Additive compositions and methods of use thereof
By using additive compositions of polyol and zeolite composites in polyurethane polymers and foams, the problem of release of volatile organic compounds in polyurethane foams is solved, significantly reducing the emission of aldehyde and amine compounds, and improving the odor and health of the product Security.
Patent Information
- Application Number
- CN202380034873.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-18
- Filing Date
- 2023-04-17
- Publication Date
- 2024-12-03
AI Technical Summary
The volatile organic compounds (such as aldehydes) released by polyurethane polymers and foams during manufacturing lead to undesirable odors and potential health risks, and prior art is difficult to effectively reduce their detectable levels.
Using additive compositions containing polyols and zeolite composites, the zeolite composite consisting of a zeolite substrate with a microporous structure and nitrogen-containing compounds adsorbed on its surface, used to prepare polyurethane polymers and foams to adsorb and reduce volatility. Release of organic compounds.
The release of volatile organic compounds in polyurethane foams, especially aldehyde and amine compounds, improves the odor and health and safety performance of the product.
Smart Images

Figure BDA0005090857810000131 
Figure BDA0005090857810000151
Abstract
Description
Technical Field
[0001] The present application relates to additive compositions for reducing volatile organic emissions (eg, aldehyde emissions) from polymeric materials such as polyurethane polymers and foams. The present application also relates to methods of making polyurethane polymers and foams using such additive compositions. Background Art
[0002] Polyurethane polymers are used in a variety of applications, such as the production of polyurethane foams. These polyurethane foams are in turn used for many different end uses. For example, polyurethane foams are often used as cushioning and padding in, for example, transportation seats (e.g., car seats) and furniture, such as mattresses and other furniture with seat cushions. When these polyurethane foams are used in closed environments such as the interior of an automobile or other vehicle, the foams must generally pass a test that limits the amount of volatile organic compounds that the foam can release. The volatile organic compounds released by the polyurethane foam during the test can be produced as a by-product of the reaction that produces the polyurethane polymer. Volatile organic compounds (e.g., aldehydes, such as formaldehyde, acetaldehyde, and propionaldehyde) may also be present in the raw materials (e.g., polyols) used to make the foam. These volatile organic compounds can bring undesirable odors to the raw materials and the polyurethane polymers / foams made from those raw materials. Therefore, it is desirable to find a composition or method that reduces the detectable level of volatile organic compounds present in the polyurethane polymer / foam. The present application attempts to provide such a composition and method. Summary of the invention
[0003] In a first embodiment, the present invention provides an additive composition comprising a polyol and a zeolite composite material. Preferably, the additive composition comprises:
[0004] (a) polyols;
[0005] (b) a zeolite composite material dispersed in the polyol, the zeolite composite material comprising:
[0006] (i) a zeolite substrate having a surface and a plurality of pores in the surface; and
[0007] (ii) a nitrogen-containing compound adsorbed in at least a portion of the pores in the surface of the zeolite substrate, the nitrogen-containing compound comprising: (A) a first functional group comprising a carbon atom double-bonded to a nitrogen atom, and (B) a second functional group comprising a hydrogen atom covalently bonded to the nitrogen atom.
[0008] In a second embodiment, the present invention provides a method for preparing a polyurethane polymer (e.g., polyurethane foam) using the additive composition of the first embodiment. Preferably, the method comprises the following steps:
[0009] (a) providing a first polyol;
[0010] (b) providing an isocyanate compound comprising two or more isocyanate groups;
[0011] (c) providing an additive composition comprising:
[0012] (i) a second polyol; and
[0013] (ii) a zeolite composite material dispersed in the second polyol, the zeolite composite material comprising:
[0014] (A) a zeolite substrate having a surface and a plurality of pores in the surface; and
[0015] (B) a nitrogen-containing compound adsorbed in at least a portion of the pores in the surface of the zeolite substrate, the nitrogen-containing compound comprising: (1) a first functional group comprising a carbon atom doubly bonded to a nitrogen atom, and (2) a second functional group comprising a hydrogen atom covalently bonded to the nitrogen atom;
[0016] (d) mixing the first polyol, the isocyanate compound, and the additive composition to produce a reaction mixture; and
[0017] (e) reacting the isocyanate compound with first and second polyols to produce a polyurethane polymer, wherein the zeolite composite is dispersed in the polyurethane polymer. DETAILED DESCRIPTION
[0018] In a first embodiment, the present invention provides an additive composition comprising a polyol and a zeolite composite material dispersed in the polyol. The zeolite composite material comprises a zeolite substrate and a nitrogen-containing compound adsorbed within at least a portion of the pores in the surface of the zeolite substrate.
[0019] The additive composition may include any suitable polyol. Suitable polyols include polyether polyols and polyester polyols. Suitable polyether polyols include those prepared by reacting epoxides such as ethylene oxide, propylene oxide, butylene oxide and glycidol with polyfunctional initiator compounds such as polyfunctional alcohols or amines. Examples of suitable polyfunctional initiator compounds include, but are not limited to, water, glycerol, pentaerythritol, ethylene glycol, propylene glycol (e.g., 1,2-propylene glycol), trimethylolpropane and ethylenediamine. Suitable polyester polyols include those prepared by reacting polycarboxylic acids or anhydrides with polyfunctional alcohols such as glycerol, pentaerythritol, ethylene glycol, diethylene glycol, propylene glycol (e.g., 1,2-propylene glycol) and trimethylolpropane. Examples of suitable polycarboxylic acids and anhydrides include, but are not limited to, adipic acid, maleic acid, maleic anhydride, succinic acid, succinic anhydride, azelaic acid, glutaric acid, phthalic acid and phthalic anhydride. Preferably, the polyol is a polyether polyol.
