The residual rate is measured by conventional analytical methods such as DSC, X-ray diffraction or density method. For example, when DSC is used, the residual rate can be expressed by the area ratio of each melted component in the DSC chart obtained from the portion in contact with the base portion and the portion not in contact with the surface.
[0142] For example, the survival rate R associated with the high-order structure is defined using ΔHin / ΔHout.
[0143] ΔHout is the heat value obtained by DSC analysis of the surface vicinity of the surface layer of the polymer molded body. ΔHout is an indicator of the state of the high-order structure before thermal bonding. Specifically, ΔHout is measured by the following method.
[0144] 1) A portion having a thickness of 10 to 50% is collected from the surface of the surface layer portion on the opposite side to the base portion.
[0145] 2) The collected samples are subjected to DSC analysis under elevated temperature conditions, and the heat (J / g) within the range of ±5°C of the melting point in the melting profile curve is obtained, which is taken as ΔHout. Including the case where the surface layer is composed of the biaxially stretched sheet layer L and the biaxially stretched sheet layer H, the heat (J / g) within the range of ±5°C of Tmh is taken as a representative, which is taken as ΔHout. The melting point is the peak temperature in the melting profile curve.
[0146] ΔHin is the heat value obtained by DSC analysis of the interface vicinity of the surface layer of the polymer molded body. ΔHin is an indicator of the state of the high-order structure after thermal bonding. Specifically, ΔHin is measured by the following method.
[0147] 1) A portion having a thickness of 10 to 50% is collected from the interface between the surface layer and the base layer.
[0148] 2) The collected samples are subjected to DSC analysis under elevated temperature conditions, and the heat (J / g) within the melting point ±5°C range in the melting profile curve is obtained, which is taken as ΔHin. Including the case where the surface layer is composed of the biaxially stretched sheet L and the biaxially stretched sheet H, the heat (J / g) within the range of Tmh ±5°C is represented and taken as ΔHin.
[0149] The larger the value of R (ΔHin / ΔHout), the longer the high-order structure of the surface layer is maintained after thermal bonding. The value of the residual rate is not limited, but is preferably 60 to 100%, and its lower limit is more preferably 70% or more, 80% or more, 90% or more, or 95% or more. The value of ΔHin is not limited, but is preferably 5 to 8 J / g.
[0150] 2. Manufacturing method
[0151] The polymer molded article is preferably produced by a production method comprising the steps of preparing the surface layer portion 1, thermoforming the base portion raw material to form the base portion, and simultaneously thermally bonding the surface layer portion to the surface thereof 2.
[0152] (1) Process 1
[0153] This process will be described by taking the above-mentioned preferred second embodiment as an example. This manufacturing method and multilayer sheet are proposed in PCT / JP2021 / 041525. The contents of this document are cited in this specification.
[0154] As for the surface layer, it is preferred to prepare a multilayer sheet having the aforementioned filler layer F and surface layer N. The multilayer sheet is preferably manufactured by a method having the following steps: step i: preparing a precursor formed by laminating a filler layer F and a surface layer N in a manner such that the filler layers F are not adjacent to each other; step ii: allowing a heating body to contact the outermost layer of the precursor to heat and fuse the layers of the sheet. The melting point TmF of the filler layer F and the melting point TmN of the surface layer N satisfy the relationship of TmF>TmN, preferably satisfying the relationship of TmF-TmN≥1(℃). Due to the difference in melting points, the adhesion between the layers is better. Next, refer to Figure 4 and Figure 5 Each process is explained. In the figure, f and n are the resin compositions that ultimately constitute layer F and layer N. F" and N" are the unstretched sheets (raw sheets) that ultimately constitute layer F and layer N. F' and N' are biaxially stretched sheet components that ultimately constitute layer F and layer N. 1' is a precursor, 1 is a multilayer sheet, F is a filler layer, and N is a surface layer. In addition, 2 is the unstretched sheet preparation process, 3 is the stretching process, 4 is the lamination process, and 5 is the interlayer welding process. The melting points Tmf and Tmn of the resin composition, the melting points TmF" and TmN" of the unstretched sheet, the melting points TmF' and TmN' of the biaxially stretched sheet component, and the melting points TmF and TmN of the layer have the following relationship.
[0155] Tmf=TmF”
[0156] TmF'=TmF=Tmf+x(℃)
[0157] Tmn=TmN”
[0158] TmN'=TmN=Tmn+y(℃)
[0159] Although x and y vary depending on the stretching state and the like, they are each independently preferably 1 to 10°C, more preferably about 2 to 7°C.
[0160] 1) Process i
[0161] In this step, the precursor is prepared. A part of the layers constituting the precursor may be constituted by the aforementioned co-extruded layer. All layers of the precursor are not fused or are partially fused.
