Polylactic acid grafted copolymer as well as preparation method and application thereof

CN119072513APending Publication Date: 2024-12-03CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202380017638.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-01-29
Filing Date
2023-01-04
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

In the existing technology, maleic anhydride-grafted polylactic acid has low molecular weight and low grafting rate, resulting in poor mechanical properties and heat resistance, which limits its application in industrial production.

Method used

Using the method of first grafting and then ring-opening copolymerization, the grafting monomer and lactide are grafted in the nucleophilic addition reaction, followed by low-temperature prepolymerization in the ring-opening polymerization reaction, and chain growth reaction at high temperature. , increase the molecular weight and grafting rate of the polymer.

Benefits of technology

It significantly improves the right-angle tear strength, elongation at break and glass transition temperature of the polylactic acid graft copolymer. It has good flexibility and heat resistance, is suitable for industrial production, and can further regulate its properties through functional group modification.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119072513A_ABST
    Figure CN119072513A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of polymer synthesis, and particularly relates to a polylactic acid grafted copolymer as well as a preparation method and application thereof. The polylactic acid grafted copolymer is characterized in that the polylactic acid grafted copolymer contains a repetitive structural unit with a structure as shown in a formula (A), wherein R1 is H or a grafting group, at least part of R1 in the repetitive structure units is a grafting group, and the right-angle tear strength of the polylactic acid grafted copolymer is not lower than 120 kN / m, preferably 135-150 kN / m; and the elongation at break is not less than 30%, preferably 35-45%. According to the polylactic acid grafted copolymer prepared by the method recorded by the technical scheme of the invention, the grafting efficiency is greatly improved, the toughness, elongation at break and glass transition temperature of the polylactic acid material are improved, and the prepared grafted modified polylactic acid copolymer material can be green and fully biodegradable.
Need to check novelty before this filing date? Find Prior Art

Description

Polylactic acid graft copolymer and its preparation method and application

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the benefit of Chinese patent application No. 202210110898.2 filed on January 29, 2022, the contents of which are incorporated herein by reference. Technical Field

[0003] The invention belongs to the technical field of polymer synthesis, and particularly relates to a polylactic acid graft copolymer and a preparation method and application thereof. Background Art

[0004] In recent years, research on bio-based composites has become a hot topic in academia and industry, aiming to reduce the environmental impact of fossil fuels. Compared to polyolefins and polyethylene terephthalate (PET), commonly used in industrial products, polylactic acid (PLA) is a thermoplastic resin with superior strength and processability. PLA is produced by polymerizing lactic acid monomers, which can be fermented from plants such as corn, potatoes, cotton, and hemp. Lactic acid is a renewable raw material, and PLA polymerized from renewable lactic acid exhibits high strength, good processability, and excellent mechanical properties. However, PLA also has several drawbacks, such as brittleness, strong hydrophobicity, low impact strength, and high price. Furthermore, PLA exhibits poor stability at high temperatures and certain humidity levels. These drawbacks hinder its direct use in industrial products, as with general-purpose plastics such as polyethylene and polypropylene, requiring modification. Currently, a common modification method to optimize the performance of PLA is to blend it with other plastics. While this method is simple, it does not fundamentally alter the properties of the PLA material. Other methods have also been attempted to modify the polylactic acid material itself, such as grafting. Because maleic anhydride is a polar monomer with a five-membered ring structure, it is a highly effective grafting modifier. Grafting polylactic acid with maleic anhydride can not only increase the polarity of the polylactic acid material but also, due to its cyclic structure, improve the toughness of the polylactic acid macromolecular chain.

[0005] Currently, the commonly used method for modifying the properties of other materials with maleic anhydride is to first graft maleic anhydride onto polyethylene, polystyrene, starch, lignin, etc. to obtain a pre-grafted material; then, the pre-grafted material is added to the polylactic acid material through blending to improve the toughness of the polylactic acid. However, this modification method is not very effective. Some researchers have directly grafted maleic anhydride onto the polylactic acid macromolecular chain through reactive extrusion, thereby changing the non-polar structure of the polylactic acid.

[0006] CN108192033A discloses a method for preparing a polylactic acid (PLLGC) copolymer directly grafted with maleic anhydride. The method involves polymerizing L-lactide, glycolide, and ε-caprolactone in a specific ratio under the action of a catalyst to produce crude PLLGC. The crude PLLGC is dissolved in chloroform, reprecipitated with methanol, and filtered to obtain a white solid, thereby obtaining refined PLLGC. Maleic anhydride is then added to the refined PLLGC and reacted in solution to graft the maleic anhydride onto the PLLGC copolymer. While the polylactic acid synthesized by this method is highly pure, the grafting rate of maleic anhydride is less than 1%. Furthermore, the reaction is performed using solution polymerization, which results in several drawbacks, including the high toxicity of the organic solvent used and the low molecular weight of the resulting polymer, making it unsuitable for industrial production.

