Amorphous copolycarbonates having phenolic structural units
Through the transesterification process, amorphous copolycarbonate was prepared by combining with m, m-bisphenol of lignin, which solved the crystallization trend and production problems of polycarbonate in the prior art, and realized the application and industry in standard processes Large-scale production improves the processability and stability of the product.
Patent Information
- Application Number
- CN202380035864.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-27
- Filing Date
- 2023-04-20
- Publication Date
- 2024-12-03
AI Technical Summary
The prior art is difficult to produce amorphous polycarbonate based on natural and renewable resources, and it is difficult to produce on an industrial scale, difficult to use in standard extrusion or injection molding processes, and there is a crystallization trend and high reactivity problem.
Amorphous copolycarbonate was obtained by using at least one comonomer and m,m-bisphenol from lignin by transesterification process, and a simple dropping solution was applied to the solution for production through the standard transesterification process of bisphenol A, which achieved the Economic and eco-friendly craftsmanship on industrial scale.
The obtained copolycarbonate has a reasonable molecular weight, is soluble in common solvents, is suitable for standard extrusion or injection molding processes, avoids crystallization shrinkage, and has a single peak molecular weight distribution, improving the predictability of processing and stability of properties.
Smart Images

Figure BDA0005098007610000041 
Figure BDA0005098007610000081 
Figure BDA0005098007610000101
Abstract
Description
[0001] The present invention relates to an amorphous copolycarbonate comprising specific phenolic structural units and at least one further aliphatic or aromatic structural unit different from the first, a molding material comprising the copolycarbonate, a molded article comprising the copolycarbonate, and a process for preparing an amorphous copolycarbonate comprising specific phenolic structural units and at least one further aliphatic or aromatic structural unit different from the first.
[0002] Polycarbonates, in particular aromatic polycarbonates, are known to exhibit a good profile of properties in terms of mechanical and optical properties, heat resistance and weathering resistance. Due to this profile of properties, they are used in a variety of indoor and outdoor applications. Typically, polycarbonates are prepared by an interphase phosgenation process or a melt transesterification process.
[0003] Lignocellulosic biomass has been recognized as having potential use in the production of chemicals and biomaterials. It contains cellulose, hemicellulose and lignin. Lignin is a highly cross-linked macromolecule consisting of different types of substituted phenols. The corresponding processing of lignin can provide various bisphenols, so lignin is expected to become a potential substitute for compounds used in petrochemicals, but based on natural and renewable sources at an affordable cost.
[0004] Some studies have been conducted focusing on the provision of bisphenols from lignin. For example, WO2019 / 002503A1 describes a method for producing o-alkoxybisphenols, which can be used as starting products for the preparation of biopolymers. The document mentions the reaction of these bisphenol compounds with phosgene or diaryl carbonates to form polycarbonates. However, no such reaction was performed in the experimental part.
[0005] WO2018 / 134427A1 relates to the production of high-purity meta, meta-coupled bis(4-alkylphenol) derivatives from lignin-derived sources. The resulting bisphenols are said to be useful monomers for the production of polycarbonates, in particular using phosgene or diphenyl carbonate. However, polycarbonates are not prepared in this document either.
[0006] In CN 105461912 A, the reaction of certain bisphenols with triphosgene is described.
[0007] WO 2015 / 183892 A1 describes the synthesis of novel reactive functionalized phenolic building blocks. The synthesis of bisguaiacol polycarbonate is described in Example 46. Bisguaiacol F is reacted with nitrochloroformate in acetonitrile.
[0008] WO2015 / 168225A2 describes the reaction of alkoxy bisphenols to polycarbonates by interphase phosgenation. In Example 5 of this document, a polycarbonate based on 4,4'-(2,2'-isopropylidene-bis(o-methoxy)phenol (PBMP) is prepared using interphase phosgenation and p-cumylphenol as a capping agent. This document mentions that alkoxy bisphenols exhibit a half-maximal inhibitory concentration (IC ) of less than 0.00025 M for α or β in vitro estradiol receptors. 50 ) of the additional monomers.
[0009] As can be seen from the prior art cited above, the skilled person knows how to prepare specific bisphenols from lignin. In the examples of those documents, clear indications of the facts on how to prepare these bisphenols can be found. In order to provide bisphenols from lignin, those examples are incorporated herein by reference. In particular, Green Chem., 2017, 19, 2561-2570 shows how to prepare 5,5'-methylenebis(4-n-propylguaiacol), 5,5'-methylenebis(4-ethylguaiacol) and 5,5'-methylenebis(4-methylguaiacol).
[0010] Furthermore, in this paper, polycarbonates are prepared using triphosgene via a standard laboratory-scale procedure. The polycarbonate obtained from m,m'-bis(4-methylguaiacol) is reported to be highly crystalline and quasi-insoluble despite its good thermal properties. It is only soluble in hexafluoroisopropanol. In contrast, commercial bisphenol A-based polycarbonates are amorphous and are well known for their optical transparency. In order to counteract the crystallization tendency, the structure of the bisphenols from lignin is altered to inhibit alignment and promote the desired disorder and entanglement of the polycarbonate chains. It was found that polycarbonates from m,m'-bis(4-ethylguaiacol) indeed exhibit a lower crystallization tendency than the corresponding methyl bisphenol, while m,m'-bis(4-n-propylguaiacol) even has a low crystallization tendency. Moreover, in CHCl 3 The solubility in , DCM and THF also improved. However, with increasing alkyl chain length, the glass transition temperature decreased, but in all cases the melting temperature was still measurable, indicating that the resulting polycarbonates were still semi-crystalline despite the reduced crystallization tendency. In addition, for polycarbonates based on m,m'-bis(4-n-propylguaiacol) and m,m'-bis(4-ethylguaiacol), a bimodal molecular weight distribution was reported. This may indicate that a large amount of oligomeric structures are still present in the resulting polycarbonates. It can be seen that the specific meta, meta-bisphenol does not show high reactivity in the polymerization.
[0011] Commercial amorphous bisphenol A-based polycarbonates are generally used to obtain molded articles by extrusion or injection molding. For both processes, the fact that polycarbonate is amorphous is beneficial because there is no need to consider crystallization shrinkage. The term "crystallization shrinkage" is well known to those skilled in the art. Preferably, it refers to the fact that the formation of crystals when cooling the polymer melt leads to shrinkage after molding. If the polymer is amorphous, this situation can be avoided. Crystalline polymers can also be used for extrusion or injection molding processes, but the crystallization shrinkage of the final shape and volume of the molded article needs to be considered. Therefore, crystalline polymers cannot be simply used in standard processes designed for amorphous polymers (such as bisphenol A-based polycarbonates). However, since the use of amorphous polymers in such processes is prior art, it is not possible to simply replace bisphenol A-based polycarbonates with crystalline polycarbonates based on bisphenols from lignin.
[0012] Based on this prior art, it is necessary to provide and prepare polycarbonates based at least in part on natural and renewable resources. In addition, it is necessary to provide such amorphous and / or common solvent-soluble polycarbonates. In addition, it would be advantageous to prepare such polycarbonates on an industrial scale. In addition, such polycarbonates should exhibit properties comparable to standard bisphenol A-based polycarbonates on the market (e.g., regarding solubility, processing properties, mechanical properties, and optical properties, especially xanthochromia). In addition, it would be beneficial if polycarbonates could be easily (e.g., without many adjustments) used in standard extrusion or injection molding processes designed for bisphenol A-based polycarbonates. Finally, it would be desirable to have an efficient, economical, and ecologically advantageous method for preparing such polycarbonates.
[0013] The present invention has addressed at least one, and preferably all, of the above objects.
[0014] Surprisingly, the inventors have found that when at least one comonomer (aliphatic or aromatic) is used together with m,m-bisphenol from lignin in an ester exchange process, an amorphous copolycarbonate can be obtained. In addition, due to the fact that it contains m,m-bisphenol from lignin, the resulting copolycarbonate contains at least some structure based on natural and renewable resources. Therefore, the ester exchange process itself seems to be particularly suitable for polymerizing non-reactive meta, meta-bisphenols, but only if comonomers are used in addition. In addition, due to the fact that the copolymerization effect using the ester exchange method is good, the copolycarbonate of the present invention can be produced on an industrial scale. It can even be produced by a simple drop-in solution using the standard ester exchange process of bisphenol A. Therefore, this leads to an economically and ecologically favorable process. Copolycarbonates with reasonable molecular weights are obtained. Such a molecular weight is reasonable because the copolycarbonates of the present invention can be used in many applications. This is particularly true because the copolycarbonates obtained are soluble in common solvents such as THF, CHCl even at room temperature.3 And / or dichloromethane. In addition, since the copolycarbonate is amorphous, the copolycarbonate can be easily used (e.g., without many adjustments) in standard extrusion or injection molding processes designed for bisphenol A-based polycarbonates. Using the copolycarbonate according to the present invention in such standard extrusion or injection molding processes provides an advantage method over using crystalline / semi-crystalline homopolycarbonates as disclosed in Green Chem. 2017, 19, 2561. The energy required to melt the copolycarbonates of the present invention is less because they do not show a melting temperature. Therefore, less energy is required to obtain molded articles. In addition, the copolycarbonate of the present invention has a unimodal molecular weight distribution. This is beneficial because this can explain why the copolycarbonate obtained does not show a melting temperature. In addition, the properties of such polymers with a unimodal weight distribution (when compared with a bimodal weight distribution) are easier to handle and predict.