[0162] This step can be performed, for example, by separately preparing a biaxially stretched polypropylene sheet member F' for the filler layer F and a biaxially stretched polypropylene sheet member N' for the surface layer N and alternately laminating them. For example, the precursor 1' can be prepared by laminating in the order of N' / F' / N' / ... / N'. In this case, it is preferred that all layers are not fused.
[0163] One implementation method of this process is as follows Figure 4 As shown. In this embodiment, biaxially stretched polypropylene sheet components F' and N' are prepared separately and alternately laminated to prepare the precursor 1'. At this time, in this case, preferably, all layers are not fused, but one or more layers may be fused. From the viewpoint of improving the thermal adhesion with the obtained sheet base portion, at least one side of the outermost layer is preferably a biaxially stretched polypropylene sheet component N'.
[0164] The biaxially stretched polypropylene sheet component N' can be prepared by conventional methods. For example, a raw sheet (unstretched polypropylene sheet component N") can be prepared from a raw resin composition n, and biaxially stretched by a conventional method to obtain a biaxially stretched polypropylene sheet component N'. The thickness of the raw sheet is preferably greater than 0.15 mm, and there is no upper limit, but it is preferably 6 mm or less from the viewpoint of ease of operation. The temperature during biaxial stretching is not limited, but is preferably in the range of (TmN"-10°C) to TmN".
[0165] The biaxially stretched polypropylene sheet member F' can be produced in the same manner as the biaxially stretched polypropylene sheet member N'. However, when the biaxially stretched polypropylene sheet member F' contains an inorganic filler, the temperature V during biaxial stretching preferably satisfies the following relationship in order to contain more inorganic filler than N'.
[0166] -3≤V-TmF”≤3
[0167] TmF" is the melting point (°C) of the raw material sheet. The melting point Tmf of the resin composition can be determined by DSC measurement at a heating rate of 10°C / min from 30°C to 230°C, and TmF" can be determined based on the aforementioned relationship of Tmf=TmF".
[0168] The thickness of the raw material sheet is preferably greater than 0.15 mm, and there is no upper limit, but it is preferably less than 6 mm from the viewpoint of ease of operation. In addition, from the viewpoint of rigidity, the stretching ratio is preferably 4 to 8 times of one axis. The ratio of one axis and the ratio of the other axis may be the same or different. The two axes are preferably orthogonal.
[0169] This step is preferably carried out using a coextruded sheet member having layer F and layer N. In this case, step ii can be omitted or simplified. Figure 5 The figure shows a simplified implementation method. Specifically, the raw material of layer F and the raw material of layer N are coextruded to prepare a coextruded raw material sheet C" having multiple layers, and the coextruded raw material sheet C" is biaxially stretched to prepare a coextruded biaxially stretched sheet component C'. The temperature V when the coextruded raw material sheet C" is biaxially stretched preferably satisfies the above relationship. Next, a plurality of coextruded biaxially stretched sheet components C', or a coextruded biaxially stretched sheet component C' is laminated with the aforementioned biaxially stretched sheet component F' or N' to prepare a precursor 1'. At this time, the total number of coextruded layers in the precursor 1' is not limited, but is preferably 2 to 6 layers. The thickness of the coextruded biaxially stretched sheet component C' is preferably 0.01 to 0.50 mm, and more preferably 0.02 to 0.50 mm.
[0170] like Figure 5 As shown, a precursor is prepared by laminating a plurality of coextruded biaxially stretched sheet members C', and a 5-layer multilayer sheet can be produced by welding the central N layers.
[0171] Precursor: C'[N / F / N] / C'[N / F / N]
[0172] Multilayer sheet: N / F / N / F / N
[0173] Each of the single-layer biaxially stretched sheet member and the coextruded biaxially stretched sheet member can be placed in any direction. By this placement method, the orientation direction in the plane of the multilayer sheet can be adjusted.
[0174] 2) Process ii
[0175] In this process ( Figure 4 and Figure 5 In 5), the heating body is brought into contact with the outermost layer of the precursor 1' of the multilayer sheet to heat and fuse the layers. The temperature T preferably satisfies the relationship of Tmh≥T≥Tml(TmF≥T≥TmN), and more preferably satisfies the relationship of Tmh≥T≥Tml+10(℃)(TmF≥T≥TmN+10(℃)). If T exceeds the upper limit, the laminate may melt, thereby reducing the mechanical properties. If T is lower than the lower limit, the layers cannot be fully fused, thereby reducing the mechanical properties. As a specific temperature of the heating body, it is preferably about 120 to 190℃, more preferably 140 to 170℃, and further preferably 150 to 165℃. T can be measured by any method, but it is preferably measured using a non-contact thermometer such as a radiation thermometer. The melting point is defined as the peak temperature of the melting curve obtained by measuring from 30℃ to 230℃ by DSC at a heating rate of 10℃ / min.
