Method for producing reactive silicon group-containing organic polymer

By using Group 8 metal catalyst and carbon-carbon triple bond carboxylic acid compound cocatalyst in the hydrosilylation reaction, combined with silane compounds, the problem of poor promotion effect of the hydrosilylation reaction is solved, and high silylation rate is achieved The polymer manufacturing meets the needs of bonding and sealing materials for industrial purposes.

CN119072501APending Publication Date: 2024-12-03AGC INC +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380035755.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-27
Filing Date
2023-04-24
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

In the prior art, the promotion effect of the hydrosilylation reaction is insufficient, resulting in a decrease in the silylation rate of the reactive silicon groups, which is difficult to meet the needs of industrial applications.

Method used

In the hydrosilylation reaction, the Group 8 metal catalyst and a carboxylic acid compound with a carbon-carbon triple bond are used as a cocatalyst. The reaction conditions are optimized to improve the silylation rate.

Benefits of technology

The silylation rate of the hydrosilylation reaction is significantly improved, forming a high molecular weight crosslinked product, and is suitable for industrial applications such as adhesives and sealing materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005097225160000291
    Figure BDA0005097225160000291
  • Figure BDA0005097225160000301
    Figure BDA0005097225160000301
  • Figure BDA0005097225160000331
    Figure BDA0005097225160000331
Patent Text Reader

Abstract

The present invention relates to a method for producing an organic polymer containing a reactive silicon group by reacting an organic polymer containing an unsaturated group with a silylating agent in the presence of a cocatalyst comprising a Group 8 metal catalyst and a carboxylic acid compound having a carbon-carbon triple bond, the reactive silicon group-containing organic polymer has a reactive silicon group represented by formula (1). -SiRaX3-a formula (1) [In formula (1), R represents a monovalent organic group having 1-20 carbon atoms and is an organic group other than a hydrolyzable group, and X represents a hydroxyl group, a halogen atom, or a hydrolyzable group. And a represents an integer of 0-2. And when a is 2, R may be the same as or different from each other, and when a is 0 or 1, X may be the same as or different from each other.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing an organic polymer containing reactive silicon groups.

[0002] This application claims priority based on Japanese Patent Application No. 2022-073452 filed in Japan on April 27, 2022, the contents of which are incorporated herein by reference. Background Art

[0003] It is known that polymers having reactive silicon groups have a property of obtaining a rubbery cured product by crosslinking through the formation of siloxane bonds accompanied by a hydrolysis reaction of the reactive silicon groups caused by moisture or the like even at room temperature.

[0004] Among these polymers having reactive silicon groups, oxyalkylene polymers, saturated hydrocarbon polymers, alkyl acrylate polymers, and alkyl methacrylate polymers have been industrially produced and widely used in sealing materials, adhesives, coatings, etc. The polymers having reactive silicon groups are increased in molecular weight by silanol condensation reaction between the polymers to form crosslinked products.

[0005] A polymer having a reactive silicon group is produced, for example, by hydrosilylation with a silylating agent after producing a polymer having an unsaturated group as an end group. However, the hydrosilylation reaction is accompanied by many side reactions and has the following problems: the reactive silicon group is not introduced into all the end groups, and the silylation rate, which is the ratio of the reactive silicon group in the end group, decreases. Therefore, the promotion of the hydrosilylation reaction has been studied before, and it is known that the silylation rate can be increased by adding a carboxylic acid compound to the Group 8 metal catalyst used in the hydrosilylation reaction (for example, Patent Document 1, Patent Document 2).

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2000-95785

[0009] Patent Document 2: Japanese Patent Application Laid-Open No. 2000-143679 Summary of the invention

[0010] Problem that the invention aims to solve

[0011] However, the accelerating effect of the hydrosilylation reaction in Patent Documents 1 and 2 is not sufficient, and further improvement of the accelerating effect is required.

[0012] The present invention has been accomplished based on the above circumstances, and an object of the present invention is to provide a method for producing an organic polymer containing a reactive silicon group, which can promote the hydrosilylation reaction of an organic polymer containing an unsaturated group more than the conventional method when the hydrosilylation reaction is carried out using a silylating agent.

[0013] Solutions for solving problems

[0014] The present invention is as follows [1] to

[12] .

[0015] [1] A method for producing an organic polymer containing a reactive silicon group, wherein the organic polymer containing a reactive silicon group has a reactive silicon group represented by the following formula (1), wherein the organic polymer containing an unsaturated group is reacted with a silylating agent in the presence of a co-catalyst comprising a Group 8 metal catalyst and a carboxylic acid compound having a carbon-carbon triple bond.

[0016] -SiR a X 3-a Formula (1)

[0017] [In formula (1), R represents a monovalent organic group having 1 to 20 carbon atoms and is an organic group other than a hydrolyzable group, and X represents a hydroxyl group, a halogen atom or a hydrolyzable group. a is an integer from 0 to 2. When a is 2, R may be the same or different from each other, and when a is 0 or 1, X may be the same or different from each other.]

[0018] [2] The method for producing an organic polymer containing a reactive silicon group according to [1], wherein the Group 8 metal catalyst comprises at least one metal selected from the group consisting of cobalt, nickel, ruthenium, rhodium, palladium, iridium and platinum, or comprises at least one metal selected from the group consisting of ruthenium, palladium and platinum, or comprises platinum.

[0019] [3] The method for producing a reactive silicon group-containing organic polymer according to [1] or [2], wherein the carboxylic acid compound having a carbon-carbon triple bond has a carbon number of 3 or more and 17 or less, 3 or more and 10 or less, or 4 or more and 10 or less.

[0020] [4] The method for producing a reactive silicon group-containing organic polymer according to any one of [1] to [3], wherein the carboxylic acid compound having a carbon-carbon triple bond is a carboxylic acid compound having a carbon-carbon triple bond at the α-position carbon.

[0021] [5] The method for producing a reactive silicon group-containing organic polymer according to any one of [1] to [4], wherein the molar ratio of the carboxylic acid compound having a carbon-carbon triple bond to the Group 8 metal catalyst is 0.01 to 25, 0.05 to 20, or 0.1 to 10.

[0022] [6] The method for producing a reactive silicon group-containing organic polymer according to any one of [1] to [5], wherein the co-catalyst further comprises a carboxylic acid compound having a carbon-carbon double bond.

[0023] [7] The method for producing a reactive silicon group-containing organic polymer according to [6], wherein the carboxylic acid compound having a carbon-carbon double bond is a carboxylic acid compound having a carbon-carbon double bond at the α-position carbon.

[0024] [8] The method for producing a reactive silicon group-containing organic polymer according to [6] or [7], wherein the amount of the carboxylic acid compound having a carbon-carbon double bond used is 0.1 to 10 mol or 0.5 to 5 mol relative to 1 mol of the unsaturated group of the unsaturated group-containing organic polymer.

[0025] [9] The method for producing a reactive silicon group-containing organic polymer according to [1] to [8], wherein the co-catalyst further comprises a silane compound represented by the following formula (2).

[0026] HkDJ 1 Formula 3 (2)

[0027] [In formula (2), R 1 R represents a monovalent organic group having 1 to 20 carbon atoms, and is an organic group other than a hydrolyzable group. 1 are optionally the same as or different from each other.]

[0028]

[10] The method for producing a reactive silicon group-containing organic polymer according to [9], wherein the molar ratio of the silane compound to the carboxylic acid compound having a carbon-carbon triple bond is 0.05 to 20, or 0.1 to 10.

[0029]

[11] The method for producing a reactive silicon group-containing organic polymer according to [1] to

[10] , wherein the reactive silicon group-containing organic polymer is a polymer having a unit based on an oxyalkylene monomer.

[0030]

[12] The method for producing a reactive silicon group-containing organic polymer according to [1] to

[10] , wherein the reactive silicon group-containing organic polymer is a polymer having a unit based on an alkyl acrylate monomer or an alkyl methacrylate monomer.

[0031] Effects of the Invention

[0032] According to the present invention, there can be provided a method for producing a reactive silicon group-containing organic polymer, which can promote the hydrosilylation reaction of an unsaturated group-containing organic polymer using a silylating agent more than in conventional methods. DETAILED DESCRIPTION

[0033] The meanings and definitions of the terms in this specification are as follows.

[0034] The numerical range represented by "to" means a numerical range having the numerical values ​​before and after "to" as the lower limit and the upper limit.

[0035] The α-carbon refers to a carbon atom bonded to the carbon atom of the carboxyl group of the carboxylic acid compound or the carbonyl group derived from the carboxyl group.

[0036] The "unit" constituting a polymer refers to an atomic group directly formed by polymerization of a monomer.

[0037] "Oxyalkylene polymer" is a polymer consisting of a main chain and terminal groups. The "main chain" in the oxyalkylene polymer contains the residue of the initiator and the repeating unit (polyoxyalkylene chain) based on the oxyalkylene monomer. The "terminal group" in the oxyalkylene polymer refers to the atomic group containing the oxygen atom closest to the molecular end among the oxygen atoms in the polyoxyalkylene chain. However, in the case where the atomic group contains the residue of the initiator, it is not regarded as an terminal group.

[0038] The “(meth)acrylate polymer” refers to a polymer having one or both of a polymer chain formed of repeating units based on an alkyl acrylate monomer and a polymer chain formed of repeating units based on an alkyl methacrylate monomer.

[0039] “(Meth)acrylic acid” means one or both of acrylic acid and methacrylic acid.

[0040] The "unsaturated group" refers to a monovalent group containing a carbon-carbon double bond or a carbon-carbon triple bond at a molecular terminal.

[0041] The "carboxylic acid compound" refers to a compound having a carboxyl group and a derivative thereof. Examples of the derivative include esters and carboxylic anhydrides.

[0042] “USV” refers to the unsaturation value of a polymer, which can be determined according to the unsaturation value determination method (Wijs method).

[0043] The "silylation rate" can be measured by NMR analysis and determined by the following formula.

[0044] Silylation rate = number of reactive silicon groups / [number of reactive silicon groups + (number of carbon-carbon double bonds) + (number of carbon-carbon triple bonds) × 2.

[0045] The number average molecular weight (Mn) and mass average molecular weight (Mw) in this specification refer to the polystyrene-equivalent molecular weight measured by gel permeation chromatography (GPC) using tetrahydrofuran as the eluent, using a polystyrene polymer with a known molecular weight to prepare a calibration curve. The molecular weight distribution (Mw / Mn) is the ratio of Mw to Mn.