[0020] The polyol may have any suitable molar mass. In a preferred embodiment, the polyol has a molar mass of about 400 g / mol or more. More preferably, the polyol has a molar mass of about 500 g / mol or more, about 750 g / mol or more, or about 1,000 g / mol or more. Preferably, the polyol has a molar mass of about 20,000 g / mol or less, more preferably about 15,000 g / mol or less, or about 10,000 g / mol or less. Thus, in a series of preferred embodiments, the polyol has a molar mass of about 400 g / mol to about 20,000 g / mol (e.g., about 400 g / mol to about 15,000 g / mol or about 400 g / mol to about 10,000 g / mol), about 500 g / mol to about 20,000 g / mol (e.g., about 500 g / mol to about 15,000 g / mol or about 500 g / mol to about 10,000 g / mol), about 750 g / mol to about 20,000 g / mol (e.g., about 750 g / mol to about 15,000 g / mol or about 750 g / mol to about 10,000 g / mol), or about 1,000 to about 20,000 g / mol (e.g., about 1,000 g / mol to about 15,000 g / mol or about 1,000 g / mol to about 10,000 g / mol).
[0021] As described above, the additive composition comprises a zeolite composite material comprising a zeolite substrate and a nitrogen-containing compound. The zeolite substrate may include any suitable zeolite. Zeolites may contain various cations such as H + 、Na + , Ca 2+ Mg 2+ and other cations. Zeolites are members of a family of microporous solids known as "molecular sieves", which are a group of materials that can selectively sort molecules based primarily on size exclusion methods. This sorting ability is due to the very regular pore structure of molecular size in the zeolite. The maximum size of a molecule or ionic species that can enter the pores of the zeolite is determined by the size of the zeolite channels, which is defined by the size of the rings of tetrahedrally coordinated silicon / aluminum and oxygen atoms from which the zeolite is prepared. The zeolite substrate may include any naturally occurring or synthetic zeolite, with synthetic zeolites being preferred because they are not contaminated by other minerals, etc. In a preferred embodiment, the zeolite is H + Cationic zeolites (i.e., aluminosilicate minerals in which at least a portion of the counter cations are H + cationic zeolite).
[0022] As mentioned above, zeolite has microporous structure, and the hole constituting this microporous structure can be any suitable size.Preferably, the pore diameter of zeolite is about 0.1nm or larger, more preferably about 0.2nm or larger or 0.3nm or larger.The pore diameter of zeolite is generally no more than about 1nm and is preferably about 0.9nm or less.Therefore, in a series of preferred embodiments, the pore diameter of zeolite is about 0.1nm to about 1nm (for example, about 0.1nm to about 0.9nm), about 0.2nm to about 1nm (for example, about 0.2nm to about 0.9nm) or about 0.3nm to about 1nm (for example, about 0.3nm to about 0.9nm).
[0023] The microporous structure of a zeolite may also (or alternatively) be characterized using the BET specific surface area. Zeolites suitable for use in making zeolite composites preferably have a microporous structure of about 100 m 2 / g or more, about 150m 2 / g or more, or about 200m 2 / g or more. The zeolite preferably has a BET specific surface area of about 1,000 m 2 / g or less, about 900m 2 / g or less, or about 800m 2 / g or less. Therefore, in a series of preferred embodiments, the zeolite used in preparing the zeolite composite material has a BET specific surface area of about 100 m 2 / g to about 1,000m 2 / g (e.g., about 100 m 2 / g to about 900m 2 / g or about 100m 2 / g to about 800m 2 / g), about 150m 2 / g to about 1,000m 2 / g (e.g., about 150 m 2 / g to about 900m 2 / g or about 150m 2 / g to about 800m 2 / g), or about 200m 2 / g to about (e.g., about 200 m 2 / g to about 900m 2 / g or about 200m 2 / g to about 800m 2 / g) of BET specific area.
[0024] The zeolite used in preparing the zeolite composite material can have any suitable particle size. Suitable zeolites preferably have a particle size of about 2 μm or greater. Suitable zeolites preferably have a particle size of about 10 μm or greater. Therefore, the zeolite preferably has a particle size of about 2 μm to about 10 μm.
[0025] The zeolite composite material comprises a nitrogen-containing compound. The nitrogen-containing compound is preferably adsorbed in at least a portion of the pores in the surface of the zeolite substrate. The nitrogen-containing compound can be any suitable organic compound comprising a nitrogen atom. Preferably, the nitrogen-containing compound comprises a first functional group, and the first functional group comprises a carbon atom double-bonded to the nitrogen atom (i.e., an imine group). More preferably, the nitrogen-containing compound comprises a first functional group (i.e., an imine group) comprising a carbon atom double-bonded to the nitrogen atom and (B) a second functional group (e.g., a primary amine group or a secondary amine group) comprising a hydrogen atom covalently bonded to the nitrogen atom. In a preferred embodiment, the nitrogen-containing compound comprises at least two second functional groups, and the second functional group comprises a hydrogen atom covalently bonded to the nitrogen atom (i.e., the nitrogen-containing compound comprises two or more primary amine groups or secondary amine groups). Preferred nitrogen-containing compounds include any compound with the above-mentioned properties. Suitable examples of such preferred nitrogen-containing compounds include, but are not limited to, guanidine compounds, aminoguanidine compounds, biguanidine compounds, guanamine compounds, and mixtures thereof. Suitable guanidine compounds include, but are not limited to, guanidine itself and its salts, such as guanidine hydrochloride, guanidine carbonate, guanidine nitrate, guanidine sulfate, and the above-mentioned mixture. Suitable aminoguanidine compounds include, but are not limited to, aminoguanidine itself and its salts, such as aminoguanidine sulfate, aminoguanidine hydrochloride, aminoguanidine nitrate, diaminoguanidine hydrochloride, diaminoguanidine sulfate, triaminoguanidine hydrochloride, and the above-mentioned mixture. Suitable biguanide compounds include, but are not limited to, biguanide and its salts, metformin and its salts (such as metformin hydrochloride), buformin and its salts (such as buformin hydrochloride), phenformin and its salts (such as phenformin hydrochloride), and the above-mentioned mixture. Suitable guanamine compounds include, but are not limited to, benzoguanamine and its salts, acetoguanamine and its salts, adipoguanamine (i.e., 6,6'-(1,4-butanediyl)bis-1,3,5-triazine-2,4-diamine) and its salts, 2-methylpentanediguanamine (i.e., 6,6'-(2-methyl-1,3-propanediyl)bis-1,3,5-triazine-2,4-diamine) and its salts, isohexanediguanamine and its salts, 6,6'-(1-ethyl-1,2-ethanediyl)bis-1,3,5-triazine-2,4-diamine and its salts, 6,6'-(1-methyl-1,3-propanediyl)bis-1,3,5-triazine-2,4-diamine and its salts, and mixtures thereof. In a preferred embodiment, the nitrogen-containing compound is selected from aminoguanidine compounds, biguanide compounds, guanamine compounds, and mixtures thereof. Preferably, the nitrogen-containing compound is soluble in water, meaning that it exhibits a solubility in water of 500 g / L or greater. In another preferred embodiment, the nitrogen-containing compound is an aminoguanidine compound, more preferably a water-soluble aminoguanidine compound selected from aminoguanidine sulfate, aminoguanidine hydrochloride, aminoguanidine nitrate, diaminoguanidine hydrochloride, diaminoguanidine sulfate, triaminoguanidine hydrochloride, and mixtures thereof.
