Surface activation of silicones
By introducing amino groups on the silicone surface using primary or secondary amino silanizing reagents, the problem that the surface of silicone materials is easily colonized by bacteria and fungi, simplifying the modification process and improving the antibacterial performance, and suitable for various silicones Materials, including filler reinforcement types.
Patent Information
- Application Number
- CN202380029140.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-21
- Filing Date
- 2023-03-21
- Publication Date
- 2024-12-03
AI Technical Summary
The hydrophobic surface of silicone materials is prone to colonization of bacteria and fungi and biofilm formation, leading to contamination problems in the medical and food fields. The existing modification methods require pre-oxidation treatment and the efficacy of antibacterial agents decreases over time.
Using a method that does not require pre-oxidation treatment, a silanizing reagent of primary or secondary amino groups and nucleophilic groups is used for silicone surface treatment, amino groups are introduced for further modification, and a mild condition and environmentally friendly solvent is used, which is suitable for various Such silicone surfaces include materials with mineral fillers.
The effective introduction of amino groups to the silicone surface without pre-oxidation treatment is achieved, simplifies the modification process, improves the antibacterial properties of the surface, and can be further modified in subsequent steps to enhance biocompatibility and function.
Smart Images

Figure BDA0005052235370000011 
Figure BDA0005052235370000041 
Figure BDA0005052235370000051
Abstract
Description
Technical Field
[0001] The field of the present invention relates to silicone chemistry, and in particular to the surface modification of silicones to introduce amino groups which can further react with desired substituents. Background Art
[0002] Silicones, also known as polysiloxanes, are a class of synthetic polymers consisting of an "inorganic" backbone of alternating silicon and oxygen atoms and two organic side chains attached to the silicon atoms. The most common type is PDMS (polydimethylsiloxane; Formula I). Formula I shows a description of the basic PDMS structure (note that the terminal Si atom can have one or more -OH groups instead of methyl groups in some cases). Silicones are chemically and thermally stable and are widely used in insulators, packaging, building materials, cosmetics, drug delivery systems, and medical devices. Silicones come in a variety of different forms, including elastomers, gels, lubricants, foams, and adhesives. Liquid silicone rubbers and elastomers can be made from linear polymers by crosslinking. Commercial silicone materials also typically contain various additives that affect properties (e.g., color, rheology, adhesion, etc.). Commercial silicone elastomers are often reinforced with mineral additive fillers such as silica, calcium carbonate, montmorillonite, carbon black, zinc oxide, titanium dioxide, glass, and graphene (as well as other material enhancement treatments such as boric acid and polyhydric alcohols (see, e.g., U.S. Pat. No. 4,252,709)). Medical grade silicones are biocompatible and bioinert and are therefore common materials in medical implants, including prostheses, artificial heart valves, and various catheters.
[0003]
[0004] Although flexibility and other properties are favorable for medical uses of silicone, the hydrophobic surface of silicone is susceptible to bacterial and fungal colonization and biofilm formation. Fungal or bacterial biofilm growth on silicone surfaces can be a problem for in vivo medical applications, such as catheter-associated urinary tract infection (CAUTI) (Siddiq & Darouiche, NATURE REVIEWS UROLOGY 20129 305 DOI10.1038 / nrurol.2012.68), which is the most common nosocomial infection and causes a significant health burden. Microbial contamination of silicone surfaces can also be a risk factor for applications in the food sector.
[0005] Surface modification: The surface of silicone can be chemically modified to increase resistance to bacterial colonization and biofilm formation. The most common approach is to introduce some hydrophilic parts such as polyethylene glycol (PEG) to reduce hydrophobicity and repel bacteria, thereby slowing colonization and biofilm formation. Another approach is to load lipophilic disinfectants or antimicrobial drugs in the polymer matrix, which can be leached from the material to kill infectious microorganisms (Kottmann et al., CHEMISTRY-AN ASIAN JOURNAL 2017 12 1168DOI10.1002 / asia.201700244). The disadvantage of the latter approach is that the efficacy will decrease over time with the loss of antimicrobial agents, and the leaching of bioactive agents will also affect the regulatory state of the device. Coating silicone surfaces with biocompatible polymers and proteins can also be used to improve biocompatibility and reduce problems associated with implants (such as the formation of scar tissue).
[0006] Silicone coating: Silicone is generally considered chemically inert because it lacks reactive groups, so to coat silicone, the surface is usually first activated to introduce groups that can serve as targets for chemical modification. A common method is plasma (ozone) treatment to oxidize the surface and introduce -OH groups, but the use of other oxidants (such as H 2 O 2 ) can also be used for the same purpose ( et al., Bioactive Functionalisation of Silicones with Polysaccharides, Springer Briefs in Molecular Science Biobased Polymers ISBN 978-3-030-02275-4 (eBook) 2018 https: / / doi.org / 10.1007 / 978-3-030-02275-4). This is usually followed by a second step using a silanization reagent (R-Si-(OR') 3) such as APTMS ((3-aminopropyl) trimethoxysilane) to treat the surface to introduce more nucleophilic amino groups on the surface. The silicone surface can then be coated in a manner that includes using nucleophilic groups on the surface to initiate polymerization of monomer building blocks, or reacting with electrophilic moieties on the polymer used for coating or electrophilic moieties on other compounds, or reacting them with a crosslinking agent and then reacting with electrophilic moieties on the polymer used for coating or electrophilic moieties on other compounds. Thus, a stable coating is obtained in which the polymer coating is covalently attached to the surface. Alternatively, the oxidized surface can be treated with a silanizing agent such as (3-glycidyloxypropyl)-trimethoxysilane to introduce electrophilic epoxy groups on the surface. This can further react with nucleophilic polymers or other compounds to covalently coat the surface. US2016 / 0130403 (Brook et al.) discloses that hydrophilic or reactive polymers connected to linear or branched hydrophobic silicone polymer chains can be physically adsorbed onto the surface of a silicone elastomer to form a stable hydrophilic coating. US 10,465,055 discloses treating a silicone substrate with a polymer containing at least three reactive sites to promote "covalent grafting" of the polymer to the substrate, provided that the substrate has accessible Si-H groups, which according to the disclosure can be obtained by immersing the silicone surface in an aqueous solution of hydrogen fluoride. Summary of the invention
[0007] The present invention provides a new process for surface modification of silicone materials and for coating silicone materials. The present invention provides a simple process for activating a surface so that it can be easily further modified. The process is based on the surprising discovery that amino groups can be introduced onto the surface of silicone without prior surface oxidation using the process described herein.