[0007] CN103570884A discloses a method for preparing maleic anhydride-modified poly(lactide-glycolide). The method comprises adding L / D-lactide, glycolide, and maleic anhydride to an ampoule in a certain proportion, polymerizing the mixture at 130-170°C for 12-60 hours under the action of a stannous octoate catalyst, and preparing crude poly(lactide-glycolide) (MPLGA). The MPLGA is dissolved in chloroform, reprecipitated with methanol, and filtered to obtain refined MPLGA. Although the polymer prepared by this method has a narrow molecular weight distribution, the maleic anhydride grafting reaction is carried out simultaneously during the polymerization process, resulting in a low grafting rate of the product, a long polymerization reaction time, and a low polymer molecular weight, which is not conducive to industrial production.

[0008] In summary, the maleic anhydride grafted polylactic acid in the prior art generally has the problems of low molecular weight and low maleic anhydride grafting rate, resulting in poor mechanical properties and heat resistance.

[0009] Summary of the Invention

[0010] The purpose of the present invention is to provide a polylactic acid graft copolymer, the molecular weight and the content of the grafted groups of the polylactic acid graft copolymer are significantly improved, so that the polylactic acid graft copolymer material has good mechanical properties, heat resistance and green degradability, and is easy to industrialize and produce.

[0011] In order to achieve the above-mentioned object, the first aspect of the present invention provides a polylactic acid graft copolymer, characterized in that the polylactic acid graft copolymer contains repeating structural units of the structure represented by formula (A);

[0012]

[0013] Among them, R 1 is H or a grafted group, and at least part of the R 1The polylactic acid graft copolymer has a right-angle tearing strength of not less than 120 kN / m, preferably 135-150 kN / m; and an elongation at break of not less than 30%, preferably 35-45%.

[0014] A second aspect of the present invention provides a method for preparing a polylactic acid graft copolymer, characterized in that the method comprises the following steps:

[0015] (1) contacting lactide with a grafting monomer under nucleophilic addition reaction conditions to obtain a nucleophilic addition product;

[0016] (2) under ring-opening polymerization conditions, mixing the nucleophilic addition product obtained in step (1) with a catalyst and an initiator, and performing low-temperature prepolymerization to obtain a ring-opening polymerization product;

[0017] (3) In the presence of an antioxidant, the ring-opening polymerization product obtained in step (2) is subjected to high-temperature polymerization under chain growth reaction conditions.

[0018] The third aspect of the present invention provides a polylactic acid graft copolymer prepared by the above method.

[0019] The fourth aspect of the present invention provides a use of the polylactic acid graft copolymer described in the first aspect or the third aspect in the production of agricultural mulch films, food packaging materials and medical hygiene products.

[0020] Compared to the existing technology, the present invention provides a new route for synthesizing polylactic acid graft copolymers. First, under the conditions of a nucleophilic addition reaction, lactide is grafted with a grafting monomer to obtain a nucleophilic addition product rich in graft groups. Then, under the conditions of a ring-opening polymerization reaction, the nucleophilic product rich in graft groups is prepolymerized at low temperature to obtain a ring-opening polymerization product. Finally, under the conditions of a chain growth reaction, the ring-opening polymerization product is polymerized at high temperature to obtain a high-molecular-weight maleic anhydride-grafted polylactic acid copolymer. Compared with the existing method of first ring-opening copolymerization followed by grafting, the present invention's method of first grafting followed by ring-opening copolymerization can effectively increase the content of graft groups (i.e., the grafting rate), and through subsequent high-temperature polymerization, it can effectively increase the molecular weight of the polymer.

[0021] The preparation method of the polylactic acid graft copolymer provided by the present invention can theoretically obtain a polylactic acid graft copolymer with a grafting rate of 50% or even 100%. By adjusting the raw material ratio, the content of the grafted group in the polylactic acid graft copolymer can be effectively controlled, thereby adjusting the performance of the polylactic acid graft copolymer.

[0022] The polylactic acid graft copolymer provided by the present invention has both a high molecular weight and strong flexibility. It exhibits excellent right-angle tear strength and elongation at break, and the resulting graft-modified polylactic acid copolymer is environmentally friendly and fully biodegradable. Because the terminal hydroxyl groups of the polylactic acid graft copolymer are retained, the polylactic acid graft copolymer can be further modified using these functional groups to further control the properties of the polylactic acid graft copolymer. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] FIG1 is the infrared absorption spectra of the corresponding substances in Example 1, wherein: (a) L-lactide (LA), (b) maleic anhydride (MAH), and (c) maleic anhydride-grafted lactide;

[0024] FIG2 is the infrared absorption spectra of the corresponding substances in Example 1, including: (a) polylactic acid (PLA), (b) maleic anhydride (MAH), (c) maleic anhydride-grafted polylactic acid, and (d) the infrared difference spectrum after subtraction of the spectrum of maleic anhydride-grafted polylactic acid and polylactic acid;

[0025] Figure 3 is the corresponding substance in Example 1 13 CNMR spectra, where: (a) L-lactide, (b) maleic anhydride grafted lactide;

[0026] Figure 4 is the corresponding substance in Example 1 13 CNMR spectra, including: (a) polylactic acid (PLA), (b) maleic anhydride grafted polylactic acid. DETAILED DESCRIPTION

[0027] The endpoints of the ranges and any values ​​disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoints of each range, the endpoints of each range and individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered to be specifically disclosed herein.

