Flame retardant copolyester composition
By using polyphosphonate compounds and melamine cyanurate and other additives in copolyesters, the copolyester composition formed solves the problem of difficult to take into account both flame retardancy and physical properties in the prior art, and achieves high-level fire resistance performance and good physical properties.
Patent Information
- Application Number
- CN202280095259.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-26
- Publication Date
- 2024-12-03
AI Technical Summary
When existing polymers improve flame retardancy, it is difficult to meet fire retardant standards and maintain physical properties at the same time. Especially under UL94 V-O or higher standards, the use of flame retardants often leads to embrittlement or plasticization of the polymer, affecting the Heat deformation resistance.
A copolyester composition is adopted, comprising 45% to 95% of the copolyester, combined with a polyphosphonate compound as a flame retardant additive, and melamine cyanurate and a multifunctional chain extender are added to match an appropriate amount of drip inhibition. The composition formed by the agent has good flame retardancy and physical properties.
It achieves the fire resistance standard of UL94 V-0 or higher while maintaining physical properties, and improves the flame retardant performance and impact resistance of polymers.
Smart Images

Figure BDA0005097690070000351 
Figure BDA0005097690070000361 
Figure BDA0005097690070000362
Abstract
Description
Technical Field
[0001] The present invention relates to the use of certain combinations of additives in copolyesters to improve the flame retardant properties of the copolyester compositions. More specifically, the present invention relates to the use of non-halogenated flame retardants in copolyesters to improve the flame retardant properties while maintaining adequate physical properties for molded part applications. Background Art
[0002] Flame retardant materials are added to some polymers to improve flame retardancy, especially to meet specific fire protection standards, such as UL94 V-2 or higher standards. However, adding flame retardant materials in an amount sufficient to meet the fire protection standards may have a harmful effect on certain physical properties of the copolyester containing an effective amount of flame retardant materials. In addition, no matter how much flame retardant material is added, it is impossible to meet the UL94 VO or higher fire protection standards, let alone maintain the necessary physical properties of the polymer composition.
[0003] Copolyesters can be flame-retarded in a variety of ways, but these methods also have some disadvantages. Certain halogen compounds of decabromodiphenyl oxide or decabromodiphenyl ether can be effective flame retardants, but may be opposed in the market due to potential bioaccumulation issues. Other halogen compounds may not have the same problem, but may cause embrittlement when used in sufficient amounts to make copolyesters flame retardant. Liquid phosphorus compounds such as triphenyl phosphite or triphenyl phosphate can make copolyesters flame retardant, but at effective use levels, they plasticize and soften the copolyesters, thereby reducing heat deformation resistance. Solid flame retardants of the melamine and phosphorus types can also be used alone, but in the past such additives have not been able to meet UL94 VO or higher fire protection standards at 1.5mm or thinner. Plastics used in many applications such as electronic applications, housings for handheld and fixed appliances, and housings or shells for handheld and fixed power tools have flammability requirements specified in various specifications or standards. In addition to flammability requirements, these applications also have durability or physical property requirements.
[0004] There is a need for improved copolyester compositions comprising effective flame retardants that exhibit good flame retardancy and have acceptable physical properties. Summary of the invention
[0005] Applicants have unexpectedly discovered an improved copolyester composition comprising an effective amount of certain non-halogenated flame retardants for use in making articles such as films, sheets, molded parts or profiles which exhibit good flame retardancy while maintaining glass transition temperature and otherwise providing acceptable physical properties.
[0006] In one aspect, a copolyester composition is provided, comprising:
[0007] (a) an amount of about 45 weight percent to about 95 weight percent of a copolyester comprising:
[0008] (i) a diacid component comprising
[0009] 70 mol % to 100 mol % of terephthalic acid residues,
[0010] 0 to 30 mol% of a modified aromatic diacid residue having 8 to 12 carbon atoms, and
[0011] 0 to 10 mol% of aliphatic dicarboxylic acid residues; and
[0012] (ii) a diol component comprising
[0013] 45 mol% to 95 mol% cyclohexanedimethanol (CHDM) residues
[0014] 5 to 65 mol% 2,2,4,4-tetramethylcyclobutane-1,3-diol (TMCD) residues, and
[0015] 0 to 10 mol% of a modifying diol having 2 to 20 carbon atoms;
[0016] wherein the copolyester has an intrinsic viscosity of 0.5 dL / g to 1.2 dL / g, as measured at 25° C. in 60 / 40 (wt / wt) phenol / tetrachloroethane at a concentration of 0.5 g / 100 ml,
[0017] wherein weight % is based on the weight of the copolyester, and
[0018] wherein the total mole % of the dicarboxylic acid component is 100 mole % and the total mole % of the diol component is 100 mole %;
[0019] (b) a flame retardant additive comprising a polyphosphonate compound, the flame retardant additive being present in an amount from about 5 wt % to about 55 wt %;
[0020] (c) at least one of: a flame retardant synergist comprising melamine cyanurate, the synergist being present in an amount of 10 wt % to 40 wt %, and / or a multifunctional chain extender in an amount of about 0.1 wt % to about 2 wt %; and
[0021] (d) 0 wt % to about 0.5 wt % of a drip suppressant additive;
[0022] The copolyester composition has a UL 94 V-0 rating or higher.
[0023] In various embodiments, the copolyester composition further comprises: (e) from about 1 wt % to about 10 wt % of an impact modifier component.
[0024] In various embodiments, the diol component comprises 60 mol% to 95 mol% cyclohexanedimethanol residues and 5 mol% to 40 mol% 2,2,4,4-tetramethylcyclobutane-1,3-diol residues. In certain embodiments, the diol component comprises 70 mol% to 95 mol% cyclohexanedimethanol residues and 5 mol% to 30 mol%, or 10 mol% to 30 mol%, or 15 mol% to 30 mol%, or 20 mol% to 30 mol%, or 15 mol% to 25 mol% 2,2,4,4-tetramethylcyclobutane-1,3-diol residues. In certain embodiments, the diol component comprises 60 mol% to 75 mol% cyclohexanedimethanol residues and 25 mol% to 40 mol% or 30 mol% to 40 mol% 2,2,4,4-tetramethylcyclobutane-1,3-diol residues.
[0025] In various embodiments, the intrinsic viscosity of the copolyester is from 0.55 dL / g to 0.85 dL / g, or from 0.55 dL / g to 0.65 dL / g, or from 0.65 dL / g to 0.80 dL / g, or from 0.65 dL / g to 0.75 dL / g.
[0026] In various embodiments, the flame retardant additive is present in an amount from 10 wt % to 20 wt %, or from 10 wt % to 18 wt %, or from 10 wt % to 15 wt % of the copolyester composition.
[0027] In various embodiments, the flame retardant additive comprises a compound containing a polyphosphonate. In various embodiments, the polyphosphonate compound is selected from a polyphosphonate homopolymer, a polyphosphonate copolymer, a polyphosphonate oligomer, or a combination thereof. In certain embodiments, the flame retardant additive may be a polyphosphonate homopolymer selected from Nofia HM1100 or HM9000. In certain embodiments, the flame retardant additive may be a polyphosphonate copolymer, for example, Nofia AVG-4.
[0028] In various embodiments, the copolyester composition further comprises a drip inhibitor additive in an amount of 0.05 wt % to 0.4 wt %, or 0.05 wt % to 0.25 wt %, or 0.1 wt % to 0.2 wt %. The drip inhibitor may comprise a fluoropolymer. The fluoropolymer may include, but is not limited to, polytetrafluoroethylene (PTFE), for example, Teflon TMPolytetrafluoroethylene. In various embodiments, the copolyester composition further comprises a flame retardant (FR) synergist component in an amount of 15 wt % to 35 wt % or 20 wt % to 30 wt %. In various embodiments, the FR synergist component comprises a FR synergist selected from melamine cyanurate, aluminum phosphinate compounds, melamine polyphosphate (MPP), liquid phosphorus compounds (such as PhireGuard RDP and PhireGuard BDP), other organic phosphorus compounds (e.g., compounds containing phosphorus (V) with a double bond between P and N), or combinations thereof. In various embodiments, the FR synergist comprises or is melamine cyanurate.
[0029] In various embodiments, the copolyester composition further comprises a chain extender. In certain embodiments, the chain extender comprises a multifunctional epoxide chain extender.
[0030] In various embodiments, the copolyester composition has a notched Izod impact strength of 30 J / m, or 40 J / m, or 50 J / m, or 60 J / m, or 70 J / m, or 80 J / m, or 90 J / m, or 100 J / m, or 120 J / m, or 130 J / m, or 140 J / m, or 150 J / m, or 175 J / m, or 200 J / m, or 225 J / m, or 250 J / m, or 275 J / m, or 300 J / m or more, measured according to ASTM D256.
[0031] In another aspect, an article is provided, comprising a copolyester composition according to one or more or any combination of the embodiments described herein. In various embodiments, the article is in the form of a film, sheet, molded part or profile. DETAILED DESCRIPTION
[0032] The present invention may be understood more readily by reference to the following detailed description of certain embodiments and working examples of the invention.
[0033] In accordance with the purposes of the present invention, certain embodiments of the present invention are described in the Summary of the Invention and are further described below. Other embodiments of the present invention are also described herein.
[0034] The present invention provides a copolyester composition comprising a copolyester and a flame retardant additive, wherein the copolyester composition exhibits good flame retardancy, an article made from the copolyester composition, and a method of making the composition and the article. The present invention relates to the use of a certain class of flame retardant additives to improve flame retardant properties while maintaining certain other physical properties. In various embodiments, the flame retardant additive comprises a polyphosphonate compound. When the flame retardant is added with the copolyester at an appropriate concentration, the flame retardant composition possesses a Tg of about 100°C or higher while achieving a UL94 V-0 rating or higher.
[0035] In various embodiments, the polyphosphonate compound is selected from a polyphosphonate homopolymer, a polyphosphonate copolymer, a polyphosphonate oligomer, or a combination thereof. In various embodiments, the polyphosphonate homopolymer may have one or more of the following properties: a phosphorus content in the range of 5 wt % to 15 wt %, or 8 wt % to 14 wt %, or 10 wt % to 12 wt %; a weight average molecular weight of 10,000 g / mole to 150,000 g / mole measured using a polystyrene standard; and / or a Tg of 90C to 100C, or 95C to 105C. In various embodiments, the polyphosphonate copolymer may have one or more of the following properties: a phosphorus content in the range of 1 wt % to 10 wt %, or 2 wt % to 8 wt %, or 3 wt % to 7 wt %; a weight average molecular weight of 40,000 to 100,000 g / mole as measured using polystyrene standards; and / or a Tg of 100C to 155C, or 110C to 145C, or 120C to 135C. In various embodiments, the polyphosphonate oligomer may have one or more of the following properties: an average weight average molecular weight of 500 to 8,000 g / mole, or 750 to 7,000 g / mole, or 1,000 to 6,000 g / mole, as measured using polystyrene standards; and / or an acid value of 25 to 80 KOH / g, or 30 to 75 KOH / g, or 35 to 70 KOH / g.