[0008] Therefore, the present invention proposes a new method for modifying silicone surfaces and thereby making the surfaces suitable for further modification. Specifically, the method proposed herein comprises treating the silicone surface with a substance selected from a specified group further described below, the substance containing amino groups. The inventors have tested a variety of substances and different conditions and settings, which can vary depending on the specific surface type and / or the object to be modified and the type of subsequent modification required and expected chemically and functionally. Advantageously, the method can be carried out using readily available and economical reagents, mild conditions and environmentally friendly solvents.
[0009] Thus, in a first aspect, the present invention relates to a method for modifying a solid silicone surface, in particular a silicone elastomer surface, to introduce amino groups into the surface so that it can be further modified, the method comprising treating the silicone elastomer surface with a substance selected from the group consisting of
[0010] - a molecule comprising at least one primary or secondary amino group and at least one further nucleophilic group selected from the group consisting of OH, SH, COOH and NH 2 , amides and NHR, wherein R is alkyl;
[0011] - having the formula Si-(OR 1 )(OR 2 )(OR 3 )R 5 NHR 4 A silylating agent, wherein the group R 1 , R 2 , R 3 are independently selected from linear or branched alkyl or alkylene groups and are preferably methyl or ethyl, R 5 is a straight-chain or branched alkyl or alkylene group which may be further substituted, R 4 is H or an organic group,
[0012] Therein, at least in the case where the substance is a silanization agent, the surface is not pre-treated with an oxidizing agent (including ozone, hydrogen peroxide) or plasma treatment prior to the above treatment step.
[0013] The term "silicone surface" encompasses any type of surface on a solid silicone object, which encompasses objects that may be made essentially only of silicone as well as silicone objects that contain common additives and other ingredients known in the art as minor ingredients in silicones, such as fillers, reinforcing agents, for example mineral fillers such as silica, alumina, calcium carbonate, carbon black, zinc oxide, titanium dioxide, glass, graphene crosslinking agents, catalysts, boric acid, polyhydroxy alcohols, etc. Thus, silicone objects as used herein include objects made of silicone elastomers or silicone rubbers.
[0014] The reagent material may optionally be dissolved in a solvent selected from water miscible solvents, such as, but not limited to, methanol, ethanol, propanol, isopropanol, 1-butanol, 2-butanol, tert-butanol, glycerol, water or an aqueous solution, and any miscible mixture of one or more of these. The silicone surface is then placed in the solvent with the dissolved reagent.
[0015] A variety of amines have been found to be useful as reagents in the methods described herein. Table 1 lists non-limiting examples of specific reagents.
[0016] Table 1
[0017]
[0018]
[0019] Thus, in some embodiments, the reagent is an amine comprising a linear or branched alkane or alkene chain, at least one primary or secondary amino group and / or amide group and at least one additional nucleophilic group selected from OH, SH, COOH and NH 2 , amides and NHR, wherein R is an alkyl group. In some embodiments, the reagent is an ester, ether or alcohol having at least one primary or secondary amino group. The reagent can also be an amine having two or more primary or secondary amino groups, some examples of which are shown in Table 4.
[0020] Useful agents also include amino acids and amino acid derivatives, including naturally occurring amino acids and their derivatives, such as salts and esters thereof. Preferred amino acids are amino acids with nucleophilic groups on the side chains, such as basic amino acids (histidine, lysine) and amino acids with -OH or -SH groups on the side chains (tyrosine, serine, threonine, cysteine). Also useful are small peptides, such as but not limited to dipeptides, tripeptides and other soluble oligopeptides, preferably including at least one amino acid of the preferred type with basic side chains -OH or -SH, or polyethyleneimine oligomers or polymers containing a large number of primary and secondary amino groups.
[0021] The present invention adopts silanization reagent Si-(OR 1 )(OR 2 )(OR 3 )R 5 NHR 4 In the embodiment, R 4 Can be selected from H, straight chain or branched alkyl, and the straight chain or branched alkyl can be further substituted by amide, benzyl, carbamate and amine. In a specific embodiment, such reagents can include trimethoxysilane or triethoxysilane. Specific non-limiting examples include the compounds shown in Table 2.
[0022] Table 2
[0023]
[0024]
[0025] In some embodiments, the reagent substance is a compound of formula W(X)-NHR 4 The molecules shown, where W is a molecule containing an aromatic structure, and X represents OH, SH, COOH, amide, NH 2 or NHR (wherein R is alkyl or alkenyl), and R 4 As defined above. Groups X and NHR 4 Each of can be independently directly connected to the carbon atom of the aromatic structure or connected to the side chain of the alkyl or alkylene. Non-limiting examples include the compounds shown in Table 3.
[0026] Table 3
[0027]
[0028]
[0029] Table 4 shows a non-limiting list of other useful reagents.
[0030] Table 4
[0031]
[0032]
[0033]
[0034]
[0035] As mentioned above, the method of the present invention has the significant advantage that the silicone surface to be treated according to the present invention does not need to be pre-treated with an oxidizing agent (e.g. ozone, hydrogen peroxide) or plasma treatment before being treated with the reagent according to the method of the present invention. This makes the method of the present invention much simpler than the prior art methods for modifying silicone surfaces discussed in the background section above. This applies to any reagent that can be selected, but in particular, when a silanizing agent as defined above is selected, a pre-oxidation step is not adopted. When other reagents are used, a pre-oxidation step may or may not be adopted, but as mentioned above, a pre-oxidation step is not necessary.