[0015] The present invention therefore provides an amorphous copolycarbonate comprising at least one structural unit (A) and at least one aliphatic or aromatic unit (B)
[0016]
[0017] in
[0018] Each X in the structural unit (A) independently represents a single bond, -O-, -S-, -S(O)-, -S(O)- 2 -, -C(O)- or an organic group having 1 to 18 carbon atoms, wherein the organic group having 1 to 18 carbon atoms may be linear, branched or cyclic, aromatic or non-aromatic, and may further contain heteroatoms such as halogen, oxygen, nitrogen, sulfur, silicon or phosphorus,
[0019] R 1 and R 3 Each independently represents a monovalent hydrocarbon group, preferably C 1 -C 26 -alkyl, C 7 -C 26 Alkyl aryl or C 7 -C 26 -aralkyl,
[0020] R 2 and R 4 Each independently represents a hydrogen atom, an alkoxy group or a monovalent hydrocarbon group, preferably a hydrogen atom, C 1 -C 6 -alkoxy or C 1 -C 6 -alkyl,
[0021] p and q are each independently 1 or 2, preferably 1, and
[0022] n represents the average number of repeating units, wherein the molar ratio of structural unit (A) to structural unit (B) is 95:5 to 5:95.
[0023] According to the present invention, the term "amorphous" means that the copolycarbonate does not show a melting point, but only a glass transition temperature. The fact that the copolycarbonate shows a melting point can be determined, for example, by DSC. Preferably, the presence or absence of a melting point is determined by differential scanning calorimetry using ISO 11357-2:2013-05 at a heating rate of 10 ° C / min. More preferably, the upper temperature limit of the temperature range used in the DSC is at least 20 ° C higher than the melting point of all the corresponding monomers used. For example, the upper temperature limit of the temperature range used in the DSC is 350 ° C. This limit is particularly applicable to copolycarbonates based in particular on bisphenol A. Due to the fact that the copolycarbonates of the present invention are amorphous, the copolycarbonates can be used in standard extrusion or injection molding processes, which are usually designed for amorphous polymers that do not show crystallization shrinkage. Preferably, in such processes, the copolycarbonates of the present invention can simply replace other amorphous polymers in view of the glass transition temperature. Finally, since the copolycarbonates of the present invention do not show a melting temperature, the temperature used for extrusion or injection molding is lower than the temperature used for crystalline or semi-crystalline polymers.
[0024] The copolycarbonates of the present invention may be linear or branched, depending on the type of monomers used in the process of the present invention.
[0025] Preferably, the copolycarbonate according to the present invention is at least partially bio-based. For the purposes of the present invention, the expression "bio-based" is understood to mean that the relevant compound is available and / or obtainable via renewable and / or sustainable raw materials on the application date. Renewable and / or sustainable raw materials are preferably understood to mean raw materials that are regenerated by natural processes at a rate comparable to their consumption rate (see CEN / TS16295:2012). This expression is particularly used to distinguish it from raw materials produced from fossil raw materials (also referred to as fossil-based according to the present invention). As an example, most bisphenol A-based polycarbonates represent commonly known fossil-based polycarbonates. Whether a raw material is bio-based or fossil-based can be determined by measuring the carbon isotopes in the raw materials, because the carbon isotopes C in fossil raw materials are 14 The relative amount of is low. This can be done, for example, according to ASTM D6866-18 (2018) or ISO 16620-1 to -5 (2015) or DIN SPEC 91236 2011-07. Exemplary bio-based materials are bisphenols such as those obtained from lignin.
[0026] "Alkyl" in the context of the present invention, for example and if not mentioned otherwise, refers to an alkane structure from which one hydrogen atom has been removed. An "alkyl" according to the present invention, which may be linear or branched, is saturated and therefore contains only single bonds between adjacent carbon atoms. Preferably, the alkyl group according to the present invention comprises methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, n-pentyl, 1-methylbutyl, 2-methylbutyl, 3-methylbutyl, neopentyl, 1-ethylpropyl, n-hexyl, 1,1-dimethylpropyl, 1,2-dimethylpropyl, 1,2-dimethylpropyl, 1-methylpentyl, 2-methylpentyl, 3-methylpentyl, 4-methylpentyl, 1,1-dimethylbutyl, 1,2-dimethylbutyl, 1,3-dimethylbutyl, 2,2-dimethylbutyl, 2,3-dimethylbutyl, 3,3-dimethylbutyl, 1-ethylbutyl, 2-ethylbutyl, 1,1,2-trimethylpropyl, 1,2,2-trimethylpropyl, 1-ethyl-1-methylpropyl, 1-ethyl-2-methylpropyl, 1-ethyl-2-methylpropyl, and the like. In the case where the carbon atoms of the alkyl group are defined in various ways in the present invention, these structures may be limited in selection.
[0027] "Alkylene" in the context of the present invention, for example and if not mentioned otherwise, refers to a bridged alkane structure in which two hydrogen atoms are removed from different carbon atoms. In this context, the two carbon atoms from which the two hydrogen atoms are removed can be any carbon atoms present in the alkane structure. This means that the two carbon atoms can, but do not necessarily have to, be adjacent to each other. The alkylene structure can be straight or branched and is saturated. In the case where the alkylene contains only one carbon atom, the alkylene is a methylene group (-CH 2Preferably, the alkylene group according to the present invention comprises methylene, ethylene, n-propylene, isopropylene, n-butylene, sec-butylene, tert-butylene, n-pentylene, 1-methylbutylene, 2-methylbutylene, 3-methylbutylene, neopentylene, 1-ethylpropylene, n-hexylene, 1,1-dimethylpropylene, 1,2-dimethylpropylene, 1,2-dimethylpropylene, 1-methylpentylene, 2-methylpentylene, 3-methylpentylene, 4-methylpentylene, 1-ethylpropylene, 1 ...methylpentylene, 2-methylpentylene, 3-methylpentylene, 4-methylpentylene, 4-methylpentylene, 1-ethylpropylene, 1-ethylpropylene, 1-hexylene, 1,1-dimethylpropylene, 1,2-dimethylpropylene, 1 -methylpentylene, 1,1-dimethylbutylene, 1,2-dimethylbutylene, 1,3-dimethylbutylene, 2,2-dimethylbutylene, 2,3-dimethylbutylene, 3,3-dimethylbutylene, 1-ethylbutylene, 2-ethylbutylene, 1,1,2-trimethylpropylene, 1,2,2-trimethylpropylene, 1-ethyl-1-methylpropylene, 1-ethyl-2-methylpropylene, 1-ethyl-2-methylpropylene, etc. In the case where the present invention defines the carbon atoms of the alkylene in different ways, these structures may be limited in selection. In addition, the alkylene according to the present invention optionally contains at least one carbonyl group, optionally contains at least one halogen atom and / or is optionally interrupted by at least one heteroatom. Examples of such alkylenes are -C(=O)-(CH 2 ) 4 -C(=O)-, -C(=O)-(CH 2 ) 3 -C(=O)-, -C(=O)-(CH 2 ) 2 -C(=O)-, -C(CF 3 ) 2 、-O-(CH 2 ) 4 -O-, -O-(CH 2 ) 3 -O-, -O-(CH 2 ) 2 -O- etc.
[0028] "Alkylidene" in the context of the present invention, for example and if not mentioned differently, refers to a bridged alkane structure in which two hydrogen atoms are removed from the same carbon atom. Alkylidene optionally contains at least one carbon-carbon double bond, optionally contains at least one carbonyl group and / or optionally contains at least one halogen atom. Preferably, the alkylidene according to the present invention and / or in formula (3) contains CH 2 =C*, C(CH 3 ) 2 =C*, isopropylidene, n-propylidene, isoheptylidene, C*(CH 3 )(C(=O)CH3 )、C(Cl 2 )=C*、C(Br 2 )=C*, etc., wherein "C*" represents the carbon atom at the position indicated as "Z" in formula (3).
[0029] "Cycloalkylene" in the context of the present invention, for example and if not mentioned otherwise, refers to a bridged cycloalkane structure in which two hydrogen atoms are removed from different carbon atoms in the ring. In this context, the two carbon atoms from which the two hydrogen atoms are removed can be any carbon atoms present in the cycloalkane structure. This means that the two carbon atoms can, but do not necessarily have to, be adjacent to each other. According to the present invention, the alicyclic radical of the cycloalkylene is fused to at least one further alicyclic ring. An example of such a cycloalkylene is adamantylene (tricyclo[3.3.1.13,7]decanediyl).
[0030] "Cycloalkylidene" in the context of the present invention, for example and if not mentioned otherwise, refers to a bridged cycloalkane structure in which two hydrogen atoms are removed from the same carbon atom in the ring. The alicyclic radical of the cycloalkylidene is optionally fused with at least alicyclic and / or at least one aromatic ring. Examples of such cycloalkylidene are cyclopentylidene, cyclohexylidene, 3,3,5-trimethylcyclohexylidene, cyclodecylidene, cyclododecylidene, tetrahydrodicyclopentylidene, 9-fluorenylidene, etc.