[0036] In various embodiments, the polyphosphonate compound is present in an amount of 5 wt % to 55 wt % based on the total weight of the copolyester composition. In certain embodiments, the copolyester composition comprises a polyphosphonate compound in an amount of 5 wt % to 25 wt %, or 5 wt % to 20 wt %, or 5 wt % to 15 wt %, or 6 wt % to 12 wt % and a FR synergist component in an amount of 15 wt % to 45 wt %, or 15 wt % to 35 wt %, or 20 wt % to 30 wt %, based on the total weight of the copolyester composition. In certain embodiments, the copolyester composition comprises a polyphosphonate compound in an amount greater than 25 wt% to 55 wt%, or 30 wt% to 55 wt%, or 35 wt% to 55 wt%, or 40 wt% to 55 wt%, or 45 wt% to 55 wt%, or 30 wt% to 50 wt%, or 35 wt% to 50 wt%, or 40 wt% to 50 wt%, or 45 wt% to 50 wt% and a chain extender component in an amount from 0.1 wt% to 5 wt%, or 0.1 wt% to 4 wt%, or 0.1 wt% to 3 wt%, or 0.1 wt% to 2 wt%, or 0.1 wt% to 1 wt%, or 0.1 wt% to 0.5 wt%, based on the total weight of the copolyester composition.
[0037] In certain embodiments, the polyphosphonate compound may be a commercially available polyphosphonate homopolymer product such as HM1100, HM9000, HM5000 and / or HM7000 (from FRX Polymers). In certain embodiments, the polyphosphonate compound may be a commercially available polyphosphonate copolymer product, such as CO3000, CO6000 and / or AVG-4 (from FRX Polymers). In certain embodiments, the polyphosphonate compound may be a commercially available polyphosphonate oligomer product such as OL1000, OL1001 and / or OL3001 (from FRX Polymers).
[0038] In various embodiments, the copolyester composition further comprises a small amount of a drip inhibitor additive (as described herein), but less than 1 wt%, or less than 0.5 wt%, or less than 0.25 wt%, or less than 0.1 wt%, or less than 0.05 wt%, or contains no flame retardant synergist additive.
[0039] In various embodiments, the flame retardant synergist additive may include melamine cyanurate, aluminum phosphinate compounds, melamine polyphosphate (MPP), liquid phosphorus compounds (such as PhireGuard RDP and PhireGuard BDP), other organic phosphorus compounds (e.g., compounds containing phosphorus (V) with a double bond between P and N), or combinations thereof. In one embodiment, the FR synergist includes or is melamine cyanurate.
[0040] In other embodiments, the FR synergist additive may include a FR synergist selected from ammonium polyphosphate, melamine phosphate, melamine pyrophosphate, melamine polyphosphate, zinc melamine polyphosphate, aluminum melamine polyphosphate, DOPO and DOPO derivatives, p-methylphenyl phosphate, or combinations thereof.
[0041] For component (e) impact modifier, this compound is usually an elastic compound or polymer, which plays a role in absorbing or dissipating impact kinetic energy. A variety of known materials are useful for component (e). Various impact modifiers can be used to practice the present invention. Preferred impact modifiers are those impact modifiers including at least one functional group capable of reacting with at least one end group of a macrocyclic polyester oligomer. Examples of suitable impact modifiers include, but are not limited to, various known graft copolymers, core-shell polymers, and block copolymers. These polymers may include at least one monomer selected from the group consisting of olefins, dienes, aromatic hydrocarbons, acrylates, and alcohols. (See, for example, EP 1,694,771B1). An example includes core-shell polymers, wherein the core is composed of a rubbery polymer and the shell is composed of a styrene copolymer (see, for example, U.S. Patent No. 5,321,056, which is incorporated herein by reference.) Other examples include core-shell polyolefins and functional polyolefins, such as those described in US2014 / 0256848 A1, which are incorporated herein by reference. See also EP 2139948 B1.
[0042] Examples of impact modifiers that can be used include, but are not limited to, ethylene / propylene terpolymers; functionalized polyolefins, such as those containing methyl acrylate and / or glycidyl methacrylate; styrene-based block copolymer impact modifiers, and various acrylic core / shell impact modifiers. Residues of such additives are also considered part of the polyester composition.
[0043] While not exclusive or exhaustive, some examples of commercially available impact modifiers may include:
[0044] Available from Nippon Oil & Fat Corporation 4300 and 4400; Kane available from Kaneka Americas Holding, Inc. M300; Kane available from Kaneka Americas Holding, Inc. B564; Kane available from Kaneka Americas Holding, Inc. ECO 1000; and available from Arkema 8900.
[0045] The impact modifier used as component (e) is generally present in an amount of about 1 to about 10 weight percent. In other embodiments, they are present in an amount of about 2 weight % to 10 weight %, or 3 weight % to 9 weight %, or 4 weight % to 8 weight %.
[0046] In various embodiments, the copolyester composition further comprises a compatibilizer that improves the compatibility of the flame retardant additive and / or FR additive synergist with the copolyester composition matrix. In various embodiments, the compatibilizer may comprise a silicone resin. In various embodiments, the silicone resin is liquid at 25°C.
[0047] Copolyesters useful in the present invention comprise the residues of an aromatic diacid and the residues of two or more diols.
[0048] As used herein, the term "copolyester" is intended to include "polyester" and is understood to refer to a synthetic polymer prepared by the reaction of one or more difunctional carboxylic acids and / or polyfunctional carboxylic acids with one or more difunctional hydroxy compounds and / or polyfunctional hydroxy compounds. The difunctional carboxylic acid can be a dicarboxylic acid, and the difunctional hydroxy compound can be a diol, such as, for example, a diol. In addition, as used in this application, the interchangeable terms "diacid" or "dicarboxylic acid" include polyfunctional acids, such as branching agents. As used in this application, the term "diol" includes, but is not limited to, diols, glycols, and / or polyfunctional hydroxy compounds. Alternatively, the difunctional carboxylic acid can be a hydroxycarboxylic acid, such as, for example, p-hydroxybenzoic acid, and the difunctional hydroxy compound can be an aromatic core with 2 hydroxy substituents, such as, for example, hydroquinone. As used herein, the term "residue" refers to any organic structure incorporated into a polymer by polycondensation and / or esterification of the corresponding monomers. As used herein, the term "repeat unit" refers to an organic structure having a dicarboxylic acid residue and a diol residue bonded by a carbonyl group. Thus, for example, the dicarboxylic acid residue can be derived from a dicarboxylic acid monomer or its associated acid halide, ester, salt, anhydride or mixture thereof. Thus, as used herein, the term "dicarboxylic acid" is intended to include dicarboxylic acids useful for the reaction process with diols to make polyesters and any derivatives of dicarboxylic acids, including their associated acid halides, esters, half esters, salts, half salts, anhydrides, mixed anhydrides or mixtures thereof. As used herein, the term "terephthalic acid" is intended to include terephthalic acid itself and its residues useful for the reaction process with diols to make polyesters and any derivatives of terephthalic acid, including their associated acid halides, esters, half esters, salts, half salts, anhydrides, mixed anhydrides or mixtures thereof or residues thereof. The term "modified aromatic diacid" refers to an aromatic dicarboxylic acid other than terephthalic acid. The term "modified glycol" refers to a glycol other than cyclohexanedimethanol (CHDM) or 2,2,4,4-tetramethylcyclobutane-1,3-diol (TMCD).
[0049] In one embodiment, terephthalic acid can be used as a starting material. In another embodiment, dimethyl terephthalate can be used as a starting material. In another embodiment, a mixture of terephthalic acid and dimethyl terephthalate can be used as a starting material and / or intermediate material.
[0050] The copolyester used in the present invention can generally be prepared from dicarboxylic acids and diols, which react in substantially equal proportions and are incorporated into the copolyester polymer as their corresponding residues. Therefore, the copolyester of the present invention can contain substantially equal molar proportions of acid residues (100 mole %) and diol (and / or multifunctional hydroxy compound) residues (100 mole %), so that the total mole number of repeating units is equal to 100 mole %. Therefore, the mole percentage provided in the present disclosure can be based on the total mole number of acid residues, the total mole number of diol residues, or the total mole number of repeating units. For example, a copolyester containing 30 mole % of isophthalic acid (based on total acid residues) means that the copolyester contains 30 mole % of isophthalic acid residues in a total of 100 mole % of acid residues. Therefore, there are 30 moles of isophthalic acid residues in every 100 moles of acid residues. In another example, a copolyester containing 30 mole % of 1,4-cyclohexanedimethanol (based on total diol residues) means that the copolyester contains 30 mole % of 1,4-cyclohexanedimethanol residues in a total of 100 mole % of diol residues. Thus, there are 30 moles of 1,4-cyclohexanedimethanol residues per 100 moles of diol residues.
[0051] In various embodiments, the copolyester comprises 70 mol % to 100 mol % of terephthalic acid (TPA). Alternatively, the copolyester comprises 80 mol % to 100 mol % TPA, or 90 mol % to 100 mol % TPA, or 95 mol % to 100 mol % TPA, or 100 mol % TPA. For purposes of this disclosure, the terms "terephthalic acid" and "dimethyl terephthalate" are used interchangeably herein.
[0052] In addition to terephthalic acid, the dicarboxylic acid component of the copolyester useful for the present invention can contain up to 30 mol%, up to 20 mol%, up to 10 mol%, up to 5 mol%, or up to 1 mol% of one or more modified aromatic dicarboxylic acids. Another embodiment contains 0 mol% modified aromatic dicarboxylic acids. Therefore, if present, it is envisioned that the amount of one or more modified aromatic dicarboxylic acids can be within the range of any of the aforementioned endpoint values, including, for example, 0.01 mol% to 30 mol%, 0.01 mol% to 20 mol%, 0.01 mol% to 10 mol%, 0.01 mol% to 5 mol%, and 0.01 mol% to 1 mol. In one embodiment, the modified aromatic dicarboxylic acids that can be used in the present invention include, but are not limited to, those aromatic dicarboxylic acids having up to 20 carbon atoms and that can be linear, para or symmetrical. Examples of modified aromatic dicarboxylic acids that can be used in the present invention include, but are not limited to, isophthalic acid, 4,4'-biphenyl dicarboxylic acid, 1,4-naphthalene dicarboxylic acid, 1,5-naphthalene dicarboxylic acid, 2,6-naphthalene dicarboxylic acid, 2,7-naphthalene dicarboxylic acid, and trans-4,4'-stilbene dicarboxylic acid and their esters. In one embodiment, the modified aromatic dicarboxylic acid is isophthalic acid.