[0036] In addition, the use of strong bases (e.g., NaOH, KOH, LiOH, BaOH, NH 4 OH and CaOH 2 ) is pre-treated and is omitted in a preferred embodiment.
[0037] The method can be advantageously carried out by using any one of a plurality of common solvents or solvent mixtures. The advantage of the present invention is that harmless and environmentally friendly solvents can be easily used, such as common alcohol solvents (these solvents do not have severe toxicity or serious carcinogenicity and will not cause harm to the environment when discarded). In some embodiments, an organic solvent is used, the organic solvent can be selected from but not limited to diethylene glycol, ether, diethylene glycol, dimethyl ether, methyl tert-butyl ether (MTBE), tetrahydrofuran (THF), dimethylformamide (DMF), N-methyl-2-pyrrolidone (NMP), dimethyl sulfoxide (DMSO), ethylene glycol, ethanol, propanol, isopropanol, 1-butanol, 2-butanol, the tert-butyl alcohol, ethyl acetate and acetone. Alternatively, water or an aqueous solution, or a miscible solution of water and one or more organic solvents can be used. In these embodiments, the silicone surface to be treated is placed in a solvent, and the reagent is mixed in a solvent. Tests show that the method can be successfully operated at ambient room temperature, but in some embodiments higher temperatures can be advantageous for faster reactions. After a period of time, the treated silicone surface is preferably rinsed, preferably using the same solvent used for the reaction or another solvent, and preferably using water or an aqueous solution or a non-toxic alcohol or other environmentally friendly solvent.
[0038] In embodiments using vapor phase reagents, the silicone surface is placed in a suitable closed atmosphere, which in some embodiments is air but in other embodiments is an inert atmosphere such as nitrogen, and the reagent is injected or infiltrated into the closed atmosphere.
[0039] Applicable reaction conditions vary and can be suitably optimized according to the specific reagent and solvent selected.Therefore, in some embodiments, reaction can be carried out at ambient room temperature (about 20-25 ℃), in other embodiments, reaction is carried out in the temperature range of about 10 °-100 ℃, for example, from about 10 °, or from about 15 °, or from about 20 °, or from about 25 °, or from about 30 ° to about 100 °, or to about 90 °, or to about 70 °, or more preferably to about 50 °, or to about 40 °.In some embodiments, using suitable solvent is useful for applying lower temperature, so reaction can occur in the temperature range of about -30 ° to about 10 ℃.
[0040] The reaction may also be assisted by the application of ultrasound and / or microwave heating.
[0041] The resulting surface-modified silicone with reactive amino groups can be advantageously further modified to obtain silicone with desired modified properties. Therefore, in some embodiments, the method of the present invention includes further steps of modifying the silicone surface. In one embodiment, the method includes treating the silicone surface with a diazo transfer reagent (sometimes referred to as an azide transfer reagent) to convert at least some of the introduced amino groups into azido groups. These azido groups can then selectively react with alkynes in a 1,3-dipolar cycloaddition (i.e., a "click reaction") to obtain 1,2,3-triazole derivatives (see, e.g., US9302997B2). This 1,3-dipolar cycloaddition has been used to covalently attach alkyne derivatives of various bioactive molecules (e.g., proteins, peptides, biotin, and polymers) to the surface (Escorihuela et al., Adv. Mater. Interfaces 2015, 2, 1500135-https: / / doi.org / 10.1002 / admi.201500135). Thus, in some embodiments of the method, the silicone surface, after reacting with a selected azide transfer reagent, is reacted with a selected desired molecule that binds to the introduced azide group via a 1,3-dipolar cycloaddition. The diazide transfer reagent may be selected from, but not limited to, imidazole-1-sulfonyl azide, trifluoromethanesulfonyl azide, trimethylsilyl azide, and sodium azide. Molecules bound in this manner may be selected from, but not limited to, peptides, proteins, biotin, polymers (e.g., PEG), but other agents are also suitable.
[0042] In another embodiment, the method includes the step of treating the surface with the amino group introduced with a cross-linking agent, and the cross-linking agent is preferably selected from but not limited to glutaraldehyde, ethylene glycol dimethacrylate, genepin, tannic acid and polyethylene glycol diglycidyl ether. After the selected cross-linking agent is reacted with the modified surface by methods known in the art, the desired biopolymer can be connected thereto, or when there is a nucleophilic reactive group in the structure, other polymers, peptides, proteins or other bioactive molecules are connected thereto. Therefore, this surface of the present invention with the cross-linking agent introduced can react with, for example, synthetic polymers (for example PEG), proteins, peptides, carbohydrates, small bioactive molecules (for example, but not limited to bioactive drug molecules, cytokines or hormones, etc.).
[0043] The process described herein introduces amino groups onto the accessible surface of the treated silicone. The exact structure and nature of the amino group binding to the silicone has not been elucidated and is under investigation by the inventors; the tests contained in the examples below show that significant activity is retained after extensive washing, indicating that covalent binding plays a role, although non-covalent binding may also play a role.
[0044] One aspect of the invention provides a silicone object having a modified surface obtained by the above method. Such objects of the invention can be commercially produced and provided as useful intermediates for subsequent use, or the silicone object can be treated with the method of the invention and further modified by subsequent steps to bind selected useful parts thereto, as described above. Therefore, the present invention also covers silicone objects obtainable by the method of the invention, wherein one or more molecules have been bound (preferably covalently bound) to amino groups introduced on at least some of the silicone surfaces. Such molecules can include, but are not limited to, any of the above, such as synthetic polymers, proteins, peptides, carbohydrates and small biologically active molecules (such as but not limited to biologically active drug molecules, cytokines or hormones) or any combination of one or more of these.
[0045] As used herein (including in the claims), unless the context indicates otherwise, singular forms of terms should be interpreted as also including plural forms, and vice versa. Therefore, it should be noted that, as used herein, the singular forms "a", "an", and "the" include plural references unless the context clearly indicates otherwise.