[0026] Zeolite composite material can contain nitrogenous compound of any suitable amount.Preferably, based on the gross weight of zeolite substrate and nitrogenous compound, nitrogenous compound is present in zeolite composite material with the amount of about 5 weight % or more.More preferably, based on the gross weight of zeolite substrate and nitrogenous compound, nitrogenous compound is present in zeolite composite material with the amount of about 10 weight % or more, about 15 weight % or more or about 20 weight % or more.There seems to be no upper limit for the amount of nitrogenous compound that can be present in zeolite composite material.More specifically, the maximum amount of nitrogenous compound seems to depend on the structure of zeolite substrate and the ability of nitrogenous compound adsorption thereof.Having said that, it is believed that when the mass of nitrogenous compound added is equal to or exceeds the mass of zeolite substrate, increasing the amount of nitrogenous compound provides the return of reduction.Therefore, in a preferred embodiment, based on the gross weight of zeolite substrate and nitrogenous compound, nitrogenous compound is present in zeolite composite material with the amount of about 50 weight % or less. In a series of preferred embodiments, the nitrogen-containing compound is present in the zeolite composite in an amount of about 5 wt % to 50 wt %, about 10 wt % to about 50 wt %, about 15 wt % to about 50 wt %, or about 20 wt % to about 50 wt %, based on the total weight of the zeolite substrate and the nitrogen-containing compound.
[0027] Zeolite composite material can be prepared by any suitable method. Preferably, zeolite composite material is prepared by dissolving the nitrogen-containing compound of the desired amount in a suitable solvent (e.g., water). Then the zeolite substrate is added to the solution of the obtained nitrogen-containing compound, and the obtained slurry is mixed / stirred. When the slurry is stirred, the zeolite substrate is thoroughly wetted with the solution, which causes the nitrogen-containing compound to be adsorbed in at least a portion of the pores of the zeolite substrate. Then the wetted zeolite substrate is dried to remove the residual solvent and obtain the above-mentioned zeolite composite material. Any suitable method can be used to dry the wetted zeolite substrate, for example, the wetted zeolite substrate is heated to an elevated temperature (e.g., when the solvent is water, the temperature is heated to about 120° C. for about 8 hours). Preferably, the wetted zeolite is dried so that the residual solvent content (e.g., the moisture content when water is used as a solvent) is less than 2 weight %. The obtained zeolite composite material can be used as is, or the zeolite composite material can be ground or pulverized to reduce the particle size of any agglomerates that may have been formed during the production process.
[0028] The zeolite composite material can be present in the additive composition in any suitable amount. Preferably, based on the total weight of the polyols and zeolite composite material present in the additive composition, the zeolite composite material is present in the additive composition in an amount of about 1 wt % or more. More preferably, based on the total weight of the polyols and zeolite composite material present in the additive composition, the zeolite composite material is present in the additive composition in an amount of about 2 wt % or more, about 3 wt % or more, about 4 wt % or more, about 5 wt % or more, about 6 wt % or more, about 7 wt % or more, about 8 wt % or more, about 9 wt % or more, or about 10 wt % or more. Preferably, based on the total weight of the polyols and zeolite composite material present in the additive composition, the zeolite composite material is present in the additive composition in an amount of about 50 wt % or less. More preferably, based on the total weight of the polyols and zeolite composite material present in the additive composition, the zeolite composite material is present in the additive composition in an amount of about 45 wt % or less, about 40 wt % or less, about 35 wt % or less, about 30 wt % or less, or about 25 wt % or less.Thus, in a series of preferred embodiments, the zeolite composite is present in an amount of about 1 wt % to about 50 wt % (e.g., about 1 wt % to about 45 wt %, about 1 wt % to about 40 wt %, about 1 wt % to about 35 wt %, about 1 wt % to about 30 wt %, or about 1 wt % to about 25 wt %), about 2 wt % to about 50 wt % (e.g., about 2 wt % to about 45 wt %, about 2 wt % to about 40 wt %, about 2 wt % to about 35 wt %, about 2 wt % to about 30 wt %, or about 2 wt % to about 25 wt %), about 3 wt % to about 50 wt % (e.g., about 2 wt % to about 45 wt %, about 2 wt % to about 40 wt %, about 2 wt % to about 35 wt %, about 2 wt % to about 30 wt %, or about 2 wt % to about 25 wt %), or about 3 wt % to about 5 0 wt % (e.g., about 3 wt % to about 45 wt %, about 3 wt % to about 40 wt %, about 3 wt % to about 35 wt %, about 3 wt % to about 30 wt %, or about 3 wt % to about 25 wt %), about 4 wt % to about 50 wt % (e.g., about 4 wt % to about 45 wt %, about 4 wt % to about 40 wt %, about 4 wt % to about 35 wt %, about 4 wt % to about 30 wt %, or about 4 wt % to about 25 wt %), about 5 wt % to about 50 wt % (e.g., about 5 wt % to about 45 wt %, about 5 wt % to about 40 wt %, about 5 wt % to about 35 wt %, about 5 wt % to about 30 wt %, or about 5 wt % to about 25 wt %), %, or about 5 wt % to about 25 wt %), about 6 wt % to about 50 wt % (e.g., about 6 wt % to about 45 wt %, about 6 wt % to about 40 wt %, about 6 wt % to about 35 wt %, about 6 wt % to about 30 wt %, or about 6 wt % to about 25 wt %), about 7 wt % to about 50 wt % (e.g., about 7 wt % to about 45 wt %, about 7 wt % to about 40 wt %, about 7 wt % to about 35 wt %, about 7 wt % to about 30 wt %, or about 7 wt % to about 25 wt %), about 8 wt % to about 50 wt % (e.g., about 8 wt % to about 45 wt %, about 8 wt % to about 40 wt %, about % to about 30 wt %, or about 8 wt % to about 25 wt %), about 9 wt % to about 50 wt % (e.g., about 9 wt % to about 45 wt %, about 9 wt % to about 40 wt %, about 9 wt % to about 35 wt %, about 9 wt % to about 30 wt %, or about 9 wt % to about 25 wt %), or about 10 wt % to about 50 wt % (e.g., about 10 wt % to about 45 wt %, about 10 wt % to about 40 wt %, about 10 wt % to about 35 wt %, about 10 wt % to about 30 wt %, or about 10 wt % to about 25 wt %).In a preferred embodiment, the zeolite composite is present in the additive composition in an amount of about 5 wt % to about 30 wt % (e.g., about 10 wt % to about 30 wt %, about 10 wt % to about 25 wt %, about 15 wt % to about 30 wt %, or about 15 wt % to about 25 wt %), based on the total weight of the polyol and the zeolite composite present in the additive composition.