[0053] The carboxylic acid component of the copolyester useful for the present invention can be further modified with up to 10 mol % (such as up to 5 mol % or up to 1 mol %) of one or more aliphatic dicarboxylic acids containing 2 to 16 carbon atoms (such as, for example, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid and dodecanedioic acid). Certain embodiments can also include 0.01 mol % or more (such as 0.1 mol % or more, 1 mol % or more, 5 mol % or more or 10 mol % or more) of one or more modified aliphatic dicarboxylic acids. Another embodiment contains 0 mol % modified aliphatic dicarboxylic acids. Therefore, if present, it is envisioned that the amount of one or more modified aliphatic dicarboxylic acids can be within the scope of any one of these aforementioned endpoint values, including, for example, 0.01 mol % to 10 mol % and 0.1 mol % to 10 mol %. The total mol % of the dicarboxylic acid component is 100 mol %.
[0054] The esters of terephthalic acid and other modified dicarboxylic acids or their corresponding esters and / or salts can be used to replace the dicarboxylic acids. Suitable examples of dicarboxylic acid esters include, but are not limited to, dimethyl esters, diethyl esters, dipropyl esters, diisopropyl esters, dibutyl esters, and diphenyl esters. In one embodiment, the esters are selected from at least one of the following: methyl esters, ethyl esters, propyl esters, isopropyl esters, and phenyl esters.
[0055] The copolyesters useful for the copolyester compositions of the present invention may contain 0 to 10 mole %, e.g., 0.01 to 5 mole %, 0.01 to 1 mole %, 0.05 to 5 mole %, 0.05 to 1 mole %, or 0.1 to 0.7 mole %, based on the total mole percentage of diol or diacid residues; respectively contain one or more residues of a branching monomer (also referred to herein as a branching agent) having 3 or more carboxyl substituents, hydroxyl substituents, or a combination thereof. In certain embodiments, branching monomers or branching agents may be added before and / or during and / or after the polymerization of the polyester. Thus, the copolyesters useful for the present invention may be linear or branched.
[0056] Examples of branching monomers include, but are not limited to, polyfunctional acids or polyfunctional alcohols such as trimellitic acid, trimellitic anhydride, pyromellitic dianhydride, trimethylolpropane, glycerol, pentaerythritol, citric acid, tartaric acid, 3-hydroxyglutaric acid, and the like. In one embodiment, the branching monomer residues may include 0.1 mol % to 0.7 mol % of one or more residues selected from at least one of the following: trimellitic anhydride, pyromellitic dianhydride, glycerol, sorbitol, 1,2,6-hexanetriol, pentaerythritol, trimethylolethane, and / or trimesic acid. The branching monomers may be added to the polyester reaction mixture or blended with the polyester in the form of a concentrate, as described, for example, in U.S. Pat. Nos. 5,654,347 and 5,696,176, the disclosures of which regarding branching monomers are incorporated herein by reference.
[0057] In various embodiments, CHDM can be 1,4-cyclohexanedimethanol. 1,4-cyclohexanedimethanol can be cis, trans or a mixture thereof, for example, a cis / trans ratio of 60:40 to 40:60. In another embodiment, trans-1,4-cyclohexanedimethanol can be present in an amount of 60 mol % to 80 mol %. Alternatively, 1,2-cyclohexanedimethanol and / or 1-3-cyclohexanedimethanol can be used alone or in combination with each other and / or with 1,4-cyclohexanedimethanol.
[0058] The diol component of the copolyester portion of the copolyester compositions useful for the various embodiments may contain modifying diols other than CHDM or TMCD; in one embodiment, the copolyesters useful for the invention may contain less than 15 mole %, or 10 mole % or less of one or more modifying diols.
[0059] Modifying glycols useful for the copolyesters herein refer to glycols other than CHDM or TMCD and may contain 2 to 20 or 2 to 16 carbon atoms. Examples of suitable modifying glycols include, but are not limited to, ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, neopentyl glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, p-xylene glycol, isosorbide, or mixtures thereof. In another embodiment, the modifying glycol is 1,3-propylene glycol and / or 1,4-butanediol.
[0060] In various embodiments, the copolyester composition comprises at least one polyester comprising:
[0061] (a) a dicarboxylic acid component comprising:
[0062] i) 70 to 100 mole % of terephthalic acid residues;
[0063] ii) 0 to 30 mol % of aromatic dicarboxylic acid residues having up to 20 carbon atoms; and
[0064] iii) 0 to 10 mol % of residues of aliphatic dicarboxylic acids having up to 16 carbon atoms; and
[0065] (b) a diol component comprising:
[0066] i) 5 to 55 mole % of 2,2,4,4-tetramethyl-1,3-cyclobutanediol (TMCD) residues; and
[0067] ii) 45 mol % to 95 mol % of 1,4-cyclohexanedimethanol (CHDM) residues,
[0068] wherein the total mole % of the dicarboxylic acid component is 100 mole % and the total mole % of the diol component is 100 mole %; and
[0069] wherein the polyester has an intrinsic viscosity of 0.5 dL / g to 1.2 dL / g as measured at 25°C in 60 / 40 (wt / wt) phenol / tetrachloroethane at a concentration of 0.5 g / 100 ml; and wherein the polyester has a Tg of 100°C to 200°C.
[0070] In various embodiments, the polyester composition comprises at least one polyester comprising:
[0071] (a) a dicarboxylic acid component comprising:
[0072] i) 70 to 100 mole % of terephthalic acid residues;
[0073] ii) 0 to 30 mol % of aromatic dicarboxylic acid residues having up to 20 carbon atoms; and
[0074] iii) 0 to 10 mol % of residues of aliphatic dicarboxylic acids having up to 16 carbon atoms; and
[0075] (b) a diol component comprising:
[0076] i) 20 to 40 mole % of 2,2,4,4-tetramethyl-1,3-cyclobutanediol residues; and
[0077] ii) 60 mol % to 80 mol % of 1,4-cyclohexanedimethanol residues,
[0078] wherein the total mole % of the dicarboxylic acid component is 100 mole % and the total mole % of the diol component is 100 mole %; and
[0079] wherein the polyester has an intrinsic viscosity of 0.35 dL / g to 0.85 dL / g as measured at 25°C in 60 / 40 (wt / wt) phenol / tetrachloroethane at a concentration of 0.5 g / 100 ml; and wherein the polyester has a Tg of 100°C to 120°C.
[0080] In various embodiments, the polyester composition comprises at least one polyester comprising:
[0081] (a) a dicarboxylic acid component comprising:
[0082] i) 70 to 100 mole % of terephthalic acid residues;
[0083] ii) 0 to 30 mol % of aromatic dicarboxylic acid residues having up to 20 carbon atoms; and
[0084] iii) 0 to 10 mol % of residues of aliphatic dicarboxylic acids having up to 16 carbon atoms; and
[0085] (b) a diol component comprising:
[0086] i) 40 to 55 mol % of 2,2,4,4-tetramethyl-1,3-cyclobutanediol residues;
[0087] as well as
[0088] ii) 45 mol % to 60 mol % of 1,4-cyclohexanedimethanol residues,
[0089] wherein the total mole % of the dicarboxylic acid component is 100 mole % and the total mole % of the diol component is 100 mole %; and
[0090] wherein the polyester has an intrinsic viscosity of 0.35 dL / g to 0.85 dL / g as measured at 25°C in 60 / 40 (wt / wt) phenol / tetrachloroethane at a concentration of 0.5 g / 100 ml; and wherein the polyester has a Tg of 120°C to 140°C.
[0091] In various embodiments, the polyester composition comprises at least one polyester comprising:
[0092] (a) a dicarboxylic acid component comprising:
[0093] i) 70 to 100 mole % of terephthalic acid residues;
[0094] ii) 0 to 30 mol % of aromatic dicarboxylic acid residues having up to 20 carbon atoms; and
[0095] iii) 0 to 10 mol % of residues of aliphatic dicarboxylic acids having up to 16 carbon atoms; and
[0096] (b) a diol component comprising:
[0097] i) 15 to 70 mol % of 2,2,4,4-tetramethyl-1,3-cyclobutanediol residues;
[0098] as well as
[0099] ii) 30 mol % to 85 mol % of 1,4-cyclohexanedimethanol residues,
[0100] wherein the total mole % of the dicarboxylic acid component is 100 mole % and the total mole % of the diol component is 100 mole %; and
[0101] wherein the polyester has an intrinsic viscosity of 0.35 dL / g to 0.85 dL / g, as measured at 25°C in 60 / 40 (wt / wt) phenol / tetrachloroethane at a concentration of 0.5 g / 100 ml; and wherein the polyester has a Tg of 100°C to 140°C.
[0102] In various embodiments, the polyester composition comprises at least one polyester comprising:
[0103] (a) a dicarboxylic acid component comprising:
[0104] i) 70 to 100 mole % of terephthalic acid residues;
[0105] ii) 0 to 30 mol % of aromatic dicarboxylic acid residues having up to 20 carbon atoms; and
[0106] iii) 0 to 10 mol % of residues of aliphatic dicarboxylic acids having up to 16 carbon atoms; and
[0107] (b) a diol component comprising:
[0108] i) 15 to 90 mole % of 2,2,4,4-tetramethyl-1,3-cyclobutanediol residues; and
[0109] ii) 10 to 85 mol % of 1,4-cyclohexanedimethanol residues,
[0110] wherein the total mole % of the dicarboxylic acid component is 100 mole % and the total mole % of the diol component is 100 mole %; and
[0111] wherein the polyester has an intrinsic viscosity of 0.1 dL / g to 1.2 dL / g, as measured at 25°C in 60 / 40 (wt / wt) phenol / tetrachloroethane at a concentration of 0.5 g / 100 ml; and wherein the polyester has a Tg of 100°C to 200°C.
[0112] In various embodiments, any of the polyesters or polyester compositions described herein may further comprise the residue of at least one branching agent. In various embodiments, any of the polyesters or polyester compositions described herein may comprise at least one thermal stabilizer or a reaction product thereof.