[0046] Throughout the specification and claims, the terms "comprises," "comprising," "having," and "containing" and variations thereof should be understood to mean "including but not limited to," and are not intended to exclude other components.
[0047] The term "at least one" should be understood to mean "one or more", thus including both embodiments containing one or more components. In addition, when an independent claim cited by a dependent claim uses "at least one / kind" to describe a feature and the dependent claim uses "the" and "the at least one / kind" to indicate the corresponding feature, it has the same meaning as in the independent claim.
[0048] It should be understood that the foregoing embodiments of the present invention may be modified while still falling within the scope of the present invention. Unless otherwise specified, the features disclosed in the specification may be replaced by alternative features for the same, equivalent or similar purposes. Therefore, unless otherwise specified, each feature disclosed is merely an example of a series of equivalent or similar features.
[0049] The use of exemplary language (e.g., "such as", "for example", "such as") is only intended to better illustrate the present invention, and does not limit the scope of the present invention, unless otherwise specified. Any steps described in the specification can be implemented in any order or simultaneously, unless the context clearly indicates otherwise.
[0050] All features and / or steps disclosed in the specification can be combined arbitrarily, except for combinations in which at least some features and / or steps are mutually exclusive. In particular, the preferred features of the present invention are applicable to all aspects of the present invention and can be used in any combination. BRIEF DESCRIPTION OF THE DRAWINGS
[0051] Figure 1 :Used to quantify free amino groups (-NH 2 ) calibration curve for the ninhydrin test.
[0052] Figure 2: Shows the effect of reaction time on the three steps of surface modification. A: APTMS; B: glutaraldehyde; and C: chitosan.
[0053] Figure 3 : FT-IR spectra of untreated silicone (F), chitosan-coated silicone (G), and chitosan (H).
[0054] Figure 4 : Samples at each step; A: untreated silicone after ninhydrin test, B: after 2 hours of silanization with 2% APTMS, C: after 24 hours of treatment with 2% APTMS, D: APTMS-treated silicone after ninhydrin test, E: after APTMS treatment and glutaraldehyde treatment, F: chitosan coating (after APTMS and glutaraldehyde treatment).
[0055] Figure 5 : Effect of washing with different solvents on the ninhydrin response of silicone samples treated with 2% APTMS.
[0056] Figure 6 : FT-IR spectrum of a silicone sample reacted with APTMS, then with an azide reagent and finally subjected to a cycloaddition reaction (see Example 6). Example
[0057] Example 1. Silicone Samples, Ninhydrin Test and FT-IR
[0058] 1-1 Silicone sample
[0059] NuSil Technology medical silicone elastomer sheets (MED82-5010-80 and MED82-5010-40) were used in the experiment. Silicone discs were cut from the sheets using a hollow punch to obtain a diameter of 1.2 cm, a thickness of 0.2 cm (thin disc) or 0.4 cm (thick disc) and a total surface area of 3.0 cm 2 or 3.8cm 2The weight of the thin disk sample was 0.14 g and the weight of the thick disk sample was 0.26 g. Thin disks were used, immersed in acetone and sonicated for 30 min to remove all surface contaminants, rinsed with deionized water, and dried in an 80 °C oven before use, unless otherwise stated.
[0060] In the second set of experiments, we fabricated 2 mm thick silicone sheets by pouring a silicone mixture made of two liquid silicones (one containing a catalyst and the other containing a crosslinker and a curing inhibitor) into a mold and heating the mold at 100 °C to cure the silicone into an elastomer. Three silicone films with different stiffness (Shore OO) were fabricated, named A (CF1350), B (CF15), and C (CF13).
[0061] 1-2 Ninhydrin test
[0062] Ninhydrin reagent was used to quantify the free amino groups (-NH 2 ):
[0063] Lithium acetate dihydrate is dissolved in deionized water, pH is adjusted to 5.2 with glacial acetic acid, obtain 4M lithium acetate buffer solution.Ninhydrin (1.0g) and reduced ninhydrin (0.15g) are directly weighed in a round-bottomed flask and dissolved in DMSO (37.5mL).Then stopper the flask with a diaphragm.The syringe connected to a nitrogen balloon is inserted into the solution through the diaphragm, and oxygen is discharged by inserting another syringe into the diaphragm.Then add 12.5mL 4M lithium acetate buffer solution, and once again use nitrogen purging solution.
[0064] 1-3 Calibration of the Ninhydrin Test with Glucosamine Hydrochloride
[0065] 0.1 ml CH 3 COOH added 25 ml H 2 Prepare 25 ml of CH 2 O 3 COOH / H 2 O (1:250 v / v) solution. Then 0.25 g of chitosan was added to the solution and the solution was stirred with a magnetic stirrer until the chitosan was completely dissolved to prepare a stock solution with a concentration of 1 mg / ml. Then, the stock solution was used to prepare six standard solutions of specified concentrations: 15.62 μg / ml, 31.25 μg / ml, 62.5 μg / ml, 125 μg / ml, 250 μg / ml and 500 μg / ml.
[0066] A similar process was also performed to prepare the glucosamine standard solution.
[0067] A blank sample was prepared by mixing 1 ml of deionized water with 1 ml of ninhydrin reagent. The test tube was then placed in a water bath (90°C) and heated for 30 minutes to complete the reaction. After cooling in another water bath, 5 ml of 50% (v / v) EtOH / H 2 O mixture diluted solution to a final volume of 7 ml. These solutions were vortexed again for 15 s to oxidize excess reduced ninhydrin. The absorbance at 570 nm was measured using a UV-visible spectrophotometer (GENESYS150). The results were used to prepare a calibration curve ( Figure 1 ).