[0031] "Aralkylidene" in the context of the present invention, for example and if not mentioned otherwise, refers independently in each case to a bridged linear, cyclic, branched or unbranched alkyl structure having two hydrogen atoms removed from the same carbon atom and mono-, multi- or polysubstituted by aryl groups. At the same time, "aralkylene" refers independently in each case to a bridged linear, cyclic, branched or unbranched alkyl structure having two hydrogen atoms removed from different carbon atoms and mono-, multi- or polysubstituted by aryl groups. "Aryl" in the context of the present invention, for example and if not mentioned otherwise, is a carbocyclic aromatic group. Examples of "aryl" are phenyl, o-, p-, m-tolyl, naphthyl, phenanthrenyl or anthracenyl. In particular in the context of formula (3), examples of such aralkylidene groups are phenyl-CH*, phenyl-C*(CH 3 ), naphthyl-CH*, phenyl-C*-phenyl, etc., wherein "C*" represents the carbon atom at the position indicated as "Z" in formula (3). Examples of such aralkylene groups are m-diisopropylidene phenylene and p-diisopropylidene phenylene.
[0032] "Arylalkyl" in the context of the present invention, for example and if not mentioned otherwise, may be an aryl group as defined above having an alkyl, alkynyl or alkenyl group attached to an aromatic group.
[0033] "Alkoxy" in the context of the present invention, for example and if not mentioned otherwise, refers to a straight-chain, cyclic or branched alkyl group (-OR) which is singly bonded to oxygen. Preferably, the alkoxy group according to the invention has 1 to 6 carbon atoms and thus includes methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, sec-butoxy, tert-butoxy, n-pentoxy, 1-methylbutoxy, 2-methylbutoxy, 3-methylbutoxy, neopentoxy, 1-ethylpropoxy, cyclohexyloxy, cyclopentyloxy, n-hexyloxy, 1,1-dimethylpropoxy, 1,2-dimethylpropoxy, 1,2-dimethylpropoxy, 1-methylpentyloxy, 2-methylpentyloxy. In the case where the present invention defines the carbon atom of the alkoxy group in different ways, these structures may be limited in selection.
[0034] "Halogen atom" in the context of the present invention, if not mentioned otherwise, refers to fluorine (F), chlorine (Cl), bromine (Br) or iodine (I). Preferably, the halogen atom is F, Cl, Br or I, more preferably it is Cl or Br.
[0035] Based on the definitions given above, the skilled person knows how to understand additional definitions that are not explicitly defined in the above paragraphs.
[0036] The term "average number of repeating units" is known to the skilled person. The skilled person knows how to determine this parameter. Typically, it is determined by using a GPC method. Preferably, it is determined using a GPC method as outlined in the context of the present invention.
[0037] Preferably, each X in the structural unit (A) independently represents a substituted or unsubstituted C 3 -C 18 Cycloalkylidene; Formula—C(R c )(R d )—C 1 -C 18 Alkylene, where R c and R d are independently hydrogen, C 1 -C 12 Alkyl, C 1 -C 12 Cycloalkyl, C 7 -C 12 Arylalkyl, C1 -C 12 -heteroalkyl or cyclic C 7 -C 12 Heteroarylalkyl; or a c )—, wherein R c It is a two-price C 1 -C 12 Hydrocarbon.
[0038] More preferably, each X in the structural unit (A) independently represents a substituted or unsubstituted C 3 -C 18 Cycloalkylidene; Formula—C(R c )(R d )—C1-C18 alkylidene group, wherein R c and R d are independently hydrogen, C 1 -C 12 Alkyl, C 1 -C 12 Cycloalkyl, C 7 -C 12 Arylalkyl, C 1 -C 12 -heteroalkyl or cyclic C 7 -C 12 Heteroarylalkyl; or a c )—, wherein R c It is a two-price C 1 -C 12 Hydrocarbon,
[0039] R 1 and R 3 Each independently represents C 1 -C 26 -alkyl, C 7 -C 26 Alkyl aryl or C 7 -C 26 -aralkyl,
[0040] R 2 and R 4 Each independently represents a hydrogen atom, C 1 -C 6 -alkoxy or C 1 -C 6 -alkyl, and
[0041] p and q are each independently 1 and n represents the average number of repeating units.
[0042] More preferably, R in structural unit (A) 2 and R 4 Each is methyl, ethyl or propyl.
[0043] Even more preferably, the structural unit (A) is represented by formula (A1)
[0044]
[0045] Each X 1 Independently represents a straight or branched chain C 1 -C 10 -alkylidene or C 1 -C 10 -alkylene, preferably straight chain C 1 -C 4 -alkylene, or straight or branched C 1 -C 6 - alkylene, still more preferably methylene,
[0046] R 1 and R 3 Each independently represents C 1 -C 26 -alkyl, C 7 -C 26 -alkylaryl or C 7 -C 26 - aralkyl, preferably methyl, ethyl, propyl, octyl, isooctyl, benzyl, ethylphenyl, butylphenyl, propyldiphenyl or cyclohexylphenyl,
[0047] R 2 and R 4 Each independently represents a hydrogen atom, C 1 -C 6 -alkoxy or C 1 -C 6 -alkyl, preferably C 1 -C 4 -alkyl, still more preferably methyl, ethyl, propyl, most preferably methyl, still most preferably ethyl or still most preferably propyl, and
[0048] n represents the average number of repeating units.
[0049] More preferably, each X in formula (A1) 1 Independently represents the straight chain C 1 -C 4 -Alkyl or straight chain or branched C 1 -C 6 -alkylene, and even more preferably, each R 1 and R 3 independently represents a methyl group or an ethyl group,
[0050] R 2 and R 4 each independently represents a hydrogen atom, a methyl group, an ethyl group or a propyl group, and
[0051] n represents the average number of repeating units.
[0052] Preferably, X in structural unit (A) or X in structural unit (A1) 1 Can be substituted or unsubstituted C 3 -C 18 -cycloalkylidene; formula—C(R c )(R d )—C 1 -C 18 -alkylidene, where R c and R d are independently hydrogen, C 1 -C 12 -alkyl, C 1 -C 12 -cycloalkyl, C 7 -C 12 -Arylalkyl, C 1 -C 12 -heteroalkyl or cyclic C 7 -C 12 -heteroarylalkyl; or a group of formula -C(=R c )—, wherein R c It is a two-price C 1 -C 12 -hydrocarbon group. Preferably, R 1 and R 3 Each independently represents C 1 -C 26 -alkyl, C 7 -C 26 -alkylaryl or C 7 -C 26 -aralkyl. Even more preferably, R 1 and R 3 Each independently represents a methyl group, an ethyl group, a propyl group, an octyl group, an isooctyl group, a benzyl group, an ethylphenyl group, a butylphenyl group, a propyldiphenyl group or a cyclohexylphenyl group. 1 and R 3 Each is a methyl group.
[0053] Preferably, X in structural unit (A) or X in structural unit (A1) 1 represents methylene, cyclohexyl-methylene, 2-[2.2.1]-bicycloheptylidene, ethylene, isopropylidene, neopentylene, cyclohexylene, cyclopentadecylene, cyclododecylene or adamantylene. More preferably, X represents the formula—C(R c )(R d )—C 1 -C 18 -alkylidene, where Rc and R d are independently hydrogen, C 1 -C 12 -alkyl, C 1 -C 12 -cycloalkyl, C 7 -C 12 -Arylalkyl, C 1 -C 12 -heteroalkyl or cyclic C 7 -C 12 -heteroarylalkyl, preferably hydrogen or C 1 -C 12 -alkyl. Even more preferably, R c and R d are independently hydrogen or C 1 -C 6 -alkyl. Most preferably, R c is hydrogen and R d is methyl, ethyl, propyl or butyl. 1 and R 3 Each is a methyl group.
[0054] Preferably, R in structural unit (A) or (A1) 2 and R 4 Each independently represents a hydrogen atom, an alkoxy group or a monovalent hydrocarbon group, preferably a hydrogen atom, C 1 -C 6 -alkoxy or C 1 -C 6 -alkyl, even more preferably a hydrogen atom or a C 1 -C 4 -alkyl.
[0055] Preferably, p and q in the structural unit (A) or (A1) are each 1. In this case, it is most preferred that R 2 and R 4 Both are C 1 -C 4 -alkyl.
[0056] Preferably, each X in structural unit (A) or X in structural unit (A1) 1 Independent expression—C(R c )(R d )—C 1 -C 6 -alkylidene, where R c and R d are independently hydrogen or C 1 -C 5 -alkyl.
[0057] More preferably, each X in structural unit (A) or X in structural unit (A1) 1 Independent expression—C(R c )(R d )—C 1 -C 4 -alkylidene, where R c and R d are independently hydrogen or C 1 -C 3 -alkyl, preferably hydrogen
[0058] R 1 and R 3 each independently represents a methyl group or an ethyl group,
[0059] R 2 and R 4 Each independently represents a hydrogen atom, a methyl group, an ethyl group or a propyl group.