[0176] This process is preferably carried out continuously using a heated roller as a heating body. Specifically, the precursor of the multilayer sheet is passed between two heated rollers to fuse the layers. It is also possible to set the two rollers as a group and use a heated roller combining the two groups of rollers as a heating body to fuse. The pressure applied at this time can be appropriately adjusted. The winding speed in the roll forming is not limited, but is preferably about 0.05 to 10 m / min.
[0177] As methods other than roll forming, pressure forming, welding forming, etc. can be cited. In addition, when the sheet-like components are heated and welded, in order to further promote orientation while suppressing thermal shrinkage, it is preferable to apply pressure. The pressure at this time is adjusted according to the welding temperature.
[0178] 3) Other processes
[0179] The manufacturing method of the present invention may further include a known step of cooling the multilayer sheet obtained in the previous step. The cooling method is not limited, but examples thereof include a method of natural cooling at room temperature, a method of cold pressing at room temperature or 10 to 20°C, and the like.
[0180] (2) Process 2
[0181] In this process, the base portion raw material is thermoformed to form the base portion, and the surface portion is thermobonded on its surface. The thermoforming method is not limited, and injection molding, stamping molding, and vacuum molding can be listed. Among them, injection molding is preferred, so injection molding will be used as an example below. Figure 6 This process will be described below.
[0182] In the figure, 90 is an injection molding machine, 92 is a mold, 1 is a multilayer sheet, and 10' is a molten polymer forming the base part. In this process, the multilayer sheet 1 will first be arranged in the mold cavity of the mold. Next, the mold is closed, and the molten polymer constituting the base part is injected into the mold to thermally bond the surface part and the base part. The molding conditions can be appropriately adjusted according to the polymer used to satisfy Tms<Tp, or to satisfy the residual rate R(ΔHin / ΔHout)≥60% as needed. When using polypropylene resin, as an embodiment, the barrel temperature of the molding machine can be set to 180-250°C, and the mold temperature can be set to about 30-60°C. Tp is the temperature of the molten polymer for the base part ejected from the nozzle of the molding machine, which can be set to 180-250°C. This molding method is also called insert molding.
[0183] 3. Purpose
[0184] The surface layer of the polymer molded body has a high degree of orientation and a specific high-order structure in the in-plane direction, and the degree of orientation has a low dependence on the thickness direction, so it can have excellent mechanical properties while maintaining a relatively light weight, especially excellent rigidity and scratch resistance. In addition, if the surface layer contains a filler layer F, the layer has easy peeling properties. Therefore, if the surface layer has a top layer, the top layer is easily peeled off from the polymer molded body and has excellent recyclability. Therefore, the polymer molded body has excellent recyclability as well as rigidity and scratch resistance, and can be used as a steel plate substitute for automotive parts, motor and electronic parts or housing parts. In addition, the polymer molded body can also be used for food packaging materials, containers or lids that are lightweight, reduced in weight and have excellent unsealing properties. Since the polymer molded body has high rigidity, it can be used for groceries, daily necessities, home appliance parts, toy parts, furniture parts, building materials, packaging parts, industrial materials, logistics materials or agricultural materials.
[0185] The polymer molded body has the aforementioned rigidity. In addition, the surface impact strength (-30°C, JIS K7211-2) of the polymer molded body when standardized with a thickness of 3 mm is preferably 5 J / mm or more, more preferably 7 J / mm or more, and further preferably 9 J / mm or more. In the scratch resistance test, the sample is scratched and evaluated by its scratch width. In one embodiment, the scratching conditions are as follows. Scratch speed 100 min / m, load 10 N, tip diameter 1.0 mm, scratch length 50 mm.
[0186] [Example]
[0187] 1. Preparation of biaxially stretched sheet parts
[0188] The biaxially stretched sheet member was prepared as follows
[0189] [Polymer 1]
[0190] A solid catalyst for polymerization is prepared by the method described in Example 1 of European Patent Gazette No. 674991. The solid catalyst is supported on MgCl2 by Ti and diisobutyl phthalate as an internal donor according to the method described in the above patent gazette. The solid catalyst (1), triethylaluminum (TEAL) and dicyclopentyldimethoxysilane (DCPMS) are contacted at -5°C for 5 minutes in an amount of TEAL weight ratio of 11 to the solid catalyst and TEAL / DCPMS weight ratio of 10. The obtained catalyst system is kept in a suspended state at 20°C in liquid propylene for 5 minutes, thereby performing prepolymerization. After the obtained prepolymer is introduced into a polymerization reactor, hydrogen and propylene are added, and the polymerization temperature and hydrogen concentration are set to 75°C and 0.15 mol%, respectively, and the polymer 1 as a propylene homopolymer is obtained by adjusting the pressure.
