Method for applying a coating composition to a substrate

The durability of the paint is solved by using a combination of high Tg non-film-forming second polymer particles and low Tg film-forming first polymer particles in the water-based traffic sign paint, combined with an appropriate amount of incremental agent and pigment. The problem of taking into account both color retention achieves higher stability and pollution resistance.

CN119072459APending Publication Date: 2024-12-03ROHM & HAAS CO +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202280095142.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2022-05-20
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The durability of existing water-based traffic sign paints on the road is difficult to take into account both the durability and color retention of the road. When conventional methods reduce the volume fraction of film-forming latex to increase the level of non-film-forming pigments or fillers, the durability of the paint will be affected. Influence.

Method used

A colored coating composition containing high Tg non-film-forming second polymer particles and low Tg film-forming first polymer particles ensures that the solid content of the composition is 60%. The ratio of the first polymer to the second polymer is in the range of 30:70 to 90:10, and the particle size measured by dynamic light scattering and the selection of polymers are optimized to optimize the solid content and pH of the polymer. value.

Benefits of technology

The color retention and stability of the paint for traffic signs is achieved without sacrificing the durability of the paint, which enhances resistance to dirt, tire marks and other stains, and accelerates drying under high humidity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005093456780000031
    Figure BDA0005093456780000031
  • Figure BDA0005093456780000051
    Figure BDA0005093456780000051
Patent Text Reader

Abstract

The present invention relates to a method comprising the steps of: a) applying a layer of a pigmented coating composition having a thickness of 0.1 mm to 2 mm onto a cement, concrete or asphalt substrate, and b) drying the coating composition. The method of the present invention can be used to prepare traffic sign paints with improved color retention and durability.
Need to check novelty before this filing date? Find Prior Art

Description

Background Art

[0001] The present invention relates to a method for applying a coating composition to a substrate, more particularly to a concrete or asphalt substrate.

[0002] Waterborne fast-drying traffic marking paints are a common and low-cost product used to improve road safety. In order to be effective as traffic marking paints, four key properties are required: (i) durability of the paint on the road, as measured by presence and retroreflectivity over time; (ii) color retention and resistance to dirt, tire marks and other stains; (iii) drying time under high humidity; and (iv) paint stability. Among these, color retention is a particular challenge. Although this property can be improved by reducing the volume fraction of film-forming latex in the paint in order to increase the level of non-film-forming pigments or fillers, it is often found that the durability of the paint on the road is catastrophically affected. Therefore, it would be an advancement in the field of waterborne traffic marking paints to find a method to improve color retention without sacrificing paint durability. Summary of the invention

[0003] The present invention relates to a method comprising the steps of: a) applying a 0.1 mm to 2 mm thick layer of a pigmented coating composition to a cement, concrete or asphalt substrate, and b) allowing the coating composition to dry;

[0004] The colored coating composition comprises an aqueous dispersion of: 1) a calculated T g first polymer particles in the range of -25°C to 50°C; 2) calculated T g second polymer particles in the range of 30°C to 110°C; 3) extender particles; 4) pigment particles; and 5) ammonia or a volatile amine or salt thereof;

[0005] The prerequisite is that the second polymer particles have a T of at least 20°C higher than the first polymer particles. g , wherein, based on the weight of the composition:

[0006] the first polymer particles and the second polymer particles together have a solids content in the range of 10 wt % to 20 wt %;

[0007] The extender particles have a solids content in the range of 45 wt % to 70 wt %;

[0008] The pigment particles have a solids content in the range of 3 wt % to 15 wt %; and

[0009] The composition has a total solids content in the range of 60 wt % to 85 wt %;

[0010] wherein a w / w ratio of the first polymer particles to the second polymer particles is in the range of 30:70 to 90:10.

[0011] The method of the present invention for preparing a coated concrete substrate provides a coated traffic marking paint having excellent color retention and durability. DETAILED DESCRIPTION

[0012] The present invention is a method comprising the steps of: a) applying a 0.1 mm to 2 mm thick layer of a pigmented coating composition to a cement, concrete or asphalt substrate, and b) allowing the coating composition to dry;

[0013] The colored coating composition comprises an aqueous dispersion of: 1) a calculated T g first polymer particles in the range of -25°C to 50°C; 2) calculated T g second polymer particles in the range of 30°C to 110°C; 3) extender particles; 4) pigment particles; and 5) ammonia or a volatile amine or salt thereof;

[0014] The prerequisite is that the second polymer particles have a T of at least 20°C higher than the first polymer particles. g , wherein, based on the weight of the composition:

[0015] The first polymer particles and the second polymer particles together have a solids content in the range of 10 wt % to 20 wt %;

[0016] The extender particles have a solids content in the range of 45 wt % to 70 wt %;

[0017] The pigment particles have a solids content in the range of 3 wt % to 15 wt %; and

[0018] The composition has a total solids content in the range of 60 wt % to 85 wt %;

[0019] wherein the w / w ratio of the first polymer particles to the second polymer particles is in the range of 30:70 to 90:10.