[0060] Preferably, the copolycarbonates of the invention are characterized in that the at least one aliphatic or aromatic unit (B) is selected from structural units of the formulae (3) to (10), wherein
[0061]
[0062] Wherein each Z in formula (3) independently represents a single bond, -S(=O) 2 -, -C(=O)-, -O-, -S-, -S(=O)-, -CH(CN)-, a straight or branched C 1 -C 6 -alkylene, optionally containing at least one carbon-carbon double bond, optionally containing at least one carbonyl group and / or optionally containing at least one halogen atom 2 -C 10 -alkylidene, C-alkylidene, wherein the alicyclic group is fused to at least one additional alicyclic ring 5 -C 12 -cycloalkylene, C-cycloalkylene, wherein the alicyclic group is optionally fused to at least one alicyclic and / or at least one aromatic ring 5 -C 15 -cycloalkylidene, C 7 -C 20 -Arylalkylidene, C 8 -C 20 -aralkylene, optionally fused to a further aromatic ring which may optionally contain at least one heteroatom 6 -C 12 -arylene group, formula (B1-A), formula (B1-B), formula (B1-C) or formula (B1-D)
[0063]
[0064] In formulas (B1-A), (B1-B) and (B1-C), each R' independently represents a linear C 1 -C 4 -Alkyl, branched C 3 -C 4 -alkyl, aralkyl or aryl, and "C*" represents a quaternary carbon atom at the position indicated as "Z" in formula (3), and
[0065] In formula (B1-D), each R' independently represents a linear C 1 -C 4 -Alkyl, branched C 3 -C 4 -alkyl, each R" independently represents a linear C 1 -C 4 -Alkylene, branched C 3 -C 4 -alkylene, each R"' independently represents H or a linear C 1 -C 3 -alkyl, s is 0 to 2, and each s1 is independently 0 or 1, and "*" represents a bond connecting "Z" to the aromatic ring in formula (3),
[0066] Each R 5 and R 6 Independently represent H, C 1 -C 18 -alkyl, C 5 -C 6 -cycloalkyl, C 1 -C 5 -alkenyl-, C 1 -C 18 -alkoxy, phenoxy, halogen atom, C 6 -C 18 -Aryl or C 7 -C 18 -aralkyl,
[0067] p1 and q1 are each 1 to 4, and
[0068] m2 represents the average number of repeating units;
[0069]
[0070] Wherein in formulas (4) to (6), m2 represents the average number of repeating units;
[0071]
[0072] Each Rx Independently represents a straight or branched chain C 1 -C 6 -alkyl, C 1 -C 12 -Aryl, C 1 -C 8 - an aralkyl group or a halogen atom, t is 0 to 4, and m2 represents the average number of repeating units;
[0073]
[0074] In formulae (8) and (9), each Y1 independently represents oxygen, sulfur or NR y , where R y is H or -CH 3 , each Y2 represents a single bond, oxygen, sulfur or NR as defined above y and m2 represents the average number of repeating units, and each R' in formula (8) independently represents a linear C 1 -C 4 -Alkyl, branched C 3 -C 4 -alkyl, aralkyl or aryl and s is 0 to 2;
[0075]
[0076] Where m3 represents the average number of repeating units.
[0077] The obtained polycarbonate is a copolycarbonate according to the present invention. It is understood by those skilled in the art that there may be overlap between the structures of the chemical formula (A) and the formula (3). However, according to the present invention, the expression "comprising at least one structural unit (A) and at least one aliphatic or aromatic unit (B)" is preferably understood to mean that the structure of the formula (A) needs to be compulsorily different from the structure of the formula (B). Only in this way can a copolycarbonate comprising two different structural units be obtained. Therefore, preferably, the structure of the chemical formula (A) is different from the structure of the chemical unit (B), especially the structure of the formula (3).
[0078] Preferably, the at least one aliphatic or aromatic unit (B) of the copolycarbonate of the present invention is selected from one of the structural units of the formulae (3), (4), (7) and (10),
[0079] Wherein each Z in formula (3) independently represents a single bond, -S(=O) 2 -, -C(=O)-, -O-, -S-, -S(=O)-, straight chain or branched chain C 1 -C 6 -alkylene, optionally containing at least one carbon-carbon double bond, C 2 -C 10-alkylidene, wherein the alicyclic group is optionally fused to at least alicyclic and / or at least one aromatic ring 5 -C 15 -cycloalkylidene, C 7 -C 15 -aralkylidene group, C of formula (B1-E) 8 -C 15 -Arylene
[0080]
[0081] In formula (B1-E), each R' independently represents a linear C 1 -C 4 -Alkyl, branched C 3 -C 4 Alkyl, each R" independently represents a straight chain C 1 -C 4 -Alkylene, branched C 3 -C 4 alkyl, s is 0 to 2, and each s1 is independently 0 or 1, and "*" represents a bond connecting "Z" to the aromatic ring in formula (3),
[0082] Formula (B1-A), Formula (B1-B), Formula (B1-C),
[0083] Each R 5 and R 6 Independently represent H, C 1 -C 18 -alkyl, C 5 -C 6 -cycloalkyl, C 1 -C 18 -alkoxy, phenoxy, C 6 -C 18 -Aryl or C 7 -C 18 -aralkyl,
[0084] p1 and q1 are each 1 to 4, and m2 represents the average number of repeating units.
[0085] Preferably, the polycarbonate of the present invention further comprises at least one structural unit selected from the structural units of formula (3), wherein each Z independently represents a single bond, C 2 -C 6 Alkylene, C 5 -C 12 Cycloalkylidene, wherein the alicyclic group is optionally fused to at least one aromatic ring,
[0086] Formula (B1-A), Formula (B1-B), Formula (B1-C),
[0087] Each R 5 and R 6 Independently represent H, C 1 -C 3 -alkyl, C 1 -C 18 - alkoxy,
[0088] p1 and q1 are each 1 to 4, and m2 represents the average number of repeating units.
[0089] More preferably, the at least one aliphatic or aromatic unit (B) is selected from the structural units of formula (3) or (10), wherein the structural unit of formula (3) is represented by at least one structural unit selected from the structural units of formulae (3a) to (3k).
[0090]
[0091] In formulae (3g), (3h) and (3i), R' represents a methyl group or a phenyl group.
[0092] Most preferably still, the at least one aliphatic or aromatic unit (B) is selected from structural units of formula (3b), (3f) or (10).
[0093] Structural units (A) and (B) list "n" and "m2" or "m3" as the number of repeating units. Preferably, the average sum of all ns and all m2s in a polymer chain of the copolycarbonate of the present invention is 20 to 80, more preferably 25 to 75, even more preferably 30 to 70, even more preferably 35 to 65, and most preferably 40 to 60. This does not mean that this copolycarbonate cannot contain any end groups or any other structures caused by impurities, etc. However, this copolycarbonate is basically composed of the structure of formula (A) and (B), and is composed of repeating units of only one type of structural units (A) and (B). The technician can convert this average sum of n and m2 into a number average molecular weight. Therefore, the technician can also calculate n and m2 based on the ratio of molecular weight and structural units (A) and (B).
[0094] According to the present invention, copolycarbonate preferably has a weight average molecular weight of 4000 g / mol to 50000 g / mol, preferably 8000 g / mol to 40000 g / mol, and more preferably 10000 g / mol to 35000 g / mol as determined by gel permeation chromatography using bisphenol A-polycarbonate calibration in dichloromethane. Preferably, the gel permeation chromatography is calibrated using bisphenol A polycarbonate and dichloromethane as eluents. Typically, linear polycarbonates (obtained from BPA and phosgene) with known molecular weight distribution of PSS Polymer Standards Service GmbH, Deutschland can be used for calibration. Most preferably, calibration is performed according to method 2301-0257502-09D (2009 German version) from Currenta GmbH & Co. OHG, Leverkusen. The eluent is dichloromethane. Preferably, a combination of columns based on crosslinked styrene divinylbenzene resins is used. More preferably, the diameter of the analytical column is 7.5 mm and the length is 300 mm. The particle size of the column material is preferably 3 μm to 20 μm. The concentration of the solution is preferably 0.2 wt %. The flow rate is preferably 1.0 ml / min. The temperature of the solution is preferably 30° C. Preferably, UV- and / or RI-detection is used. Preferably, the copolycarbonate of the present invention has a unimodal molecular weight distribution. This preferably means that the copolycarbonate of the present invention shows only one M at a GPC curve greater than 1000 g / mol. 峰 / has only one maximum value.
[0095] The weight average molecular weight as defined according to the invention ensures that the obtained copolycarbonate exhibits good mechanical properties in terms of tensile strength and processing parameters. It has been surprisingly found that the obtained tensile strength is comparable to that of bisphenol A based polycarbonates of comparable number average molecular weight. In addition, the fact that the copolycarbonate of the present invention preferably shows a unimodal molecular weight distribution indicates that the polymerization itself can be easily handled and the content of monomers and / or oligomers in the obtained copolycarbonate can be reduced. This is also conducive to the processing of the obtained copolycarbonate. This shows that the meta, meta-bisphenol from lignin can be polymerized as a drop solution in existing equipment, for example for the polymerization of bisphenol A by transesterification.
[0096] In particular, the glass transition temperature of the polycarbonate cocondensates of the present invention is above 100° C., preferably above 110° C., and more preferably above 112° C., most preferably above 130° C. This glass transition temperature ensures that the copolycarbonates of the present invention can be used for all applications in which BPA-based polycarbonates are also used. Preferably, the glass transition temperature can be determined by differential scanning calorimetry ISO 11357-2:2013-05 at a heating rate of 10° C. / min. It is known to those skilled in the art that the type of comonomer (structural unit (B)) has an influence on the resulting glass transition temperature.