[0046] 《Method for producing organic polymer containing reactive silicon group》

[0047] The method for producing a reactive silicon group-containing organic polymer of the present embodiment reacts an unsaturated group-containing organic polymer with a silylating agent in the presence of a co-catalyst comprising a Group 8 metal catalyst and a carboxylic acid compound having a carbon-carbon triple bond.

[0048] The reactive silicon group-containing organic polymer contains a reactive silicon group represented by formula (1) described later.

[0049] <Organic polymers containing unsaturated groups>

[0050] Examples of the unsaturated group-containing organic polymer include, but are not limited to, unsaturated group-containing polyether polymers and unsaturated group-containing vinyl polymers.

[0051] As the unsaturated group-containing polyether polymer, an unsaturated group-containing oxyalkylene polymer is preferred. As the unsaturated group-containing vinyl polymer, an unsaturated group-containing (meth)acrylate polymer is preferred.

[0052] The Mn of the unsaturated group-containing organic polymer is preferably 500 to 200,000, and Mw / Mn is preferably 1.80 or less. The number of unsaturated groups in one molecule of the unsaturated group-containing organic polymer is preferably 1.0 to 8.0, and more preferably 1.0 to 6.0.

[0053] (Oxyalkylene polymer containing unsaturated group)

[0054] The oxyalkylene polymer containing unsaturated groups is a polymer having unsaturated groups and repeating units based on oxyalkylene monomers. The oxyalkylene polymer containing unsaturated groups is composed of a main chain and terminal groups, the main chain having the residue of an initiator and repeating units based on oxyalkylene monomers, and the terminal groups having unsaturated groups. Preferably, the main chain is composed of the residue of an initiator and repeating units based on oxyalkylene monomers, and the terminal groups have oxygen atoms and unsaturated groups. As oxyalkylene monomers, ethylene oxide monomers, propylene oxide monomers, butylene oxide monomers, and tetramethylene oxide monomers can be listed. Preferred propylene oxide monomers. When the polyoxyalkylene chain in the main chain of the oxyalkylene polymer containing unsaturated groups is a copolymer chain of two or more oxyalkylene monomers, it can be a block polymer chain or a random polymer chain.

[0055] The number of terminal groups in one molecule of the unsaturated group-containing oxyalkylene polymer is preferably 1 to 8, more preferably 2 to 6, and even more preferably 2 to 4.

[0056] The number of unsaturated groups in one molecule of the unsaturated group-containing oxyalkylene polymer is preferably 1.0 to 8.0, more preferably 2.0 to 6.0, and further preferably 2.0 to 4.0.

[0057] The number of unsaturated groups per terminal group of the unsaturated group-containing oxyalkylene polymer is preferably 0.5 to 4.0, more preferably 0.6 to 2.0.

[0058] The Mn of the unsaturated group-containing oxyalkylene polymer is preferably from 2,000 to 100,000, more preferably from 5,000 to 50,000.

[0059] The Mw / Mn of the unsaturated group-containing oxyalkylene polymer is preferably 1.80 or less, more preferably 1.50 or less, further preferably 1.40 or less, and particularly preferably 1.20 or less. The Mw / Mn of the unsaturated group-containing oxyalkylene polymer is preferably 1.00 to 1.80, more preferably 1.00 to 1.50, further preferably 1.00 to 1.40, and particularly preferably 1.00 to 1.20.

[0060] (Method for producing unsaturated group-containing oxyalkylene polymer)

[0061] The method for producing the oxyalkylene polymer containing unsaturated groups can use a conventionally known method. For example, it can be produced by subjecting one or more oxyalkylene monomers to ring-opening addition polymerization with an initiator, and converting the hydroxyl group of the terminal group of the obtained polymer into an alkeneoxy group or an alkynyloxy group. As auxiliary materials such as an initiator required for the polymerization, conventionally known auxiliary materials can also be used, and reaction conditions such as reaction temperature and reaction pressure can also be appropriately selected.

[0062] As the ring-opening polymerization catalyst when one or more oxyalkylene monomers and an initiator are subjected to ring-opening addition polymerization, a conventionally known catalyst can be used. For example, a base catalyst such as KOH, a metal compound-porphyrin complex catalyst such as a complex obtained by reacting an organic aluminum compound with porphyrin, a composite metal cyanide complex catalyst, and a catalyst formed from a phosphazene compound can be listed.

[0063] From the perspective of being able to narrow the molecular weight distribution of the polymer and being easy to obtain a curable composition with low viscosity, it is preferably a composite metal cyanide complex catalyst. Composite metal cyanide complex catalysts can use compounds known in the past. The manufacturing method of the polymer using the composite metal cyanide complex can also adopt a known method. For example, compounds and manufacturing methods disclosed in International Publication Gazette No. 2003 / 062301, International Publication Gazette No. 2004 / 067633, Japanese Patent Publication No. 2004-269776, Japanese Patent Publication No. 2005-15786, International Publication Gazette No. 2013 / 065802, and Japanese Patent Publication No. 2015-010162 can be used.

[0064] As methods for converting the hydroxyl group of the terminal group of the polymer into an alkeneoxy group or an alkynyloxy group, for example, the following three methods can be cited. The first method is a method in which an alkali metal salt is allowed to act on the polymer, and then a halogenated hydrocarbon compound having a carbon-carbon double bond is reacted. The second method is a method in which an alkali metal salt is allowed to act on the polymer, and then an epoxy compound having an unsaturated group is reacted, and then a halogenated hydrocarbon compound having an unsaturated group is reacted. The third method is a method in which an alkali metal salt is allowed to act on the polymer, and then a halogenated hydrocarbon compound having a carbon-carbon triple bond is reacted.

[0065] (Unsaturated group-containing (meth)acrylate polymer)

[0066] The unsaturated group-containing (meth)acrylate polymer is a polymer having an unsaturated group and a repeating unit based on an alkyl acrylate monomer or an alkyl methacrylate monomer. The unsaturated group-containing (meth)acrylate polymer may have a repeating unit based on other monomers copolymerizable with the alkyl acrylate monomer or the alkyl methacrylate monomer.

[0067] As the monomer constituting the (meth)acrylate polymer, for example, a conventionally known monomer described in JP-A-11-130931 can be used.

[0068] The content of the unit based on the alkyl (meth)acrylate monomer is preferably 50% by mass or more, more preferably 70% by mass or more, and may be 100% by mass relative to all the monomer units constituting the (meth)acrylate polymer containing an unsaturated group. The content of the unit based on the alkyl (meth)acrylate monomer is preferably 50 to 100% by mass, more preferably 70 to 100% by mass relative to all the monomer units constituting the (meth)acrylate polymer containing an unsaturated group.

[0069] The number of unsaturated groups in one molecule of the unsaturated group-containing (meth)acrylate polymer is preferably 1.0 to 8.0, more preferably 1.0 to 6.0.

[0070] The Mn of the unsaturated group-containing (meth)acrylate polymer is preferably 500 to 100,000, more preferably 1,000 to 80,000.

[0071] The Mw / Mn of the (meth)acrylate polymer containing an unsaturated group is preferably 1.80 or less, more preferably 1.50 or less, further preferably 1.40 or less, and particularly preferably 1.20 or less. The Mw / Mn of the oxyalkylene polymer containing an unsaturated group is preferably 1.00 to 1.80, more preferably 1.00 to 1.50, further preferably 1.00 to 1.40, and particularly preferably 1.00 to 1.20.

[0072] (Method for producing unsaturated group-containing (meth)acrylate polymer)

[0073] The method for producing the (meth)acrylate polymer containing an unsaturated group can be a conventionally known method. For example, there can be cited a method of polymerizing an alkyl (meth)acrylate monomer with a compound having an unsaturated group, a method of reacting with a compound having two alkenyl groups in the final stage of the polymerization reaction using a living radical polymerization method, etc. In particular, the living radical polymerization method is preferred because it has an arbitrary molecular weight, a narrow molecular weight distribution, and a low-viscosity polymer can be obtained.

[0074] As a living radical polymerization method, for example, atom transfer radical polymerization (ATRP method) can be cited, which is to polymerize (meth) alkyl acrylate monomers using organic halides or sulfonyl halide compounds as initiators and transition metal complexes as catalysts. As atom transfer radical polymerization (ATRP method), polymerization can be carried out by a previously known polymerization method described in Japanese Patent Publication No. 11-130931. The (meth) acrylate polymer containing an unsaturated group can be obtained by polymerizing the (meth) alkyl acrylate monomer using atom transfer radical polymerization (ATRP method), and then reacting with a compound having at least two alkenyl groups such as 1,5-hexadiene, 1,7-octadiene, 1,9-decadiene, etc. to introduce an unsaturated group. The "terminal group" in the (meth) acrylate polymer obtained by the ATRP method refers to an atomic group containing the carbon atom closest to the molecular end among the carbon atoms in the chain of the (meth) acrylate polymer. When the atomic group contains the residue of the initiator, it is not regarded as an end group.

[0075] <Silylating agent>

[0076] Examples of the silylating agent include compounds having both a group capable of reacting with an unsaturated group to form a bond (e.g., a sulfanyl group) and a reactive silicon group represented by formula (1) described below, and hydrosilane compounds (e.g., HSiR a X 3-a , R, X, and a are defined in the same manner as in the formula (1) described below). Specifically, trimethoxysilane, triethoxysilane, triisopropoxysilane, tri(2-propyleneoxy)silane, triacetoxysilane, dimethoxymethylsilane, diethoxymethylsilane, dimethoxyethylsilane, diisopropoxymethylsilane, (α-chloromethyl)dimethoxysilane, and (α-chloromethyl)diethoxysilane can be exemplified. From the perspective of high activity and good curability, trimethoxysilane, triethoxysilane, dimethoxymethylsilane, and diethoxymethylsilane are preferred, and dimethoxymethylsilane or trimethoxysilane is more preferred.