[0028] In order to achieve the above-mentioned object, the first aspect of the present invention provides a polylactic acid graft copolymer, characterized in that the polylactic acid graft copolymer contains repeating structural units of the structure represented by formula (A);

[0029]

[0030] Among them, R 1 is H or a grafted group, and at least part of the R 1 The polylactic acid graft copolymer has a right-angle tearing strength of not less than 120 kN / m, preferably 135-150 kN / m; and an elongation at break of not less than 30%, preferably 35-45%.

[0031] The polylactic acid graft copolymer can also be represented by the following general formula:

[0032]

[0033] Among them, R1”, R2”, ... and R n " are each independently selected from H, a grafted group represented by formula (I), and a grafted group represented by formula (II).

[0034] According to the present invention, the content of the grafted group is 1 The content is 10 mol% or more of the total amount, preferably 30 mol% or more, and more preferably 40 mol% or more.

[0035] According to the present invention, the grafting group can be any group that can be grafted onto lactide / polylactic acid and make the resulting polylactic acid material have a right-angle tear strength of not less than 120 kN / m, preferably 135-150 kN / m, and an elongation at break of not less than 30%, preferably 35-45%. Preferably, the grafting group is a structure represented by formula (I) and / or formula (II).

[0036]

[0037] Wherein, R1, R2, R3, R4, and R5 are each independently hydrogen, a C1-C4 substituted or unsubstituted alkyl group, and R6 is a C1-C6 substituted or unsubstituted alkyl group, or a C6-C20 aryl group.

[0038] In the present invention, the C1-C6 substituted or unsubstituted alkyl group may be any one of methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl, tert-butyl, n-pentyl, isopentyl, tert-pentyl, neopentyl, n-hexyl, and isohexyl. The alkyl group may be substituted by one or more of halogen, nitro, primary amino, secondary amino, and tertiary amino groups. The halogen may be one or more of fluorine, chlorine, bromine, and iodine.

[0039] The C6-C20 aryl group may be any one of phenyl, methylphenyl, ethylphenyl, dimethylphenyl, diphenyl, biphenyl, and polyphenyl.

[0040] According to the present invention, taking the graft copolymer with maleic anhydride as the branch group as an example, the polylactic acid graft copolymer 13CNMR spectra show peaks at chemical shifts near 169 ppm, indicating anhydride carbon atoms, and near 72 ppm, indicating maleic anhydride carbon-carbon double bond cleavage. These peaks are unique to the mid-chain grafting method of the present invention. In this context, "near" refers to an acceptable error in the art, typically ±5 ppm, due to factors such as instrumentation and individual operation. Accordingly, the present invention refers to the prior art method of ring-opening polymerization followed by grafting as chain-end grafting.

[0041] According to the present invention, the weight average molecular weight of the polylactic acid graft copolymer is 1×10 5 -4×10 5 The polylactic acid graft copolymer provided by the present invention has a high molecular weight and strong flexibility. The molecular weight of the polylactic acid grafted by the chain end in the prior art is usually 3×10 5 Below, the right-angle tearing strength is lower than 100kN / m, usually 80-95kN / m, and the elongation at break does not exceed 10%, usually 5-10%.

[0042] According to the present invention, the glass transition temperature of the polylactic acid graft copolymer is 80-100° C. The glass transition temperature of the polylactic acid graft copolymer provided by the present invention is higher than that of the polylactic acid grafted with chain ends in the prior art, which is beneficial to improving the temperature resistance of the material.

[0043] According to the present invention, at least one terminal group of the polylactic acid graft copolymer contains a hydroxyl group. Thus, the polylactic acid graft copolymer can be further modified by this functional group. The presence of the terminal hydroxyl group can be determined by chemical titration.

[0044] In the present invention, right-angle tear strength and elongation at break were measured using a universal mechanical tester; weight-average molecular weight was measured using gel permeation chromatography; glass transition temperature was measured using differential scanning calorimetry; and grafting rate was measured using chemical titration. Details are described below.

[0045] A second aspect of the present invention provides a method for preparing a polylactic acid graft copolymer, characterized in that the method comprises the following steps:

[0046] (1) contacting lactide with a grafting monomer under nucleophilic addition reaction conditions to obtain a nucleophilic addition product;

[0047] (2) under ring-opening polymerization conditions, mixing the nucleophilic addition product obtained in step (1) with a catalyst and an initiator, and performing low-temperature prepolymerization to obtain a ring-opening polymerization product;

[0048] (3) In the presence of an antioxidant, under the condition of chain growth reaction, the ring-opening polymerization product obtained in step (2) is subjected to high-temperature polymerization to increase the molecular weight of the polylactic acid graft copolymer.

[0049] The present invention adopts a method of first grafting and then ring-opening polymerization, which can effectively ensure the grafting rate. Through high-temperature polymerization, it can ensure that a polylactic acid graft copolymer with a higher molecular weight is obtained, so that the obtained polymer has higher flexibility and heat resistance.