[0113] In various embodiments, the polyester composition contains at least one polycarbonate. In other embodiments, the polyester composition does not contain a polycarbonate.
[0114] In various embodiments, the polyesters may contain less than 15 mol% ethylene glycol residues, such as, for example, 0.01 mol% to less than 15 mol% ethylene glycol residues. In various embodiments, the polyesters useful for the present invention contain less than 10 mol%, or less than 5 mol%, or less than 4 mol%, or less than 2 mol%, or less than 1 mol% ethylene glycol residues, such as, for example, 0.01 mol% to less than 10 mol%, or 0.01 mol% to less than 5 mol%, or 0.01 mol% to less than 4 mol%, or 0.01 mol% to less than 2 mol%, or 0.01 mol% to less than 1 mol% ethylene glycol residues. In one embodiment, the polyesters useful for the present invention contain no ethylene glycol residues.
[0115] In other embodiments, the diol component of the polyester may include, but is not limited to, at least one of the following range combinations: 5 mol% to less than 55 mol% 2,2,4,4-tetramethyl-1,3-cyclobutanediol and greater than 45 mol% and up to 95 mol% 1,4-cyclohexanedimethanol; 5 mol% to less than 50 mol% 2,2,4,4-tetramethyl-1,3-cyclobutanediol and greater than 50 mol% and up to 95 mol% 1,4-cyclohexanedimethanol; 5 mol% to less than 45 mol% 2,2,4,4-tetramethyl-1,3-cyclobutanediol and greater than 55 mol% and up to 95 mol% 1 ,4-cyclohexanedimethanol; 5 mol% to less than 40 mol% 2,2,4,4-tetramethyl-1,3-cyclobutanediol and greater than 60 mol%, up to 95 mol% 1,4-cyclohexanedimethanol; 10 mol% to 40 mol% 2,2,4,4-tetramethyl-1,3-cyclobutanediol and 60 mol% to 90 mol% 1,4-cyclohexanedimethanol; 10 mol% to 35 mol% 2,2,4,4-tetramethyl-1,3-cyclobutanediol and 65 mol% to 90 mol% 1,4-cyclohexanedimethanol; 10 mol% to 30 mol% 2,2,4,4-tetramethyl-1,3- cyclobutanediol and 70 mol % to 90 mol % 1,4-cyclohexanedimethanol; 10 mol % to 25 mol % 2,2,4,4-tetramethyl-1,3-cyclobutanediol and 75 mol % to 90 mol % 1,4-cyclohexanedimethanol; 15 mol % to 40 mol % 2,2,4,4-tetramethyl-1,3-cyclobutanediol and 60 mol % to 85 mol % 1,4-cyclohexanedimethanol; 15 mol % to 35 mol % 2,2,4,4-tetramethyl-1,3-cyclobutanediol and 65 mol % to 85 mol % 1,4-cyclohexanedimethanol; 15 mol % to 30 mol % 2,2 ,4,4-tetramethyl-1,3-cyclobutanediol and 70 mol % to 85 mol % 1,4-cyclohexanedimethanol; 15 mol % to 25 mol % 2,2,4,4-tetramethyl-1,3-cyclobutanediol and 75 mol % to 85 mol % 1,4-cyclohexanedimethanol; 15 mol % to 20 mol % 2,2,4,4-tetramethyl-1,3-cyclobutanediol and 75 mol % to 80 mol % 1,4-cyclohexanedimethanol; and 17 mol % to 23 mol % 2,2,4,4-tetramethyl-1,3-cyclobutanediol and 77 mol % to 83 mol % 1,4-cyclohexanedimethanol.
[0116] In certain embodiments, the diol component of the polyester portion of the polyester composition may contain 25 mol % or less of one or more modified diols that are not 2,2,4,4-tetramethyl-1,3-cyclobutanediol or 1,4-cyclohexanedimethanol; in one embodiment, the polyester useful for the present invention may contain less than 15 mol % of one or more modified diols. In another embodiment, the polyester may contain 10 mol % or less of one or more modified diols. In another embodiment, the polyester may contain 5 mol % or less of one or more modified diols. In another embodiment, the polyester may contain 3 mol % or less of one or more modified diols. In another embodiment, the polyester may contain 0 mol % of modified diols. Certain embodiments may also contain 0.01 mol % or more (such as 0.1 mol % or more, 1 mol % or more, 5 mol % or more, or 10 mol % or more) of one or more modified diols. Thus, it is contemplated that the amount of modifying glycol(s), if present, can range within any of these aforementioned endpoints, including, for example, 0.01 to 15 mole % and 0.1 to 10 mole %.
[0117] In various embodiments, the modified glycol in the polyester may refer to a glycol other than 2,2,4,4,-tetramethyl-1,3-cyclobutanediol and 1,4-cyclohexanedimethanol and may contain 2 to 16 carbon atoms. In certain embodiments, examples of suitable modified glycols include, but are not limited to, ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, neopentyl glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, p-xylene glycol, or mixtures thereof. In one embodiment, the modified glycol is ethylene glycol. In another embodiment, the modified glycol is 1,3-propylene glycol and / or 1,4-butanediol. In another embodiment, ethylene glycol is excluded as a modified glycol. In another embodiment, 1,3-propylene glycol and 1,4-butanediol are excluded as modified glycols. In another embodiment, 2,2-dimethyl-1,3-propanediol is excluded as a modified glycol.
[0118] In various embodiments, the mole percent of cis-2,2,4,4-tetramethyl-1,3-cyclobutanediol in certain polyesters is greater than 50 mole percent, or greater than 55 mole percent of cis-2,2,4,4-tetramethyl-1,3-cyclobutanediol, or greater than 70 mole percent of cis-2,2,4,4-tetramethyl-1,3-cyclobutanediol; wherein the total mole percent of cis-2,2,4,4-tetramethyl-1,3-cyclobutanediol and trans-2,2,4,4-tetramethyl-1,3-cyclobutanediol equals a total of 100 mole percent.
[0119] In various embodiments, the mole percent of isomers of 2,2,4,4-tetramethyl-1,3-cyclobutanediol in certain polyesters is from 30 mole percent to 70 mole percent cis-2,2,4,4-tetramethyl-1,3-cyclobutanediol or from 30 mole percent to 70 mole percent trans-2,2,4,4-tetramethyl-1,3-cyclobutanediol, or from 40 mole percent to 60 mole percent cis-2,2,4,4-tetramethyl-1,3-cyclobutanediol or from 40 mole percent to 60 mole percent trans-2,2,4,4-tetramethyl-1,3-cyclobutanediol, wherein the total mole percent of cis-2,2,4,4-tetramethyl-1,3-cyclobutanediol and trans-2,2,4,4-tetramethyl-1,3-cyclobutanediol equals a total of 100 mole percent.
[0120] In certain embodiments, the polyester can be amorphous or semi-crystalline. In one aspect, some polyesters can have a relatively low degree of crystallinity. Thus, some polyesters can have a substantially amorphous morphology, meaning that the polyester comprises substantially disordered polymer regions.
[0121] In various embodiments, the Tg of the polyester may be at least one of the following ranges: 100°C to 200°C; 100°C to 190°C; 100°C to 180°C; 100°C to 170°C; 100°C to 160°C; 100°C to 155°C; 100°C to 150°C; 100°C to 145°C; 100°C to 140°C; 100°C to 138°C; 100°C to 135°C; 100°C to 130°C; 100°C to 125°C; 100°C to 120°C; 100°C to 115°C; 100°C to 110°C; 105°C to 200°C; 105°C to 190°C; 105°C to 180°C; 105°C to 170°C; 105°C to 160°C; 105°C to 155°C; 1 05℃ to 150℃; 105℃ to 145℃; 105℃ to 140℃; 105℃ to 138℃; 105℃ to 135℃; 105℃ to 130℃; 105℃ to 125℃; 105℃ to 120℃; 105℃ to 115℃; 105℃ to 110℃ greater than 105℃ to 125℃; greater than 105℃ to 120℃; greater than 105℃ to 115℃; greater than 105℃ to 110℃; 110℃ to 200℃; 110℃ to 190℃; 110℃ to 180℃; 110℃ to 170℃; 110℃ to 160℃; 110℃ to 155℃; 110℃ to 150℃; 110℃ to 145℃; 110℃ to 140℃; 110℃ to 138℃; 110 ℃ to 135℃; 110℃ to 130℃; 110℃ to 125℃; 110℃ to 120℃; 110℃ to 115℃; 115℃ to 200℃; 115℃ to 190℃; 115℃ to 180℃; 115℃ to 170℃; 115℃ to 160℃; 115℃ to 155℃; 115℃ to 150℃; 115℃ to 14 5℃; 115℃ to 140℃; 115℃ to 138℃; 115℃ to 135℃; 110℃ to 130℃; 115℃ to 125℃; 115℃ to 120℃; 120℃ to 200℃; 120℃ to 190℃; 120℃ to 180℃; 120℃ to 170℃; 120℃ to 160℃; 120℃ to 155℃; 1 20℃ to 150℃; 120℃ to 145℃; 120℃ to 140℃; 120℃ to 138℃; 120℃ to 135℃; 120℃ to 130℃; 125℃ to 200℃; 125℃ to 190℃; 125℃ to 180℃; 125℃ to 170℃; 125℃ to 160℃; 125℃ to 155℃; 125℃ to 150℃; 125℃ to 145℃; 125℃ to 140℃; 125℃ to 138℃; 125℃ to 135℃; 127℃ to 200℃; 127℃ to 190℃; 127℃ to 180℃; 127℃ to 170℃; 127℃ to 160℃; 127℃ to 150℃; 127℃ to 145℃; 127℃ to 140℃;127℃ to 138℃; 127℃ to 135℃; 130℃ to 200℃; 130℃ to 190℃; 130℃ to 180℃; 130℃ to 170℃; 130℃ to 160℃; 130℃ to 155℃; 130℃ to 150℃; 130℃ to 145℃; 130℃ to 140℃; 130℃ to 138℃; 130℃ to 135℃; 135℃ to 200℃; 135℃ to 190℃; 135℃ to 180℃; 135℃ to 170℃; 135℃ to 160℃; 135℃ to 155℃; 135℃ to 150℃; 135℃ to 145℃; 135℃ to 140℃; 140℃ to 200℃ ; 140°C to 190°C; 140°C to 180°C; 140°C to 170°C; 140°C to 160°C; 140°C to 155°C; 140°C to 150°C; 140°C to 145°C; 148°C to 200°C; 148°C to 190°C; 148°C to 180°C; 148°C to 170°C; 148°C to 160°C; 148°C to 155°C; 148°C to 150°C; 150°C to 200°C; 150°C to 190°C; 150°C to 180°C; 150°C to 170°C; 150 to 160; 155°C to 190°C; 155°C to 180°C; 155°C to 170°C; and 155°C to 165°C. ;
[0122] The glass transition temperature (Tg) of the polyester can be measured using a TADSC2920 from Thermal Analyst Instrument at a scanning rate of 20°C / min.