[0068] Table 5. Calibration data for the ninhydrin test
[0069] Table 5
[0070]
[0071]
[0072] (The molecular weight of glucosamine hydrochloride used in the calculation is 215.63 g / mol)
[0073] 1-4 Ninhydrin test for quantification of amino groups in silicone disc samples
[0074] Treated or untreated disks were inserted into test tubes containing 1 ml of ninhydrin reagent and 1 ml of water. The test tubes were placed in a water bath (90° C.) and heated for 30 minutes to complete the ninhydrin reaction. The disks were then removed, the solution cooled and subsequently diluted to a final volume of 7 ml with 5 ml of a 50% (v / v) ethanol / water mixture. The absorbance of the diluted solution was measured in a 1 cm pathlength cuvette using a UV spectrophotometer. In the case of a strong response (absorbance>1-2), the solution was further diluted with 50% (v / v) ethanol / water to allow measurement within the optimal 0-2 absorbance range.
[0075] 1-5FT-IR
[0076] Surface functionalization and coatings were investigated using a Nicolet iZ10 FT-IR spectrometer (Thermo Fisher Scientific) in reflectance mode, and spectra were analyzed using OMNIC software.
[0077] Example 2. Silicone treated with ATPMS in toluene, crosslinked with glutaraldehyde and coated with chitosan.
[0078] 2-1 Treatment with ATPMS dissolved in toluene
[0079] In this experiment, 1%, 2%, and 4% (3-aminopropyl)trimethoxysilane (APTMS) solutions were prepared by adding 0.5, 1, and 2 mL of APTMS to 49.5, 49, and 48 mL of toluene, respectively.
[0080] 1 ml of (3-aminopropyl)trimethoxysilane (APTMS) was diluted in 50 ml of toluene to obtain a 2% APTMS solution. The thin silicone disc was penetrated with a 19G BD Microlance syringe needle to weight it so that it was completely immersed in the APTMS solution. The disc was then immersed in the APTMS solution in a conical flask and the solution was stirred with a magnetic stirrer. The disc was removed after the set treatment time (20min, 40min, 1h, 1.5h, 2h or 24h), rinsed thoroughly with water, and then washed 6 times on each side using a pipette to remove any excess reagent. It was then dried in an oven (80°C) for 2 hours. The response to ninhydrin increased for up to 24 hours (Figure 2-A). However, such a long reaction time also had a negative impact on the performance of the silicone material. After 24 hours of reaction, the treated disc became white and brittle, indicating that a large amount of covalent cross-linking had occurred. Therefore, the 2 h reaction was considered optimal, as the response in the ninhydrin experiment was approximately 65% of the 24 h response. No effect of the 2 h treatment on the properties of the silicone material was observed.
[0081] 2-2 ATPMS-treated silicone containing glutaraldehyde crosslinker
[0082] The silicone disk treated with 2% APTMS in toluene solution for 2 hours and rinsed was immersed in 25% glutaraldehyde H 2 O solution with occasional stirring. After 20min, 40min, 1h, 1.5h, 2h or 3h, the disk was removed from the solution and washed 4 times with methanol on each side with a pipette and air-dried overnight. The slices were analyzed by FT-IR and ninhydrin test. All tests were performed three times. Before coating the amino-functionalized silicone with chitosan, the sample must be treated with a suitable crosslinker that can react with the amino groups and polysaccharides on the silicone surface. Glutaraldehyde is a crosslinker that readily reacts with primary amino groups to form imines. The imines can then be reduced to form stable dialkylamines. This reagent blocks the amino groups on the silicone surface, so the response to the ninhydrin test should decrease as the reaction proceeds. Due to the conversion of amino groups to imines, the ninhydrin response of the sample decreases with increasing reaction time in the glutaraldehyde solution. After 3 hours of reaction, there was almost no response to the ninhydrin test. Therefore, the crosslinking reaction is almost complete after 3 hours of crosslinking (Figure 2-B).
[0083] 2-3 ATPMS treated with chitosan and silicone treated with glutaraldehyde.
[0084] The silicone disk treated with 2% APTMS in toluene solution for 2 hours and rinsed was immersed in 25% glutaraldehyde solution as described above, and then immersed in a 25% glutaraldehyde solution containing 0.04 g / ml chitosan and 0.001 g / ml NaBH 4 2% (v / v) acetic acid / H 2 O solution for 2 minutes, 40 minutes, 1 hour, 1.5 hours or 2 hours. This was done at room temperature with occasional stirring with a needle. It was then removed from the solution, rinsed thoroughly in deionized water, washed 10 times on each side using a plastic pipette filled with the same solvent and dried in an oven (80°C) for 1 hour. The slices were analyzed by FT-IR and ninhydrin test. All tests were performed three times.
[0085] Chitosan polymer chains contain many amino groups (-NH 2 ), when the silicone sample treated with glutaraldehyde is immersed in the chitosan solution, the response in the ninhydrin test should increase again. An increase in the ninhydrin response was observed (Figure 2-C). The response increased rapidly within the first hour, but slowed down and approached a stable level within 2 hours. After the ninhydrin reaction, the sample was diluted 10 times to obtain a significant measurement value and fit the calibration curve.
[0086] FIG. 2 shows the effect of reaction time on the response of all three coating steps in the ninhydrin test. A: APTMS, B: glutaraldehyde, and C: chitosan. All measurements were performed three times and standard error bars are shown. After the ninhydrin test, the ninhydrin reagent was diluted 7 times (to 7 ml) for the APTMS treated disk (A) and the glutaraldehyde treated disk (B). After the ninhydrin reaction of the chitosan treated disk, the reagent was diluted 70 times (first to 7 ml, then diluted 10 times) so that the measured absorbance could fit the calibration curve.
[0087] 2-4 FT-IR results
[0088] Untreated silicone disks were measured to identify characteristic peaks that could be compared to the spectrum of the treated silicone. The peak at 2961 cm was observed in the untreated silicone sample. -1 (CH 3 The characteristic peak of silicone at Figure 3 -F). Additional peaks can be observed in the spectrum of chitosan-coated silicone and these peaks are similar to those observed in the spectrum of pure chitosan. The characteristic peaks of chitosan are as follows: 3292 cm -1 (NH and CH stretching), 2871cm -1 (CH 3 Symmetrical expansion and contraction), 1647cm -1 (C=O stretching) and 1375cm -1(CN telescopic)( Figure 3 -H). Similar to chitosan, the characteristic peaks of chitosan-coated silicone ( Figure 3 G) is as follows: 3262cm -1 (NH and CH stretching), 2961cm -1 (CH 3 Symmetrical telescopic), 1558cm -1 (C=O stretch) and 1402.52cm -1 (CN telescopic).