[0077] For example, when dimethoxymethylsilane is used to hydrosilylate an organic polymer containing an unsaturated group, a polymer having a dimethoxymethylsilyl group (a type of reactive silicon group) can be obtained. The polymer having a reactive silicon group provides a crosslinked product by a hydrolysis reaction of the silyl group caused by moisture in the air, etc., and a subsequent silanol condensation reaction with other polymer molecules. The polymer having a reactive silicon group is used for applications such as adhesives, adhesives, coatings, sealing materials, waterproof materials, etc. that require weather resistance, heat resistance, and moisture permeability resistance.

[0078] When the unsaturated group of the organic polymer containing an unsaturated group is a carbon-carbon double bond, the amount of the silylating agent used is preferably 1 to 20 mol, more preferably 1 to 2 mol, relative to 1 mol of the unsaturated group. When the unsaturated group of the organic polymer containing an unsaturated group is a carbon-carbon triple bond, the amount of the silylating agent used is preferably 2 to 40 mol, more preferably 2 to 4 mol, relative to 1 mol of the unsaturated group. If it is below the above upper limit, the cost is reduced and the operation of removing the silylating agent after the reaction becomes simple, so it is preferred. If it is above the above lower limit, the silylation rate becomes high, so it is preferred.

[0079] <Group 8 Metal Catalyst>

[0080] The Group 8 metal catalyst is a catalyst having a Group 8 metal in the short-period periodic table. As the Group 8 metal, it is preferably at least one metal selected from the group consisting of cobalt, nickel, ruthenium, rhodium, palladium, iridium and platinum, more preferably at least one metal selected from the group consisting of ruthenium, palladium and platinum, and further preferably platinum. As the Group 8 metal catalyst, it is preferably a Group 8 metal monomer, a carrier in which the Group 8 metal is supported on a carrier, a Group 8 metal salt or a complex of a Group 8 metal and an organic compound. Specifically, for example, preferred are platinum monomers, platinum metal on a carrier in which solid platinum is supported on a carrier such as alumina, silica, carbon black, chloroplatinic acid complexes with alcohols, aldehydes, ketones, etc. as ligands or chloroplatinic acid complexes, platinum-olefin complexes [for example, Pt(CH2=CH2)2(PPh3), Pt(CH2=CH2)2Cl2], platinum-acetylacetone complexes [Pt(C5H7O2)2], platinum-vinylsiloxane complexes [Pt{(vinyl)Me2SiOSiMe2(vinyl)}, Pt{Me(vinyl)SiO}4], platinum-phosphine complexes [Ph(PPh3)4, Pt(PBu3)4], platinum-phosphite complexes [Pt{P(OPh)3}4] and other platinum complexes.

[0081] These Group 8 metal catalysts can be used alone or in combination of two or more. Chloroplatinic acid, platinum olefin complexes, platinum-acetylacetone complexes, and platinum-vinylsiloxane complexes are preferred due to their high reactivity. Specifically, hexachloroplatinic (IV) acid hexahydrate and platinum (0)-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complexes are preferred.

[0082] There is no particular limitation on the amount of the Group 8 metal catalyst used, but the amount of the Group 8 metal catalyst used is preferably 1.0 to 20 mass ppm, more preferably 1.5 to 10 mass ppm, relative to the total mass of the organic polymer containing an unsaturated group. When the amount of the Group 8 metal catalyst used is at least the lower limit of the above range, the hydrosilylation reaction is easy to proceed sufficiently, and when the amount is at most the upper limit of the above range, it is preferred from the perspective of cost.

[0083] <Promoter>

[0084] The co-catalyst includes a carboxylic acid compound having a carbon-carbon triple bond. Examples of the carboxylic acid compound having a carbon-carbon triple bond include monocarboxylic acids having a carbon-carbon triple bond, dicarboxylic acids having a carbon-carbon triple bond, carboxylic anhydrides having a carbon-carbon triple bond, and esters having a carbon-carbon triple bond.

[0085] The monocarboxylic acid having a carbon-carbon triple bond is a compound in which a hydrogen atom bonded to a carbon in a hydrocarbon compound having a carbon-carbon triple bond is substituted with a carboxyl group.

[0086] The dicarboxylic acid having a carbon-carbon triple bond is a compound in which two hydrogen atoms bonded to carbon in a hydrocarbon compound having a carbon-carbon triple bond are substituted with carboxyl groups.

[0087] The carboxylic acid anhydride having a carbon-carbon triple bond is a compound obtained by dehydration condensation of two carboxyl groups of the carboxylic acid having a carbon-carbon triple bond, a compound obtained by dehydration condensation of a carboxyl group of the carboxylic acid having a carbon-carbon triple bond and a carboxyl group of a carboxylic acid not having a carbon-carbon triple bond, or a compound obtained by dehydration condensation of two carboxyl groups in one molecule of a dicarboxylic acid having a carbon-carbon triple bond.

[0088] The ester having a carbon-carbon triple bond is a compound in which the hydrogen atom in the carboxyl group of the carboxylic acid having a carbon-carbon triple bond is replaced by a monovalent hydrocarbon group. The monovalent hydrocarbon group is preferably a monovalent saturated hydrocarbon group, and examples thereof include a linear or branched alkyl group and a cycloalkyl group. Among them, a methyl group and an ethyl group are preferred.

[0089] As the hydrocarbon compound having a carbon-carbon triple bond, an example may be a compound having a carbon-carbon triple bond in which at least one carbon-carbon single bond in a saturated hydrocarbon compound is replaced by a carbon-carbon triple bond. As the saturated hydrocarbon compound, an example may be a straight chain or branched alkane or cycloalkane. The hydrogen atom in the compound having a carbon-carbon triple bond may be substituted by a substituent. As the substituent, an aromatic group, a hydroxyl group, etc. may be cited.

[0090] The carbon number of the carboxylic acid compound having a carbon-carbon triple bond is preferably 3 or more and 17 or less, more preferably 3 or more and 10 or less, and particularly preferably 4 or more and 10 or less. The carbon number of the monocarboxylic acid compound having a carbon-carbon triple bond is preferably 3 or more and 17 or less, and more preferably 3 or more and 10 or less. The carbon number of the dicarboxylic acid having a carbon-carbon triple bond is preferably 4 or more and 10 or less. The carbon number of the carboxylic anhydride having a carbon-carbon triple bond is preferably 4 or more and 10 or less. The carbon number of the ester having a carbon-carbon triple bond is preferably 4 or more and 17 or less, and more preferably 4 or more and 10 or less.

[0091] The number of triple bonds in one molecule of the carboxylic acid compound having a carbon-carbon triple bond is preferably 1 or 2, and more preferably 1.

[0092] As the carboxylic acid compound having a carbon-carbon triple bond, a carboxylic acid compound having a carbon-carbon triple bond at the α-position carbon is preferred. As the carboxylic acid compound having a carbon-carbon triple bond at the α-position carbon, monocarboxylic acids having a carbon-carbon triple bond at the α-position carbon, dicarboxylic acids having a carbon-carbon triple bond at the α-position carbon, carboxylic anhydrides having a carbon-carbon triple bond at the α-position carbon, or esters having a carbon-carbon triple bond at the α-position carbon can be cited, preferably monocarboxylic acids having a carbon-carbon triple bond at the α-position carbon and esters having a carbon-carbon triple bond at the α-position carbon, more preferably monocarboxylic acids having a carbon-carbon triple bond at the α-position carbon. In the case of dicarboxylic acids, there are dicarboxylic acids having a carbon-carbon triple bond at two α-positions and dicarboxylic acids having a carbon-carbon triple bond only at one α-position, preferably dicarboxylic acids having a carbon-carbon triple bond at two α-positions.

[0093] The carbon number of the carboxylic acid compound having a carbon-carbon triple bond at the α-carbon is preferably 3 or more and 17 or less, more preferably 3 or more and 10 or less, and particularly preferably 4 or more and 10 or less.

[0094] As the monocarboxylic acid having a carbon-carbon triple bond at the α-position carbon, preferably phenylpropiolic acid, propiolic acid, 2-butiolic acid, 2-heptiolic acid, 2-methyl-3-butiolic acid, 2-hydroxy-3-butiolic acid, 3-butiolic acid, more preferably phenylpropiolic acid. As the dicarboxylic acid having a carbon-carbon triple bond at the α-position carbon, acetylene dicarboxylic acid can be listed. As the carboxylic anhydride having a carbon-carbon triple bond at the α-position carbon, propiolic anhydride can be listed. As the ester having a carbon-carbon triple bond at the α-position carbon, phenylpropiolic acid methyl ester can be listed.

[0095] When the carboxylic acid compound having a carbon-carbon triple bond at the α-position carbon has two or more triple bonds in one molecule, it may have a carbon-carbon triple bond other than the α-position carbon.

[0096] As a co-catalyst, if a carboxylic acid compound with a carbon-carbon double bond is also included, higher silylation can be achieved, so it is preferred. However, in the case of a carboxylic acid compound with a carbon-carbon triple bond and a carbon-carbon double bond in one molecule, it is regarded as a carboxylic acid compound with a carbon-carbon triple bond. That is, "a carboxylic acid compound with a carbon-carbon double bond" in this specification is a carboxylic acid compound with a carbon-carbon double bond and without a carbon-carbon triple bond.

[0097] Examples of the carboxylic acid compound having a carbon-carbon double bond include monocarboxylic acids having a carbon-carbon double bond, dicarboxylic acids having a carbon-carbon double bond, carboxylic acid anhydrides having a carbon-carbon double bond, and esters having a carbon-carbon double bond.

[0098] The monocarboxylic acid having a carbon-carbon double bond is a compound in which a hydrogen atom bonded to carbon in a hydrocarbon compound having a carbon-carbon double bond is substituted with a carboxyl group.

[0099] The dicarboxylic acid having a carbon-carbon double bond is a compound in which two hydrogen atoms bonded to carbon in a hydrocarbon compound having a carbon-carbon double bond are substituted with carboxyl groups.

[0100] The carboxylic acid anhydride having a carbon-carbon double bond is a compound obtained by dehydration condensation of two carboxyl groups of the carboxylic acid having a carbon-carbon double bond, a compound obtained by dehydration condensation of a carboxyl group of the carboxylic acid having a carbon-carbon double bond and a carboxyl group of a carboxylic acid not having a carbon-carbon double bond, or a compound obtained by dehydration condensation of two carboxyl groups contained in one molecule of a dicarboxylic acid having a carbon-carbon double bond.