[0191] [Resin composition (e)] (Talc-containing resin composition)
[0192] To 60 parts by weight of polymer 1, 40 parts by weight of talc (Neo Talc UNI05 manufactured by Neoraito Kosan Co., Ltd. (volume average particle size measured by laser diffraction method: 5 μm)), 0.2 parts by weight of antioxidant (B225 manufactured by BASF) and 0.05 parts by weight of neutralizer (calcium stearate manufactured by Tamnan Chemical Industry Co., Ltd.) were added, and the mixture was stirred for 1 minute using a Henschel mixer. The mixture was melt-kneaded in a single-screw extruder at a barrel temperature of 230°C, and the extruded strands were cooled in water and cut using a pelletizer to obtain a pelletized resin composition (e). The MFR (temperature 230°C, load 2.16 kg) of the resin composition (e) was 4.6 g / 10 minutes.
[0193] [Polymer 2-1]
[0194] The solid catalyst (1), TEAL and dicyclopentyldimethoxysilane (DCPMS) were contacted at -5°C for 5 minutes in an amount of 1:1 weight ratio of TEAL to the solid catalyst and 3 weight ratio of TEAL / DCPMS. The obtained catalyst system was kept in a suspended state in liquid propylene at 20°C for 5 minutes to perform prepolymerization. After the obtained prepolymer was introduced into a polymerization reactor, hydrogen, propylene and ethylene were added. Thereafter, under the conditions of a polymerization temperature of 75°C, a hydrogen concentration of 0.20 mol% and an ethylene concentration of 0.45 mol%, the polymerization pressure was adjusted to obtain a polymer 2-1 as a propylene-ethylene copolymer.
[0195] [Resin composition (b1)]
[0196] To 100 parts by weight of polymer 2-1, 0.2 parts by weight of an antioxidant (B225 manufactured by BASF), 0.05 parts by weight of a neutralizer (calcium stearate manufactured by Tamnan Chemical Industry Co., Ltd.), and 0.25 parts by weight of a nonol-based nucleating agent (Millad NX8000J manufactured by Milliken) were added and mixed with stirring for 1 minute using a Henschel mixer. The mixture was melt-kneaded in a single-screw extruder at a barrel temperature of 230°C, and the extruded strands were cooled in water and cut using a pelletizer to obtain a pelletized resin composition (b1). The resin composition (b1) contained 1.7% by weight of ethylene-derived units and had an MFR (temperature 230°C, load 2.16 kg) of 4.9 g / 10 minutes.
[0197] [Polymer 2-2]
[0198] The solid catalyst (1), TEAL and dicyclopentyldimethoxysilane (DCPMS) were contacted at -5°C for 5 minutes in an amount of 1:1 weight ratio of TEAL to the solid catalyst and 3 weight ratio of TEAL / DCPMS. The obtained catalyst system was kept in a suspended state in liquid propylene at 20°C for 5 minutes to perform prepolymerization. After the obtained prepolymer was introduced into a polymerization reactor, hydrogen, propylene and ethylene were added. Thereafter, under the conditions of a polymerization temperature of 75°C, a hydrogen concentration of 0.44 mol% and an ethylene concentration of 1.07 mol%, the polymerization pressure was adjusted to obtain a polymer 2-2 which is a propylene-ethylene copolymer.
[0199] [Resin composition (b2)]
[0200] 0.2 parts by weight of an antioxidant (B225 manufactured by BASF) and 0.05 parts by weight of a neutralizer (calcium stearate manufactured by Tamnan Chemical Industry Co., Ltd.) were added to 100 parts by weight of polymer 2-2, and the mixture was stirred and mixed for 1 minute using a Henschel mixer. The mixture was melt-kneaded in a single-screw extruder at a barrel temperature of 230°C, and the extruded strands were cooled in water and cut using a pelletizer to obtain a pelletized resin composition (b2). The resin composition (b2) contained 4.0 wt% of ethylene-derived units and had an MFR (temperature 230°C, load 2.16 kg) of 7.5 g / 10 minutes.
[0201] [Polymer 3]
[0202] The solid catalyst (1), TEAL and methylcyclohexyldimethoxysilane (CHMMS) were contacted at -5°C for 5 minutes in an amount of TEAL weight ratio of 8 to the solid catalyst and TEAL / CHMMS weight ratio of 8. The obtained catalyst system was kept in a suspended state in liquid propylene at 20°C for 5 minutes to carry out prepolymerization, and the catalyst obtained was used as a prepolymerized catalyst.
[0203] After the obtained prepolymerized catalyst was introduced into a polymerization reactor, hydrogen, propylene and ethylene were added, and then, under the conditions of polymerization temperature of 75° C., hydrogen concentration of 0.068 mol %, and ethylene concentration of 0.08 mol %, the polymerization pressure was adjusted to obtain polymer 3 which is a propylene-ethylene copolymer.