[0089] Figure 3 FT-IR spectra of F: untreated silicone; G: chitosan coated silicone and H: chitosan are shown.
[0090] 2-3 Visual Analysis
[0091] Digital images show the appearance of silicone disc samples after different treatments. Untreated silicone has an opaque light grey color that darkens after treatment with the ninhydrin reagent ( Figure 4 -A). After being treated with 2% APTMS solution for 2 hours, the appearance did not change visually ( Figure 4 -B), but after 24 hours of treatment, the sample turned white and brittle ( Figure 4 -C). The disk treated with 2% APTMS for 2 hours turned blue after treatment with ninhydrin reagent ( Figure 4 -D). The APTMS-treated disks turned brown-orange after treatment with glutaraldehyde ( Figure 4 -E), became more red after treatment with chitosan.
[0092] The results are as follows Figure 4 Shown are A: untreated silicone after ninhydrin test, B: after 2 h silanization with 2% APTMS, C: after 24 h treatment with 2% APTMS, D: APTMS-treated silicone after ninhydrin test, E: glutaraldehyde treatment, and F: chitosan coating.
[0093] Example 3. Stability of amino modification of silicone.
[0094] Samples of silicone disks treated with 2% APTMS for 2 hours were washed thoroughly with different solvents in an attempt to extract reagents that were not firmly (covalently) attached to the silicone ( Figure 5). When the initial wash was done with water, methanol, and toluene, the ninhydrin response was similar (~1.2), but when the initial wash was done with ethanol, the ninhydrin response was reduced by 50% from the initial response (~0.6). Extensive washing for up to a week further reduced the ninhydrin response, but this occurred mainly within the first 24 hours, and after a further week of washing, the reduction in the ninhydrin response was limited. After washing with the different solvents, the samples were also heated in water (90°C) for 20 minutes. Heating resulted in a reduction of about 50% in the initial response for all samples.
[0095] Figure 5 The effect of washing with different solvents on the ninhydrin response of a silicone sample treated with 2% APTMS is shown. The Y-axis represents the absorbance at 570 nm and the X-axis represents the time in days.
[0096] Example 4. Treatment of silicone using pure APTMS and different APTMS solutions.
[0097] Toluene solution process. The silicone disc was immersed in a toluene standard solution containing 2% (v / v) ATPMS for 20 min at room temperature. Subsequently, the disc was thoroughly rinsed with anhydrous toluene to remove excess reagent residues. The silicone sample was then heated in an oven (80°C) to dryness and subjected to the ninhydrin test as described in Example 1.
[0098] Deionized water solution process: The sample was immersed in a 5% APTMS solution (heated to 85°C) for 5 or 30 minutes and dried with nitrogen. The sample was then kept at 65°C for 10 minutes.
[0099] Process of pure APTMS liquid. The silicone sample was immersed in 97% APTMS for 5 minutes, then rinsed with deionized water and dried in an 80 °C oven.
[0100] Procedure for ethanol solution and ethyl acetate solution: Anhydrous solution was prepared by mixing APTMS with anhydrous ethanol or ethyl acetate to obtain a 1% solution. The solution was stirred for 10 min at room temperature under nitrogen. The silicone disk was then placed in the solution under nitrogen at room temperature. After 20 minutes, the substrate was rinsed with ethanol and dried with nitrogen. The results are shown in Table 6.
[0101] Table 6. Treatment results of APTMS in different solvents and pure APTMS
[0102]
[0103] *-NH 2 The calculation of molar amounts was based on the extinction coefficient obtained from the glucosamine hydrochloride calibration curve equation (Example 1).
[0104] Example 5. Azide transfer reaction with modified silicones and azide-alkyne cyclization reactions.
[0105] Azide transfer reaction protocol: A silicone disk sample treated with 2% APTMS toluene solution for 2 hours was penetrated with a syringe needle and immersed in 50 mL of MeOH in a 100 ml round bottom flask. Imidazolesulfonyl azide (50 mg) was then added to the reaction medium during stirring. Subsequently, 50 mg of K dissolved in 1 ml of deionized water was added. 2 CO 3 and 5.75 mg CuSO dissolved in 1 ml deionized water 4 .5H 2 O. The flask is stoppered and the reaction medium is stirred for 16 h to 20 h. Once the reaction time is over, the sample is washed with acetone, then with water and again with acetone and finally dried at room temperature for one hour. The treated disks are analyzed using FT-IR. The spectrum of the treated disks is consistent with that of the disks with the azide groups introduced on the surface, since the peak at 2097 cm -1 A new peak was observed.
[0106] Cycloaddition reaction protocol: 15 mL of DMSO was added to a 25 mL round bottom flask equipped with a reflux condenser. Heat until the solvent reaches 50°C. Then the azide functionalized disk (threaded on a needle) was added to the reaction medium which was stirred with a magnetic stirrer. Then 1.5 mg of CuSO 4 and 4.7 mg of sodium ascorbate were dissolved in 1 mL of deionized water, respectively, and added to the reaction medium. Finally, 23.3 mg of N,N,N-trimethylprop-2-yn-1-ammonium was added under a nitrogen atmosphere. The reaction solution was then stirred at 50 °C for 48 h. Thereafter, the sample was removed from the medium and washed with deionized water at least 3 times. The sample was then dried in the open air. The treated disks were analyzed by FT-IR. After the cycloaddition reaction, the azide peak disappeared, but in the spectrum at 2922 cm -1 A new peak in the CH stretching region can be observed at , consistent with triazole functionalization.
[0107] Figure 6 Shown is the FT-IR spectrum used to study the azide-alkyne cycloaddition reaction.