[0123] For certain embodiments, the polyester may exhibit at least one of the following intrinsic viscosities as measured in 60 / 40 (wt / wt) phenol / tetrachloroethane at a concentration of 0.5 g / 100 ml at 25° C.: 0.10 dL / g to 1.2 dL / g; 0.10 dL / g to 1.1 dL / g; 0.10 dL / g to 1 dL / g; 0.10 dL / g to less than 1 dL / g; 0.10 dL / g to 0.98 dL / g; 0.10 dL / g to 0.95 dL / g; 0.10 dL / g to 0.90 dL / g; 0.10 dL / g to 0.85 dL / g; 0.10 dL / g to 0.80 dL / g; 0.10 dL / g to 0.75 dL / g; 0. .10dL / g to less than 0.75dL / g; 0.10dL / g to 0.72dL / g; 0.10dL / g to 0.70dL / g; 0.10dL / g to less than 0.70dL / g; 0.10dL / g to 0.68dL / g; 0.10dL / g to less than 0.68dL / g; 0.10dL / g to 0.65dL / g; 0.20dL / g to 1.2dL / g; 0.20dL / g to 1.1dL / g; 0.20dL / g to 1dL / g; 0.20dL / g to less than 1dL / g; 0.20dL / g to 0.98dL / g; 0.20dL / g to 0.95dL / g; 0.20dL / g to 0.90dL / g; 0.20dL / g to 0.85dL / g; 0.20dL / g to 0.80dL / g; 0.20dL / g to 0.75dL / g; 0.20dL / g to less than 0.75dL / g; 0.20dL / g to 0.72dL / g; 0.20dL / g to 0.70dL / g; 0.20dL / g to less than 0.70dL / g; 0.20dL / g to 0.68dL / g; 0.20dL / g to less than 0.68dL / g; 0.20dL / g to 0.65dL / g; 0.35dL / g to 1.2dL / g; 0.35dL / g to 1.1dL / g; 0.35dL / g to 1dL / g; 0.35dL / g to less than 1dL / g; 0.35dL / g to 0.98dL / g; 0.35dL / g to 0.95dL / g; 0.35dL / g to 0.90dL / g; 0.35dL / g to 0.85dL / g; 0.35dL / g to 0.80dL / g; 0.35dL / g to 0.75dL / g; 0.35dL / g to Less than 0.75 dL / g; 0.35 dL / g to 0.72 dL / g; 0.35 dL / g to 0.70 dL / g; 0.35 dL / g to less than 0.70 dL / g; 0.35 dL / g to 0.68 dL / g; 0.35 dL / g to less than 0.68 dL / g; 0.35 dL / g to 0.65 dL / g; 0.40dL / g to 1.2dL / g; 0.40dL / g to 1.1dL / g; 0.40dL / g to 1dL / g; 0.40dL / g to less than 1dL / g; 0.40dL / g to 0.98dL / g; 0.40dL / g to 0.95dL / g; 0.40dL / g to 0.90dL / g; 0.40dL / g to 0.85dL / g; 0.40dL / g to 0.80dL / g; 0. 40dL / g to 0.75dL / g; 0.40dL / g to less than 0.75dL / g; 0.40dL / g to 0.72dL / g; 0.40dL / g to 0.70dL / g; 0.40dL / g to less than 0.70dL / g; 0.40dL / g to 0.68dL / g; 0.40dL / g to less than 0.68dL / g; 0.40dL / g to 0.65dL / g; greater than 0.42dL / g g to 1.2 dL / g; greater than 0.42 dL / g to 1.1 dL / g; greater than 0.42 dL / g to 1 dL / g; greater than 0.42 dL / g to less than 1 dL / g; greater than 0.42 dL / g to 0.98 dL / g; greater than 0.42 dL / g to 0.95 dL / g; greater than 0.42 dL / g to 0.90 dL / g; greater than 0.42 dL / g to 0.85 dL / g; greater than 0.42 dL / g to 0.80 dL / g; greater than 0.42 dL / g to 0.75 dL / g; greater than 0.42 dL / g to less than 0.75 dL / g; greater than 0.42 dL / g to 0.72 dL / g; greater than 0.42 dL / g to less than 0.70 dL / g; greater than 0.42 dL / g to 0.68 dL / g; greater than 0.42 dL / g to less than 0.68 dL / g; and greater than 0.42 dL / g to 0.65 dL / g.
[0124] For certain embodiments, the polyester may exhibit at least one of the following intrinsic viscosities as measured in 60 / 40 (wt / wt) phenol / tetrachloroethane at a concentration of 0.5 g / 100 ml at 25° C.: 0.45 dL / g to 1.2 dL / g; 0.45 dL / g to 1.1 dL / g; 0.45 dL / g to 1 dL / g; 0.45 dL / g to 0.98 dL / g; 0.45 dL / g to 0.95 dL / g; 0.45 dL / g to 0.90 dL / g; 0.45 dL / g to 0.85 dL / g; 0.45 dL / g to 0.80 dL / g; 0.45 dL / g to 0.75 dL / g; 0.45 dL / g to less than 0.75 dL / g g; 0.45dL / g to 0.72dL / g; 0.45dL / g to 0.70dL / g; 0.45dL / g to less than 0.70dL / g; 0.45dL / g to 0.68dL / g; 0.45dL / g to less than 0.68dL / g; 0.45dL / g to 0.65dL / g; 0.50dL / g to 1.2dL / g; 0.50dL / g to 1.1dL / g; 0.50dL / g to 1dL / g; 0.50dL / g to less than 1dL / g; 0.50dL / g to 0.98dL / g; 0.50dL / g to 0.95dL / g; 0.50dL / g to 0.90dL / g; 0.50dL / g to 0.85dL / g L / g; 0.50dL / g to 0.80dL / g; 0.50dL / g to 0.75dL / g; 0.50dL / g to less than 0.75dL / g; 0.50dL / g to 0.72dL / g; 0.50dL / g to 0.70dL / g; 0.50dL / g to less than 0.70dL / g; 0.50dL / g to 0.68dL / g; 0.50dL / g to less than 0.68dL / g; 0.50dL / g to 0.65dL / g; 0.55dL / g to 1.2dL / g; 0.55dL / g to 1.1dL / g; 0.55dL / g to 1dL / g; 0.55dL / g to less than 1dL / g; 0.55dL / g to 0 .98dL / g; 0.55dL / g to 0.95dL / g; 0.55dL / g to 0.90dL / g; 0.55dL / g to 0.85dL / g; 0.55dL / g to 0.80dL / g; 0.55dL / g to 0.75dL / g; 0.55dL / g to less than 0.75dL / g; 0.55dL / g to 0.72dL / g; 0.55dL / g to 0.70dL / g; 0.55dL / g to less than 0.70dL / g; 0.55dL / g to 0.68dL / g; 0.55dL / g to less than 0.68dL / g; 0.55dL / g to 0.65dL / g; 0.58dL / g to 1.2dL / g; 0.58dL / g to 1.1dL / g; 0.58dL / g to 1dL / g; 0.58dL / g to less than 1dL / g; 0.58dL / g to 0.98dL / g; 0.58dL / g to 0.95dL / g; 0.58dL / g to 0.90dL / g; 0.58dL / g to 0.85dL / g; 0.58dL / g to 0.80dL / g; 0.58dL / g to 0.75dL / g; 0.58dL / g to less than 0.75dL / g; 0.58dL / g to 0.72dL / g; 0.58dL / g to 0.70dL / g; 0.58dL / g to less than 0.70dL / g; 0.58dL / g to 0.68dL / g; 0 .58dL / g to less than 0.68dL / g; 0.58dL / g to 0.65dL / g; 0.60dL / g to 1.2dL / g; 0.60dL / g to 1.1dL / g; 0.60dL / g to 1dL / g; 0.60dL / g to less than 1dL / g; 0.60dL / g to 0.98dL / g; 0.60 dL / g to 0.95dL / g; 0.60dL / g to 0.90dL / g; 0.60dL / g to 0.85dL / g; 0.60dL / g to 0.80dL / g; 0.60dL / g to 0.75dL / g; 0.60dL / g to less than 0.75dL / g; 0.60dL / g to 0.72dL / g; 0 .60dL / g to 0.70dL / g; 0.60dL / g to less than 0.70dL / g; 0.60dL / g to 0.68dL / g; 0.60dL / g to less than 0.68dL / g; 0.60dL / g to 0.65dL / g; 0.65dL / g to 1.2dL / g; 0.65dL / g to 1.1dL / g; 0.65dL / g to 1dL / g; 0.65dL / g to less than 1dL / g; 0.65dL / g to 0.98dL / g; 0.65dL / g to 0.95dL / g; 0.65dL / g to 0.90dL / g; 0.65dL / g to 0.85dL / g; 0.65dL / g to 0.80dL / g; 0 .65dL / g to 0.75dL / g; 0.65dL / g to less than 0.75dL / g; 0.65dL / g to 0.72dL / g; 0.65dL / g to 0.70dL / g; 0.65dL / g to less than 0.70dL / g; 0.68dL / g to 1.2dL / g; 0.68dL / g to 1.1dL / g; 0.68dL / g to 1dL / g; 0.68dL / g to less than 1dL / g; 0.68dL / g to 0.98dL / g; 0.68dL / g to 0.95dL / g; 0.68dL / g to 0.90dL / g; 0.68dL / g to 0.85dL / g; 0.68dL / g to 0.80dL / g; 0.68dL / g to 0.75dL / g; 0.68dL / g to less than 0.75dL / g; 0.68dL / g to 0.72dL / g; greater than 0.76dL / g to 1.2dL / g; greater than 0.76dL / g to 1.1dL / g; greater than 0.76dL / g to 1dL / g; greater than 0.76dL / g to less than 1dL / g; greater than 0.76dL / g to 0.98dL / g; greater than 0.76dL / g to 0.95dL / g; greater than 0.76dL / g to 0.90dL / g; greater than 0.80dL / g to 1.2dL / g; greater than 0.80dL / g to 1.1dL / g; greater than 0.80dL / g to 1dL / g; greater than 0.80dL / g to less than 1dL / g; greater than 0.80dL / g to 1.2dL / g; greater than 0.80dL / g to 0.98dL / g; greater than 0.80dL / g to 0.95dL / g; greater than 0.80dL / g to 0.90dL / g. .