[0204] [Resin composition (a)]
[0205] Relative to 100 parts by weight of polymer 3, 0.2 parts by weight of B225 manufactured by BASF was added as an antioxidant, 0.05 parts by weight of calcium stearate manufactured by Tamnan Chemical Industry Co., Ltd. was added as a neutralizer, and 0.05 parts by weight of a nonol-based nucleating agent (Millad NX8000J manufactured by Milliken) was added, and the mixture was mixed by stirring for 1 minute using a Henschel mixer. An NVC extruder manufactured by Nakatani Machinery Co., Ltd. was used to melt-mix at a barrel temperature of 230°C, and the extruded strands were cooled in water and cut using a pelletizer to obtain a granular resin composition (a). The resin composition (a) contained 0.36% by weight of ethylene-derived units, and the MFR (temperature 230°C, load 2.16 kg) was 4.4 g / 10 minutes.
[0206] [Biaxially stretched sheet LHL100]
[0207] use 3 types of 3-layer film / sheet molding machines (manufactured by Thermo Plastics Industries, Ltd.) were used to co-extrude the resin composition (b1) / resin composition (a) / resin composition (b1) at a molding temperature of 230°C to obtain a raw material sheet (size 10 cmX10 cm or more) with a thickness of 3.8 mm. Using a film stretching device (KARO-Ⅳ manufactured by Bruckner), the raw material sheet was successively biaxially stretched (5 times X8 times) at 165°C to obtain a coextruded biaxially stretched sheet LHL100 with a thickness of 0.1 mm. The thickness ratio was 1 / 20 / 1. The rigidity and melting points Tmh (TmF), Tml (TmN), and Tms of the stretched sheet were measured. The rigidity and melting point were also measured for the following stretched sheets.
[0208] [Biaxially stretched sheet LHL30]
[0209] A coextruded biaxially stretched sheet LHL30 having a thickness of 0.03 mm was obtained by the same method as the biaxially stretched sheet LHL100 except that (b2) was used instead of the resin composition (b1). However, the ratio of the successive biaxial stretching was set to 5 times × 8 times. The thickness ratio was 1 / 10 / 1.
[0210] [Biaxially stretched sheet LHL50]
[0211] The coextruded biaxially stretched sheet LHL50 with a thickness of 0.05 mm was obtained in the same manner as the biaxially stretched sheet LHL100. However, the ratio of the successive biaxial stretching was set to 5 times x 8 times. The thickness ratio was 1 / 18 / 1.
[0212] [Biaxially stretched sheet LHL200]
[0213] use Three 3-layer film-sheet molding machines (manufactured by Thermo Plastics Industries, Ltd.) were used to coextrude the resin composition (b2) / resin composition (a) / resin composition (b2) at a molding temperature of 230°C to obtain a raw material sheet (size 10 cmX10 cm or more) with a thickness of 2.0 mm. Using a film stretching device (Karo-IV manufactured by Bruckner), the raw material sheet was simultaneously biaxially stretched (3 times X3 times) at 165°C to obtain a coextruded biaxially stretched sheet LHL200 with a thickness of 0.2 mm. The thickness ratio was 1 / 18 / 1.
[0214] [Biaxially stretched sheet NFN150] (Biaxially stretched sheet with talc layer)
[0215] use Three 3-layer film / sheet molding machines (manufactured by Thermo Plastics Industries, Ltd.) were used to coextrude the resin composition (b2) / resin composition (e) / resin composition (b2) at a molding temperature of 230°C to obtain a raw sheet (size 10 cm x 10 cm or more) having a thickness of 1.5 mm. The raw sheet was simultaneously biaxially stretched (3 times x 3 times) at 165°C using a film stretching device (manufactured by Bruckner) to obtain a coextruded biaxially stretched sheet NFN150 having a thickness of 0.15 mm. The thickness ratio was 1 / 18 / 1.
[0216] [Unstretched sheet NFN_U] (unstretched sheet with talc layer)
[0217] use Three 3-layer film / sheet molding machines (manufactured by Thermo Plastics Industries, Ltd.) were used to coextrude the resin composition (b2) / resin composition (e) / resin composition (b2) at a molding temperature of 230° C. to obtain a sheet (size of 10 cm×10 cm or more) having a thickness of 0.4 mm, which was used as an unstretched sheet NFN_U. The thickness ratio was 1 / 10 / 1.
[0218] [Unstretched sheet LHL_U]
[0219] use Three 3-layer film / sheet molding machines (manufactured by Thermo Plastics Industries, Ltd.) were used to co-extrude the resin composition (b1) / resin composition (a) / resin composition (b1) at a molding temperature of 230° C. to obtain a sheet (size 10 cm×10 cm or more) having a thickness of 0.4 mm, which was used as an unstretched sheet LHL_U. The thickness ratio was 1 / 10 / 1.