[0101] The ester having a carbon-carbon double bond is a compound in which the hydrogen atom in the carboxyl group of the monocarboxylic acid having a carbon-carbon double bond is replaced by a monovalent hydrocarbon group. The monovalent hydrocarbon group is preferably a monovalent saturated hydrocarbon group, and examples thereof include a straight-chain or branched alkyl group and a cycloalkyl group. Among them, a methyl group and an ethyl group are preferred.

[0102] The carbon number of the carboxylic acid compound having a carbon-carbon double bond is preferably 3 or more and 18 or less, more preferably 4 or more and 18 or less, and even more preferably 4 or more and 10 or less.

[0103] As the carboxylic acid compound having a carbon-carbon double bond, a carboxylic acid compound having a carbon-carbon double bond at the α-position carbon is preferred. As the carboxylic acid compound having a carbon-carbon double bond at the α-position carbon, monocarboxylic acids having a carbon-carbon double bond at the α-position carbon, dicarboxylic acids having a carbon-carbon double bond at the α-position carbon, carboxylic anhydrides having a carbon-carbon double bond at the α-position carbon, and esters having a carbon-carbon double bond at the α-position carbon can be listed, preferably monocarboxylic acids having a carbon-carbon double bond at the α-position carbon and esters having a carbon-carbon double bond at the α-position carbon, more preferably monocarboxylic acids having a carbon-carbon double bond at the α-position carbon, and particularly preferably monocarboxylic acids having a carbon number of 3 or more and 7 or less and having a carbon-carbon double bond at the α-position carbon. As monocarboxylic acids having a carbon number of 3 or more and 7 or less and having a carbon-carbon double bond at the α-position carbon, 2-hexenoic acid and crotonic acid can be listed.

[0104] As the hydrocarbon compound having a carbon-carbon double bond, an example may be a compound having a carbon-carbon double bond in which at least one carbon-carbon bond in a saturated hydrocarbon compound is replaced by a carbon-carbon double bond. As the saturated hydrocarbon compound, an example may be a straight chain or branched chain alkane, a cycloalkane. The hydrogen atom in the compound having a carbon-carbon double bond may be substituted by a substituent. As the substituent, an aromatic group, a hydroxyl group, etc. may be cited.

[0105] The number of double bonds in one molecule of the carboxylic acid compound having a carbon-carbon double bond is preferably 1 or 2, and more preferably 1.

[0106] When the carboxylic acid compound having a carbon-carbon double bond at the α-position carbon has two or more double bonds in one molecule, it may have a carbon-carbon double bond other than the α-position carbon.

[0107] When a silane compound represented by the following formula (2) is further contained as a co-catalyst, higher silylation can be achieved, which is preferred.

[0108] HkDJ 1 Formula 3 (2)

[0109] In the formula (2), R 1 R represents a monovalent organic group having 1 to 20 carbon atoms, and is an organic group other than a hydrolyzable group. 1 They are optionally the same as or different from each other.

[0110] R 1 It is preferably at least one selected from the group consisting of an alkyl group, a cycloalkyl group, and an aryl group. It is more preferably at least one selected from the group consisting of a linear or branched alkyl group having 1 to 4 carbon atoms, a cyclohexyl group, a phenyl group, and a benzyl group. It is preferably a methyl group or an ethyl group, and particularly preferably an ethyl group. In addition, R 1 same.

[0111] Examples of the silane compound include trimethylsilane, triethylsilane, triisopropylsilane, triphenylsilane, dimethylethylsilane, and dimethylphenylsilane, and triethylsilane is preferred.

[0112] As a co-catalyst, when the silane compound is included, it can be a carboxylic acid compound having a carbon-carbon triple bond and the silane compound, or any combination of a carboxylic acid compound having a carbon-carbon triple bond, a carboxylic acid compound having a carbon-carbon double bond and the silane compound, preferably comprising a carboxylic acid compound having a carbon-carbon triple bond, a carboxylic acid compound having a carbon-carbon double bond and the silane compound.

[0113] The molar ratio of the carboxylic acid compound having a carbon-carbon triple bond to the Group 8 metal catalyst is preferably 0.01 to 25, more preferably 0.05 to 20, and particularly preferably 0.1 to 10. If it is above the lower limit of the range, the silylation rate is further improved. If it is below the upper limit of the range, the amount of acid in the solution is suppressed and thickening is suppressed.

[0114] When a carboxylic acid compound having a carbon-carbon double bond is included as a co-catalyst, the amount of the carboxylic acid compound having a carbon-carbon double bond is preferably 0.1 to 10 mol, more preferably 0.5 to 5 mol, relative to 1 mol of the unsaturated group of the organic polymer containing an unsaturated group. If it is above the lower limit of the range, the silylation rate is further improved. If it is below the upper limit of the range, the amount of acid in the solution is suppressed, and the thickening of the composition containing the organic polymer containing an unsaturated group or the organic polymer containing a reactive silicon group is suppressed.

[0115] When the silane compound represented by the formula (2) is included as a co-catalyst, the molar ratio of the silane compound to the carbon-carbon triple bond carboxylic acid compound is preferably 0.05 to 20, and more preferably 0.1 to 10. If it is above the lower limit of the range, the silylation rate is further improved. In addition, the amount of acid in the solution is suppressed, and thickening is suppressed.

[0116] It is preferred that the Group 8 metal catalyst and the co-catalyst be dissolved and diluted in various solvents to stabilize the Group 8 metal catalyst and the co-catalyst, so that the catalyst and the co-catalyst are easy to handle. As preferred solvents, for example, hydrocarbon solvents such as hexane, cyclohexane, heptane, benzene, toluene, and xylene, halogenated hydrocarbon compounds, alcohols, glycols, ethers, esters, ketones, nitriles, amides, etc. can be cited. Among them, alcohols, ketones, nitriles, and amides are preferred, and isopropanol, acetone, N,N-dimethylformamide (DMF), acetonitrile are more preferred, and acetonitrile is particularly preferred. The Group 8 metal catalyst and the co-catalyst can be diluted by two or more solvents.

[0117] <Method for adding Group 8 metal catalyst, co-catalyst and silylating agent>

[0118] There is no particular limitation on the order of addition of the Group 8 metal catalyst, co-catalyst, and silylating agent during the hydrosilylation reaction. As a preferred method, the following is an example. As a method for adding a Group 8 metal catalyst, co-catalyst, and silylating agent during the hydrosilylation reaction, a method can be cited in which a Group 8 metal catalyst and a carboxylic acid compound having a carbon-carbon triple bond are dissolved in the solvent as a premix, and colloidal particles of the Group 8 metal catalyst are formed in advance, and added to a reaction solution containing an organic polymer containing an unsaturated group, and then a silylating agent is added to perform hydrosilylation. In addition, as a method for adding a Group 8 metal catalyst, co-catalyst, and silylating agent during the hydrosilylation reaction, a method can be cited in which a Group 8 metal catalyst and a carboxylic acid compound having a carbon-carbon triple bond are respectively added to a reaction solution containing an organic polymer containing an unsaturated group, and then a silylating agent is added to perform hydrosilylation. Since the colloidal particles of the 8th group metal catalyst are formed in advance, the dispersibility of the metal catalyst is improved, and it is easy to promote the hydrosilylation reaction, so the premix is ​​preferably added to the reaction solution. In addition, when the carboxylic acid compound with a carbon-carbon double bond is included as a co-catalyst, the carboxylic acid compound with a carbon-carbon double bond is preferably added to the reaction solution, and then, the premix is ​​added to the reaction solution. And then, when the silane compound is included as a co-catalyst, it is preferred that the silane compound is included in the premix.

[0119] <Reaction conditions>

[0120] The hydrosilylation reaction can be carried out in a solvent-free system or in the presence of a solvent. As the solvent for the hydrosilylation reaction, hydrocarbons, halogenated hydrocarbons, ethers, esters can be used, but heptane, hexane, cyclohexane, benzene, toluene, xylene, etc. are preferably used. In addition, when the organic polymer containing unsaturated groups is a solid or a high-viscosity liquid, a solvent is preferably used in order to reduce the viscosity of the reaction solution.

[0121] The gas phase of the reactor during the hydrosilylation reaction may be composed only of an inert gas such as nitrogen or helium, or may contain oxygen or the like.

[0122] In the case of introducing oxygen into the gas phase, from the perspective of suppressing the oxidation of the reaction solvent, the hydrosilylation reaction can be carried out in the presence of an antioxidant. As an antioxidant, there is no particular limitation, and phenolic antioxidants and amine antioxidants having a free radical chain inhibitor function can be used. As a phenolic antioxidant, for example, 2,6-di-tert-butyl-p-cresol, 2,6-di-tert-butylphenol, 2,4-dimethyl-6-tert-butylphenol, 2,2'-methylenebis(4-methyl-6-tert-butylphenol), 4,4'-butylenebis(3-methyl-6-tert-butylphenol), 4,4'-thiobis(3-methyl-6-tert-butylphenol), tetra{methylene-3(3,5-di-tert-butyl-4-hydroxyphenyl)propionate}methane, 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, etc. can be used. As the amine antioxidant, for example, phenyl-β-naphthylamine, α-naphthylamine, N,N′-di-sec-butyl-p-phenylenediamine, phenothiazine, N,N′-diphenyl-p-phenylenediamine, etc. can be used.

[0123] The reaction temperature of the hydrosilylation reaction is preferably 40°C or higher and 150°C or lower, and more preferably 40°C or higher and 100°C or lower.

[0124] <Reactive silicon group-containing organic polymer>

[0125] The type of organic polymer, Mn, and Mw / Mn of the reactive silicon group-containing organic polymer are the same as those described in the above-mentioned unsaturated group-containing organic polymer, and the preferred ranges are also the same.

[0126] The number of reactive silicon groups per molecule is preferably 0.8 to 8.0, more preferably 0.8 to 6.0.

[0127] The silylation rate is preferably 80 to 100 mol %, more preferably 85 to 100 mol %, and particularly preferably 90 to 100 mol %.

[0128] <Reactive silicon group-containing oxyalkylene polymer>

[0129] The reactive silicon group-containing oxyalkylene polymer is a polymer having a reactive silicon group and a repeating unit based on an oxyalkylene monomer. The reactive silicon group-containing oxyalkylene polymer is composed of a main chain and a terminal group, the main chain having a residue of an initiator and a repeating unit based on an oxyalkylene monomer, and the terminal group having a reactive silicon group. Preferably, the main chain is composed of a residue of an initiator and a repeating unit based on an oxyalkylene monomer.