[0125] In certain embodiments, it is contemplated that the polyester composition may possess at least one of the intrinsic viscosity ranges described herein and at least one of the monomer ranges for the composition described herein, unless otherwise stated. It is also contemplated that the polyester composition may possess at least one of the Tg ranges described herein and at least one of the monomer ranges for the composition described herein, unless otherwise stated. It is also contemplated that the polyester composition may possess at least one of the Tg ranges described herein, at least one of the intrinsic viscosity ranges described herein, and at least one of the monomer ranges for the composition described herein, unless otherwise stated.
[0126] In various embodiments, the molar ratio of cis / trans 2,2,4,4-tetramethyl-1,3-cyclobutanediol may vary depending on the respective pure form or mixtures thereof. In certain embodiments, the mole percentage of cis- and / or trans-2,2,4,4-tetramethyl-1,3-cyclobutanediol is greater than 50 mole % cis and less than 50 mole % trans; or greater than 55 mole % cis and less than 45 mole % trans; or from 30 mole % to 70 mole % cis and from 70 mole % to 30 % trans; or from 40 mole % to 60 mole % cis and from 60 mole % to 40 mole % trans; or from 50 mole % to 70 mole % trans and from 50 % to 30 % cis or from 50 mole % to 70 mole % cis and from 50 % to 30 % trans; or from 60 mole % to 70 mole % cis and from 30 mole % to 40 mole % trans; or greater than 70 mole % cis and less than 30 mol % trans; wherein the sum of the mole percentages of cis- and trans-2,2,4,4-tetramethyl-1,3-cyclobutanediol is equal to 100 mole %. The molar ratio of cis / trans 1,4-cyclohexanedimethanol may vary within the range of 50 / 50 to 0 / 100, such as between 40 / 60 and 20 / 80.
[0127] The polyester part of the polyester composition can be made by methods known in the literature, such as by methods in homogeneous solution, by transesterification methods in the melt and by two-phase interface methods. Suitable methods include those disclosed in US Published Application 2006 / 0287484, the contents of which are incorporated herein by reference.
[0128] In various embodiments, the polyester may be prepared by a process comprising reacting one or more dicarboxylic acids (or derivatives thereof) with one or more diols under conditions that provide the polyester, including but not limited to the step of reacting one or more dicarboxylic acids (or derivatives thereof) with one or more diols at a temperature of 100° C. to 315° C. at a pressure of 0.1 to 760 mm Hg for a time sufficient to form the polyester. For methods of producing polyesters, see U.S. Pat. No. 3,772,405, which is incorporated herein by reference for its disclosure of such methods.
[0129] In various embodiments, the polyester composition can be a polymer blend, wherein the blend comprises: (a) 5 wt % to 95 wt % of at least one of the polyesters described herein; and (b) 5 wt % to 95 wt % of at least one polymeric component. Although not exclusive or exhaustive, some examples of potential polymeric components include, but are not limited to, nylon, polyesters other than the polyesters described herein (e.g., polyethylene or polybutylene terephthalate (PET or PBT)), polyamides (such as DuPont's ); polystyrene, polystyrene copolymers, styrene acrylonitrile copolymers, acrylonitrile butadiene styrene copolymers, poly(methyl methacrylate), acrylic acid copolymers, such as Poly(ether-imides) such as POLY(ETHER-IMIDE) (from General Electric); polyphenylene ethers such as poly(2,6-dimethylphenylene ether), or poly(phenylene ether) / polystyrene blends such as NORYL (a blend of poly(2,6-dimethylphenylene oxide) and polystyrene resin from General Electric); polyphenylene sulfide; polyphenylene sulfide / sulfone; poly(ester-carbonate); polycarbonates such as (polycarbonate from General Electric); polysulfone; polysulfone ether; and poly(ether ketone) of an aromatic dihydroxy compound; or a mixture of any of the foregoing polymers. The blends can be prepared by conventional processing techniques known in the art, such as melt blending or solution blending. In one embodiment, polycarbonate is not present in the polyester composition. However, polyester compositions useful for the present invention also contemplate excluding polycarbonate as well as including polycarbonate.
[0130] Additionally, the copolyester composition may further comprise one or more additional additives selected from colorants, dyes, mold release agents, additional flame retardants, plasticizers, processing aids, rheology modifiers, nucleating agents, antioxidants, light stabilizers, fillers, and reinforcing materials.
[0131] In various embodiments, the polyester composition and the polymer blend composition may also contain 0.01% to 25% by weight of the total composition of commonly used additives such as colorants, dyes, mold release agents, additional flame retardants, plasticizers, nucleating agents, stabilizers (including but not limited to UV stabilizers, heat stabilizers and / or reaction products thereof), fillers and impact modifiers. For example, UV additives can be incorporated into articles (e.g., ophthalmic products) by addition to the bulk or hard coating. Examples of typical commercially available impact modifiers that are well known in the art and useful for the present invention include but are not limited to ethylene / propylene terpolymers; functionalized polyolefins, such as polyolefins containing methyl acrylate and / or glycidyl methacrylate; styrene-based block copolymer impact modifiers, epoxide functionalized impact modifiers, and various acrylic core / shell impact modifiers. The residues of such additives are also considered to be part of the polyester composition. In one embodiment, the composition comprises an epoxide functionalized impact modifier.
[0132] In one aspect, the copolyester composition of the present invention comprises a copolyester composition comprising any one of the above copolyesters and a polyphosphonate compound flame retardant.
[0133] In various embodiments, the polyester may include at least one chain extender additive. Suitable chain extender additives may include, but are not limited to, multifunctional (including but not limited to difunctional) isocyanates, multifunctional epoxides (including, for example, epoxy phenolic resins) and phenoxy resins. Examples of other chain extender additives may include thioethers, carbodiimides, ethylene glycol dimers and mellitic anhydride. In various embodiments, the chain extender additive has an epoxide side group. In one embodiment, the chain extender additive may be one or more styrene-acrylate copolymers with epoxy functionality. In one embodiment, the chain extender additive may be one or more copolymers of glycidyl methacrylate and styrene. In various embodiments, the chain extender additive may be selected from epoxides modified with glycidyl methacrylate, random copolymers of styrene and glycidyl methacrylate, or a combination thereof. In various embodiments, the chain extender additive may be a glycidyl methacrylate modified epoxide having a weight average molecular weight (Mw) in the range of 5,000 g / mol to 10,000 g / mol or 6,000 g / mol to 8,000 g / mol measured using a polystyrene standard. In various embodiments, the chain extender additive may be a random copolymer of styrene and glycidyl methacrylate having a weight average molecular weight (Mw) ranging from 40,000 to 60,000 g / mole or from 45,000 to 55,000 g / mole as measured using polystyrene standards.
[0134] In various embodiments, the chain extender additive may include a polymeric additive having a plurality of pendant epoxy (or epoxide) groups per molecule. For purposes of this application, epoxy and epoxide pendant groups may be used interchangeably. In one embodiment, the polymeric chain extender additive may have an average of greater than or equal to 2 pendant epoxy groups per molecule, an average of greater than or equal to 3 pendant epoxy groups per molecule; or an average of greater than or equal to 4 pendant epoxy groups per molecule; or an average of greater than or equal to 5 pendant epoxy groups per molecule; or an average of greater than or equal to 6 pendant epoxy groups per molecule; or an average of greater than or equal to 7 pendant epoxy groups per molecule; or more specifically, an average of greater than or equal to 8 pendant epoxy groups per molecule, or more specifically, an average of greater than or equal to 11 pendant epoxy groups per molecule, or more specifically, an average of greater than or equal to 15 pendant epoxy groups per molecule, or more specifically, an average of greater than or equal to 17 pendant epoxy groups per molecule. The lower limit of the number of pendant epoxy groups may be determined by one of ordinary skill in the art to apply to specific manufacturing conditions and / or specific end-use applications. In certain embodiments, the chain extender additive may have 2 to 20 pendant epoxy groups per molecule, or 5 to 20 pendant epoxy groups per molecule, or 2 to 15 pendant epoxy groups per molecule, or 2 to 10 pendant epoxy groups per molecule, or 2 to 8 pendant epoxy groups per molecule, or 3 to 20 pendant epoxy groups per molecule, or 3 to 15 pendant epoxy groups per molecule, or 5 to 15 pendant epoxy groups per molecule, or 3 to 10 pendant epoxy groups per molecule, or 5 to 10 pendant epoxy groups per molecule, or 3 to 8 pendant epoxy groups per molecule, or 3 to 7 pendant epoxy groups per molecule.
[0135] In certain embodiments, the chain extender can be added at the end of the polymerization process or after the polymerization process. If added after the polymerization process, the chain extender can be incorporated by compounding or by adding during a conversion process such as injection molding or extrusion. The amount of the chain extender used can vary depending on the specific monomers used in the composition and the desired physical properties, but is generally 0.1 to 10 weight percent based on the total weight of the polyester, such as 0.1 to 5 weight percent. In various embodiments, the chain extender is present in an amount of 0.1 to 5 weight percent, or 0.1 to 4 weight percent, or 0.1 to 3 weight percent, or 0.1 to 2 weight percent, or 0.1 to 1 weight percent, or 0.1 to 0.75 weight percent, or 0.1 to 0.5 weight percent based on the total weight of the polyester composition.
[0136] In certain embodiments, the polyester composition (or the polyester contained in the polyester composition) may contain a heat stabilizer. In various embodiments, the heat stabilizer is a compound that can stabilize the polyester during polyester manufacturing and / or post-polymerization, and the compound includes, but is not limited to, phosphorus compounds, including, but not limited to, phosphoric acid, phosphorous acid, phosphonic acid, phosphinic acid, phosphous acid, phosphonic acid, and various esters and salts thereof. Esters can be alkyl, branched alkyl, substituted alkyl, difunctional alkyl, alkyl ether, aryl, and substituted aryl. In one embodiment, the number of ester groups present in a particular phosphorus compound can vary from zero to the maximum value allowed based on the number of hydroxyl groups present on the heat stabilizer used. The term "heat stabilizer" is intended to include its reaction products. The term "reaction product" as used in conjunction with the heat stabilizer of the present invention refers to any product of a polycondensation or esterification reaction between a heat stabilizer and any monomer used to make polyester, as well as a product of a polycondensation or esterification reaction between a catalyst and any other type of additive. In various embodiments, these may be present in a polyester composition.