[0220] [Example 1]
[0221] In the EC160NⅡ injection molding machine manufactured by Toshiba Machine Co., Ltd., a mold having a cavity with a thickness of 150mmX300mmX2.5mm and a film gate is installed. The mold temperature is set to 40°C, and a biaxially stretched sheet LHL100 is arranged on one inner surface of the cavity (150mmX300mm). Next, polypropylene (YC582P manufactured by Sunallomer Co., Ltd.) is injected into the cavity for insert molding. A polymer molded body having a base portion and a surface portion (biaxially stretched sheet LHL100) thermally bonded to the base portion is manufactured by the above method. The molded body is evaluated as listed in Table 1. Tp (resin temperature during thermal bonding) is 210°C. As Figure 7 As shown in FIG. 1 , after thermal bonding, the cross section of the molded product was cut to obtain a slice Sin with a thickness of about 30% from the interface between YC582P and the surface layer toward the surface. In addition, a slice Sout with a thickness of about 30% was obtained from the surface of the surface layer toward the interface. These slices were subjected to DSC analysis, and the residual rate R was measured by the method described below. The residual rate R was 95%.
[0222] The molding conditions were as follows.
[0223] Cylinder temperature: 180~240℃
[0224] Mold temperature: 40℃
[0225] Shot time: 15 seconds
[0226] Cooldown: 25 seconds
[0227] [Example 2]
[0228] A polymer molded body was manufactured and evaluated in the same manner as in Example 1, except that biaxially stretched sheet LHL30 was used instead of biaxially stretched sheet LHL100, the thickness of the mold cavity was changed to 3 mm, and the resin temperature was changed as shown in Table 1.
[0229] [Example 3]
[0230] A polymer molded body was produced and evaluated in the same manner as in Example 1, except that the biaxially stretched sheet LHL30 was used instead of the biaxially stretched sheet LHL100 and the thickness of the mold cavity was changed to 3 mm.
[0231] [Example 4]
[0232] Except that the resin temperature was changed as shown in Table 1, a polymer molded body was produced and evaluated in the same manner as in Example 3.
[0233] [Example 5]
[0234] A polymer molded article was produced and evaluated in the same manner as in Example 3 except that the biaxially stretched sheet LHL50 was used instead of the biaxially stretched sheet LHL30.
[0235] [Examples 6 and 7]
[0236] Two precursors were prepared by stacking 2 and 3 layers of the biaxially stretched sheet LHL50. A stamping machine manufactured by Shoji Co., Ltd. heated to 160°C was used as a heating body, and the layers of each precursor were heated and fused to produce multilayer sheets as laminates. During stamping, a 3mm thick aluminum plate and a 1mm thick steel plate were used to clamp and insert the two sides of the above-mentioned precursor from the outside, and pressurized at 4MPa for 2 minutes. Multilayer sheets with a thickness of 0.1 and 0.15mm were manufactured and evaluated by the above method. Using the multilayer sheet instead of the biaxially stretched sheet LHL30, polymer moldings were manufactured and evaluated in the same manner as in Example 3.
[0237] [Examples 8 and 9]
[0238] Polymer molded bodies were produced and evaluated in the same manner as in Examples 5 and 6, except that the biaxially stretched sheet LHL200 was used instead of the biaxially stretched sheet LHL50.
[0239] [Example 10]
[0240] A polymer molded article was produced and evaluated in the same manner as in Example 3 except that the biaxially stretched sheet NFN150 was used instead of the biaxially stretched sheet LHL30.
[0241] [Example 11]
[0242] A precursor was prepared by stacking 19 layers of LHL50 and overlapping NFN150 on the top layer. A stamping machine manufactured by Shoji Co., Ltd. heated to 160°C was used as a heating body to heat and fuse the layers of the precursor to produce a multilayer sheet as a laminate. During stamping, a 3mm thick aluminum plate and a 1mm thick steel plate were used to clamp and insert the two sides of the above-mentioned precursor from the outside, and pressurized at 4MPa for 2 minutes. A 1.1mm thick multilayer sheet was manufactured by the above method. A polymer molded body was manufactured and evaluated in the same manner as in Example 3, except that the multilayer sheet obtained by the above method was used instead of the biaxially stretched sheet LHL30, and it was configured so that the top layer was opposite to the inner surface of the mold cavity.
[0243] [Example 12]
[0244] Except that the resin temperature was changed as shown in Table 1, a polymer molded body was produced and evaluated in the same manner as in Example 3.
[0245] [Comparative Example 1]
[0246] A molded body was obtained by injection molding without using a multilayer sheet and evaluated. The molding conditions were the same as those in Example 3.
[0247] [Comparative Example 2]
[0248] A polymer molded body was produced and evaluated in the same manner as in Example 3 except that the unstretched sheet NFN_U was used.
[0249] [Comparative Example 3]
[0250] A polymer molded body was produced and evaluated in the same manner as in Example 3 except that the unstretched sheet LHL_U was used.
[0251] [Table 1-1]
[0252]
[0253] *Normalized according to the thickness of the molded body
[0254] [Table 1-2]
[0255]
[0256] *Normalized according to the thickness of the molded body
[0257] Each assessment was performed as described below.