[0108] Example 6. Modification of silicone with ethanolamine in different solvents.
[0109] Cleaning of silicone discs
[0110] The silicone disc was cut from a 0.4 mm thick silicone sheet. The silicone disc was immersed in deionized water in a conical flask and shaken. The water wash solution was replaced and the disc was immersed at room temperature for one hour. This process was repeated twice. Finally, the disc was dried in an oven at 80 °C for 2 hours.
[0111] Mix ethanolamine (EA) with water, isopropanol, ethanol, or ethyl acetate to make a treatment solution of the desired concentration. Soak the disk in the treatment solution and gently stir every 1 hour (thick disks will not float in the solution, so there is no need to pass the needle through them).
[0112] After the reaction, the disk was removed and thoroughly rinsed 4 times in water (total rinse time 15 minutes) and then subjected to the ninhydrin test as described above (in Example 1).
[0113] The results are shown in Table 7.
[0114] Table 7
[0115]
[0116]
[0117] *-NH 2 The calculation of molar amounts was based on the extinction coefficient obtained from the glucosamine hydrochloride calibration curve equation (Example 1).
[0118] Example 7. Modification of silicone with APTMS
[0119] In the present embodiment, the silicone disc made of preformed sheets A, B, and C is modified with APTMS. Silicone discs are made using a 12mm hollow steel punch, cleaned with deionized water, and finally dried in an 80°C oven. The sample (silicone disc) is added to a 50ml APTMS solution or only solvent (control), and stirred at room temperature for 1 hour. The supernatant is then discarded, and the sample is washed six times with toluene (for this purpose, an appropriate amount of toluene is added to each disc to completely cover the disc (20mL) and shake for about 30 seconds, then the solution is replaced with 20ml fresh toluene, and the process is repeated six times). The sample is then washed 6 times with methanol and deionized water, respectively, as described above to remove any remaining traces. Finally, the sample is dried in an 80°C oven and used for the ninhydrin test.
[0120] The method for the ninhydrin test using the silicone disk is the same as the standard method for the calibration curve. The disk is immersed in 1 ml of water and 1 ml of ninhydrin reagent in a test tube. The test tube is then placed in a water bath (90°C) and heated for 30 minutes to complete the reaction. The sample is then washed with 26 ml of 50% (v / v) EtOH / H2O before UV measurement. 2 O mixture dilution solution. All tests were performed three times. The results are shown in Table 8.
[0121] Table 8
[0122]
[0123]
[0124] Example 8. Silicone modified with DAP (1.3 diaminopropane), EA (ethanolamine), A12P (3-amino-1,2-propanediol), 3AP (3-amino-1-propanol) and EDA solution (ethylenediamine) isopropanol.
[0125] In this experiment, five different reagents were prepared by adding 2.2 mL of DAP, EA, A12P, 3AP, and EDA to 20 mL of isopropanol, respectively.
[0126] Disks were made from Type A silicone sheets using a 12 mm hollow steel punch as before and washed twice (30 minutes) with 20 mL of isopropanol and water respectively as before.
[0127] The samples (silicone disks) were added to DAP, EA, A12P, 3AP and EDA solutions (3 disks were treated each time) and stirred for 24 hours. The supernatant was then discarded and the samples were washed twice with isopropanol and water as described above. Finally, the samples were dried in an oven at 80°C and used for the ninhydrin test.
[0128] The ninhydrin assay was performed as described in Example 8, except that after heating, 40 mL of 50% (v / v) EtOH / H 2 O mixture dilution solution. All tests were performed three times. The results are shown in Table 9.
[0129] Table 9
[0130]
Claims
1. A method for modifying a silicone solid surface to introduce amino groups into the surface to make it suitable for further modification, the method comprising treating the silicone elastomer surface with a reagent substance selected from the group consisting of - a molecule comprising at least one primary or secondary amino group and at least one further nucleophilic group selected from OH, SH, NH2 and NHR, wherein R is an alkyl group; - having the formula Si-(OR 1 )(OR 2 )(OR 3 )R 5 NHR 4 A silylating agent, wherein the group R 1 , R 2 , R 3 are independently selected from linear or branched alkyl or alkylene groups and are preferably methyl or ethyl, R 5 is a straight chain or branched alkyl or alkylene group, and R 4 is H or an organic group, in, The reagent substance is optionally dissolved in a solvent and the silicone elastomer surface is placed in the solvent with the dissolved reagent, wherein the solvent is a water-miscible solvent, preferably selected from methanol, ethanol, propanol, isopropanol, 1-butanol, 2-butanol, tert-butanol, glycerol, water or an aqueous solution, and any miscible mixture of one or more of these, At least in the case where the reagent substance is a silanization agent, the surface is not pre-treated with an oxidizing agent including ozone, hydrogen peroxide, or plasma treatment prior to the above treatment step.
2. The method of claim 1, wherein the reagent substance is a silanization agent and wherein R 4 is selected from H, straight chain or branched alkyl groups, which may be further substituted with amide, benzyl, carbamate and amine.
3. The method of claim 1, wherein the reagent substance is of the formula W(X)-NHR 1 A molecule represented by a molecular structure in which W is -((CY 1 ) n -Z-(CY 2 ) m ) l - a linear or branched molecule, wherein Y 1 and Y 2 Independently selected from H, OH, SH, NH2, alkyl (CH2) k CH3, wherein n, m, l are independently integers from 1 to 10 and k is an integer from 1 to 5, including polyethyleneimine, O-(2-aminoethyl)polyethylene glycol, O,O'-bis(3-aminopropyl)polyethylene glycol and poly-L-ornithine, and Z is selected from -S-, -O- and -NH-, and X is optionally present but requires that Y 1 and Y 2 is a non-nucleophilic group and represents OH, SH, COOH, amide, NH2 or NHR, wherein R is an alkyl group.