[0097] The molar ratio of the structural unit (A) to the structural unit (B) of the copolycarbonate is 95:5 to 5:95, preferably 75:25 to 8:92, more preferably 71:29 to 9:91, even more preferably 60:40 to 10:90, even more preferably 50:50 to 11:89, even more preferably 40:60 to 12:88, and most preferably 30:70 to 15:85. Compared with the prior art, the molar ratio range of the structural unit (A) to the structural unit (B) can be widely selected. For short alkyl chains (X in formula (A) is methylene), the situation remains the same. Preferably, the molar ratio of structural units (A) and (B) can be determined by total hydrolysis. Preferably, the respective copolycarbonates are subjected to complete hydrolysis to form corresponding degradation products, which are the corresponding monomer structural units (A) and (B). The ratio of those degradation products can be determined by 1 H-NMR or HPLC determination, the latter can be achieved, for example, as follows: A sample of the copolycarbonate is hydrolyzed under reflux with the aid of sodium methoxide. The corresponding solution is acidified and concentrated to dryness. The dry residue is dissolved in acetonitrile and the phenolic compounds are determined by means of HPLC with UV detection.
[0098] According to the invention, the resulting properties can be fine-tuned by selecting the molar ratio of structural units (A) and (B). However, in order for the copolycarbonate to have a high content of bio-based structural units, it is preferred to have a high content of structural units (A).
[0099] Preferably, the copolycarbonate of the present invention comprises at least 30 wt. %, more preferably at least 60 wt. %, even more preferably at least 80 wt. %, and most preferably at least 90 wt. % of the sum of the structural units (A) and (B), wherein the wt. % are based on the total weight of the copolycarbonate. Most preferably, the copolycarbonate consists essentially of the structural units (A) and (B) or consists of the structural units (A) and (B). Obviously, the term "consisting of" in this case does not include the terminal groups that are additionally present.
[0100] In another aspect of the present invention, a molding compound is provided, which is included in the copolycarbonate of the present invention provided in each definition given as above. By adding other thermoplastic polymers and / or additives, such molding compounds can be obtained. In addition, another aspect of the present invention provides a molded article, which is included in the copolycarbonate of the present invention provided in each definition given as above. Such molded articles can be obtained by methods known to those skilled in the art, such as extrusion, injection molding, blow molding or thermoforming of sheets or plates. As mentioned above, the copolycarbonate of the present invention provides a more ecological method for preparing molded articles because it is amorphous. In addition, the copolycarbonate of the present invention can be used in standard methods and equipment that already exist and are used for, for example, BPA-based polycarbonates. Preferably, the molded article of the present invention is obtained by extrusion or injection molding.
[0101] In another aspect of the present invention, a method is provided, which produces an amorphous copolycarbonate comprising the structural unit (A) as defined above. Preferably, the method of the present invention obtains the copolycarbonate of the present invention in each of the definitions given as described above. This means that, in particular, the molecular weight of the copolycarbonate as defined above can be obtained by the method of the present invention.
[0102] Therefore, a method for preparing an amorphous copolycarbonate is provided, characterized in that:
[0103] (I) 5 to 95 mol % of at least one diol of formula (1)
[0104]
[0105] in
[0106] Each X independently represents a single bond, -O-, -S-, -S(O)-, -S(O)2-, -C(O)-, or an organic group having 1 to 18 carbon atoms, wherein the organic group having 1 to 18 carbon atoms may be cyclic or acyclic, aromatic or non-aromatic, and may further contain heteroatoms such as halogen, oxygen, nitrogen, sulfur, silicon or phosphorus,
[0107] R 1 and R 3 Each independently represents a monovalent hydrocarbon group, preferably C 1 -C 26 Alkyl, C 7 -C 26 Alkyl aryl or C 7 -C 26 Aralkyl, and
[0108] R 2 and R 4 Each independently represents a hydrogen atom, an alkoxy group or a monovalent hydrocarbon group, preferably a hydrogen atom, C 1-C 6 -alkoxy or C 1 -C 6 -alkyl, and
[0109] p and q are each independently 1 or 2, preferably 1, and
[0110] (II) 95 to 5 mol % of at least one aromatic or aliphatic diol, wherein the mol % is based on the sum of (I) and (II)
[0111] (I) and (II) in the melt
[0112] (III) at least one diaryl carbonate of formula (2)
[0113]
[0114] Where R 5 and R 6 Each independently represents H, C 1 -C 34 -alkyl, C 7 -C 34 -Arylalkyl, C 6 -C 34 -aryl or -COO-R', where R' represents C 1 -C 34 -alkyl, C 7 -C 34 -aralkyl or C 6 -C 34 -aryl, and
[0115] r and s represent 1 to 5, respectively.
[0116] Preferably, for the diol of formula (1)
[0117] Each X independently represents a substituted or unsubstituted C 3 -C 18 Cycloalkylidene; Formula—C(R c )(R d )—C 1 -C 18 Alkylene, where R c and R d are independently hydrogen, C 1 -C 12 Alkyl, C 1 -C 12 Cycloalkyl, C 7 -C 12 Arylalkyl, C 1 -C 12 -heteroalkyl or cyclic C 7 -C 12Heteroarylalkyl; or a c )—, wherein R c It is a two-price C 1 -C 12 Hydrocarbon;
[0118] R 1 and R 3 Each independently represents C 1 -C 26 -alkyl, C 7 -C 26 Alkyl aryl or C 7 -C 26 -aralkyl,
[0119] R 2 and R 4 Each independently represents a hydrogen atom, C 1 -C 6 -alkoxy or C 1 -C 6 -alkyl, and p and q are each independently 1.
[0120] Preferably, X in formula (1) can be substituted or unsubstituted C 3 -C 18 -cycloalkylidene; formula—C(R c )(R d )—C 1 -C 18 -alkylidene, where R c and R d are independently hydrogen, C 1 -C 12 -alkyl, C 1 -C 12 -cycloalkyl, C 7 -C 12 -Arylalkyl, C 1 -C 12 -heteroalkyl or cyclic C 7 -C 12 -heteroarylalkyl; or a group of formula -C(=R c )—, wherein R c It is a two-price C 1 -C 12 -hydrocarbon group. Preferably, R 1 and R 3 Each independently represents C 1 -C 26 -alkyl, C 7 -C 26 -alkylaryl or C 7 -C 26 -aralkyl. Even more preferably, R 1and R 3 Each independently represents a methyl group, an ethyl group, a propyl group, an octyl group, an isooctyl group, a benzyl group, an ethylphenyl group, a butylphenyl group, a propyldiphenyl group or a cyclohexylphenyl group. 1 and R 3 Each is a methyl group.
[0121] Preferably, X in formula (1) represents methylene, cyclohexyl-methylene, 2-[2.2.1]-bicycloheptylidene, ethylidene, isopropylidene, neopentylidene, cyclohexylidene, cyclopentadecylidene, cyclododecylidene or adamantylidene. More preferably, X represents the formula—C(R c )(R d )—C 1 -C 18 -alkylidene, where R c and R d are independently hydrogen, C 1 -C 12 -alkyl, C 1 -C 12 -cycloalkyl, C 7 -C 12 -Arylalkyl, C 1 -C 12 -heteroalkyl or cyclic C 7 -C 12 -heteroarylalkyl, preferably hydrogen or C 1 -C 12 -alkyl. Even more preferably, R c and R d are independently hydrogen or C 1 -C 6 -alkyl. Most preferably, R c is hydrogen and R d is methyl, ethyl, propyl or butyl. 1 and R 3 Each is a methyl group.
[0122] Preferably, R in formula (1) 2 and R 4 Each independently represents a hydrogen atom, an alkoxy group or a monovalent hydrocarbon group, preferably a hydrogen atom, C 1 -C 6 -alkoxy or C 1 -C 6 -alkyl, even more preferably a hydrogen atom or a C 1 -C 4 -alkyl.
[0123] Preferably, p and q in formula (1) are each 1. In this case, it is most preferred that R 2 and R 4 Both are C1 -C 4 -alkyl.
[0124] Preferably, each X in formula (1) independently represents the formula: c )(R d )—C 1 -C 6 -alkylidene, where R c and R d are independently hydrogen or C 1 -C 5 -alkyl.
[0125] More preferably, each X in the structural unit (A) in formula (1) independently represents the formula—C(R c )(R d )—C 1 -C 4 -alkylidene, where R c and R d are independently hydrogen or C 1 -C 3 -alkyl, preferably hydrogen
[0126] R 1 and R 3 each independently represents a methyl group or an ethyl group,
[0127] R 2 and R 4 Each independently represents a hydrogen atom, a methyl group, an ethyl group or a propyl group.
[0128] Preferably, the process according to the invention is characterized in that at least one aromatic or aliphatic diol (II) is selected from structural units of the formulae (III) to (X), wherein
[0129] Wherein in formula (III), Z, R 5 , R 6 , p1 and q1 are each defined as in formula (3),
[0130]
[0131] Wherein each R in formula (VII) x and each t is defined as in equation (7),
[0132] Wherein in formula (VIII), Y1, Y2, R' and s are each as defined in formula (8),
[0133] Wherein in formula (IX), Y1 and Y2 are each as defined in formula (9),
[0134]
[0135] A person skilled in the art will be able to see the relationship between the above diols and the respective structures of formulae (3) to (10). A person skilled in the art will therefore also be able to transfer all the preferences given for the copolycarbonates of the invention to the diols shown above.
[0136] Most preferably, the process according to the invention is characterized in that the at least one aromatic or aliphatic diol (II) is bisphenol A or isosorbide.