[0029] The additive composition may include other components in addition to the polyol and the zeolite composite material. Suitable other components for the additive composition include, but are not limited to, antioxidants, dispersants (e.g., surfactants such as polydimethylsiloxane-polyoxyalkylene block copolymers, silicone oils, and alcohol ethoxylates [e.g., nonylphenol ethoxylates]), aldehyde scavengers, and mixtures thereof. In a preferred embodiment, the additive composition includes a dispersant, such as those listed above.
[0030] As mentioned above, it has been observed that many polyurethane foams release various volatile organic compounds, such as aldehyde compounds and amine compounds. These volatile organic compounds may have pungent odors, and long-term exposure to such compounds may have adverse health effects. When the foam is placed in a closed space such as a vehicle interior, these odors and exposure hazards are generally exacerbated. In such a closed space, the volatile organic compounds (e.g., aldehyde compounds and amine compounds) released by the polyurethane foam can quickly accumulate and rise to concentrations that are unpleasant or cause health hazards to vehicle occupants. When used as an additive in the manufacture of polyurethane foam, the additive composition of the present invention has been shown to significantly reduce the amount of aldehyde compounds and amine compounds released by the polyurethane foam. As shown in the following examples, experimental observations show that the additive composition of the present invention reduces the level of formaldehyde, acetaldehyde and triethylenediamine, such as released by the foam. The observed reduction in the emission of these compounds is significantly lower than the emission observed by simply adding a zeolite substrate and a nitrogen-containing compound. The results show that the described zeolite composite material (wherein the nitrogen-containing compound is absorbed into the pores of the zeolite) exhibits a synergistic effect that exceeds the effect brought about by the components themselves.
[0031] Thus, in a second embodiment, the present invention provides a method for preparing a polyurethane polymer (e.g., polyurethane foam) using the additive composition of the first embodiment. The method generally requires mixing the additive composition with a suitable polyol and an isocyanate compound, and reacting the resulting mixture to prepare the polyurethane polymer. When a suitable blowing agent is included in the reaction mixture, the polyurethane polymer is foamed to produce a polyurethane foam.
[0032] Preferably, the method comprises the following steps: (a) providing a first polyol; (b) providing an isocyanate compound comprising two or more isocyanate groups; (c) providing an additive composition; (d) mixing the first polyol, the isocyanate compound and the additive composition to produce a reaction mixture; and (e) reacting the isocyanate compound with the first and second polyols to produce a polyurethane polymer, wherein the zeolite composite material is dispersed in the polyurethane polymer. As described above, the additive composition used in the method is the additive composition described above. Therefore, the additive composition comprises: (i) a second polyol; and (ii) a zeolite composite material dispersed in the second polyol. The zeolite composite material comprises: (A) a zeolite substrate having a surface and a plurality of pores in the surface; and (B) a nitrogen-containing compound adsorbed in at least a portion of the pores in the surface of the zeolite substrate. The nitrogen-containing compound preferably comprises (1) a first functional group comprising a carbon atom double-bonded to a nitrogen atom, and (2) a second functional group comprising a hydrogen atom covalently bonded to a nitrogen atom.
[0033] The first polyol used in the method can be any suitable polyol or a mixture of polyols. Suitable polyols used in the method include polyether polyols and polyester polyols. Suitable polyether polyols include those prepared by reacting epoxides such as ethylene oxide, propylene oxide, butylene oxide and glycidol with polyfunctional initiator compounds such as polyfunctional alcohols or amines. Examples of suitable polyfunctional initiator compounds include but are not limited to water, glycerol, pentaerythritol, ethylene glycol, propylene glycol (e.g. 1,2-propylene glycol), trimethylolpropane and ethylenediamine. Suitable polyester polyols include those prepared by reacting polycarboxylic acids or anhydrides with polyfunctional alcohols such as glycerol, pentaerythritol, ethylene glycol, diethylene glycol, propylene glycol (e.g. 1,2-propylene glycol) and trimethylolpropane. Examples of suitable polycarboxylic acids and anhydrides include, but are not limited to, adipic acid, maleic acid, maleic anhydride, succinic acid, succinic anhydride, azelaic acid, azelaic anhydride, glutaric acid, glutaric anhydride, phthalic acid and phthalic anhydride. The polyol or mixture of polyols used to produce the polyurethane polymer depends at least in part on the desired properties of the final polyurethane polymer. Preferably, the first polyol is a polyether polyol.