[0130] The oxyalkylene monomer, the number of terminal groups in one molecule, Mn, and Mw / Mn in the reactive silicon group-containing oxyalkylene polymer are the same as those described in the unsaturated group-containing oxyalkylene polymer, and the preferred ranges are also the same.

[0131] The number of reactive silicon groups in one molecule of the reactive silicon group-containing oxyalkylene polymer is preferably 0.72 to 8.0, more preferably 0.8 to 6.0.

[0132] The number of reactive silicon groups per terminal group of the reactive silicon group-containing oxyalkylene polymer is preferably 0.8 to 3.0, more preferably 0.9 to 2.0.

[0133] <Reactive silicon group-containing (meth)acrylate polymer>

[0134] The reactive silicon group-containing (meth)acrylate polymer is a polymer having a reactive silicon group and having a repeating unit based on an alkyl acrylate monomer or an alkyl methacrylate monomer.

[0135] The monomers constituting the reactive silicon group-containing (meth)acrylate polymer, the number of terminal groups in one molecule, Mn, and Mw / Mn are the same as those described in the unsaturated group-containing (meth)acrylate polymer.

[0136] The number of reactive silicon groups in one molecule of the reactive silicon group-containing (meth)acrylate polymer is preferably 0.8 to 8.0, and more preferably 0.8 to 6.0.

[0137] (Reactive Silicon Group)

[0138] The reactive silicon group has a hydrolyzable group bonded to a silicon atom and is obtained by crosslinking by forming a siloxane bond. The reaction of forming the siloxane bond is accelerated by a curing catalyst. The reactive silicon group is represented by the following formula (1).

[0139] -SiR a X 3-a Formula (1)

[0140] [In formula (1), R represents a monovalent organic group having 1 to 20 carbon atoms and is an organic group other than a hydrolyzable group, and X represents a hydroxyl group, a halogen atom or a hydrolyzable group. a is an integer from 0 to 2. When a is 2, R may be the same or different from each other, and when a is 0 or 1, X may be the same or different from each other.]

[0141] In the above formula (1), R represents a monovalent organic group having 1 to 20 carbon atoms. R does not include a hydrolyzable group.

[0142] R is preferably at least one selected from the group consisting of a hydrocarbon group having 1 to 20 carbon atoms and a triorganosiloxy group.

[0143] R is preferably at least one selected from the group consisting of an alkyl group, a cycloalkyl group, an aryl group, an α-chloroalkyl group, and a siloxytriorganosiloxy group. More preferably, it is at least one selected from the group consisting of a linear or branched alkyl group having 1 to 4 carbon atoms, a cyclohexyl group, a phenyl group, a benzyl group, an α-chloromethyl group, a trimethylsiloxy group, a triethylsiloxy group, and a triphenylsiloxy group. From the perspective of good curability of the polymer having a reactive silicon group and good stability of the curable composition, it is preferably a methyl group, an ethyl group, or an α-chloromethyl group, and from the perspective of easy availability, it is more preferably a methyl group.

[0144] In the above formula (1), X represents a hydroxyl group, a halogen atom or a hydrolyzable group. X's may be the same or different from each other.

[0145] Examples of the hydrolyzable group include an alkoxy group, an acyloxy group, a ketoximo group, an amino group, an amide group, an acid amide group, an aminooxy group, a sulfanyl group, and an alkenyloxy group.

[0146] From the perspective of stable hydrolysis and easy handling, an alkoxy group is preferred. The alkoxy group is preferably a methoxy group, an ethoxy group, or an isopropoxy group, and more preferably a methoxy group or an ethoxy group. When the alkoxy group is a methoxy group or an ethoxy group, a siloxane bond is quickly formed, and a cross-linked structure is easily formed in the cured product, and the physical property values ​​of the cured product are easily improved.

[0147] In the formula (1), a is an integer of 0 to 2. When a is 2, R may be the same or different. When a is 0 or 1, X may be the same or different. Since the physical properties of the cured product are likely to be excellent, a is preferably 0 or 1, and more preferably 1.

[0148] As the reactive silicon group represented by the formula (1), trimethoxysilyl, triethoxysilyl, triisopropoxysilyl, tri(2-propyleneoxy)silyl, triacetoxysilyl, dimethoxymethylsilyl, diethoxymethylsilyl, dimethoxyethylsilyl, methyldiisopropoxysilyl, (α-chloromethyl)dimethoxysilyl, (α-chloromethyl)diethoxysilyl can be cited as examples. From the perspective of high activity and good curability, trimethoxysilyl, triethoxysilyl, dimethoxymethylsilyl, diethoxymethylsilyl are preferred, and dimethoxymethylsilyl and trimethoxysilyl are more preferred.

[0149] <Curable composition>

[0150] The curable composition is obtained by mixing the reactive silicon group-containing organic polymer with other necessary components.

[0151] The content of the reactive silicon group-containing organic polymer is preferably 1 to 50% by mass, more preferably 1 to 45% by mass, and further preferably 2 to 40% by mass relative to the total mass of the curable composition. When it is below the upper limit of the above range, the strength of the cured product is more excellent and the elongation characteristics are further improved.

[0152] [Other ingredients]

[0153] As the above-mentioned other components, there can be exemplified curable compounds other than organic polymers containing reactive silicon groups, curing catalysts (silanol condensation catalysts), fillers, plasticizers, thixotropy-imparting agents, stabilizers, adhesion-imparting agents, physical property regulators, dehydrating agents, adhesion-imparting resins, reinforcing materials such as fillers, surface modifiers, flame retardants, foaming agents, solvents, and silicates.

[0154] As other components, the conventionally known components described in International Publication No. 2013 / 180203, International Publication No. 2014 / 192842, International Publication No. 2016 / 002907, Japanese Patent Publication No. 2014-88481, Japanese Patent Publication No. 2015-10162, Japanese Patent Publication No. 2015-105293, Japanese Patent Publication No. 2017-039728, Japanese Patent Publication No. 2017-214541, etc. can be used in combination without limitation. Two or more components can be used in combination.

[0155] [Mechanism of action]

[0156] It is believed that by adding a carboxylic acid compound having a carbon-carbon triple bond to the Group 8 metal catalyst, the carbonyl group coordinates with the metal atom via an unsaturated bond to produce nano-sized metal catalyst colloidal particles. It is believed that the above-mentioned metal catalyst is dispersed and stabilized as colloidal particles, thereby improving the catalyst activity. As a result, it is estimated that the hydrosilylation reaction is promoted to prepare an organic polymer containing a reactive silicon group with a high silylation rate.

[0157] In the present invention, it is considered that since the carboxylic acid compound having a carbon-carbon triple bond is efficiently coordinated to the metal atom in the metal catalyst, even if the amount of the carboxylic acid compound added is smaller, high dispersion stability can be exhibited.

[0158] It can be considered that by also including a silane compound as a co-catalyst, the silane compound is added to the unsaturated bond of the carboxylic acid compound having a carbon-carbon triple bond to form a carboxylic acid silane compound addition product having a carbon-carbon triple bond, and the addition product is coordinated with the above-mentioned metal catalyst, thereby further improving the dispersion stability of the metal catalyst colloidal particles and being able to further improve the catalyst activity.

[0159] It is believed that if a carboxylic acid compound having a carbon-carbon triple bond is combined with a silane compound, even if a carboxylic acid silane compound addition product having a carbon-carbon triple bond is formed, the carbon-carbon triple bond can remain. Therefore, it is believed that the coordination to the above-mentioned metal catalyst and the dispersion stability of the colloid particles of the coordinated metal catalyst can be taken into account at a high level, and the catalytic activity can be further improved.

[0160] [use]

[0161] As the application of the curable composition containing the organic polymer containing a reactive silicon group of the present invention, adhesives, sealing materials (such as elastic sealing materials for construction, sealing materials for multi-layer glass, rust-proofing / waterproofing sealing materials for glass ends, solar cell back sealing materials, building sealing materials, ship sealing materials, automobile sealing materials, road sealing materials), and electrical insulating materials (insulating coating materials for wires / cables) are suitable. It is particularly suitable for adhesive applications that require high modulus, good tensile strength and elongation properties of the cured product.

[0162] Example

[0163] Hereinafter, the present invention will be specifically described by way of Examples, but the present invention is not limited to the following description.

[0164] 《Measurement method / evaluation method》

[0165] <Mn、Mw / Mn>

[0166] HLC-8220GPC (product name of Tosoh Corporation) was used, TSKgel SupermultiporeHZ-M (product name of Tosoh Corporation) was used as the chromatographic column, tetrahydrofuran was used as the solvent, the sample pump was set to 0.350 mL / min, the reference pump was set to 0.350 mL / min, the detector temperature was set to 40°C, and the collection time was set to 6 minutes to 15 minutes. Mw, Mn and Mw / Mn were determined by analyzing the peaks that appeared during the collection time of 6 minutes to 11 minutes.

[0167] <Hydroxy value of oxyalkylene polymer>

[0168] The hydroxyl value (mgKOH / g) present in the oxyalkylene polymer was analyzed by the hydroxyl value measuring method in accordance with JIS K1557:2007.

[0169] <Method for measuring unsaturated group value>

[0170] The unsaturated group value (hereinafter referred to as USV) of the polymer is determined by the unsaturated group value determination method (Wijs method). That is, a polymer (about 2g) is placed in a conical flask, accurately weighed, and 40ml of chloroform is added to dissolve it. After accurately weighing 20ml of Wei's reagent using a quantitative pipette and adding it, the flask is placed in a cool place for 1 hour. A few drops of starch solution are added to an aqueous solution of potassium iodide prepared by dissolving potassium iodide (2g) in 100ml of water. After the resulting solution is added to the flask, N / 10 sodium thiosulfate is added dropwise while stirring, and the moment when the solution in the flask becomes colorless and transparent is taken as the end point. According to the end point, the unsaturated group value is obtained according to the following formula. It should be noted that the blank test titration uses chloroform without the addition of the polymer to implement the above operation.

[0171] Unsaturated group value (mmol / g) = ((blank test titration (ml) - sample solution titration (ml)) × titration of sodium thiosulfate solution) ÷ (20 × sample (g))

[0172] <Silylation rate>

[0173] The silylation rate of the polymer is based on 1 The calculation was performed by the internal standard method of H-NMR.