[0137] In the method of the present invention, a diaryl carbonate of formula (2) is used. Preferably, in formula (2), R 5 and R 6 Each independently represents H, C 1 -C 10 -alkyl, C 7 -C 15 -Arylalkyl, C 6 -C 12 -aryl or -COO-R', where R' represents C 1 -C 5 -alkyl, C 7 -C 12 -aralkyl or C 6 -C 12 -aryl and R and s each represent 1 to 3. More preferably, the diaryl carbonate of formula (2) is selected from diphenyl carbonate, 4-tert-butylphenyl carbonate, di-(4-tert-butylphenyl) carbonate, biphenyl-4-ylphenyl carbonate, di-(biphenyl-4-yl)-carbonate, 4-(1-methyl-1-phenylethyl)-phenyl-phenyl carbonate and di-[4-(1-ethyl-1-phenylethyl)-phenyl]-carbonate.
[0138] Preferably, in the process of the present invention, the molar ratio of the diaryl carbonate of formula (2) to the sum of the diol of formula (1) and at least one aromatic or aliphatic diol is from 1.01 to 1.09, preferably from 1.03 to 1.07.
[0139] The method of the present invention is characterized in that the reaction is carried out in the melt. This preferably means that the process is carried out at a temperature above the melting / glass transition temperature of all educts and products. Those skilled in the art know how to carry out this process in the melt (so-called melt transesterification). For example, it is described in "Schnell", Chemistry and Physics of Polycarbonates, Polymer Reviews, Vol. 9, Interscience Press, New York, London, Sydney 1964, DC Prevorsek, BT Debona and Y. Kersten, Corporate Research Center, Allied Chemical Corporation, Moristown, New Jersey 07960, "Synthesis of Poly (ester) Carbonate Copolymers" in Journal of Polymer Science, Polymer Chemistry Edition, Vol. 19, 75-90 (1980), in D. Freitag, U. Grigo, PR M ü ller, N. Nouvertne, BAYER AG, "Polycarbonates" in Encyclopedia of Polymer Science and Engineering, Volume 11, 2nd edition, 1988, pages 648-718, and finally in Dr. U. Grigo, K. Kircher and PRMüller "Polycarbonate" in Becker / Braun, Kunststoff-Handbuch [Plastics Handbook], Volume 3 / 1, Polycarbonate, Polyacetale, Polyester, Celluloseester [Polycarbonates, polyacetals, polyesters, cellulose esters], Carl Hanser Verlag, Munich, Vienna 1992, pages 117-299.
[0140] The preparation of certain copolycarbonates by melt transesterification is generally more economical than by interphase phosgenation, since these products are smaller in volume. In addition, educts (e.g. phosgene) requiring special handling can be avoided. Finally, polymerization by melt transesterification does not require the use of solvents, so that the purification requirements of the resulting products are lower.
[0141] In the melt transesterification, the reactants are preferably melted under reduced pressure. Depending on the equipment configuration, atmospheric pressure, preferably a mild vacuum, i.e. an absolute pressure below 200 mbar, particularly preferably 100-200 mbar, and most preferably less than 100 mbar, can be applied during the melting stage. However, the reactants can also be melted at standard pressure, preferably under a protective gas atmosphere, such as nitrogen. The melting is preferably carried out at a temperature in the range of 175 to 400° C., more preferably in the range of 180 to 350° C., most preferably in the range of 185 to 320° C. For the reaction or condensation stage, the above-mentioned temperatures and pressures apply. Preferably, the values given above are valid for the aromatic or aliphatic diol (II) being bisphenol A. However, a person skilled in the art is able to adjust the corresponding parameters according to the melting temperature of the diol (II) used.
[0142] To carry out the process according to the invention, it is possible, for example, to use an apparatus design as shown in WO-A 02 / 077067.
[0143] According to the present invention, the method is preferably carried out in the absence of an additional organic solvent. Therefore, the method according to the present invention can preferably be carried out in the absence of a solvent. According to the present invention, this does not exclude the possibility that the used diaryl carbonate and the condensation product formed in the reaction can be present in these reaction steps as a solvent (if possible). This is especially true if the used carbonate is in excess relative to the stoichiometric amount of diols. This preferred method variant is particularly gentle. However, according to the present invention, it is preferred not to add an additional organic solvent to the method. Due to the absence of an additional organic solvent, the method can be carried out advantageously and in an environmentally friendly manner.
[0144] The diols of formula (1) and diols (I) and (II) can be reacted using at least one catalyst according to the method of the present invention. In principle, a reaction mode without using a catalyst is possible, but the result may have to accept higher temperatures and longer residence times. Preferably, the method of the present invention is characterized in that the reaction is carried out in the presence of at least one catalyst selected from ammonium catalysts, phosphonium catalysts and organic bases. The technician can consider the reactivity of the monomers used to select the correct catalyst.
[0145] Catalysts suitable for the process according to the invention are for example
[0146] Ammonium catalysts, such as tetramethylammonium hydroxide, tetramethylammonium acetate, tetramethylammonium fluoride, tetramethylammonium tetraphenylborate, dimethyldiphenylammonium hydroxide, tetraethylammonium hydroxide, hexadecyltrimethylammonium tetraphenylborate and hexadecyltrimethylammonium phenolate. Particularly suitable are phosphonium catalysts of formula (K):
[0147]
[0148] Where R a , R b , R c And R d Can be the same or different C 1 -C 10 -alkyl, C 6 -C 14 -Aryl, C 7 -C 15 -aralkyl or C 5 -C 6 -cycloalkyl, preferably methyl or C 6 -C 14 -aryl, particularly preferably methyl or phenyl, and X- may be an anion such as hydroxide, sulfate, bisulfate, bicarbonate, carbonate or a halide, preferably chloride or an alkylate or arylate of the formula -OR, wherein R may be C 6 -C 14 -Aryl, C 7 -C 15 -Arylalkyl or C 5 -C 6 - Cycloalkyl, preferably phenyl.
[0149] Preferably, the organic base is a tertiary nitrogen base. More preferably, it is selected from a base derived from guanidine, 4-dimethylaminopyridine (DMAP), 1,8-diazabicyclo[5.4.0]undec-7-ene, 1,5-diazabicyclo[4.3.0]non-5-ene, 1,5,7-triazabicyclo[4.4.0]dec-5-ene, hexamethylphosphoramidite triamide, 1,2-dimethyl-1,4,5,6-tetrahydropyridine, 7-methyl-1,5,7-triheterobicyclodec-5-ene, 1,8-diheterobicyclo[5.4.0]undec-7-ene (DBU), DBN, ethylimidazole, N,N-diisopropylethylamine (Hünig base), pyridine, TMG and a mixture of these substances. Further preferably, the catalyst is selected from bases derived from guanidine, 4-dimethylaminopyridine (DMAP), 1,8-diazabicyclo[5.4.0]undec-7-ene, 1,5-diazabicyclo[4.3.0]non-5-ene and 1,5,7-triazabicyclo[4.4.0]dec-5-ene. Particular preference is given to using 4-dimethylaminopyridine.
[0150] Particularly preferred catalysts are tetraphenylphosphonium hydroxide, 4-dimethylaminopyridine and phenoxytetraphenylphosphonium, with phenoxytetraphenylphosphonium being very particularly preferred. Particular preference is given to using alkali metal or alkaline earth metal salts of the ammonium and / or phosphonium catalysts mentioned.
[0151] The amount of the catalyst is preferably 1 to 10 moles based on 1 mole of the sum of all diols. -8 mole, preferably 10-8 Up to 10 -3 mole, particularly preferably 10 -7 Up to 10 -4 Moore.
[0152] The catalysts can be used individually or as catalyst mixtures and can be added in pure form or as a solution, for example in water or in phenol (for example as a solid solution with phenol).
[0153] In the process of the present invention, the molar ratio of (I) at least one diol of the formula (1) to (II) at least one aromatic or aliphatic diol is from (I) 5 to 95 mol % and (II) 95 to 5 mol %, preferably from (I) 75 to 8 mol % and (II) 25 to 92 mol %, more preferably from (I) 71 to 9 mol % and (II) 29 to 91 mol %, still more preferably from (I) 60 to 10 mol % and (II) 40 to 90 mol %, still more preferably from (I) 50 to 11 mol % and (II) 50 to 89 mol %, still more preferably from (I) 40 to 12 mol % and (II) 60 to 88 mol %, and most preferably from (I) 30 to 15 mol % and (II) 70 to 85 mol %, based on the sum of (I) and (II). Example
[0154] Size exclusion chromatography was performed using a PSS SECurity System; polycarbonate calibration (according to method 2301-0257502-09D of Currenta GmbH & Co. OHG, Leverkusen), dichloromethane as eluent, column 1 (PL-PC5), concentration 2 g / l, flow rate 1.0 ml / min, at a temperature of 30°C, using UV and / or RI detection.
[0155] The glass transition temperature (Tg) and the melting temperature (Tm) present were determined by DSC at a heating rate of 10°C / min using ISO 11357-2:2013-05. The glass transition temperature represents the onset temperature of the second heating at 10°C / min measured on a Mettler Toledo DSC. In the case of the copolymerization of BPL and BPA, the temperature was raised to 350°C. When a temperature limit of 350°C was used, decomposition was observed in the case of the copolymerization of BPL and ISB. Therefore, in this case, the upper temperature limit was set to 250°C.
[0156] BPL1: 5,5'-methylenebis(4-ethylguaiacol)
[0157] BPL2: 5,5'-methylenebis(4-methylguaiacol)
[0158] BPL3: 5,5'-methylenebis(4-n-propylguaiacol)
[0159] BPA: Bisphenol A
[0160] ISB: (3R,3aR,6S,6aR)-Hexahydrofuran[3,2-b]furan-3,6-diol (isosorbide)
[0161] Embodiment of the present invention - copolymerization of BPL and BPA
[0162] Copolycarbonates are prepared by transesterification of diphenyl carbonate.