[0050] Preferably, the grafting monomer is a monomer represented by formula (i) and / or formula (ii):

[0051]

[0052] Among them, R1', R2', R3', R4', R5', and R6' respectively correspond to and are the same as R1, R2, R3, R4, R5, and R6 defined above, and are not repeated here.

[0053] According to the present invention, step (1) is to achieve a grafting reaction between lactide and a grafting monomer such as maleic anhydride, wherein maleic anhydride is grafted onto lactide via double bond cleavage through a nucleophilic addition reaction to obtain a grafted product. The nucleophilic addition reaction in step (1) is carried out in the presence of an initiator.

[0054] The lactide described in the present invention is at least one selected from L-lactide, D-lactide and meso-lactide, preferably L-lactide and / or D-lactide.

[0055] According to the present invention, the initiator is a peroxide initiator, preferably dicumyl peroxide and / or 2,5-dimethyl-2,5-bis-(tert-butylperoxy)hexane.

[0056] According to the present invention, the amount of the initiator added is 0.1-5 wt %, preferably 0.5-2 wt %, of the amount of the lactide used.

[0057] According to the present invention, step (1) is a constant temperature reaction under an inert gas flow, preferably a nitrogen flow and vacuum conditions, and the conditions of the nucleophilic addition reaction include: a reaction temperature of 50-150°C, preferably 80-120°C; a reaction pressure of 2-100kPa, preferably 20-60kPa; a reaction time of 0.5-10h, preferably 2-6h; and a gas flow rate of 0.5-6m / s, preferably 2-4m / s, for the nitrogen flow protection.

[0058] In the present invention, unless otherwise specified, the pressures mentioned refer to absolute pressures.

[0059] According to the present invention, the optical purity of the lactide in step (1) can be 99.0-99.6%, preferably 99.4-99.6%, and either homemade or purchased lactide can be used.

[0060] According to the present invention, in order to obtain better toughness and increase the grafting rate of the grafting group (ie the content of the grafting group in the polylactic acid material), the amount of grafting monomer added is preferably 100-300wt% of the amount of lactide used, preferably 150-200wt%.

[0061] Taking maleic anhydride and L-lactide as an example, the main reactions occurring in step (1) are shown in the following formulas (a) and (b):

[0062]

[0063] Theoretically, the grafting rate of the product obtained by formula (a) is 100%, and the grafting rate of the product obtained by formula (b) is 50%.

[0064] According to the present invention, the method further comprises removing the lactide that has not participated in the nucleophilic addition reaction by means of reduced pressure distillation after step (1), and then subjecting the obtained product to the reaction of step (2).

[0065] According to the present invention, the conditions for the reduced pressure distillation include: temperature of 100-200° C., preferably 120-150° C.; pressure of 0-100 kPa, preferably 10-50 kPa; and time of 1-10 h, preferably 2-6 h.

[0066] According to the present invention, the catalyst in step (2) is used to catalyze the ring-opening reaction of the lactide after the grafted group is grafted, and is preferably at least one of stannous octoate, zinc lactate, trialkylaluminum, triisobutylaluminum and stannous chloride, and more preferably stannous octoate.

[0067] According to the present invention, the amount of the catalyst added may be 0.1-5 wt%, preferably 0.5-3 wt%, based on the total weight of the nucleophilic addition product.

[0068] According to the present invention, the initiator in step (2) is an alkylhydroxy or aromatic hydroxy initiator, which is used to initiate the polymerization reaction of the lactide after the introduction of the grafted group and the ring-opening reaction. The initiator is preferably selected from at least one of glycerol, xylitol, ethylene glycol and triphenylphosphine, preferably triphenylphosphine.

[0069] According to the present invention, the amount of the initiator added may be 0.05-5 wt %, preferably 0.3-2 wt %, based on the total weight of the nucleophilic addition product.

[0070] According to the present invention, step (2) is a low-temperature polymerization in an inert gas flow, preferably a nitrogen flow and negative pressure conditions, and the conditions of the ring-opening polymerization reaction in step (2) include: a reaction temperature of 100-150°C, preferably 120-140°C; a reaction pressure of 100-1000kPa, preferably 200-500kPa; a reaction time of 2-15h, preferably 3-8h; and a gas flow rate of the nitrogen flow of 0.5-6m / s, preferably 2-4m / s.

[0071] According to the present invention, the antioxidant in step (3) is used to prevent oxidation of the polylactic acid oligomer in step (2), thereby ensuring further polymerization at a higher temperature and performing a chain growth reaction. The antioxidant can be any substance that can prevent oxidation of polylactic acid at high temperatures and does not adversely affect the polylactic acid material. For example, it can be selected from at least one of phosphite antioxidants, alkyl polyphenol antioxidants, and thiobisphenol antioxidants, preferably triphenyl phosphite.

[0072] According to the present invention, the amount of the antioxidant added is 0.1-5 wt%, preferably 0.5-2 wt%, of the total weight of the ring-opening polymerization product.