[0174] The number of terminal groups per molecule in the oxyalkylene polymers in Tables 1 and 2 is the number of hydroxyl groups in the initiator.

[0175] The number of reactive silicon groups per molecule is given by 1 H-NMR was determined by the internal standard method.

[0176] <Evaluation of tensile properties (H-type test)>

[0177] An H-type test body was prepared according to the test method for building sealing materials of JIS A1439:2016, and the tensile properties were evaluated.

[0178] The curable composition to be measured was filled into a template with a thickness of 2 mm, and aged for 7 days at a temperature of 23° C. and a humidity of 50%, and further aged for 7 days at a temperature of 50° C. and a humidity of 65%. The obtained cured product was subjected to a tensile test at a tensile speed of 500 mm / min using a Tensilon tester, and the modulus (M50, unit: N / mm2) as the stress at 50% elongation was measured. 2 ), as the modulus of stress at 100% elongation (M100, unit: N / mm 2 ), as the tensile strength of the maximum point aggregation force (Tmax, unit: N / mm 2 ), maximum elongation (Emax, unit: %).

[0179] The larger the value of M50 and M100, the harder the cured product is; the larger the value of the maximum point cohesion, the higher the tensile strength of the cured product is; the larger the value of the maximum point elongation, the better the elongation of the cured product is.

[0180] Examples 1 to 24 are embodiments, and Examples 25 to 38 are comparative examples.

[0181] (Example 1: Polymer A1)

[0182] Using polyoxypropylene glycol as an initiator and a zinc hexacyanocobaltate complex (hereinafter also referred to as "TBA-DMC catalyst") whose ligand is tert-butyl alcohol as a catalyst, propylene oxide is polymerized to obtain a hydroxyl-containing oxyalkylene polymer (precursor polymer P1) having two hydroxyl groups at the end. The hydroxyl value of the obtained precursor polymer P1 is 6.2 mgKOH / g.

[0183] Sodium methoxide was added in an amount of 1.05 molar equivalents relative to the hydroxyl groups of the precursor polymer P1, and methanol was distilled off under reduced pressure. Allyl chloride was added in an excess amount relative to the hydroxyl groups of the precursor polymer P1 and reacted, and unreacted allyl chloride was removed under reduced pressure. The metal salt was purified to remove the unsaturated group-containing oxyalkylene polymer (precursor polymer Q1) in which the hydroxyl groups were converted into allyloxy groups. The USV of the obtained precursor polymer Q1 was 0.12 mmol / g.

[0184] After adding crotonic acid as carboxylic acid compound B (carboxylic acid compound having carbon-carbon double bond, the same below) to precursor polymer Q1 in an amount of 1 mol per 1 mol of unsaturated group of precursor polymer Q1, hexachloroplatinic acid (IV) hexahydrate as platinum catalyst (6.5 mg per 1000 g of precursor polymer Q1) and phenylpropiolic acid as carboxylic acid compound A (carboxylic acid compound having carbon-carbon triple bond, the same below) (9.2 mg per 1000 g of precursor polymer Q1) (in molar ratio, platinum catalyst:carboxylic acid compound A=1:5) were mixed, and further added a solution prepared by dissolving triethylsilane as silane compound C in acetonitrile in a molar ratio of 1:1 with respect to carboxylic acid compound A. After adding 1.1 mol of dimethoxymethylsilane as silylating agent per 1 mol of unsaturated group of precursor polymer Q1, reacting at 70°C for 3 hours, unreacted silylating agent was removed under reduced pressure to obtain polymer A1 as reactive silicon group-containing oxyalkylene polymer. The number of terminal groups per molecule of the obtained polymer A1 was two, the number of reactive silicon groups introduced per molecule was 2.0, the silylation rate was 99.5%, and Mn was 23,000. The results are shown in Table 1 (hereinafter, the same is shown in Table 1 or 2).

[0185] (Example 2: Polymer A2)

[0186] In Example 1, the platinum catalyst was changed to platinum (0)-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (Karstedt catalyst) (6.1 mg per 1000 g of precursor polymer Q1). The same operation as in Example 1 was performed except that the polymer A2, which is an oxyalkylene polymer containing a reactive silicon group, was obtained.

[0187] (Example 3: Polymer A3)

[0188] In Example 1, the carboxylic acid compound A was changed to methyl phenylpropiolate. Other than that, the same operation as in Example 1 was performed (the amount of the platinum catalyst was not changed, and the amount of the carboxylic acid compound A was changed so that the molar ratio of the platinum catalyst: the carboxylic acid compound A = 1:5. The same was also true for the following Examples 4 to 10 and Examples 33 to 39, but in Examples 33 to 39, the molar ratio of the platinum catalyst: the replacement compound of the carboxylic acid compound A was set to be 1:5.), to obtain a polymer A3 which is an oxyalkylene polymer containing a reactive silicon group.

[0189] (Example 4: Polymer A4)

[0190] In Example 1, the carboxylic acid compound A was changed to propiolic acid. The same operation as in Example 1 was carried out except that the above was performed to obtain a polymer A4 which is an oxyalkylene polymer containing a reactive silicon group.

[0191] (Example 5: Polymer A5)

[0192] In Example 1, the carboxylic acid compound A was changed to 2-butynoic acid. The same operation as in Example 1 was carried out except that the above was performed to obtain a polymer A5 which is an oxyalkylene polymer containing a reactive silicon group.

[0193] (Example 6: Polymer A6)

[0194] In Example 1, the carboxylic acid compound A was changed to 2-heptynoic acid. The same operation as in Example 1 was carried out except that the above was performed to obtain a polymer A6 which is an oxyalkylene polymer containing a reactive silicon group.

[0195] (Example 7: Polymer A7)

[0196] In Example 1, the carboxylic acid compound A was changed to 2-methyl-3-butynoic acid. The same operation as in Example 1 was carried out except that the above was performed to obtain a polymer A7 which is an oxyalkylene polymer containing a reactive silicon group.

[0197] (Example 8: Polymer A8)

[0198] In Example 1, the carboxylic acid compound A was changed to 2-hydroxy-3-butynoic acid. The same operation as in Example 1 was carried out except that the above was performed to obtain a polymer A8 which is an oxyalkylene polymer containing a reactive silicon group.

[0199] (Example 9: Polymer A9)

[0200] In Example 1, the carboxylic acid compound A was changed to 3-butynoic acid. The same operation as in Example 1 was carried out except that the above was performed to obtain a polymer A9 which is an oxyalkylene polymer containing a reactive silicon group.

[0201] (Example 10: Polymer A10)

[0202] In Example 1, the carboxylic acid compound A was changed to acetylene dicarboxylic acid. The same operation as in Example 1 was carried out except that the carboxylic acid compound A was changed to acetylene dicarboxylic acid, thereby obtaining a polymer A10 which is an oxyalkylene polymer containing a reactive silicon group.

[0203] (Example 11: Polymer A11)

[0204] In Example 1, the silylating agent was changed to trimethoxysilane. The same operation as in Example 1 was carried out except that a polymer A11 which is an oxyalkylene polymer containing a reactive silicon group was obtained.

[0205] (Example 12: Polymer A12)

[0206] The same operation as in Example 1 was carried out instead of the precursor polymer P1 to obtain a hydroxyl-containing oxyalkylene polymer (precursor polymer P2) having a polymerization degree different from that of the precursor polymer P1 and having hydroxyl groups at both ends. The hydroxyl value of the obtained precursor polymer P2 was 7.5 mgKOH / g.

[0207] Sodium methoxide was added in an amount of 1.15 molar equivalents relative to the hydroxyl groups of the precursor polymer P2, and methanol was distilled off under reduced pressure. Next, allyl glycidyl ether was added in an amount of 1.05 molar equivalents relative to the hydroxyl groups of the precursor polymer P2, and the reaction was carried out at 130°C for 2 hours. Furthermore, sodium methoxide was added in an amount of 0.28 molar equivalents relative to the hydroxyl groups of the precursor polymer P2, and methanol was removed. Then, allyl chloride was added in an amount of 2.10 molar equivalents relative to the hydroxyl groups of the precursor polymer P2, and the reaction was carried out at 130°C for 2 hours, and unreacted allyl chloride was removed under reduced pressure. Purification was performed to remove the metal salt, and an oxyalkylene polymer containing unsaturated groups having 2.0 allyl groups per terminal group (precursor polymer Q2) was obtained. The USV of the obtained precursor polymer Q2 was 0.29 mmol / g.

[0208] 1 mol of crotonic acid as carboxylic acid compound B was added and dissolved relative to 1 mol of unsaturated groups of precursor polymer Q2. Next, hexachloroplatinic acid (IV) hexahydrate as a platinum catalyst (6.5 mg relative to 1000 g of precursor polymer Q2) and phenylpropiolic acid as carboxylic acid compound A (9.2 mg relative to 1000 g of precursor polymer Q2) were mixed (in terms of molar ratio, platinum catalyst: carboxylic acid compound A = 1:5), and a solution prepared by dissolving triethylsilane as a silane compound C in acetonitrile at a molar ratio of 1:1 relative to carboxylic acid compound A was further added. In addition, 1.1 mol of dimethoxymethylsilane was added relative to 1 mol of unsaturated groups of precursor polymer Q2, and after reacting at 70°C for 5 hours, unreacted dimethoxymethylsilane was removed under reduced pressure to obtain polymer A12 as an oxyalkylene polymer containing reactive silicon groups.

[0209] (Example 13: Polymer A13)

[0210] 1.05 molar equivalents of sodium methoxide were added to the hydroxyl groups of the precursor polymer P2, and methanol was distilled off under reduced pressure. Then, an excess of propargyl bromide was reacted with the hydroxyl groups of the precursor polymer P2 to obtain an oxyalkylene polymer (precursor polymer Q3) having 1.0 propargyl group per terminal group. The USV of the obtained precursor polymer Q3 was 0.29 mmol / g.