[0034] The first polyol used in the method can have any suitable molar mass. In a preferred embodiment, the first polyol has a molar mass of about 400 g / mol or more. More preferably, the first polyol has a molar mass of about 500 g / mol or more, about 750 g / mol or more, or about 1,000 g / mol or more. Preferably, the first polyol has a molar mass of about 20,000 g / mol or less, more preferably about 15,000 g / mol or less, or about 10,000 g / mol or less. Thus, in a series of preferred embodiments, the first polyol has a molar mass of about 400 g / mol to about 20,000 g / mol (e.g., about 400 g / mol to about 15,000 g / mol or about 400 g / mol to about 10,000 g / mol), about 500 g / mol to about 20,000 g / mol (e.g., about 500 g / mol to about 15,000 g / mol or about 500 g / mol to about 10,000 g / mol), about 750 g / mol to about 20,000 g / mol (e.g., about 750 g / mol to about 15,000 g / mol or about 750 g / mol to about 10,000 g / mol), or about 1,000 to about 20,000 g / mol (e.g., about 1,000 g / mol to about 15,000 g / mol or about 1,000 g / mol to about 10,000 g / mol).
[0035] The isocyanate compound used in the method can be any suitable isocyanate compound comprising two or more isocyanate groups. Suitable isocyanate compounds include but are not limited to aliphatic diisocyanates (e.g., hexamethylene diisocyanate, methylene dicyclohexyl diisocyanate and isophorone diisocyanate), aromatic diisocyanates (e.g., toluene diisocyanate and methylene diphenyl diisocyanate) and mixtures thereof. Preferably, the isocyanate compound is an aromatic diisocyanate, such as toluene diisocyanate, methylene diphenyl diisocyanate or mixtures thereof.
[0036] The additive composition used in the method can be any embodiment of the additive composition described above. In particular, the additive composition can include any suitable combination of the polyol, zeolite substrate, and nitrogen-containing compound described above with respect to the additive composition.
[0037] The additive composition can be mixed with the first polyol and the isocyanate compound in any suitable amount. The amount of the additive composition added is usually selected to provide a desired amount of zeolite composite material in the resulting reaction mixture (i.e., the combination of the first polyol, the isocyanate compound, the additive composition and any other components). The amount of the zeolite composite material present is preferably expressed as the weight parts of the zeolite composite material per 100 parts by weight of polyol (i.e., the total mass of the first polyol and the second polyol from the additive composition), which will be abbreviated as "php" hereinafter. Preferably, the additive composition is added to provide a zeolite composite material concentration of about 0.01php or higher, about 0.05php or higher, about 0.1php or higher, about 0.15php or higher, or about 0.2php or higher. Preferably, the additive composition is added to provide a zeolite composite material concentration of about 1php or lower, about 0.9php or lower, about 0.8php or lower, about 0.7php or lower, or about 0.6php or lower. Thus, in a series of preferred embodiments, the additive composition is preferably added to provide from about 0.01 php to about 1 php (e.g., from about 0.01 php to about 0.9 php, from about 0.01 php to about 0.8 php, from about 0.01 php to about 0.7 php, or from about 0.01 php to about 0.6 php), from about 0.05 php to about 1 php (e.g., from about 0.05 php to about 0.9 php, from about 0.05 php to about 0.8 php, from about 0.05 php to about 0.7 php, or from about 0.05 php to about 0.6 php), from about 0.1 php to about 1 php (e.g., from about 0.1 php to about 0.9 The zeolite composite concentration may be from about 0.1 php to about 0.8 php, from about 0.1 php to about 0.7 php, or from about 0.1 php to about 0.6 php), from about 0.15 php to about 1 php (e.g., from about 0.15 php to about 0.9 php, from about 0.15 php to about 0.8 php, from about 0.15 php to about 0.7 php, or from about 0.15 php to about 0.6 php), or from about 0.2 php to about 1 php (e.g., from about 0.2 php to about 0.9 php, from about 0.2 php to about 0.8 php, from about 0.2 php to about 0.7 php, or from about 0.2 php to about 0.6 php).
[0038] In addition to the first polyol, isocyanate compound and additive composition, the method can also use a suitable catalyst to catalyze the reaction between the polyol and the isocyanate compound. Suitable catalysts include amine catalysts (e.g., tertiary amine catalysts), Lewis acid catalysts and mixtures thereof. Amine catalysts suitable for the method include but are not limited to triethylenediamine, dimethylcyclohexylamine, dimethylethanolamine, bis-(2-dimethylaminoethyl) ether and mixtures thereof. Lewis acid catalysts suitable for the method include but are not limited to alkyltin carboxylates, oxides and mercaptides, such as dibutyltin dilaurate, stannous octoate, methyl tin mercaptide and mixtures thereof.