[0137] In various embodiments, reinforcing materials may be useful to the polyester composition. Reinforcing materials may include, but are not limited to, carbon filaments, silicates, mica, clay, talc, titanium dioxide, wollastonite, glass flakes, glass beads and fibers, cellulose fibers and polymeric fibers and combinations thereof. In one embodiment, reinforcing materials are glass, such as fiberglass filaments, a mixture of glass and talc, a mixture of glass and mica, and a mixture of glass and polymeric fibers.
[0138] In another aspect, the invention relates to a copolyester composition comprising a copolyester produced by a process comprising:
[0139] (I) heating a mixture comprising monomers useful for any copolyester of the present invention at a temperature of 150°C to 240°C for a time sufficient to produce an initial copolyester in the presence of a catalyst;
[0140] (II) heating the initial copolyester of step (I) at a temperature of 240° C. to 320° C. for 1 to 4 hours; and
[0141] (III) Removal of any unreacted diol.
[0142] Suitable catalysts for this method include, but are not limited to, organic zinc or tin compounds. The use of such catalysts is well known in the art. Examples of catalysts useful for the present invention include, but are not limited to, zinc acetate, butyltin tri-2-ethylhexanoate, dibutyltin diacetate, and dibutyltin oxide. Other catalysts may include, but are not limited to, catalysts based on titanium, zinc, manganese, lithium, germanium, and cobalt. The amount of catalyst may be in the range of 10ppm to 20,000ppm, or 10ppm to 10,000ppm, or 10ppm to 5000ppm, or 10ppm to 1000ppm, or 10ppm to 500ppm, or 10ppm to 300ppm, or 10ppm to 250 based on the catalyst metal and based on the weight of the final polymer. The method may be carried out in batch or continuous process.
[0143] Typically, step (I) can be performed until 50 weight percent or more of the diol has reacted. Step (I) can be performed at a pressure ranging from atmospheric pressure to 100 psig. The term "reaction product" as used in conjunction with any catalyst useful for the present invention refers to any product of a polycondensation or esterification reaction with the catalyst and any monomer used to make the polyester, as well as the product of a polycondensation or esterification reaction between the catalyst and any other type of additive.
[0144] Typically, step (II) and step (III) can be performed simultaneously. These steps can be performed by methods known in the art (such as by placing the reaction mixture under a pressure ranging from 0.002 psig to below atmospheric pressure, or by blowing hot nitrogen through the mixture).
[0145] In one embodiment, a copolyester composition is provided, comprising a copolyester and a polyphosphonate compound flame retardant, wherein the composition comprises 5 to 20 weight percent of the flame retardant and 10 to 40 weight percent of the synergist based on the total weight of the composition. In one embodiment, the flame retardant consists essentially of a polyphosphonate homopolymer.
[0146] In another embodiment, a copolyester composition is provided, comprising a copolyester and a polyphosphonate compound flame retardant, wherein the composition comprises greater than 25 wt % to 55 wt % of the flame retardant and 0.1 wt % to 2 wt % of the chain extender additive based on the total weight of the composition. In one embodiment, the flame retardant consists essentially of a polyphosphonate homopolymer. In one embodiment, the flame retardant consists essentially of a polyphosphonate copolymer (e.g., polyphosphonate-co-carbonate).
[0147] The flame retardant may be incorporated into the copolyester by any conventional method to ultimately form an article.
[0148] Flame retardants can be incorporated into plastic compounding lines (such as twin-screw compounding lines) to form copolyester composition concentrates. In various embodiments, copolyester pellets are dried at 150°F to 190°F (65.6°C to 87.8°C) for 4 to 6 hours to reduce moisture. The pellets can be fed to the throat of the extruder and melted at a temperature of 400°F to 570°F (204°C to 300°C) to produce a viscous thermoplastic material. Alternatively, the flame retardant can be pre-blended and then added as a single powder with a loss-in-weight feeder, or added separately in a loss-in-weight feeder. The rotation of the two screws can disperse the flame retardant into the copolyester. The mixture can be extruded through a die to produce multiple wires. In certain embodiments, the wire can be fed to a water trough to cool the pellets. After leaving the water trough, the wire can be dried and fed to a slicing machine to cut the wire into pellets. Alternatively, the mixture can be extruded into water through a circular flat die with multiple openings. The flat die has a rotating cutter that cuts the strands into thin flakes as they are extruded from the die to produce pellets. A continuous stream of water cools the pellets and conveys them to a drying section, usually a centrifuge, where the pellets are separated from the water.
[0149] Alternatively, the flame retardant can be incorporated into a plastic compounding line such as a twin-rotor continuous compounding mixer (such as a Farrell continuous mixer) to form a copolyester composition. In various embodiments, the copolyester pellets can be dried at 150°F to 190°F (65.6°C to 87.8°C) for 4 to 6 hours to reduce moisture. The copolyester pellets and flame retardant can be fed to the throat of the continuous mixer and melted into a homogeneous mixture at a temperature of 430°F to 520°F (221°C to 271°C). The output rate of the mixer is controlled by changing the area of the discharge port. The melt can be cut into "chunks" and fed to the throat of a double-roll mill or a single-screw extruder. In the case where the melt is fed to a double-roll mill, the melt covers one of the rolls to form a concentrate sheet, which is then cut into strips that are fed to the throat of a single-screw extruder. The mixture is then extruded through a die to produce multiple strands. The wire can be fed into a water trough to cool the pellets. After leaving the water trough, the wire is dried and fed to a dicing machine to cut the wire into pellets. Alternatively, the mixture can be extruded into water through a circular flat die with multiple openings. The flat die has a rotating cutter that cuts the wire into thin slices when the wire is extruded from the die to produce pellets. The continuous water flow cools the pellets and transports them to a drying area, usually a centrifuge that separates the pellets from the water. In the case where the "lumps" are fed into a single screw extruder, the mixture can be extruded through a die to produce multiple wires. The wire can be fed into a water trough to cool the pellets. After leaving the water trough, the wire is dried and fed to a dicing machine to cut the wire into pellets. Alternatively, the mixture can be extruded into water through a circular flat die with multiple openings. The flat die has a rotating cutter that cuts the wire into thin slices when the wire is extruded from the die to produce pellets. A continuous stream of water cools the pellets and conveys them to a drying area, usually a centrifuge where the pellets are separated from the water.
[0150] Alternatively, flame retardants may be incorporated into a high intensity mixer such as In a batch mixer), the copolyester composition is formed. In various embodiments, the copolyester pellets can be dried at 150°F to 190°F (65.6°C to 87.8°C) for 4 to 6 hours to reduce moisture. The copolyester pellets and flame retardant are loaded into a high-intensity mixer, and then the punch is lowered to compress the pellet / flame retardant mixture into the mixing chamber. Two rotating mixer blades melt the pellets and disperse the flame retardant into the melt. When the desired temperature is reached, the door at the bottom of the mixer is opened and the mixture is dripped onto a double-roll mill. The ribbon from the double-roll mill can then be fed to a single screw extruder. The mixture is then extruded through a die to produce multiple wires. The wire can be fed to a water trough to cool the pellets. After leaving the water trough, the wire is dried and fed to a slicing machine to cut the wire into pellets. Alternatively, the mixture can be extruded into water through a circular flat die with multiple openings. The flat die has a rotating cutter that cuts the strands into thin flakes as they are extruded from the die to produce pellets. A continuous stream of water cools the pellets and conveys them to a drying section, usually a centrifuge, where the pellets are separated from the water.
[0151] The present invention includes plastic articles comprising the copolyester composition. The plastic articles can be made by methods including, but not limited to, extruding the copolyester composition to produce continuous flat sheets or profiles, or injection molding to produce discrete articles, or calendering to produce continuous films or sheets, or additive manufacturing powders or filaments to produce three-dimensional shapes.
[0152] Films and / or sheets useful for the present invention can have any thickness that will be apparent to one of ordinary skill in the art. In one embodiment, the films of the present invention have a thickness of less than 30 mils, or less than 20 mils, or less than 10 mils, or less than 5 mils. In one embodiment, the sheets of the present invention have a thickness greater than 30 mils. In one embodiment, the sheets of the present invention have a thickness of 30 mils to 100 mils, or 30 mils to 200 mils, or 30 mils to 500 mils.
[0153] The present invention further relates to films and / or sheets comprising the polyester compositions of the present invention. Methods of forming polyester into films and / or sheets are well known in the art. Examples of films and / or sheets of the present invention include, but are not limited to, extruded films and / or sheets, calendered films and / or sheets, compression molded films and / or sheets, injection molded films or sheets, and solution cast films and / or sheets. Methods of making films and / or sheets include, but are not limited to, extrusion, calendering, extrusion molding, compression molding, and solution casting. These films or sheets may be manufactured or subjected to further processing, such as orientation (uniaxial or biaxial), heat setting, surface treatment, etc.
[0154] In one embodiment of the present invention, a flat sheet or profile is included. The sheet or profile is prepared by extruding a copolyester composition to produce a flat sheet or profile. In this case, the pellets of the copolyester composition are dried at 150°F to 190°F (65.6°C to 87.8°C) for 4 to 6 hours and then fed to a single screw extruder, a twin screw extruder or a conical twin screw extruder. The copolyester composition pellets are conveyed and compressed along the extruder barrel by the screw to melt the pellets and discharge the melt from the end of the extruder. The melt is fed through a screening device and / or a melt pump for removing debris to reduce pressure changes caused by the extruder. The melt is then fed to a die to form a continuous flat sheet, or fed to a profile die to form a continuous shape. In one embodiment of the present invention comprising a flat sheet die, the melt is extruded onto a series of metal rollers (usually three) to cool the melt and finish the sheet. The flat sheet is then conveyed in the form of a continuous sheet for a distance or a period of time sufficient to cool the sheet. The sheet is then trimmed to the desired width, then rolled into a roll or sheared or sawed into a sheet form of the desired size. The flat plate can also be mechanically formed into a shaped article to form the desired shaped article, then cooled by spraying water, conveying by a water tank or by blowing air to the shaped article. The article is then sawed or sheared to the desired length. In the case of a profile die, the die is designed to produce a profile of the desired shape. After leaving the die, the profile is then cooled by spraying water, conveying by a water tank or by blowing air to the profile. The profile is then sawed or sheared to the desired length. In the case of a fiber, the fiber can be pulled out from the extrusion die spinneret to reach the desired fiber diameter, and then crystallized to enhance physical properties.