[0163] Example 3: 0.5623 g of diphenyl carbonate, 0.34 g of BPA and 0.3164 g of BPL1 were mixed with 2.8 μl of tetraphenylphosphine phenolate solution (5 wt % TPPP, 5 wt % demineralized water and 90 wt % phenol) and subjected to intermittent transesterification under mechanical stirring (stirrer: homemade drill bit form).
[0164] Raise the temperature using a heat block and gradually increase the vacuum level as follows:
[0165] 1. Step (45 minutes): 210°C, atmospheric pressure
[0166] 2. Step (15 minutes): 240°C, 100 mbar absolute pressure
[0167] 3. Step (10 minutes): 270°C, 50 mbar absolute pressure
[0168] 4. Step (10 minutes): 280°C, 25 mbar absolute pressure
[0169] 5. Step (20 minutes): 300°C, 4 mbar absolute pressure
[0170] 6. Step (30 minutes): 300°C, absolute pressure <1 mbar
[0171] The results of this polymerization are summarized in Table 1. Comparative Example 1, Inventive Examples 2 and 4 were performed in the same manner except that the ratio of BPA and BPL1 was varied as shown in Table 1.
[0172] Table 1:
[0173]
[0174] *) Since a catalyst is added to the phenol-containing solution, a small amount of phenol is always present.
[0175] From the results in Table 1, it can be seen that the reaction of monomer BPL and monomer BPA produces a copolymer with a high molecular weight. As the BPA content increases, the molecular weight also increases. However, it can be seen that with a high content of BPL, a reasonable molecular weight can still be obtained.
[0176] Furthermore, all the obtained polymers were soluble in dichloromethane (eg, for measuring GPC, the samples were completely soluble) and THF. The GPC curve was unimodal at molecular weights > 1000 g / mol.
[0177] Embodiment of the present invention - copolymerization of BPL and ISB
[0178] Example 6: 0.675 g of diphenyl carbonate, 0.263 g of ISB, 0.346 g of BPL2 and 1.4 μl of 4-(dimethylamino)pyridine solution (5 wt % DMAP, 5 wt % deionized water and 90 wt % phenol) were melted together in an alkali-free glass flask and subjected to intermittent transesterification reaction under mechanical stirring. The temperature was raised and the vacuum degree was gradually increased as shown below:
[0179] 1. Step (45 minutes): 210°C, atmospheric pressure
[0180] 2. Step (15 minutes): 240°C, 100 mbar absolute pressure
[0181] 3. Step (10 minutes): 260°C, 50 mbar absolute pressure
[0182] 4. Step (10 minutes): 260°C, 25 mbar absolute pressure
[0183] 5. Step (20 minutes): 260°C, 4 mbar absolute pressure
[0184] 6. Step (30 minutes): 270°C, absolute pressure <1 mbar
[0185] The results of this polymerization are summarized in Table 2. Inventive Examples 5 and 7 were carried out in the same manner except that the ratio of ISB and BPL2 was varied as shown in Table 2.
[0186] Table 2:
[0187]
[0188] *) Since a catalyst is added to the phenol-containing solution, a small amount of phenol is always present.
[0189] Table 2 shows the same trend as with BPA as a comonomer. The lower the amount of BPL2, the higher the molecular weight obtained. However, the resulting polymers exhibit high glass transition temperatures while having reasonable molecular weights.
[0190] Furthermore, all the obtained polymers were soluble in dichloromethane (eg, for measuring GPC, the samples were completely soluble) and THF. The GPC curve was unimodal at molecular weights > 1000 g / mol.
[0191] Example: BPL Homopolymerization via LPC and SPC
[0192] LPC process:
[0193] BPL1, BPL2 and BPL3 were used for homopolymerization using interphase phosgenation (LPC process) respectively. The reaction was carried out in a micro glass batch reactor. The corresponding bisphenol (0.5 g) was added to deionized water dissolved with NaOH (2.0 mol NaOH per mol bisphenol) to obtain a 2.0 wt% bisphenol solution. Subsequently, dichloromethane was added to the bisphenol solution in an amount calculated to obtain a 2 wt% solution. The micro glass reactor was sealed and placed in an ice water bath, and the magnetic stirrer was set to a fixed speed to form an oil-in-water dispersion. Phosgene was added to the stirred solution in a semi-batch feed using a mass flow meter. 1.30 mol phosgene was added per mol bisphenol to ensure complete conversion of the bisphenol. Five minutes after the completion of the phosgene addition, 0.0274 mol p-tert-butylphenol per mol bisphenol was added as a chain terminator, and then NaOH was added to reach a pH of 11. After a reaction time of 30 minutes, 0.015 mol N-ethylpiperidine per mol bisphenol was added. It is normal for the pH to drop during the post-reaction time. After a post-reaction time of 30 minutes, the phases are separated. The organic phase is washed once with 10% HCl and then three times with deionized water. The polymer is dried overnight in a vacuum oven at 60° C. and 20 mbar. It is already clear at this point that no high molecular weight polymer has been formed.
[0194] The results are summarized in Table 3. GPCs were performed in dichloromethane using PC calibration. When the reaction product was dissolved in dichloromethane, no visible insoluble residue was found.
[0195] Table 3:
[0196] Bisphenol <![CDATA[M w (g / mol)]]> Tg(℃) Comparative Example 2 BPL1 -* 109.7 Comparative Example 3 BPL2 1,883 125.4 Comparative Example 4 BPL3 1,300 72.8
[0197] *No reaction occurred because BPL1 is not soluble in water or dichloromethane.
[0198] From the results in Table 3, it can be seen that no polymer can be obtained by homopolymerizing meta-, meta-BPLs using the LPC process.
[0199] SPC process:
[0200] Reference Example 1: 0.3599 g of diphenyl carbonate, 0.5062 g of BPL1 and 0.6 μl of tetraphenylphosphonium phenol (TPPP) solution (5.57 wt % TPPP, 5 wt % demineralized water and 90 wt % phenol) were melted in an alkali-free glass test tube and subjected to intermittent transesterification. The test tube was connected to a distillation bridge, which was connected to a conical column. The temperature was increased and the vacuum was gradually increased as shown below:
[0201] 1. Step (85 minutes): 228°C, atmospheric pressure
[0202] 2. Step (15 minutes): 250°C, 140 mbar absolute pressure
[0203] 3. Step (15 minutes): 266°C, 51 mbar absolute pressure
[0204] 4. Step (15 minutes): 283°C, 25 mbar absolute pressure
[0205] 5. Step (30 minutes): 297°C, 3.6 mbar absolute pressure
[0206] 6. Step (40 minutes): 296°C, absolute pressure <1 mbar
[0207] The resulting mixture was analyzed (it was removed from the test tube and dried using dichloromethane). Table 4 summarizes the results.
[0208] Reference Example 2: 0.3936 g of diphenyl carbonate, 0.5046 g of BPL2 and 0.6 μl of tetraphenylphosphonium phenol (TPPP) solution (5.57 wt % TPPP, 5 wt % demineralized water and 90 wt % phenol) were melted in an alkali-free glass test tube and subjected to intermittent transesterification. The test tube was connected to a distillation bridge, which was connected to a conical column. The temperature was increased and the vacuum was gradually increased as shown below:
[0209] 1. Step (80 minutes): 219°C, atmospheric pressure
[0210] 2. Step (15 minutes): 225°C, 900 mbar absolute pressure
[0211] 3. Step (15 minutes): 241°C, 194 mbar absolute pressure
[0212] 4. Step (15 minutes): 258°C, 99 mbar absolute pressure
[0213] 5. Step (15 minutes): 275°C, 52 mbar absolute pressure
[0214] 6. Step (15 minutes): 289°C, 25 mbar absolute pressure
[0215] 7. Step (30 minutes): 296°C, 3.8 mbar absolute pressure
[0216] 8. Step (45 minutes): 296°C, absolute pressure <1 mbar
[0217] The resulting mixture was analyzed (it was removed from the test tube with dichloromethane and dried). The results are summarized in Table 4. The polymers obtained were insoluble in dichloromethane. Therefore, they were dissolved in hexafluoroisopropanol and GPCs were performed using PMMA calibration.
[0218] Table 4:
[0219] Bisphenol <![CDATA[M w (g / mol)**]]> Reference Example 1 BPL1 21,890 Reference Example 2 BPL2 24,090
[0220] **Absolute values are similar to those given in other experiments above. W Not comparable (here: GPC calibrated with HFIP and PMMA)
[0221] As can be seen from Table 4 above, the SPC process is able to homopolymerize bisphenol lignin-based monomers. However, the resulting homopolymers are insoluble in common solvents commonly used in the context of polycarbonates, such as methylene chloride. This appears to be due to the fact that the resulting homopolymers are crystalline. The use of comonomers in the process of the present invention provides soluble amorphous copolycarbonates containing a large amount of bisphenol lignin-based structural units.