4. The method of claim 1, wherein the substance is a silanization agent selected from (3-aminopropyl)trimethoxysilane (APTMS), bis[3-(trimethoxysilyl)-propyl]-amine, trimethoxy-[3-(methylamino)propyl]silane, (3-aminopropyl)-triethoxy-silane, 1-[3-(trimethoxysilyl)propyl]urea, N-[3-(trimethoxysilyl)propyl]aniline, [3-(2-aminoethylamino)propyl]trimethoxysilane.
5. The method of claim 1, wherein the substance is of the formula W(X)-NHR 4 A molecule represented by wherein W is a molecule containing an aromatic structure, X is OH, SH, NH2 or NHR, wherein R is an alkyl group, and R 4 is a straight chain or branched alkyl group as defined in claim 1, preferably which may be further substituted by amide, benzyl, carbamate and amine.
6. The method of claim 5, wherein the substance is selected from 4-aminophenol, 3-aminophenol, 4-aminobenzyl alcohol, 4-aminophenylethanol, 4-hydroxybenzylamine, tyramine, tyrosine, L-tyrosine methyl ester.
7. The method of claim 1, wherein the substance is selected from the group consisting of ethanolamine, 2-(ethylamino)ethanol, diethanolamine, 2-amino-1-propanol, 3-methylamino-1-propanol, 3-amino-1,2-propanediol, 2-(methylamino)ethanol, 2-hydroxyethylhydrazine, 3-amino-1-propanol, 2-amino-1,3-propanediol, 3-amino-2-methylpropan-1-ol, 2-(2-aminoethoxy)ethylamine, 3,3'-azadiyldipropan-1-ol, 3-[(2-aminoethyl)amino]-1-propanol, N, N'-bis(2-hydroxyethyl)ethylenediamine, 3-(2-hydroxyethylamino)-1-propanol, ethylenediamine, N-methylethylenediamine, N,N'-diethylethylenediamine, glycinamide, triethylenetetramine, tetraethylenepentamine, N-(2-hydroxyethyl)ethylenediamine, 3-[(2-aminoethyl)amino]-1-propanol, tris(2-aminoethyl)amine, 1,1-diamino-3,6,9-trioxoundecane, 1,3-diaminopropane, 1,3-diamino-2-propanol, 1,2-diaminopropane, 2,2-dimethyl-1,3- Propylene diamine, 3-aminopropionamide, bis(3-aminopropyl)amine, N,N'-bis(3-aminopropyl)-1,3-propylene diamine, N,N'-bis(2-aminoethyl)-1,3-propylene diamine, 1,2-bis(3-aminopropylamino)ethane, 1,3-diamino-N-(2-hydroxyethyl)propane, 3-(3-aminopropoxy)propylamine, tris(3-aminopropyl)amine, 4,9-dioxa-1,12-dodecane diamine, 4-amino-1-butanol, piperazine, 1-(2-hydroxyethyl)piperazine, 4-hydroxypiperidine, 1, 4-diaminobutane, spermidine, 2,2'-(ethylenedioxy)bis(ethylamine), cysteamine, 2-((2-aminoethyl)-thio)-ethanol, cysteine, 3-amino-1-propanethiol, 2-aminobutane-1,4-dithiol, homocysteine, glycine, serine, serine methyl ester, serine ethyl ester, serine isopropyl ester, threonine, threonine methyl ester, lysine, lysine ethyl ester, lysine methyl ester, ornithine, tyrosine, L-tyrosine methyl ester, and oligopeptides of two or more of the above amino acids and / or amino acid derivatives.
8. The method of claim 1, wherein prior to the treating step, the silicone surface is not pre-treated with an oxidizing agent including ozone, hydrogen peroxide, or plasma treatment.
9. The method of any one of claims 1 to 8, wherein the surface is not pretreated with a strong base such as NaOH, KOH, LiOH, BaOH, NH4OH and CaOH2.
10. A method as claimed in any preceding claim, wherein the reagent is dissolved in a solvent and the silicone surface is placed in the solvent with the dissolved reagent, or wherein the reagent is in gaseous form and is contacted with the silicone surface in a gaseous environment.
11. The method of claim 9, wherein the solvent is selected from an organic solvent including diethylene glycol, diethyl ether, dimethyl ether, methyl tert-butyl ether (MTBE), tetrahydrofuran (THF), dimethylformamide (DMF), N-methyl-2-pyrrolidone (NMP), dimethyl sulfoxide (DMSO), ethylene glycol, ethanol, propanol, isopropanol, 1-butanol, 2-butanol, tert-butanol, ethyl acetate, acetone, water or an aqueous solution, and any miscible mixture of one or more of these.
12. A method as claimed in any preceding claim further comprising the step of treating the silicone surface with an azide transfer reagent to convert at least some of the introduced amino groups to azide groups.
13. The method of claim 12, wherein the azide transfer reagent is selected from the group consisting of imidazole-1-sulfonyl azide, trifluoromethanesulfonyl azide, trimethylsilyl azide and sodium azide.
14. The method according to any one of the preceding claims further comprises the step of treating the silicone surface with a cross-linking agent, preferably selected from glutaraldehyde, ethylene glycol dimethacrylate, genipin, tannic acid and polyethylene glycol diglycidyl ether.
15. The method of any one of the preceding claims further comprising the step of treating the silicone surface with a bioactive molecule selected from the group consisting of chitosan, chitosan derivatives, oligopeptides and proteins to form a bioactive coating.
16. A silicone object having a modified surface comprising reactive amino groups, obtainable by the method according to any one of claims 1 to 15.
17. A silicone object having a modified surface obtainable by the method of any one of claims 1 to 14, wherein one or more molecules have been bound to at least some of the amino groups introduced on the silicone surface, the molecules being selected from synthetic polymers, proteins, peptides, carbohydrates and small biologically active molecules such as antibiotic drugs, cytokines or hormones.
18. A silicone object as claimed in claim 16 or 17, wherein the silicone surface is further modified to change the physicochemical or biological properties, for example to make the surface more hydrophilic, more hydrophobic, antimicrobial to resist bacterial colonisation and / or more biocompatible.