[0258] [MFR of resin composition]
[0259] Referring to JIS K7210-1, the measurement was performed under the conditions of a temperature of 230°C and a load of 2.16 kg.
[0260] [Content of ethylene-derived units contained in the resin composition (wt%)]
[0261] The sample dissolved in the mixed solvent of 1,2,4-trichlorobenzene / deuterated benzene was analyzed using AVANCE III HD400 ( 13 The 13C-NMR spectrum was obtained under the conditions of a measurement temperature of 120°C, a flip angle of 45 degrees, a pulse interval of 7 seconds, a sample rotation rate of 20 Hz, and an accumulation number of 5000 times. The ethylene-derived unit content (weight %) contained in the resin composition was determined by the method described in M. Kakugo, Y. Naito, K. Mizunuma and T. Miytake, Macromolecules, 15, 1150-1152 (1982) using the spectrum obtained by the above method.
[0262] [Scratch resistance]
[0263] The surface of the molded body surface layer was scratched using a scratch tester KK-02 manufactured by Keskato. The scratch width was measured using a shape measuring laser microscope (“VHX-2000” manufactured by KEYENCE) as an indicator of scratch resistance. The smaller the width, the better the scratch resistance.
[0264] Scratch speed: 100 min / m, load 10N, tip diameter 1.0mm, scratch length 50mm
[0265] [Flexural modulus]
[0266] The polymer molded body with the thickness shown in Table 1 was processed into a width of 10 mm and a length of 80 mm to obtain a test piece for measurement (type B2). The bending elastic modulus of the type B2 test piece for measurement was measured using a precision universal testing machine (Autograph AG-X10kN) manufactured by Shimadzu Corporation under the conditions of a temperature of 23°C, a relative humidity of 50%, a distance between fulcrums of 48 mm, and a test speed of 2 mm / min. The measurement was performed by placing the indenter against the surface end.
[0267] [Tensile elastic modulus]
[0268] According to JIS K7161, a sample cut from a film sample is stretched at a speed of 5 mm / min using a Tensilon tester (Autocom) manufactured by T.S.E. The tensile modulus is the value obtained by dividing the load of the tangent line drawn from the zero point of the stress-strain curve at 2% elasticity by the cross-sectional area of the sample. The tensile modulus is measured in the MD direction and the TD direction of the film sample.
[0269] [Impact Strength]
[0270] The polymer molded body was processed into a square of 70 ± 2 mm to obtain a test piece for measurement. According to JIS K7211-2, a HYDRO SHOT HITS-P10 manufactured by Shimadzu Corporation was used to place the test piece for measurement in a tank adjusted to -30°C. The inner diameter of the hole is used After fixing the sample pressure plate, use a hemispherical impact surface with a diameter of The test piece was struck with an impactor at an impact speed of 4.4±0.2 m / s to obtain various energies (J) and fracture characteristics. The average puncture energy of each of the four test pieces was taken as the impact strength.
[0271] Regarding the impact fracture characteristics and the type of failure, YD / YS / YU / NY were determined in accordance with JIS K7211-2 using a test piece whose impact strength was measured under the above conditions.
[0272] Maximum impact force energy: The energy consumed to produce the displacement representing the maximum impact force FM occurring during the test (J)
[0273] Puncture energy: maximum impact force F M Energy consumed when the displacement is reduced to half (J)
[0274] Total energy: The energy consumed from the start of the test to the displacement at which the impact force becomes zero (J)
[0275] [Melting point] Melting point obtained by DSC (Tms, Tmh, Tml)
[0276] About 5 mg of the sample was weighed using an electronic balance, and then a differential thermal analyzer (DSC) (Q-200 manufactured by TA Instruments) was used to keep the sample at 30°C for 5 minutes, and then heated to 230°C at a heating rate of 10°C / min to obtain a melting curve. The peak temperature of the melting curve was taken as the melting point. When the melting heat ΔH was calculated using the above melting curve, ΔH was calculated based on the melting peak area within the specified temperature range on the baseline after the melting was completely completed in the melting profile curve after baseline correction.
[0277] Melting point of the part that joins the base part of the surface layer (Tms)
[0278] 1) Collecting a portion having a thickness of 10 to 50% from the interface between the surface layer and the base layer.
[0279] 2) Perform DSC measurement under the temperature increase conditions of the sample collected in 1) above, and take the peak temperature of the melting curve obtained as Tms. If Tmh and Tml are observed at the same time, when multiple melting point peaks are observed, the maximum peak temperature (usually Tmh) is taken as Tms.
[0280] Survival rate R (△Hin / △Hout)
[0281] 1) A portion having a thickness of 10 to 50% is collected from the surface of the surface layer portion on the side opposite to the base layer portion.
[0282] 2) The sample collected in 1) above is subjected to DSC analysis under elevated temperature conditions, and the heat (J / g) within the range of Tmh±5°C is determined as ΔHout. The melting point is the peak temperature in the melting profile curve.