[0073] According to the present invention, the temperature of the chain extension reaction in step (3) is 140-250°C, preferably 160-200°C.

[0074] According to the present invention, step (3) is preferably carried out in a twin-screw extruder. A twin-screw extruder is used to realize the reaction process, wherein the ring-opening polymerization product and the antioxidant are added to the twin-screw extruder for high-temperature reactive mixing, extrusion granulation, and finally the polylactic acid graft copolymer is obtained.

[0075] The conditions for high-temperature polymerization include an inlet temperature of 140-160° C. and an outlet temperature of 170-190° C. for the twin-screw extruder. The residence time of the material in the twin-screw extruder is preferably 13-23 minutes.

[0076] The preparation method of the polylactic acid graft copolymer provided by the present invention carries out a bulk prepolymerization reaction of lactide in a reactor and couples it with a twin-screw extruder for copolymerization. The reaction operation is simple and easy to industrialize.

[0077] Taking maleic anhydride and L-lactide as an example, the main reaction processes of steps (2) and (3) are shown in the following formulas (c) and (d):

[0078]

[0079]

[0080] In the above formulae (c) and (d), x and y represent the degree of polymerization of MA-LLA, y is greater than x, and z represents the number of moles.

[0081] The third aspect of the present invention provides a polylactic acid graft copolymer prepared by the above method.

[0082] The polylactic acid graft copolymer prepared by the above method has a right-angle tearing strength of 120-150 KN / m, an elongation at break of 30-45%, a glass transition temperature of 80-100°C, and a molecular weight of 1×10 5 -4×10 5 , the grafting rate is 40-50%.

[0083] The fourth aspect of the present invention provides a use of the polylactic acid graft copolymer described in the first aspect or the third aspect in the production of agricultural mulch films, food packaging materials and medical hygiene products.

[0084] The above-mentioned polylactic acid graft copolymer has a higher grafting rate, thereby having better flexibility and temperature resistance while ensuring a higher molecular weight, and can therefore be better used in the production of agricultural mulch films, food packaging materials and medical hygiene products.

[0085] The present invention will be described in detail below by way of examples. In the following examples, unless otherwise specified, all reagents used are commercially available products.

[0086] The following are the test methods for the performance parameters involved in the present invention:

[0087] (1) Grafting rate of grafted groups:

[0088] The grafting rate of the grafted groups in the polylactic acid graft copolymer was determined by a chemical titration method. Specifically, a certain mass of the polylactic acid graft copolymer was weighed and placed in a conical flask. A certain amount of tetrahydrofuran was added to dissolve it, and a small amount of thymol blue / DMF indicator was added dropwise. The mixture was titrated with an excess of 0.05 mol / L potassium hydroxide in ethanol and back-titrated with 0.01 mol / L HCl-isopropanol solution.

[0089] Grafting rate = n2 / n1×100%, n1 = (m0-m2) / M1, n2 = m2 / M2, that is, grafting rate = [(0.05V KOH -0.01V HCl )×2×M1] / [m0-(0.05V KOH -0.01V HCl)×2×M2]; where m0 is the mass of the weighed polylactic acid graft copolymer, in g; m2 is the total mass of the grafted groups on the polylactic acid molecular chain, calculated based on the consumed KOH; n1 is the degree of polymerization of polylactic acid, i.e., the amount of substance of the lactic acid unit, n2 is the amount of substance of the grafted groups on the polylactic acid molecular chain, M1 is the molar mass of lactic acid, M2 is the molar mass of the grafted groups, V KOH V is the volume of potassium hydroxide ethanol solution added, in mL; HCl The volume of HCl-isopropanol solution consumed in the titration, in mL.

[0090] (2) Right-angle tear strength and elongation at break: measured using a universal mechanical testing machine in accordance with GB / T1039-1992.

[0091] (3) Detection of terminal hydroxyl groups: Detected by phthalic anhydride method in accordance with GB / T 12008.3-2009.

[0092] (4) Glass transition temperature: measured using a differential scanning calorimeter (DSC) (DSC 204, NETZSCH, Germany). The test conditions are as follows: sample weight 5-10 mg, first heating the sample from room temperature to 200°C at a heating rate of 10°C / min, and isothermally maintaining the sample for 5 min to eliminate the thermal history; then rapidly cooling the sample to -20°C, and then heating it from -20°C to 200°C at a heating rate of 10°C / min; nitrogen was introduced as a protective gas throughout the test, and the nitrogen flow rate was set at 50 mL / min.

[0093] (5) Polymer weight-average molecular weight: The molecular weight of the polylactic acid graft copolymer samples was characterized by gel permeation chromatography (GPC) using a Waters 1515 system. Chromatographically pure THF was used as the mobile phase at a flow rate of 1.0 ml / min and a column temperature of 35°C. Prior to testing, the sample was dissolved in THF at a concentration of 5 mg / mL and filtered through a polytetrafluoroethylene (PTFE) membrane with a pore size of 0.22 μm before injection. Calibration was performed using a narrow distribution polystyrene (PS) standard.