[0020] The first polymer particles and the second polymer particles can be acrylic, styrene-acrylic, urethane, alkyd, vinyl ester (e.g., vinyl acetate and vinyl versatate) and vinyl acetate-ethylene (VAE) polymer dispersions and combinations thereof. The polymer particles, which are preferably acrylic or styrene-acrylic latex particles, preferably have a z-average particle size in the range of 50 nm to 600 nm, more preferably in the range of 70 nm to 300 nm, as measured by dynamic light scattering.

[0021] As used herein, "acrylic latex" comprises structural units of at least 30 wt%, preferably at least 50 wt%, and more preferably at least 80 wt% acrylate and / or methacrylate monomers. The acrylic latex preferably comprises an aqueous dispersion of polymer particles functionalized with methyl methacrylate and one or more acrylates selected from the group consisting of methyl methacrylate, ethyl acrylate, n-butyl acrylate, 2-ethylhexyl acrylate, and 2-propylheptyl acrylate. As used herein, the term "structural unit" of a designated monomer refers to the residue of the monomer after polymerization. For example, the structural unit of n-butyl acrylate is illustrated as follows:

[0022]

[0023] The dotted lines represent the connection points between the structural units and the polymer backbone.

[0024] The acrylic latex also preferably contains structural units of acid monomers, including carboxylic acid, sulfuric acid and phosphoric acid monomers, and their salts and combinations thereof. Examples of suitable carboxylic acid monomers include methacrylic acid, acrylic acid and itaconic acid and their salts; examples of suitable sulfuric acid monomers include sulfonic acid monomers such as sulfoethyl methacrylate, sulfopropyl methacrylate, styrene sulfonic acid and its salts, vinyl sulfonic acid and its salts, and 2-acrylamido-2-methylpropanesulfonic acid and its salts; examples of suitable phosphoric acid monomers include phosphonates of alcohols and dihydrogen phosphates, wherein the alcohols contain polymerizable vinyl or alkenyl groups or are substituted with polymerizable vinyl or alkenyl groups. Preferred dihydrogen phosphates are phosphates of hydroxyalkyl acrylates or hydroxyalkyl methacrylates, including 2-phosphoethyl methacrylate (PEM) and its salts.

[0025] The first polymer particles have a T in the range of -25°C, preferably -15°C and more preferably -10°C to 50°C, preferably to 30°C as calculated by the Fox formula. g The second polymer particles preferably have a T in the range of 30°C, preferably 50°C to 110°C, preferably to 90°C as calculated by the Fox formula. g The second polymer particles have a T of at least 20°C higher than the second polymer particles g .

[0026] The w / w ratio of the first polymer particles to the second polymer particles is in the range of 30:70, preferably 50:50 to 90:10, preferably to 70:30, and the first polymer particles and the second polymer particles together have a solids content in the range of 10 wt% to 20 wt%, preferably to 18 wt% and more preferably to 17 wt%.

[0027] As used herein, the term extender refers to any white, translucent or translucent particulate filler that does not impart a significant (non-white) color or hue. Examples of suitable inorganic extenders include silicon dioxide; silicates and aluminosilicates such as talc, clay, mica and sericite; CaCO3; nepheline syenite; feldspar; wollastonite; kaolinite; dicalcium phosphate; and diatomaceous earth. Preferably, the extender particles have a solids content in the range of 50% to 65% by weight based on the weight of the composition. A preferred extender is CaCO3.

[0028] Pigment particles include opaque pigments such as TiO2, ZnO and hollow opaque pigments (opaque polymers), and colorants such as yellow iron oxide, red iron oxide and carbon black. Preferred pigment particles are TiO2 particles, and their solid content concentration is in the range of 5 wt % to 10 wt % based on the weight of the composition.

[0029] The composition also comprises a sufficient amount of ammonia or a volatile amine or a salt thereof to achieve a pH in the range of 8, preferably 8.5, more preferably 9 to 12, preferably to 11. As used herein, the term "volatile amine" is an amine having a boiling point of no greater than 250° C. Examples of suitable volatile amines include 2-amino-2-methyl-1-propanol, dimethylaminoethanol and monoisopropanolamine.