[0211] Crotonic acid as a carboxylic acid compound B was added to the precursor polymer Q3 in an amount of 2 mol relative to 1 mol of the unsaturated group (carbon-carbon triple bond) of the precursor polymer Q3 and dissolved. Next, hexachloroplatinic acid (IV) hexahydrate as a platinum catalyst (6.5 mg relative to 1000 g of the precursor polymer Q3) and phenylpropiolic acid as a carboxylic acid compound A (9.2 mg relative to 1000 g of the precursor polymer Q3) were mixed (in terms of molar ratio, platinum catalyst: carboxylic acid compound A = 1:5), and a solution prepared by dissolving triethylsilane as a silane compound C in acetonitrile at a molar ratio of 1:1 relative to the carboxylic acid compound A was further added. Furthermore, 4.0 mol of dimethoxymethylsilane was added relative to 1 mol of propargyl groups of the precursor polymer Q3, and after reacting at 70°C for 3 hours, the unreacted dimethoxymethylsilane was removed under reduced pressure to obtain a polymer A13 as an oxyalkylene polymer containing a reactive silicon group.

[0212] (Example 14: Polymer A14)

[0213] 8.39 g of cuprous bromide and 112 mL of acetonitrile were added to a 2L flask, and heated and stirred at 70°C for 20 minutes under a nitrogen stream. 17.6 g of diethyl 2,5-dibromoadipate, 130 mL of ethyl acrylate, 720 mL of butyl acrylate, and 251 g of stearyl acrylate were added thereto, and further heated and stirred at 70°C for 40 minutes. 0.41 mL of pentamethyldiethylenetriamine (hereinafter also referred to as "triamine") was added thereto to start the reaction. Then, heating and stirring were continued at 70°C, and 2.05 mL of triamine was further added. 244 mL of 1,7-octadiene and 4.1 mL of triamine were added 330 minutes after the start of the reaction, and heating and stirring were continued at 70°C, and heating was stopped 570 minutes after the start of the reaction. The obtained reaction solution was diluted with toluene and filtered, and the filtrate was subjected to reduced pressure heating treatment to obtain an unpurified acrylate polymer having an alkenyl group as an end group. The number of alkenyl groups in each molecule of the unpurified acrylate polymer is 2.0. Furthermore, under a nitrogen atmosphere, the entire amount of the unpurified acrylate polymer, 17.2 g of potassium acetate, and 700 mL of N, N-dimethylacetamidomethyl (hereinafter referred to as "DMAc") were added to a 2L flask, and heated and stirred at 100°C for 10 hours. The reaction solution was heated under reduced pressure to remove DMAc, and toluene was added for filtration. The residue obtained by heating the filtrate under reduced pressure to remove the volatile components was added to a 2L flask, 100 g of an adsorbent (a mixture of Kyoward 500SN and Kyoward 700SN (both product names of Kyowa Chemical Industry Co., Ltd.) in a mass ratio of 1 to 1) was added, and heated and stirred at 130°C under a nitrogen stream for 9 hours. Dilute with toluene, filter to remove the adsorbent, and remove the toluene in the filtrate under reduced pressure to obtain an acrylate polymer containing an unsaturated group (precursor polymer Q4).

[0214] Crotonic acid as a carboxylic acid compound B was added to the precursor polymer Q4 and dissolved in such a manner that the amount was 1 mol relative to 1 mol of the unsaturated group of the precursor polymer Q4. Next, hexachloroplatinic acid (IV) hexahydrate as a platinum catalyst (0.00065 mass % relative to the precursor polymer Q4) and phenylpropiolic acid as a carboxylic acid compound A (0.00092 mass % relative to the precursor polymer Q4) were mixed at a molar ratio of 1:5, and a solution prepared by dissolving triethylsilane as a silane compound C in acetonitrile at a molar ratio of 1:1 relative to the carboxylic acid compound A was further added. Furthermore, 1.1 mol of trimethoxysilane was added relative to 1 mol of the unsaturated group of the precursor polymer Q4, and after reacting at 70°C for 3 hours, the unreacted trimethoxysilane was removed under reduced pressure to obtain a polymer A14 as a (meth)acrylate polymer containing a reactive silicon group.

[0215] (Example 15: Polymer A15)

[0216] In Example 1, the initiator was changed to n-butanol, and the same operation as in Example 1 was performed to obtain a hydroxyl-containing oxyalkylene polymer (precursor polymer P3) having a hydroxyl terminal group, an oxyalkylene polymer containing an unsaturated group (precursor polymer Q5), and a polymer A15 as an oxyalkylene polymer containing a reactive silicon group. The hydroxyl value of the obtained precursor polymer P3 was 11.2 mgKOH / g, and the USV of the precursor polymer Q5 was 0.22 mmol / g.

[0217] (Example 16: Polymer A16)

[0218] In Example 1, the initiator was changed to glycerol, and the same operation as in Example 1 was performed to obtain a hydroxyl-containing oxyalkylene polymer (precursor polymer P4) having three terminal groups as hydroxyl groups, an oxyalkylene polymer containing unsaturated groups (precursor polymer Q6), and a polymer A16 as an oxyalkylene polymer containing reactive silicon groups. The hydroxyl value of the obtained precursor polymer P4 was 7.0 mgKOH / g, and the USV of the precursor polymer Q6 was 0.14 mmol / g.

[0219] (Example 17: Polymer A17)

[0220] In Example 1, the initiator was changed to sorbitol, and the same operation as in Example 1 was performed to obtain a hydroxyl-containing oxyalkylene polymer (precursor polymer P5) having 6 terminal groups as hydroxyl groups, an oxyalkylene polymer containing unsaturated groups (precursor polymer Q7), and a polymer A17 as an oxyalkylene polymer containing reactive silicon groups. The hydroxyl value of the obtained precursor polymer P5 was 8.0 mgKOH / g, and the USV of the precursor polymer Q7 was 0.16 mmol / g.

[0221] (Example 18: Polymer A18)

[0222] In Example 1, the molar ratio of the platinum catalyst to the carboxylic acid compound A was changed to 1:0.04. Except for this, the same operation as in Example 1 was performed to obtain a polymer A18 as an oxyalkylene polymer containing a reactive silicon group. It should be noted that the amounts of the platinum catalyst and the carboxylic acid compound B were the same as in Example 1, and the amounts of the carboxylic acid compound A and the silane compound C were changed. The same applies to the following Examples 20 to 22.

[0223] (Example 19: Polymer A19)

[0224] In Example 1, the molar ratio of the platinum catalyst to the carboxylic acid compound A was changed to 1:0.05. The same operation as in Example 1 was carried out except that the above was performed to obtain a polymer A19 which is an oxyalkylene polymer containing a reactive silicon group.

[0225] (Example 20: Polymer A20)

[0226] In Example 1, the molar ratio of the platinum catalyst to the carboxylic acid compound A was changed to 1:20. The same operation as in Example 1 was carried out except that the above was performed to obtain a polymer A20 which is an oxyalkylene polymer containing a reactive silicon group.

[0227] (Example 21: Polymer A21)

[0228] In Example 1, the molar ratio of the platinum catalyst to the carboxylic acid compound A was changed to 1:21. The same operation as in Example 1 was carried out except that the above was performed to obtain a polymer A21 which is an oxyalkylene polymer containing a reactive silicon group.

[0229] (Example 22: Polymer A22)

[0230] In Example 1, silane compound C was not used (an acetonitrile solution in which silane compound C was not dissolved was added. The same procedure was applied to Examples 25 to 39 in which silane compound C was not used). Except for this, the same operation as in Example 1 was performed to obtain polymer A23, which is an oxyalkylene polymer containing a reactive silicon group.

[0231] (Example 23: Polymer A23)

[0232] In Example 1, no carboxylic acid compound B was used. Except for this, the same operation as in Example 1 was carried out to obtain a polymer A23 which is an oxyalkylene polymer containing a reactive silicon group.

[0233] (Example 24: Polymer A24)

[0234] In Example 1, the carboxylic acid compound B and the silane compound C were not used. Except for this, the same operation as in Example 1 was carried out to obtain a polymer A24 which is an oxyalkylene polymer containing a reactive silicon group.

[0235] (Example 25: Polymer A25)

[0236] In Example 1, no carboxylic acid compound A, carboxylic acid compound B and silane compound C were used. Except for this, the same operation as in Example 1 was carried out to obtain polymer A25 which is an oxyalkylene polymer containing a reactive silicon group.

[0237] (Example 26: Polymer A26)

[0238] In Example 12, no carboxylic acid compound A, carboxylic acid compound B and silane compound C were used. Except for this, the same operation as in Example 12 was carried out to obtain polymer A26 which is an oxyalkylene polymer containing a reactive silicon group.

[0239] (Example 27: Polymer A27)

[0240] In Example 13, no carboxylic acid compound A, carboxylic acid compound B and silane compound C were used. Except for this, the same operation as in Example 13 was carried out to obtain polymer A27 which is an oxyalkylene polymer containing a reactive silicon group.

[0241] (Example 28: Polymer A28)

[0242] In Example 14, no carboxylic acid compound A, carboxylic acid compound B, and silane compound C were used. Except for this, the same operation as in Example 14 was carried out to obtain polymer A28 which is a reactive silicon group-containing (meth)acrylate polymer.

[0243] (Example 29: Polymer A29)

[0244] In Example 15, no carboxylic acid compound A, carboxylic acid compound B and silane compound C were used. Except for this, the same operation as in Example 15 was carried out to obtain polymer A29 which is an oxyalkylene polymer containing a reactive silicon group.

[0245] (Example 30: Polymer A30)

[0246] In Example 16, no carboxylic acid compound A, carboxylic acid compound B, and silane compound C were used. Except for this, the same operation as in Example 16 was carried out to obtain a polymer A30 which is an oxyalkylene polymer containing a reactive silicon group.

[0247] (Example 31: Polymer A31)

[0248] In Example 17, no carboxylic acid compound A, carboxylic acid compound B and silane compound C were used. Except for this, the same operation as in Example 17 was carried out to obtain a polymer A31 which is an oxyalkylene polymer containing a reactive silicon group.

[0249] (Example 32: Polymer A32)

[0250] In Example 24, the carboxylic acid compound A was changed to butyric acid. The same operation as in Example 24 was carried out except that the above was performed to obtain a polymer A32 which is an oxyalkylene polymer containing a reactive silicon group.

[0251] (Example 33: Polymer A33)

[0252] In Example 24, the carboxylic acid compound A was changed to formic acid. The same operation as in Example 24 was carried out except that the above was performed to obtain a polymer A33 which is an oxyalkylene polymer containing a reactive silicon group.