[0094] Example 1

[0095] (1) L-lactide and maleic anhydride were added to a reactor, and dicumyl peroxide (DIPO) was added as an initiator. A nucleophilic addition reaction was carried out at a constant temperature under a nitrogen flow and vacuum conditions. The reaction temperature for the nucleophilic addition reaction was 105°C, the reaction pressure was 45 kPa, the reaction time was 3.5 h, and the nitrogen flow rate was 2 m / s. The amount of maleic anhydride added was 155 wt% of the amount of L-lactide used, and the amount of dicumyl peroxide added was 0.7 wt% of the amount of L-lactide used.

[0096] (2) The L-lactide that did not participate in the nucleophilic addition reaction in step (1) was removed by vacuum distillation to obtain a purified nucleophilic addition product; the vacuum distillation temperature was 130° C., the pressure was 25 kPa, and the time was 3.5 hours. The purified product was determined by chromatographic analysis to be maleic anhydride-grafted L-lactide (MA-LLA).

[0097] (3) The maleic anhydride grafted L-lactide (MA-LLA) obtained in step (2) is subjected to a ring-opening polymerization reaction in the presence of a catalyst and an initiator under a nitrogen flow atmosphere, and low-temperature prepolymerization is performed to obtain a ring-opening polymerization product: MA-LLA oligomer. The ring-opening polymerization reaction temperature is 140° C., the reaction time is 4.5 hours, the reaction pressure is 350 kPa, and the nitrogen flow rate is 3.5 m / s. The amount of the catalyst stannous octoate added is 0.75 wt% of the amount of MA-LLA used; the amount of the initiator triphenylphosphine added is 0.35 wt% of the amount of MA-LLA used. The weight average molecular weight of the MA-LLA oligomer is 5500.

[0098] (4) The MA-LLA oligomer obtained in step (3) and an antioxidant are added to a twin-screw extruder, subjected to high-temperature reactive mixing, causing the MA-LLA oligomer to undergo a chain growth reaction, and extruded into pellets to obtain a polylactic acid graft copolymer: a maleic anhydride grafted polylactic acid copolymer material (MA-PLLA). The amount of the antioxidant triphenyl phosphite added is 0.65 wt% of the amount of the MA-LLA oligomer, based on the weight of the MA-LLA oligomer. The reaction extrusion temperature of the twin-screw extruder for reactive mixing and extrusion pelletization is 185° C., and the residence time of the material in the twin-screw extruder is 15 minutes.

[0099] Among them, the infrared spectra of L-lactide, maleic anhydride, and maleic anhydride-grafted lactide are shown in Figure 1a, b, and c, respectively; the infrared difference spectra of PLA, maleic anhydride, maleic anhydride-grafted polylactic acid (MAH-g-PLA), and maleic anhydride-grafted polylactic acid (MAH-g-PLA) and polylactic acid after subtraction are shown in Figure 2a, b, c, and d, respectively; the infrared difference spectra of L-lactide, maleic anhydride-grafted lactide 13 The CNMR spectra are shown in Figure 3a and b respectively; 13 The CNMR spectra are shown in Figure 4a and b respectively.

[0100] As can be seen from Figure 1, the infrared spectrum of maleic anhydride grafted lactide is at 3090 cm -1 The out-of-plane bending vibration peak of olefinic hydrogen of =CH appears at 1600cm -1 The stretching vibration peak of -C=C- appears at , indicating that maleic anhydride is successfully grafted onto lactide.

[0101] As can be seen from Figure 2, the infrared difference spectrum between MAH-g-PLA and pure PLA is at 1750 cm -1 The absorption peak of C=O group appears at 1190cm -1 、1130cm -1 and 1093cm -1 The absorption peak of COC appears at ; compared with PLA, the absorption peaks of carbonyl and ether bonds in the infrared spectrum of MAH-g-PLA are enhanced, indicating that MAH is successfully grafted onto the PLA macromolecular chain.

[0102] Comparing Figure 3 a and b, it can be seen that the peaks of two carbon atoms in the anhydride group are increased at the chemical shifts of 70 ppm and 18 ppm, indicating that maleic anhydride is successfully grafted onto L-lactide.

[0103] Comparing Figure 4 a and b, it can be seen that there is a peak of anhydride carbon atoms at a chemical shift of 169 ppm, and a peak of carbon atoms after the breakage of the maleic anhydride carbon-carbon double bond at a chemical shift of 72 ppm, indicating that MAH was successfully grafted onto the PLA macromolecular chain.

[0104] The presence of terminal hydroxyl groups was determined by chemical titration.

[0105] Example 2-Example 11

[0106] A polylactic acid graft copolymer was prepared according to a procedure similar to that of Example 1, with the differences being the reaction conditions, types of materials, and amounts of materials added. See Table 1 for details.

[0107] Example 12

[0108] A polylactic acid graft copolymer was prepared according to the method of Example 1, except that the conditions for the nucleophilic addition reaction were: 170° C. and a reaction pressure of 5 kPa.