[0030] The composition advantageously also comprises 0.01 wt %, more preferably 0.05 wt % to 2 wt %, more preferably to 1 wt % and most preferably to 0.5 wt % of polyamines based on the weight of the composition, the polyamines being polymers containing at least 5 amine groups. The example of polyamines includes polyethyleneimine (polyethylenimine), and a polymer or copolymer of a monoethylenically unsaturated amine of a structural unit comprising 20 wt %, preferably 50 wt % to 100 wt %. The category of the monoethylenically unsaturated amines suitable for preparing polyamine homopolymers and copolymers includes alkylaminoalkyl acrylates and methacrylates, acrylamide, methacrylamide, N-acryloxyalkyl-oxazolidine, N-acryloxyalkyl tetrahydro-1,3-oxazine and hydroxyalkylaminoethyl acrylates and methacrylates. Specific examples of suitable monoethylenically unsaturated amines include dimethylaminoethyl acrylate, dimethylaminoethyl methacrylate, N-β-aminoethyl acrylamide, N-β-aminoethyl methacrylamide, N-(monomethylaminoethyl)-acrylamide, N-(monomethylaminoethyl)-methacrylamide, 2-(3-oxazolidinyl)ethyl methacrylate, 2-(3-oxazolidinyl)ethyl acrylate, 3-(γ-methacryloyloxypropyl)-tetrahydro-1,3-oxazine, 3-β-methacryloyloxyethyl-2-methyl-2-propyl oxazolidine, 3-(β- ...2-(3-oxazolidinyl)ethyl methacrylate, 2-(3-oxazolidinyl)ethyl acrylate, 2-(3-oxazolidinyl)ethyl methacrylate, 2-(3-oxazolidinyl)ethyl methacrylate, 2-(3-oxazolidinyl)ethyl methacrylate, 2-(3-oxazolidinyl)ethyl methacrylate, 2-(3-oxazolidinyl)ethyl methacrylate, 2-(3-oxazolidinyl)ethyl methacrylate, 2-(3-oxazolidinyl)ethyl methacrylate, 2-(3-oxazolidinyl)ethyl methacrylate, 2-(3-oxazolidinyl)ethyl methacrylate, The preferred polyamine is poly(oxazolidinylethyl methacrylate).

[0031] The weight average molecular weight (M) of the polyamines is measured using size exclusion chromatography (SEC) as described in US Pat. No. 10,662,337, column 5, lines 50 to 67. w ) is preferably in the range of 500 g / mol, more preferably 5000 g / mol and most preferably 10,000 g / mol to preferably 500,000, g / mol, more preferably to 100,000 g / mol and most preferably to 80,000 g / mol.

[0032] The pigment volume concentration of the composition is preferably in the range of 60, preferably 65 to 90, preferably to 85. The PVC is calculated by the following equation:

[0033]

[0034] The composition used in the method of the present invention advantageously comprises one or more additional materials, including surfactants, defoamers, dispersants, coalescing agents, rheology modifiers and solvents. Coagulants are particularly desirable for first polymer particles that do not readily form films at ambient temperature. For such first polymer particles, the concentration of the coalescing agent used is high enough to promote film formation of the first polymer particles at ambient temperature, but low enough so as not to promote film formation of the second polymer particles. Thus, the first polymer particles form a film alone or in the presence of a coalescing agent. As used herein, "film forming" means forming a film at or below ambient temperature, preferably at room temperature, according to ASTM D2354. < Minimal film formation at 22 °C.

[0035] The composition is advantageously applied to cement, concrete or asphalt substrates in a wet coating in the range of 0.1 mm, or 0.3 mm to 5 mm, or 3 mm, and then allowed to dry. The method may include dripping glass beads, sand, quartz, Al2O3 and alumina before the coating on the substrate dries. Methods for surface treatment with such additives are well known in the art. (See US 5,672,379, column 15, lines 3-35).

[0036] It has been surprisingly found that relatively high T g The non-film-forming second polymer particles and relatively low T g The key combination of film-forming first polymer particles provides improved color retention with little loss of durability. In contrast, higher concentrations of extender particles and lower concentrations of low T g The first polymer particles provide little improvement in color retention and have a significant loss in durability.