[0253] (Example 34: Polymer A34)

[0254] In Example 24, the carboxylic acid compound A was changed to acetic acid. The same operation as in Example 24 was carried out except that the above was performed to obtain a polymer A34 which is an oxyalkylene polymer containing a reactive silicon group.

[0255] (Example 35: Polymer A35)

[0256] In Example 24, the carboxylic acid compound A was changed to benzoic acid. The same operation as in Example 24 was carried out except that the above was performed to obtain a polymer A35 which is an oxyalkylene polymer containing a reactive silicon group.

[0257] (Example 36: Polymer A36)

[0258] In Example 24, the carboxylic acid compound A was changed to 3,6-dimethyl-4-octyne-3,6-diol. The same operation as in Example 24 was carried out except that a polymer A36 as a reactive silicon group-containing oxyalkylene polymer was obtained.

[0259] (Example 37: Polymer A37)

[0260] In Example 24, the carboxylic acid compound A was changed to 2-methyl-3-butyn-2-ol. The same operation as in Example 24 was carried out except that the above was performed to obtain a polymer A37 which is an oxyalkylene polymer containing a reactive silicon group.

[0261] (Example 38: Polymer A38)

[0262] In Example 24, the carboxylic acid compound A was changed to 3,5-dimethyl-3-hexene-1-yne. The same operation as in Example 24 was carried out except that the above was performed to obtain a polymer A38 which is an oxyalkylene polymer containing a reactive silicon group.

[0263] [Table 1]

[0264]

[0265] [Table 2]

[0266]

[0267] As shown in Examples 1 to 31, in the examples (Examples 1 to 24) where hydrosilylation was carried out in the presence of a Group 8 metal catalyst and a carboxylic acid compound A, the silylation rate was improved and the hydrosilylation reaction was promoted compared to the examples (Examples 25 to 31) where hydrosilylation was carried out in the presence of only a Group 8 metal catalyst. In addition, in the presence of a compound that does not belong to the carboxylic acid compound A (Examples 32 to 38), the silylation rate was not sufficiently improved. As can be seen from Examples 1 to 23, in the presence of a Group 8 metal catalyst and a carboxylic acid compound A, by further adding a carboxylic acid compound B or a silane compound C, the silylation rate was further improved, and the hydrosilylation reaction was further promoted.

[0268] <Other ingredients>

[0269] The additives described in Table 3 and Table 4 are as follows.

[0270] Bai Yanhua CCR: Colloidal calcium carbonate, product name of Baishi Industrial Company.

[0271] Whiton SB: Heavy calcium carbonate, product name of Whitehead Industries, Inc.

[0272] R820: Titanium oxide, product name of Ishihara Sangyo Co., Ltd.

[0273] DINP: SansocizerDINP, diisononyl phthalate, product name of Shin Nippon Chemical Co., Ltd.

[0274] DIDP: Diisodecyl phthalate, manufactured by Mitsubishi Chemical Corporation.

[0275] PMLS4012: Preminol S4012, a high molecular weight polyol having two hydroxyl groups per molecule and an Mn of 13,000, a product name of AGC Corporation.

[0276] SansocizerEPS: 4,5-epoxycyclohexane-1,2-dicarboxylic acid-di-2-ethylhexyl ester, product name of Shin Nippon Chemical Co., Ltd.

[0277] DISPARLON 6500: Hydrogenated castor oil-based thixotropic agent, product name of Kusumoto Chemicals Co., Ltd.

[0278] DISPARLON 305: Hydrogenated castor oil-based thixotropic agent, product name of Kusumoto Chemicals Co., Ltd.

[0279] Balloon80GCA: Organic ball, product name of Matsumoto Oil & Fats Co., Ltd.

[0280] M309: Aronix M-309: Photocurable resin, product name of Toa Synthetics Co., Ltd.

[0281] Glyceryl monostearate: Reagent, manufactured by Tokyo Chemical Industry Co., Ltd.

[0282] KBM-1003: Vinyltrimethoxysilane, product name of Shin-Etsu Chemical Co., Ltd.

[0283] A-171: Vinyltrimethoxysilane, product name of Momentive.

[0284] KBM-403: 3-Glycidyloxypropyltrimethoxysilane, product name of Shin-Etsu Chemical Co., Ltd.

[0285] KBM-603: 3-(2-aminoethylamino)propyltrimethoxysilane, product name of Shin-Etsu Chemical Co., Ltd.

[0286] A-1120: 3-(N-2-aminoethylamino)propyltrimethoxysilane, product name of Momentive.

[0287] TINUVIN765: Hindered amine light stabilizer containing tertiary amine, product name of BASF.

[0288] TINUVIN770: Hindered amine light stabilizer containing tertiary amine, product name of BASF.

[0289] Sanol LS770: Hindered amine light stabilizer, product name of Sankyo Lifetech.

[0290] IRGANOX1010: Hindered phenol antioxidant, product name of BASF.

[0291] TINUVIN326: Benzotriazole UV absorber, product name of BASF.

[0292] TINUVIN327: Benzotriazole UV absorber, product name of BASF.

[0293] Tung oil: Air oxidation curing compound, manufactured by Kimura Co.

[0294] DBTDL: dibutyltin dilaurate.

[0295] U-220H: Di-n-butylbis(acetylacetonato)tin, product name of Nitto Chemical Co., Ltd.

[0296] Stanoct: Stannous octoate, product name of Gifu Pharmaceuticals.

[0297] Laurylamine: Reagent, manufactured by Pure Chemical Company.

[0298] Glomax LL: Calcined kaolin, product name of Takehara Chemical Industry Co., Ltd.

[0299] 《Preparation of curable composition》

[0300] The curable composition was prepared by adding the polymers in the blending amounts (parts by mass) shown in Tables 5 to 7 and the additives in the blending amounts (parts by mass) shown in Tables 3 and 4. The blending amounts of the components shown in Tables 3 and 4 are values ​​(unit: parts by mass) relative to a total of 100 parts by mass of the polymer. It should be noted that in the additive D4, the blending amounts of the main agent shown in Table 3 and the curing agent shown in Table 4 were used.

[0301] The obtained curable composition was used to evaluate tensile properties (H-type test). The results are shown in Tables 5 to 7. In Tables 5 and 6, the value shown as (M100) indicates the value of M100.

[0302] [Table 3]

[0303]

[0304] [Table 4]

[0305]

[0306] [Table 5]

[0307]

[0308] [Table 6]

[0309]

[0310] [Table 7]

[0311]

[0312] <Evaluation Results>

[0313] As shown in Reference Examples 1 to 12, Reference Examples 15 to 26, and Reference Examples 29 to 38, good M50 was shown in the curable composition containing a polymer with a high silylation rate. As shown in Reference Examples 13, 14, 27, and 28, by comparing Reference Examples 13 and 27 and 14 and 28 with the same compounding, it can be seen that when M50 is adjusted to the same value, the curable composition of Reference Example 13 or 14 containing a polymer with a high silylation rate showed good Tmax and elongation compared with Reference Example 27 or 28.

Claims

1. A method for producing an organic polymer containing a reactive silicon group, wherein the organic polymer containing a reactive silicon group has a reactive silicon group represented by the following formula (1), wherein the organic polymer containing an unsaturated group is reacted with a silylating agent in the presence of a co-catalyst comprising a Group 8 metal catalyst and a carboxylic acid compound having a carbon-carbon triple bond, -SiR a X 3-a Formula (1), In formula (1), R represents a monovalent organic group having 1 to 20 carbon atoms and is an organic group other than a hydrolyzable group, X represents a hydroxyl group, a halogen atom or a hydrolyzable group, a is an integer from 0 to 2, when a is 2, R are optionally the same or different from each other, and when a is 0 or 1, X are optionally the same or different from each other.

2. The method for producing an organic polymer containing a reactive silicon group according to claim 1, wherein: The Group 8 metal catalyst has at least one metal selected from the group consisting of cobalt, nickel, ruthenium, rhodium, palladium, iridium and platinum.

3. The method for producing an organic polymer containing a reactive silicon group according to claim 1, wherein: The carboxylic acid compound having a carbon-carbon triple bond has 3 or more and 17 or less carbon atoms.

4. The method for producing an organic polymer containing a reactive silicon group according to claim 1, wherein: The carboxylic acid compound having a carbon-carbon triple bond is a carboxylic acid compound having a carbon-carbon triple bond at the α-position carbon.

5. The method for producing an organic polymer containing a reactive silicon group according to claim 1, wherein: The molar ratio of the carboxylic acid compound having a carbon-carbon triple bond to the Group 8 metal catalyst is 0.01 to 25.

6. The method for producing an organic polymer containing a reactive silicon group according to claim 1, wherein: The co-catalyst further comprises a carboxylic acid compound having a carbon-carbon double bond.

7. The method for producing an organic polymer containing a reactive silicon group according to claim 6, wherein: The carboxylic acid compound having a carbon-carbon double bond is a carboxylic acid compound having a carbon-carbon double bond at the α-position carbon.

8. The method for producing an organic polymer containing a reactive silicon group according to claim 6, wherein: The usage-amount of the carboxylic acid compound having a carbon-carbon double bond is 0.1 to 10 mol with respect to 1 mol of the unsaturated group of the unsaturated group-containing organic polymer.

9. The method for producing an organic polymer containing a reactive silicon group according to claim 1, wherein: The co-catalyst further comprises a silane compound represented by the following formula (2): HkDJ 1 3 Formula (2), In formula (2), R 1 represents a monovalent organic group having 1 to 20 carbon atoms, and is an organic group other than a hydrolyzable group, R 1 They are optionally the same as or different from each other.

10. The method for producing an organic polymer containing a reactive silicon group according to claim 9, wherein: The molar ratio of the silane compound to the carboxylic acid compound having a carbon-carbon triple bond is 0.05 to 20.

11. The method for producing a reactive silicon group-containing organic polymer according to any one of claims 1 to 10, wherein: The reactive silicon group-containing organic polymer is a polymer having units based on an oxyalkylene monomer.

12. The method for producing a reactive silicon group-containing organic polymer according to any one of claims 1 to 10, wherein: The reactive silicon group-containing organic polymer is a polymer having a unit based on an alkyl acrylate monomer or an alkyl methacrylate monomer.