[0109] Example 13

[0110] A polylactic acid graft copolymer was prepared according to the method of Example 1, except that the amount of maleic anhydride added was 310 wt % of the amount of L-lactide used, and the amount of dicumyl peroxide added was 6 wt % of the amount of L-lactide used.

[0111] Example 14

[0112] A polylactic acid graft copolymer was prepared according to the method of Example 1, except that the amount of stannous octoate catalyst added in the ring-opening polymerization reaction was 5 wt% of the amount of the nucleophilic addition product; and the amount of triphenylphosphine initiator added was 5 wt% of the amount of the nucleophilic addition product.

[0113] Example 15

[0114] A polylactic acid graft copolymer was prepared according to the method of Example 1, except that the amount of antioxidant added in the chain growth reaction was 5 wt % of the amount of the ring-opening polymerization product; and the ring-opening polymerization reaction temperature was 250° C.

[0115] Example 16

[0116] A polylactic acid graft copolymer was prepared according to the method of Example 1, except that maleic anhydride was replaced by methyl methacrylate.

[0117] Example 17

[0118] A polylactic acid graft copolymer was prepared according to the method of Example 1, except that L-lactide in the nucleophilic addition reaction was replaced by D-lactide.

[0119] Comparative Example 1

[0120] The polylactic acid graft copolymer is prepared by first polymerizing L-lactide and then grafting it according to the existing technology:

[0121] (1) L-lactide (LLA) is prepolymerized at low temperature in the presence of a catalyst and an initiator under a nitrogen flow and negative pressure to obtain LLA oligomers. The reaction temperature for the low temperature prepolymerization is 130° C., the reaction time is 3 hours, the reaction pressure is 300 kPa, the flow rate of the nitrogen flow is 3 m / s, and the amount of the catalyst, stannous octoate, added is 0.5 wt% of the amount of LLA used; and the amount of the initiator, triphenylphosphine, added is 0.2 wt% of the amount of LLA used.

[0122] (2) adding the LLA oligomer prepared in step (1) into a twin-screw extruder for polymerization reaction, and simultaneously adding maleic anhydride (MA) and an antioxidant, and reactively mixing and extruding and granulating at high temperature to finally obtain a maleic anhydride grafted polylactic acid material (MA-PLLA); based on the weight of the LLA oligomer, the amount of maleic anhydride added is 2.5wt% of the amount of the LLA oligomer, the amount of the antioxidant triphenyl phosphite added is 0.5wt% of the amount of the LLA oligomer, and the reaction extrusion temperature of the twin-screw extruder for reactive mixing and extrusion granulation is 180°C.

[0123] The presence of terminal hydroxyl groups could not be detected by chemical titration.

[0124] Comparative Example 2

[0125] The polymer was prepared using the method disclosed in Example 1 of CN 104371082 A.

[0126] In a high-pressure reactor, 30 g of lactide, 3 g of maleic anhydride, 9 mg of stannous octoate, 3 mg of benzoyl peroxide and 50 ml of toluene were added, nitrogen was introduced for 5 minutes to remove oxygen, and the mixture was reacted at 200° C. under sealed conditions for 20 hours. The mixture was then cooled with water, the autoclave was opened, and the solution was poured into a portion of anhydrous methanol. The unreacted substances were removed by stirring, and the mixture was then filtered. The powder obtained by filtration was vacuum dried to obtain a polylactic acid modified with maleic anhydride without discoloration.

[0127] The presence of terminal hydroxyl groups was determined by chemical titration.

[0128] Comparative Example 3

[0129] The polymer was prepared by the method disclosed in Example 1 of CN 104371082 A, except that the amount of maleic anhydride added was 140 wt % of the amount of L-lactide used.

[0130] The presence of terminal hydroxyl groups was determined by chemical titration.

[0131] Table 1

[0132]

[0133]

[0134] Table 1

[0135]

[0136]

[0137] Table 2

[0138]

[0139]

[0140] As can be seen from Table 2, by adopting the method disclosed in the present invention, by carrying out the grafting reaction of the grafting group before the polymerization of lactide, the grafting efficiency is greatly improved, the toughness, elongation at break and glass transition temperature of the polylactic acid material are improved, and the obtained grafted modified polylactic acid copolymer material is green and fully biodegradable.

[0141] The preferred embodiments of the present invention have been described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, various simple variations of the technical solution of the present invention can be made, including combining the various technical features in any other appropriate manner. These simple variations and combinations should also be regarded as the contents disclosed by the present invention and fall within the scope of protection of the present invention.

Claims

1. A polylactic acid graft copolymer, characterized in that: The polylactic acid graft copolymer contains repeating structural units of the structure represented by formula (A); Among them, R 1 is H or a grafted group, and at least part of the R 1 The polylactic acid graft copolymer has a right-angle tearing strength of not less than 120 kN / m, preferably 135-150 kN / m; and an elongation at break of not less than 30%, preferably 35-45%.

2. The polylactic acid graft copolymer according to claim 1, wherein The content of the grafted group is 1 The content is 10 mol% or more of the total amount, preferably 30 mol% or more, and more preferably 40 mol% or more.