[0037] Example

[0038] In the following examples, the dispersant refers to TAMOL TM 963 dispersant (a trademark of The Dow Chemical Company or one of its affiliates); defoamer refers to Drewplus L-493 defoamer; TiO2 refers to TiPure R-900 titanium dioxide; CaCO3 refers to Hubercarb Q6 calcium carbonate; attapulgite refers to Attagel 50 attapulgite gel; coalescing agent refers to Texanol coalescing agent; and HEC refers to Natrosol H4BR hydroxyethylcellulose.

[0039] All aqueous dispersions of polymer particles (latexes) were prepared using standard emulsion polymerization techniques. The monomer concentration used to prepare the first polymer particles was 56.3% butyl acrylate, 42.2% methyl methacrylate, and 1.5% methacrylic acid. The monomer concentration used to prepare the second polymer particles was 20% butyl acrylate, 78.7% methyl methacrylate, and 1.5% methacrylic acid. The first polymer particles and the second polymer particles had a z-average particle size of approximately 200 nm as measured by dynamic light scattering and a solids content of 50% by weight. Poly(oxazolidine ethyl methacrylate) was added to each latex (4.6 g of a 27% w / w aqueous solution per 100 g of latex solids).

[0040] The aqueous road marking composition was prepared by adding the first polymer and the second polymer to a plastic bucket while stirring with an overhead mixer. Dispersant (0.33 wt %), defoamer (0.25 wt %), attapulgite (0.08 wt %), TiO2, CaCO3, and methanol (1.6 wt %) were added sequentially under high shear stirring and then mixed for 15 min. Methanol, coalescing agent, water, and HEC (2% w / w aqueous solution) were then added sequentially at a stirring speed sufficient to maintain a deep vortex. Once all ingredients were added, the formulation was mixed for 15 min. The formulation was then allowed to stand for at least 24 h before application. The amount of HEC was varied to achieve an initial viscosity of 85 KU to 90 KU.

[0041] The aqueous composition was sprayed onto a Portland cement road by a walk-behind self-propelled striper according to ASTM D713. The composition was applied as a transverse line at a thickness of 380 μm on a lane where an average of ~10,000 vehicles cross per day over a one-year period. The lines were allowed to dry for at least 2 h before traffic was allowed to resume. The durability of the coating was measured according to ASTM D913 and recorded as the percentage of paint remaining in the rutted area of ​​the painted line.

[0042] Table 1 shows the effects of several properties on the use of high T g Polymer or CaCO3 replaces different amounts of low T g Effect of polymer. Comparative Example 1 used 15.1 wt% of low T g Inventive Examples 1, 2 and 3 use equal volume fractions of high T g The polymer replaced 20 wt%, 33.3 wt% and 50 wt% of the low T g Comparative Examples 2 and 3 used equal volumes of CaCO3 to replace 20 wt% and 33.3 wt% of the low T gPolymer. In the table, composition stability is evaluated based on the sedimentation (in mm) and viscosity change (in KU) of the aqueous composition after 7 days at 60°C, and the sedimentation (in mm) is evaluated after 1 month of shelf stability testing at room temperature. 90% relative humidity refers to Dry No Pick-Up (according to ASTM D-711) reported in minutes. WT (rutting) presence is reported as a percentage according to ASTM D913 (which is measured on an unbeaded line 55 days after application) and is a measure of durability. ΔE, as measured according to ASTM D2244, is an indicator of color retention (smaller ΔE corresponds to smaller color change) and is reported as a percentage of the color change of Comparative Example 1 containing only soft polymer at 55 days. The term high T g :Low T g refers to the v / v ratio of the two polymers; and CaCO3: low T g Refers to the v / v ratio of the above added CaCO3 used in the comparative examples. CaCO3, inorganics, polymer solids, soft polymer, hard polymer, water, solid volume and solid weight are all reported based on the weight of the total paint. The hard polymer is considered to be a pigment for the PVC calculation. The word "pass" is used to indicate the acceptable threshold of the measured property.