[0039] The reaction mixture of the method may include other components except the first polyol, the isocyanate compound, the additive composition and (if present) the catalyst. As described above, the reaction mixture may also include a blowing agent so that the method produces polyurethane foam. Suitable blowing agents used in the method include but are not limited to water, pentane, 1,1,1,2-tetrafluoroethane, 1,1,1,3,3-pentafluoropropane, 1,1-dichloro-1-fluoroethane and mixtures thereof. Preferably, the blowing agent is water. The reaction mixture may further include one or more surfactants, which can help emulsify the liquid component, adjust the cell size of the foam, and stabilize the cell structure of the foam to prevent collapse and subsurface voids. Suitable surfactants include but are not limited to polydimethylsiloxane-polyoxyalkylene block copolymers, silicone oils and alcohol ethoxylates (e.g., nonylphenol ethoxylates) and mixtures thereof. The reaction mixture may further include a chain extender, a crosslinking agent and a mixture thereof. Suitable chain extenders include, but are not limited to, diols of relatively low molar mass (e.g., typically 200 g / mol or less), such as ethylene glycol, diethylene glycol, ethylene glycol, triethylene glycol, tetraethylene glycol, propylene glycol, dipropylene glycol, tripropylene glycol, 1,3-propylene glycol, 1,3-butylene glycol, 1,4-butylene glycol, neopentyl glycol, 1,6-hexanediol, 1,4-cyclohexanedimethanol, ethanolamine, diethanolamine, methyldiethanolamine, and phenyldiethanolamine. Suitable crosslinkers include, but are not limited to, polyols of relatively low molar mass (e.g., typically 200 g / mol or less) having three or more hydroxyl groups, such as glycerol, trimethylolpropane, 1,2,6-hexanetriol, triethanolamine, pentaerythritol, and N,N,N′,N′-tetrakis(2-hydroxypropyl)ethylenediamine.
[0040] The polyurethane polymers (e.g., polyurethane foams) produced by the method can be used in any suitable application or end use. Preferably, the polyurethane foam is flexible, making it suitable for use as cushioning pads in, for example, mattresses, furniture, and vehicle seats. The foams produced by the method of the present invention are believed to be particularly suitable for use as cushioning pads in vehicle seats (e.g., car seats), wherein the reduction of volatile organic compounds released by the foam will be particularly advantageous in view of the relatively large volume of the vehicle interior occupied by such cushioning pads.
[0041] The following examples further illustrate the above subject matter, but should of course not be construed as limiting the scope thereof in any way.
[0042] Example 1
[0043] This example demonstrates the production of several zeolite composites suitable for use in preparing additive compositions according to the present invention.
[0044] The zeolite composites were prepared by the following general procedure. First, a specified amount (by weight) of a nitrogen-containing compound was added to ten (10) parts by weight of water and mixed until the nitrogen-containing compound was completely dissolved. Second, ten (10) parts by weight of zeolite were added to the solution of the nitrogen-containing compound and mixed for about ten (10) minutes. Finally, the resulting zeolite dispersion was placed in an oven maintained at a temperature of about 120°C for about 18 hours or until the moisture content of the resulting zeolite composite was less than 2% (whichever occurred last). All zeolite composites in this example were prepared using HSZ-385HUA zeolite (from Tosoh USA, Inc.). HSZ-385HUA zeolite is a zeolite reported to have a moisture content of 600 m 2 / g BET specific surface area and an average particle size of 2-3μm + Cationic zeolite.
[0045] Two (2) parts by weight of aminoguanidine were used in the above procedure to prepare a zeolite composite material designated as "Sample 1A". Four (4) parts by weight of aminoguanidine were used in the above procedure to prepare a zeolite composite material designated as "Sample 1B". Three (3) parts by weight of metformin were used in the above procedure to prepare a zeolite composite material designated as "Sample 1C". Three parts by weight of hexadiguanamine were used in the above procedure to prepare a zeolite composite material designated as "Sample 1D". The resulting zeolite composite material was used to prepare a polyurethane foam, as described in Example 2 below.
[0046] Example 2
[0047] This example demonstrates the reduction in volatile organic compound emissions resulting from the use of an additive composition comprising a zeolite composite according to the invention.
[0048] Polyurethane foams were prepared using the general recipe provided in Table 1 below in a batch size based on 200 grams of polyol. Each foam was cured in an oven maintained at a temperature of approximately 360° F. (182° C.) for 5 minutes, then removed from the oven and cooled to room temperature. Each cooled foam was then sealed in aluminum foil to capture all volatile components until emissions testing could be performed.
[0049] Table 1.
[0050] Components Commercial Sources Quantity (portion) Ether polyols Arcol 3040(Covestro) 100.0 water 2.0 Toluene diisocyanate Mondur TD 80 (Covestro) 30.9 Silicone surfactant Niax L-620(Momentive) 0.65 Amine Catalyst Niax A-1(Momentive) 0.1 Amine Catalyst Dabco 33LV(Evonik) 0.35 Stannous Octoate Dabco T-9 (Evonik) 0.05 Zeolite composite materials -- As shown in Table 2
[0051] Once the foams were produced, emissions testing was performed by cutting samples of 1.5 inch diameter and 1.0 inch height from each foam. The cylinders were placed in a microchamber and allowed to equilibrate at 65°C for 20 minutes before exhaust gas sampling. Nitrogen humidified to 50% RH was flushed through the chamber at 50 mL / min. Exhaust gas analytes were measured using The TA adsorbent resin captured and analyzed with a gas chromatograph / mass spectrometer. Identifiable emissions were quantified as toluene equivalents. The "VOC Reduction %" reported in Table 2 below was calculated by comparing the total VOC measured for the subject foams to the total VOC measured for the control foams.
[0052] Table 2.
[0053]
[0054] The data in Table 2 show that the foams made with the zeolite composites according to the present invention all exhibited much lower VOC emissions than the control foams. For example, the VOC emissions of Foam 2B were less than half of the VOC emissions of the control foam, a reduction achieved by adding only 0.4 php of the zeolite composite sample 1B.
[0055] Example 3
[0056] This example demonstrates the production of a zeolite composite and an additive composition according to the invention.
[0057] The first zeolite composite was prepared following the general procedure described in Example 1 using 3 parts by weight of aminoguanidine and 10 parts by weight of HSZ-385HUA zeolite. After drying, the resulting zeolite composite was dispersed in Carpol PGP-400 polyol at a solids level of 25% (by weight). The resulting additive composition will be referred to as "Sample 3A".