Claims
1. An amorphous copolycarbonate comprising at least one structural unit (A) and at least one aliphatic or aromatic unit (B) in Each X in the structural unit (A) independently represents a single bond, -O-, -S-, -S(O)-, -S(O)- 2 -, -C(O)- or an organic group having 1 to 18 carbon atoms, wherein the organic group having 1 to 18 carbon atoms may be linear, branched or cyclic, aromatic or non-aromatic, and may further contain heteroatoms such as halogen, oxygen, nitrogen, sulfur, silicon or phosphorus, R 1 and R 3 Each independently represents a monovalent hydrocarbon group, preferably C 1 -C 26 Alkyl, C 7 -C 26 Alkyl aryl or C 7 -C 26 Aralkyl, R 2 and R 4 Each independently represents a hydrogen atom, an alkoxy group or a monovalent hydrocarbon group, preferably a hydrogen atom, C 1 -C 6 -alkoxy or C 1 -C 6 -alkyl, and p and q are each independently 1 or 2, preferably 1, and n represents the average number of repeating units, wherein the molar ratio of structural unit (A) to structural unit (B) is 95:5 to 5:
95.
2. The amorphous copolycarbonate according to claim 1, It is characterized in that The at least one aliphatic or aromatic unit (B) is selected from structural units of formulae (3) to (10), wherein wherein each Z independently represents a single bond, -S(=O) 2 -, -C(=O)-, -O-, -S-, -S(=O)-, -CH(CN)-, a straight or branched C 1 -C 6 -alkylene, optionally containing at least one carbon-carbon double bond, optionally containing at least one carbonyl group and / or optionally containing at least one halogen atom 2 -C 10 -alkylidene, C-alkylidene, wherein the alicyclic group is fused to at least one additional alicyclic ring 5 -C 12 -cycloalkylene, C-cycloalkylene, wherein the alicyclic group is optionally fused to at least one alicyclic and / or at least one aromatic ring 5 -C 15 -cycloalkylidene, C 7 -C 20 -Arylalkylidene, C 8 -C 20 -aralkylene, optionally fused to a further aromatic ring which may optionally contain at least one heteroatom 6 -C 12 -arylene group, formula (B1-A), formula (B1-B), formula (B1-C) or formula (B1-D) In formulas (B1-A), (B1-B) and (B1-C), each R' independently represents a linear C 1 -C 4 -Alkyl, branched C 3 -C 4 -alkyl, aralkyl or aryl, and "C*" represents a quaternary carbon atom at the position indicated as "Z" in formula (3), and In formula (B1-D), each R' independently represents a linear C 1 -C 4 -Alkyl, branched C 3 -C 4 -alkyl, each R" independently represents a linear C 1 -C 4 -Alkylene, branched C 3 -C 4 -alkylene, each R"' independently represents H or a linear C 1 -C 3 -alkyl, s is 0 to 2, and each s1 is independently 0 or 1, and "*" represents the bond connecting "Z" to the aromatic ring in formula (3), R 5 and R 6 Each independently represents H, C 1 -C 18 -alkyl, C 5 -C 6 -Cycloalkyl, C 1 -C 5 -alkenyl-, C 1 -C 18 -alkoxy, phenoxy, halogen atom, C 6 -C 18 -Aryl or C 7 -C 18 -aralkyl, p1 and q1 are each 1 to 4, and m2 represents the average number of repeating units; Wherein in formulas (4) to (6), m2 represents the average number of repeating units; Among them, each R x independently represent a straight or branched chain C 1 -C 6 -alkyl, C 1 -C 12 -Aryl, C 1 -C 8 - an aralkyl group or a halogen atom, t is 0 to 4, and m2 represents the average number of repeating units; Wherein, in formula (8) and (9), each Y1 independently represents oxygen, sulfur or NR y , where R y H or -CH 3 , each Y2 independently represents a single bond, oxygen, sulfur or NR as defined above y , and m2 represents the average number of repeating units, and in formula (8), each R' independently represents a linear C 1 -C 4 -Alkyl, branched C 3 -C 4 -alkyl, aralkyl or aryl, and s is 0 to 2; Where m3 represents the average number of repeating units.
3. The amorphous copolycarbonate according to claim 1 or 2, It is characterized in that The molar ratio of structural unit (A) to structural unit (B) is 75:25 to 8:92, preferably 71:29 to 9:
91.
4. The amorphous copolycarbonate according to any one of claims 1 to 3, It is characterized in that In the structural unit (A) Each X independently represents a substituted or unsubstituted C 3 -C 18 -cycloalkylidene; formula—C(R c )(R d )—C 1 -C 18 -alkylidene, where R c and R d are independently hydrogen, C 1 -C 12 -alkyl, C 1 -C 12 -Cycloalkyl, C 7 -C 12 -Arylalkyl, C 1 -C 12 -heteroalkyl or cyclic C 7 -C 12 -heteroarylalkyl; or a group of formula -C(=R c )—, wherein R c It is a two-price C 1 -C 12 - Hydrocarbyl.
5. The amorphous copolycarbonate according to any one of claims 1 to 4, It is characterized in that The structural unit (A) is represented by the formula (A1): Each X 1 Independently represents a straight or branched chain C 1 -C 10 -alkylidene or C 1 -C 10 -alkylene, preferably straight chain C 1 -C 4 -Alkylene or branched C 1 -C 6 - alkylene, R 1 and R 3 Each independently represents C 1 -C 26 -alkyl, C 7 -C 26 -alkylaryl or C 7 -C 26 - aralkyl, preferably methyl, ethyl, propyl, octyl, isooctyl, benzyl, ethylphenyl, butylphenyl, propyldiphenyl or cyclohexylphenyl, R 2 and R 4 Each independently represents a hydrogen atom, C 1 -C 6 -alkoxy or C 1 -C 6 -alkyl, preferably C 1 -C 4 -alkyl, and n represents the average number of repeating units.
6. The amorphous copolycarbonate according to claim 5, It is characterized in that In formula (A1) Each X 1 Independently represents the straight chain C 1 -C 4 -alkylidene or straight or branched chain C 1 -C 6 -alkylene, R 1 and R 3 each independently represents a methyl group or an ethyl group, R 2 and R 4 each independently represents a hydrogen atom, a methyl group, an ethyl group or a propyl group, and n represents the average number of repeating units.
7. The amorphous copolycarbonate according to any one of claims 2 to 6, It is characterized in that The at least one aliphatic or aromatic unit (B) is selected from the structural units of formula (3) or (10), wherein the structural unit of formula (3) is represented by at least one structural unit selected from the structural units of formulae (3a) to (3k) In formulae (3g), (3h) and (3i), R' represents a methyl group or a phenyl group. 8 . A molding compound comprising the amorphous copolycarbonate according to claim 1 .
9. A molded article comprising the amorphous copolycarbonate according to any one of claims 1 to 7.
10. The molded article according to claim 9, It is characterized in that The molded article is obtained by extrusion or injection molding.
11. A method for preparing an amorphous copolycarbonate, Features: (I) 5 to 95 mol % of at least one diol of formula (1) in Each X independently represents a single bond, -O-, -S-, -S(O)-, -S(O) 2 -, -C(O)- or an organic group having 1 to 18 carbon atoms, wherein the organic group having 1 to 18 carbon atoms may be cyclic or acyclic, aromatic or non-aromatic, and may further contain heteroatoms such as halogen, oxygen, nitrogen, sulfur, silicon or phosphorus, R 1 and R 3 each independently represents a monovalent hydrocarbon group, and R 2 and R 4 each independently represents a hydrogen atom, an alkoxy group or a monovalent hydrocarbon group, p and q are each independently 1 or 2, and (II) 95 to 5 mol % of at least one aromatic or aliphatic diol, wherein the mol % is based on the sum of (I) and (II) (I) and (II) in the melt (III) at least one diaryl carbonate of formula (2) Where R 5 and R 6 Each independently represents H, C 1 -C 34 -alkyl, C 7 -C 34 -Arylalkyl, C 6 -C 34 -aryl or -COO-R', where R' represents C 1 -C 34 -alkyl, C 7 -C 34 -aralkyl or C 6 -C 34 -aryl, and r and s represent 1 to 5, respectively.
12. The method according to claim 11, It is characterized in that The at least one aromatic or aliphatic diol (II) is selected from structural units of formulae (III) to (X), wherein Wherein, Z and R in formula (III) 5 , R 6 , p1 and q1 are each as defined in formula (3) of claim 2, Wherein each R in formula (VII) x and each t is defined as in formula (7) of claim 2, Wherein in formula (VIII), Y1, Y2, R' and s are each as defined in formula (8) of claim 2, wherein in formula (IX), Y1 and Y2 are each as defined in formula (9) of claim 2, and 13. The method according to claim 12, It is characterized in that The at least one aromatic or aliphatic diol (II) is bisphenol A or isosorbide.
14. The method according to any one of claims 11 to 13, It is characterized in that The reaction is carried out in the presence of at least one catalyst selected from the group consisting of an ammonium catalyst, a phosphonium catalyst and an organic base.
15. The method according to any one of claims 11 to 14, It is characterized in that Based on the sum of (I) and (II), 75 to 8 mol % of (I) and 25 to 92 mol % of (II) are used, preferably 71 to 9 mol % of (I) and / or 29 to 91 mol % of (II).
Citation Information
Patent Citations
Preparation method of bio-based bisphenol or polycarbonate material
CN105461912A
Method for producing polycarbonates
WO2002077067A2
Alkoxy polycarbonates, bisphenol monomers and methods of making and using the same
WO2015168225A2
Bisphenol alternatives derived from renewable susbstituted phenolics and their industrial application
WO2015183892A1
Production of highly pure meta,meta-coupled BIS(4-alkylphenol) derivatives and uses thereof
WO2018134427A1