[0043] Table 1 - With high T g Properties of polymer paints

[0044] Laboratory ID Comparative Example 1 Example 1 Example 2 Example 3 Comparative Example 2 Comparative Example 3 qualified <![CDATA[High T g : Low T g > 0:100 20:80 33:67 50:50 - - <![CDATA[CaCO3: low T g > - - - - 20:80 33:67 7-day heat aging: Settling 0 0 0 0 0 8.0 <5 7 days heat aging: ΔKU 6.3 8.4 6.7 6.6 5.7 9.0 <10 1 month shelf settlement 3.0 3.0 1.0 0 4.0 12.0 <10 90%RH dry to touch 32 28 28 24 44 56 <30 WT%Presence 100 100 100 98 100 30 >80 ΔE Color Change 100.0% 83.5% 73.9% 59.4% 93.1% 92.3% <90% <![CDATA[Soft polymer T g °C]]> -4 -4 -4 -4 -4 -4 <![CDATA[Hard polymer T g °C]]> N / A 58 58 58 N / A N / A <![CDATA[wt% CaCO3]]> 54.3% 56.5% 56.5% 56.5% 59.0% 62.0% <![CDATA[wt% TiO2]]> 7.1% 7.1% 7.1% 7.1% 6.8% 6.6% Weight% Inorganic 61.4% 63.6% 63.6% 63.6% 65.8% 68.6% Weight % polymer solids 15.1% 15.1% 15.1% 15.1% 11.6% 9.4% % soft polymer 15.1% 12.1% 10.1% 7.6% 11.6% 9.4% Weight % Hard Polymer 0.0% 3.0% 5.0% 7.6% 0.0% 0.0% PVC 61.5 69.2 74.3 80.8 69.0 74.0 Weight% Water 0.2 0.2 0.2 0.2 0.2 0.2 Solid volume 60.0 60.0 60.0 60.0 59.8 59.9 Solid weight 77.0 77.0 77.0 77.0 77.7 79.4

[0045] The data show that the test values ​​for heat aging sedimentation, ΔKU, 90% RH dry to touch, and ΔE are passed across the board. In contrast, the comparative paints that did not contain non-film-forming second polymer particles as a partial replacement for the film-forming particles failed one or more of the tests conducted on the paints. Notably, all comparative paints failed ΔE (color retention) and dry to touch.

Claims

1. A method comprising the following steps: a) applying a 0.1 mm to 2 mm thick layer of a pigmented coating composition to a cement, concrete or asphalt substrate, and b) allowing the coating composition to dry; The colored coating composition comprises an aqueous dispersion of: 1) a calculated T g first polymer particles in the range of -25°C to 50°C; 2) calculated T g second polymer particles in the range of 30°C to 110°C; 3) extender particles; 4) pigment particles; and 5) ammonia or a volatile amine or salt thereof; Provided that the second polymer particles have a T of at least 20°C higher than that of the first polymer particles g , wherein, based on the weight of the composition: the first polymer particles and the second polymer particles together have a solids content in the range of 10 wt % to 20 wt %; The extender particles have a solids content in the range of 45 wt % to 70 wt %; The pigment particles have a solids content in the range of 3 wt % to 15 wt %; and The composition has a total solids content in the range of 60 wt % to 85 wt %; wherein a w / w ratio of the first polymer particles to the second polymer particles is in the range of 30:70 to 90:

10.

2. The method according to claim 1, wherein the pigment is TiO2; the first polymer particles have a T in the range of -15°C to 30°C. g , and the second polymer particles have a T in the range of 50°C to 110°C g .

3. The method of claim 2, wherein the colored coating composition further comprises 0.01 wt % to 2 wt % of a polyamine based on the weight of the composition; wherein the weight ratio of the first polymer particles to the second polymer particles is in the range of 50:50 to 90:10; And wherein the first polymer particles and the second polymer particles are acrylic or styrene-acrylic polymers.

4. The method of claim 3, wherein the composition has a pigment volume concentration (PVC) in the range of 60 to 90.

5. The method of claim 4, wherein the binder is ammonia, 2-amino-2-methyl-1-propanol, dimethylaminoethanol or monoisopropanolamine; wherein the polyamine is poly(oxazolidineethyl methacrylate); and wherein the composition has a pH in the range of 8.5 to 12.

6. The method of claim 4, wherein the composition has a PVC in the range of 65 to 85.

7. The method of claim 1, wherein the composition further comprises one or more additional materials selected from the group consisting of surfactants, defoamers, dispersants, coalescing agents, rheology modifiers, and solvents.

8. The method of claim 6, wherein the composition further comprises a surfactant, a defoamer, a dispersant, and a rheology modifier.

9. The method of claim 1, wherein the composition comprises a coalescing agent at a concentration high enough to promote film formation of the first polymer particles at ambient temperature but low enough not to promote film formation of the second polymer particles.

10. The method of claim 1, further comprising adding glass beads, sand, quartz, Al2O3, or bauxite, or a combination thereof dropwise to the substrate before step b).

Citation Information

Patent Citations

  • Method of producing wear resistant traffic markings

    US5672379A