[0058] A second zeolite composite was prepared following the general procedure described in Example 1 using 3 parts by weight of aminoguanidine and 10 parts by weight of HSZ-980HOA zeolite (from Tosoh USA, Inc.). HSZ-980HOA zeolite is a zeolite reported to have a molecular weight of 500 m / s.2 / g BET specific surface area and an average particle size of 2.5 μm + Cationic zeolite. After drying, the resulting zeolite composite was dispersed in Arcol F-3222 polyol at a solids level of 35% (by weight). The resulting additive composition will be referred to as "Sample 3B".
[0059] Example 4
[0060] This example demonstrates the reduction in volatile organic compound emissions resulting from the use of an additive composition containing a zeolite composite according to the invention.
[0061] Polyurethane foams were prepared using the general recipe provided in Table 3 below in batch sizes based on 100 grams of polyol. Each foam was cured in an oven maintained at a temperature of approximately 360°F (182°C) for 5 minutes, then removed from the oven and cooled to room temperature. Each cooled foam was then sealed in aluminum foil to capture all volatile components until emissions testing could be performed.
[0062] Table 3.
[0063] Components Commercial Sources Quantity (portion) Ether polyols Arcol 3040(Covestro) 100.0 water 4.56 Toluene diisocyanate Mondur TD 80 (Covestro) 59.8 Silicone surfactant Niax L-620(Momentive) 1.0 Amine Catalyst Dabco 33LV(Evonik) 0.15 Stannous Octoate Dabco T-9 (Evonik) 0.15 Zeolite composite materials -- As shown in Table 4
[0064] Once the foams were produced, emissions testing was performed by cutting samples of 1.5 inch diameter and 1.0 inch height from each foam. The cylinders were placed in a microchamber and allowed to equilibrate at 65°C for 20 minutes before exhaust gas sampling. Nitrogen humidified to 50% RH was flushed through the chamber at 50 mL / min. Exhaust gas analytes were measured using The TA adsorbent resin was captured and analyzed by gas chromatography / mass spectrometry. The triethylenediamine catalyst (TEDA) emissions contributing to the foam odor were quantified as toluene equivalents. (Dabco 33LV amine catalyst is a triethylenediamine catalyst.) The amounts of triethylenediamine catalyst emissions detected are reported in Table 4 below.
[0065] Table 4.
[0066] Control foam Foam 4A Foam 4B Zeolite composite materials -- Sample 3A Sample 3B Additive Composition Amount (php) -- 1.6 1.14 Zeolite composite material quantity (php) -- ~0.4 ~0.4 <![CDATA[Total TEDA (μg / m 2 hr)]]> 1,087.7 Not Detected Not Detected
[0067] As can be seen from the data in Table 4, the foams made with the additive composition according to the present invention exhibited no detectable amine catalyst (TEDA) emissions under the test conditions employed. In contrast, the control foam exhibited 1,087.7 μg / m 2 Based on these results, it is believed that foams prepared with the additive composition of the present invention will exhibit significantly reduced VOC emissions and amine odor compared to foams prepared without the additive composition.
[0068] Example 5
[0069] This example demonstrates the reduction in volatile organic compound emissions resulting from the use of an additive composition containing a zeolite composite according to the present invention.This example further demonstrates how the zeolite composite results in greater VOC reductions than the addition of zeolite and nitrogen-containing compounds alone.
[0070] The zeolite composite was prepared using 3 parts by weight of aminoguanidine and 10 parts of HSZ-385HUA zeolite following the general procedure described in Example 1. The resulting zeolite composite will be referred to hereinafter as "Sample 5A".
[0071] Polyurethane foam was prepared using the general formula provided in Table 5 below in a batch size based on 200 grams of polyol. Foam 5A was produced by adding HSZ-385HUA zeolite and aminoguanidine alone (i.e., not in the form of a composite material as described above) to the reaction mixture during foam production. Each foam was cured for 5 minutes in an oven maintained at a temperature of about 360°F (182°C), then removed from the oven and cooled to room temperature. Each cooled foam was then sealed in aluminum foil to capture all volatile components until emissions testing could be performed.
[0072] Table 5.
[0073]
[0074] Once the foams were produced, emissions testing was performed by cutting samples of 1.5 inch diameter and 1.0 inch height from each foam. The cylinders were placed in a microchamber and allowed to equilibrate at 65°C for 20 minutes before exhaust gas sampling. Nitrogen humidified to 50% RH was flushed through the chamber at 50 mL / min. Exhaust gas analytes were measured using TA adsorbent resin capture and analyzed with gas chromatography / mass spectrometer. Identifiable emissions, such as triethylenediamine catalyst (TEDA) emissions, are quantified as toluene equivalents. The amounts of VOC and TEDA emissions detected are reported in Table 6 below. The "% reduction" values reported in Table 6 below are calculated by comparing the emissions measured for the subject foams with the emissions measured for the control foams.
[0075] Table 6
[0076] Control foam Foam 5A Foam 5B Zeolite composite materials -- -- Sample 3B Zeolite composite material quantity (php) -- -- 0.4 Zeolite amount (php) 0.3 -- Aminoguanidine (php) 0.1 -- <![CDATA[Total VOC (μg / m 2 hr)]]> 31,762 29,182 13,761 Total VOC Reduction % -- 8.1% 56.7% <![CDATA[Total TEDA (μg / m 2 hr)]]> 29,113 25,753 10,719 TEDA reduction % -- 11.5% 63.2%
[0077] The data in Table 6 show that the addition of zeolite and nitrogen-containing compound alone during foam production (Foam 5A) produced only an 8.1% reduction in total VOC emissions and an 11.5% reduction in TEDA emissions. In contrast, when the same amount of zeolite and nitrogen-containing compound were added in the form of a composite material as described herein, the resulting foam (Foam 5B) showed a 56.7% reduction in total VOC emissions and a 63.2% reduction in TEDA emissions. This significant reduction in emissions is unexpected given that the only difference between the two foams is the form in which the zeolite and nitrogen-containing compound are added to the foam (i.e., composite vs. non-composite). It is believed that these data show that foams prepared with the additive composition of the present invention will show significantly reduced VOC emissions and amine emissions / odor compared to foams prepared without the additive composition.