[0283] 3) Collecting a portion having a thickness of 10 to 50% from the interface between the surface layer and the base layer.
[0284] 4) The sample collected in 3) above is subjected to DSC analysis under the above-mentioned temperature increase conditions, and the heat (J / g) within the range of Tmh±5°C is determined and taken as ΔHin.
[0285] [Explanation of symbols]
[0286] 1Surface part, multi-layer sheet
[0287] 1' Precursor
[0288] 10 Base part
[0289] 10'Molten polymer
[0290] 90 Injection molding machine
[0291] 92 Mould
[0292] 100 Polymer moldings
[0293] F Filling layer F
[0294] NSurface
[0295] H Biaxially stretched sheet H
[0296] L Biaxially stretched sheet L
[0297] T Top
[0298] C Coextrusion layer
[0299] t Coextrusion layer thickness
[0300] 2. Unstretched sheet preparation process
[0301] 20 Unstretched sheet preparation process (coextrusion)
[0302] 3 Stretching process
[0303] 4 Lamination process
[0304] 5 Interlayer welding process
[0305] f. n resin composition
[0306] F”, N” unstretched sheet (raw material)
[0307] F', N' biaxially stretched sheet parts
[0308] C" co-extrusion raw material sheet
[0309] C' Coextruded biaxially stretched sheet parts
[0310] Sin from the interface of the surface part to the surface (about 30% of the thickness of the surface part)
[0311] Sout Slice from the surface of the surface layer toward the interface (about 30% of the thickness of the surface layer)
Claims
1. A polymer molded article comprising a base portion and a surface portion thermally bonded to the base portion, which satisfies the following conditions: 1) Gs>Gb (Gs is the rigidity of the surface layer, and Gb is the rigidity of the base layer.) 2) Tms<Tp (Tms is the melting point of the bonding portion between the surface layer portion and the base portion, and Tp is the molding temperature during the thermal bonding.) 2. The molded article according to claim 1, wherein The base layer and the surface layer are composed of a polymer having the same repeating unit.
3. The molded article according to claim 1 or 2, wherein The surface layer portion has a multi-layer structure.
4. The molded article according to claim 3, wherein The surface layer has a multilayer structure, which includes a biaxially stretched sheet layer L with a melting point of Tml and a biaxially stretched sheet layer H with a melting point of Tmh. Tmh>Tml, The biaxially stretched sheet layer L forms the bonding surface.
5. The molded article according to claim 4, wherein The layer H consists of Polypropylene resin (A) or The invention comprises a resin composition comprising a polypropylene resin (A) and a plate-like inorganic filler (B), wherein the weight ratio of component (B) / [component (A)+component (B)] is greater than 0 weight % and less than 60 weight %.
6. The molded article according to claim 5, in, The polypropylene resin (A) comprises a polypropylene resin consisting of a component (A1) and an optional component (A2), The component (A1) is 100 to 50% by weight of a propylene (co)polymer, and the (co)polymer contains 0 to 10% by weight of comonomer-derived units selected from C2 to C10-alpha olefins (but excluding C3-alpha olefins); Component (A2) is 0 to 50% by weight of an ethylene-α-olefin copolymer, and the copolymer contains 10 to 90% by weight of ethylene-derived units; The MFR (230°C, load 2.16 kg) of the polypropylene resin (A) is 1 to 15 g / 10 minutes.
7. The molded article according to claim 4, wherein The outermost surface of the surface layer portion includes a top layer other than the biaxially stretched sheet layers L and H.
8. The molded article according to claim 4, wherein The total thickness of the layer L / the thickness of the surface layer is 1 to 50%.
9. The molded article according to claim 4, wherein: The surface layer portion has alternate layers in which the layer L and the layer H are alternately laminated.
10. The molded article according to claim 1 or 2, wherein: The thickness of the surface layer is above 30 μm.
11. The molded article according to claim 1 or 2, wherein The thickness of the base portion is 5 to 250 times the thickness of the surface portion.
12. A method for producing a molded body according to claim 1 or 2, wherein: The manufacturing method has the following features: Step 1 of preparing the surface layer portion, and Step 2 of forming the base portion by thermoforming the base portion raw material and simultaneously thermally bonding the surface layer portion on the surface thereof.
13. The manufacturing method according to claim 12, wherein: The process 2 also includes: the step of arranging the surface layer portion in a mold cavity, and The step of forming the base portion by injection molding the base portion material in the cavity and thermally bonding the surface layer portion on the surface of the base portion.
Citation Information
Patent Citations
Crystalline propylene copolymer compositions having a low seal temperature and good ink adhesion
EP0674991A1
Decorative laminated sheet, structure including decorative laminated sheet, and method of manufacturing the same
JP2014124940A
Polypropylene sheet production method
WO2020075755A1
Thermoplastic resin molded product and decorative panel
JP2006192620A
Decorative sheet and decorative resin molded article using the same
JP2015163479A