3. The polylactic acid graft copolymer according to claim 1 or 2, wherein The grafted group is a structure represented by formula (I) and / or formula (II), Wherein, R1, R2, R3, R4, and R5 are each independently hydrogen, a C1-C4 substituted or unsubstituted alkyl group, and R6 is a C1-C6 substituted or unsubstituted alkyl group, or a C6-C20 aryl group.

4. The polylactic acid graft copolymer according to any one of claims 1 to 3, wherein The polylactic acid graft copolymer 13 CNMR showed peaks at chemical shifts of 169 ppm and 72 ppm.

5. The polylactic acid graft copolymer according to any one of claims 1 to 4, wherein The weight average molecular weight of the polylactic acid graft copolymer is 1×10 5 -4×10 5 .

6. The polylactic acid graft copolymer according to any one of claims 1 to 5, wherein The polylactic acid graft copolymer has a glass transition temperature of 80-100°C.

7. The polylactic acid graft copolymer according to any one of claims 1 to 6, wherein The polylactic acid graft copolymer was found to contain terminal hydroxyl groups by the phthalic anhydride method.

8. A method for preparing a polylactic acid graft copolymer, characterized in that: The method comprises the following steps: (1) contacting lactide with a monomer represented by formula (i) and / or formula (ii) under nucleophilic addition reaction conditions to obtain a nucleophilic addition product; (2) under ring-opening polymerization conditions, mixing the nucleophilic addition product obtained in step (1) with a catalyst and an initiator, and performing low-temperature prepolymerization to obtain a ring-opening polymerization product; (3) subjecting the ring-opening polymerization product obtained in step (2) to high-temperature polymerization under chain growth reaction conditions in the presence of an antioxidant; Wherein, R1', R2', R3', R4', and R5' are each independently hydrogen, a C1-C4 substituted or unsubstituted alkyl group, and R6' is a C1-C6 substituted or unsubstituted alkyl group, or a C6-C20 aryl group.

9. The preparation method according to claim 8, wherein The nucleophilic addition reaction in step (1) is carried out in the presence of an initiator; Preferably, the initiator is dicumyl peroxide and / or 2,5-dimethyl-2,5-bis-(tert-butylperoxy)hexane.

10. The preparation method according to claim 9, wherein The amount of the initiator added is 0.1-5 wt % of the amount of the lactide, preferably 0.5-2 wt %.

11. The preparation method according to any one of claims 8 to 10, wherein The conditions of the nucleophilic addition reaction include: reaction temperature of 50-150° C., reaction pressure of 2-100 kPa, and reaction time of 0.5-10 h.

12. The preparation method according to any one of claims 8 to 11, wherein The total amount of the monomers represented by formula (i) and formula (ii) added is 100-300 wt %, preferably 150-200 wt %, of the amount of lactide used.

13. The preparation method according to any one of claims 8 to 12, wherein: The method further comprises removing the lactide that has not participated in the nucleophilic addition reaction by means of reduced pressure distillation after step (1), and then subjecting the obtained product to the reaction described in step (2); Preferably, the conditions for the reduced pressure distillation include: temperature of 100-200° C., pressure of 0-100 kPa, and time of 1-10 h.

14. The preparation method according to any one of claims 8 to 13, wherein: The catalyst in step (2) is selected from at least one of stannous octoate, zinc lactate, trialkylaluminum, triisobutylaluminum and stannous chloride; Preferably, the amount of the catalyst added is 0.1-5 wt%, preferably 0.5-2 wt%, of the total weight of the nucleophilic product; and / or, the initiator is selected from at least one of glycerol, xylitol, ethylene glycol and triphenylphosphine; Preferably, the amount of the initiator added is 0.05-5 wt%, preferably 0.3-2 wt%, of the total weight of the nucleophilic product.

15. The preparation method according to any one of claims 8 to 14, wherein: The conditions for the ring-opening polymerization reaction in step (2) include: reaction temperature of 100-150° C., reaction pressure of 100-1000 kPa, and reaction time of 2-15 h.

16. The preparation method according to any one of claims 8 to 15, wherein: The antioxidant in step (3) is selected from at least one of phosphites, alkyl polyphenols and thiobisphenol antioxidants; Preferably, the antioxidant is added in an amount of 0.1-5 wt%, preferably 0.5-2 wt%, based on the total weight of the ring-opening polymerization product.

17. The preparation method according to any one of claims 8 to 16, wherein: The temperature of the chain extension reaction in step (3) is 140-250°C, preferably 160-200°C.

18. The preparation method according to any one of claims 8 to 17, wherein: The step (3) is carried out in a twin-screw extruder.

19. A polylactic acid graft copolymer prepared by the preparation method according to any one of claims 8 to 18.

20. Use of the polylactic acid graft copolymer according to any one of claims 1 to 7 and claim 19 in the production of agricultural mulch films, food packaging materials and medical hygiene products.

Citation Information

Cited By

  • Modified polylactic acid oligomer as well as preparation method and application thereof

    CN120590279A