[0078] All references, including publications, patent applications, and patents, cited herein are hereby incorporated by reference to the same extent as if each reference were individually and specifically indicated to be incorporated by reference and were set forth in its entirety herein.
[0079] In the context of describing the subject matter of the present application (especially in the following claims), the use of the terms "one" and "a kind of" and "the" and similar references should be interpreted as covering both the singular and the plural, unless otherwise specified herein or clearly contradicted by the context. Unless otherwise specified, the terms "comprising", "having", "including" and "containing" should be interpreted as open terms (i.e., meaning "including but not limited to"). Unless otherwise specified herein, the description of the numerical range herein is only intended to be used as a shorthand method for referring to each individual value falling within the range, respectively, and each individual value is incorporated into the specification as if it is separately described herein. Unless otherwise specified herein or the context clearly contradicts, all methods described herein can be performed in any suitable order. Unless otherwise stated, the use of any or all examples or exemplary language (e.g., "for example") provided herein is only intended to better illustrate the subject matter of the present application, rather than to limit the scope of the subject matter. Any language in the specification should not be interpreted as indicating that any unclaimed element is essential to the practice of the subject matter described herein.
[0080] Preferred embodiments of the subject matter of the present application are described herein, including the best mode known to the inventor for implementing the claimed subject matter. After reading the foregoing description, variations of those preferred embodiments may become apparent to those skilled in the art. The inventors expect that those skilled in the art will use these variations as appropriate, and the inventors intend that the subject matter described herein be implemented in a manner different from that specifically described herein. Therefore, as permitted by applicable law, the present invention includes all variations and equivalents of the subject matter listed in the appended claims. In addition, unless otherwise indicated or the context clearly contradicts, the present invention includes any combination of the above-mentioned elements in all possible variations thereof.
Claims
1. An additive composition comprising: (a) polyols; (b) a zeolite composite material dispersed in the polyol, the zeolite composite material comprising: (i) a zeolite substrate having a surface and a plurality of pores in the surface; and (ii) a nitrogen-containing compound adsorbed in at least a portion of the pores in the surface of the zeolite substrate, the nitrogen-containing compound comprising: (A) a first functional group comprising a carbon atom double-bonded to a nitrogen atom, and (B) a second functional group comprising a hydrogen atom covalently bonded to the nitrogen atom.
2. The additive composition of claim 1, wherein the polyol has a molar mass of about 400 g / mol or greater.
3. The additive composition according to claim 1 or 2, wherein the polyol is a polyether polyol.
4. The additive composition of any one of claims 1-3, wherein the zeolite composite is present in the additive composition in an amount of about 5 wt % to about 30 wt %, based on the total weight of the polyol and the zeolite composite present in the additive composition.
5. The additive composition according to any one of claims 1 to 4, wherein the zeolite substrate is H + Cationic zeolite.
6. The additive composition of any one of claims 1-5, wherein the nitrogen-containing compound is present in the zeolite composite in an amount of about 15 wt% to about 50 wt%, based on the total weight of the zeolite substrate and the nitrogen-containing compound.
7. The additive composition of any one of claims 1-6, wherein the nitrogen-containing compound comprises at least two second functional groups comprising hydrogen atoms covalently bonded to nitrogen atoms.
8. The additive composition according to any one of claims 1 to 7, wherein the nitrogen-containing compound is selected from the group consisting of guanidine compounds, aminoguanidine compounds, biguanidine compounds, guanamine compounds, and mixtures thereof.
9. A method for preparing a polyurethane polymer, the method comprising the steps of: (a) providing a first polyol; (b) providing an isocyanate compound comprising two or more isocyanate groups; (c) providing an additive composition comprising: (i) a second polyol; and (ii) a zeolite composite material dispersed in the second polyol, the zeolite composite material comprising: (A) a zeolite substrate having a surface and a plurality of pores in the surface; and (B) a nitrogen-containing compound adsorbed within at least a portion of the pores in the surface of the zeolite substrate, the nitrogen-containing compound comprising: (1) a first functional group comprising a carbon atom doubly bonded to a nitrogen atom, and (2) a second functional group comprising a hydrogen atom covalently bonded to the nitrogen atom; (d) mixing the first polyol, the isocyanate compound, and the additive composition to produce a reaction mixture; and (e) reacting the isocyanate compound with the first and second polyols to produce a polyurethane polymer, wherein the zeolite composite is dispersed in the polyurethane polymer.
10. The method of claim 9, wherein the second polyol has a molar mass of about 400 g / mol or greater.
11. The method of claim 9 or 10, wherein the second polyol is a polyether polyol.
12. The method of any one of claims 9-11, wherein the zeolite composite is present in the additive composition in an amount of about 5 wt% to about 30 wt%, based on the total weight of the polyol and zeolite composite present in the additive composition.
13. The method according to any one of claims 9 to 12, wherein the zeolite substrate is H + Cationic zeolite.
14. The method of any one of claims 9-13, wherein the nitrogen-containing compound is present in the zeolite composite in an amount of about 15 wt% to about 50 wt%, based on the total weight of the zeolite substrate and the nitrogen-containing compound.
15. The method of any one of claims 9-14, wherein the nitrogen-containing compound comprises at least two second functional groups comprising hydrogen atoms covalently bonded to nitrogen atoms.
16. The method according to any one of claims 9 to 15, wherein the nitrogen-containing compound is selected from the group consisting of aminoguanidine compounds, biguanidine compounds, guanamine compounds, and mixtures thereof.
17. The method of any one of claims 9-16, wherein the reaction mixture comprises about 0.1 or more parts by weight of the zeolite composite material per 100 parts by weight of the polyol.