[0155] In various embodiments, the copolyester composition can be prepared by a method comprising mixing pure copolyester pellets with a flame retardant and then extruding the copolyester composition. The composition containing the flame retardant can be compounded into pellets. In various embodiments, the pellets can be dried at 150°F to 190°F (65.6°C to 87.8°C) for 4 to 6 hours before extrusion. After the pellets are blended in a low-intensity mixer (such as a ribbon blender, a drum or a conical screw blender), the pellets can be dried. The pellets can be fed to an extruder, including but not limited to a single screw extruder, a twin screw extruder or a conical twin screw extruder. The pellets are conveyed and compressed along the extruder barrel by the screw to melt the pellets and discharge the melt from the end of the extruder. The melt is usually fed through a screening device and / or a melt pump for removing debris to reduce the pressure changes caused by the extruder. The melt is then fed to a die to form a continuous flat plate, or to a profile die to form a continuous shape. In the case of a flat die, the melt is extruded onto a series of metal rollers (usually three) to cool the melt and finish the sheet. The flat plate is then transported in the form of a continuous sheet for a certain distance or a period of time sufficient to cool the sheet. The flat plate can then be trimmed to the desired width, then rolled into a roll or sheared or sawn into sheet form. The flat plate can also be mechanically formed into a certain shape to form the desired shape, and then cooled by spraying water, passing through a water tank, or by blowing air to the molded product. The flat plate can then be sawed or sheared to the desired length. In the case of a film, a film can be produced and wound into a roll. In the case of a profile die, the die is designed to produce products of the desired shape. After leaving the die, the profile can then be cooled by spraying water, passing through a water tank, or by blowing air to the profile. The flat plate can then be sawed or sheared to the desired length. In the case of a fiber, the fiber can be pulled out from the extrusion die spinneret to reach the desired fiber diameter, and then crystallized to enhance physical properties.
[0156] In various embodiments, the copolyester composition may comprise mixing pure copolyester pellets with a flame retardant, then extruding them together with short or long filament glass fiber reinforcements, or extruding them into continuous glass fiber compounded films, sheets or tapes. The flame retardant-containing composition may be compounded into a single pellet. In various embodiments, the pellets may be dried at 150°F to 190°F (65.6°C to 87.8°C) for 4 to 6 hours before extrusion. The pellets may be dried separately or together after blending in a low intensity mixer such as a ribbon blender, a drum or a conical screw blender. The pellets are then fed to a single screw extruder, a twin screw extruder or a conical twin screw extruder. The pellets are conveyed and compressed along the extruder barrel by the screw to melt the pellets and discharge the melt from the end of the extruder. The melt may be fed through a screening device for removing debris and / or a melt pump to reduce pressure changes caused by the extruder. The melt can then be fed into a die to form a continuous flat plate, or fed into a profile die to form a continuous shape. In the case of a flat die, the melt is extruded onto a series of metal rollers (usually three) to cool the melt and finish the sheet. The flat plate is then conveyed in the form of a continuous sheet to cool the sheet. The flat plate can then be trimmed to the desired width, then rolled into a roll or sheared or sawed into a sheet form. The flat plate can also be mechanically formed into a certain shape to form the desired shape, then cooled by spraying water, by a water tank or by blowing air to the profile. The flat plate can then be sawed or sheared to the desired length, or a film can be produced and wound into a roll. In the case of a profile die, the die is designed to produce products of the desired shape. After leaving the die, the profile is cooled by spraying water, by a water tank or by blowing air to the profile. The profile can then be sawed or sheared to the desired length. In the case of a fiber, the fiber can be pulled out from the extrusion die spinneret to reach the desired fiber diameter, and then crystallized to enhance physical properties.
[0157] On the other hand, a method for manufacturing an article is provided, which includes extruding a fully compounded pellet of a copolyester composition comprising a copolyester and a flame retardant to produce an injection molded article. In various embodiments, the pellets can be dried at 150°F to 190°F (65.6°C to 87.8°C) for 4 to 6 hours to dry the pellets. The pellets can be fed to a reciprocating single screw extruder. The pellets are melted by the rotation and reciprocating motion of the screw. Once the pellets reach the desired temperature, the gate at the end of the extruder is opened and the molten plastic is pumped into the heated mold through the screw to form an article of the desired shape. Once the mold is filled, a coolant is pumped into the mold to cool the mold and the molten plastic. Once the plastic solidifies, the mold is opened and the article is removed from the mold.
[0158] In another embodiment, the method may include mixing neat copolyester pellets with a flame retardant concentrate to form a copolyester composition and then extruding the copolyester composition to produce an injection molded article with or without staple or filament glass fiber reinforcement.
[0159] In another embodiment, a method of producing a product is provided, which includes mixing pure copolyester pellets with a flame retardant to form a copolyester composition, and then calendering the copolyester composition to produce a film product. Calendering is a well-known process for forming a film or sheet by continuous co-rotating parallel rolls. In various embodiments of the calendering process, the pellets do not need to be pre-dried because the processing temperature is low enough (350°F to 400°F; 177°C to 204°C) so that degradation and hydrolysis of the polyester will not occur to a large extent. The copolyester and flame retardant composition can be prepared by using a high intensity mixer or extruder (including but not limited to a Buss Ko-kneader, a planetary gear extruder, a Farrell continuous mixer, a twin screw extruder or The melt is then transferred to a calender. The calender is generally composed essentially of a system of three or more large diameter heated rollers that convert the high viscosity plastic into a film or sheet. The flat sheet or film is conveyed in a continuous roll to cool the sheet. The flat sheet or film can then be trimmed to the desired width and then rolled into a roll or sheared or sawn into sheet form.
[0160] Although the copolyester composition can be prepared by mixing or blending the flame retardant and the concentrate of the copolyester, the copolyester composition can also be prepared by blending the flame retardant directly with the copolyester, using any of the mixing or blending processes previously described for making the copolyester composition by blending the flame retardant concentrate and the copolyester. In various embodiments, two or more flame retardants can be mixed or blended with the copolyester simultaneously or sequentially.
[0161] In various embodiments, articles comprising any of the copolyester compositions (described herein) can be articles or components of articles configured for or otherwise useful in any application where flame retardant properties are beneficial, for example, in one or more of the following applications: medical device housings or components, electronic device or peripheral device housings, personal electronic components, television or monitor housings or components, power tool housings or components, power adapter housings or components, home automation device components, gaming device housings or components, building and construction building materials and components, furniture and home furnishing components, wiring and connector housings or components, and automotive structural or decorative components.
[0162] The present invention may be further illustrated by the following examples of certain embodiments thereof, but it will be understood that these examples are included for illustrative purposes only and are not intended to limit the scope of the invention unless otherwise expressly stated.
[0163] Example
[0164] The following abbreviations are used: J is joule; J / m is joule / meter; MPa is megapascal; FR is flame retardant; FRS is flame retardant synergist; DS is drip inhibitor; CE is chain extender; FOT is flame out time; wt% is weight percent; TPA is terephthalic acid; TMCD is 2,2,4,4-tetramethylcyclobutane-1,3-diol, and 1,4-CHDM is 1,4-cyclohexanedimethanol. PCTM is glycol-modified polyethylene terephthalate cyclohexanedimethanol. The materials used for the tests are listed in Table 1.
[0165] Table 1: Materials used in the tests
[0166]
[0167]
[0168] The copolyester composition was prepared by compounding the material combination via extrusion process using a 26 mm twin screw extruder (Coperion ZSK 26Mc18). All components were blended with TX1000 base resin and fed to the extruder from the main stream. The processing conditions used are shown in Table 2.
[0169] Table 2. Extrusion processing conditions
[0170] parameter unit value Mould mm 3.5mm-4 holes Zone 1 Temperature ℃ 0 Zone 2 Temperature ℃ 180 Zone 3 Temperature ℃ 260 4 Zone Temperature ℃ 260 5 Zone Temperature ℃ 260 6 Zone Temperature ℃ 260 7 Zone Temperature ℃ 260 8 Zone Temperature ℃ 260 9 Zone Temperature ℃ 260 10 zone temperature ℃ 260 Temperature in Zone 11 ℃ 260 12 zone temperature ℃ 260 Mold temperature ℃ 260 Screw speed rpm 250 Production Capacity kg / hour 14
[0171] The extruded strands are pelletized by a water bath / cutter or underwater pelletizer system to achieve the appropriate pellet size / shape for further processing.
[0172] The copolyester composition was molded into parts for testing via injection molding using a FANUC 100 injection machine. The barrel temperature ranged from 260°C to 280°C, and the water-cooled mold temperature ranged from 20°C to 80°C. Test bars were molded to a thickness of 1.5 mm and 2.0 mm (for UL 94 testing) and 3.2 mm (for other testing).
[0173] Example 1
[0174] Examples 1.1 to 1.5 (and Comparative Examples 1.1 to 1.4) were prepared as described above and molded into test parts (or plates). The composition of the test bars is listed below in Table 3. After the test bars were cured for 40 hours at 23°C and 50% RH (normal), and after the test bars were cured for 168 hours at 70°C and then cured for 4 hours at 23°C and less than 20% RH (aging), UL 94 vertical burning and notched Izod impact were measured for each example. The UL 94 vertical burning test results include FOT-flameout time (seconds for 10 test bars), FD-flame dripping (number of drips), and UL94 classification. The normal test results for vertical burning and notched Izod impact are listed below in Table 4. The aging test results for vertical burning are listed below in Table 5. Additional test results for other properties are listed below in Table 6.
[0175] Table 3 - Composition of Examples 1.1 to 1.5 and Comparative Examples 1.1 to 1.4
[0176]
[0177] Table 4 - Normal results of Examples 1.1 to 1.5 and Comparative Examples 1.1 to 1.4
[0178]
[0179]
[0180] Table 5 - Aging results of Examples 1.1 to 1.5 and Comparative Examples 1.1 to 1.4
[0181]
[0182] Table 6 - Additional results for Examples 1.1 to 1.5 and Comparative Examples 1.1 to 1.4
[0183]
[0184]
[0185] Review of Tables 3 and 4 shows that EX.1 to EX.5 show that the combination of HM1100, Budit 315 and FA5601 (PTFE) has a positive effect on improving flame retardancy, with EX.4 and EX.5 demonstrating a strong UL 94 V0 rating. Comparative Examples C.1 and C.2, which only have Budit 315 and PTFE, are far from reaching the V0 rating. As for Comparative Examples C.3 and C.4, although the V0 rating is achieved, these formulations use brominated flame retardants, which are not suitable for use in certain applications.
[0186] Example 2
[0187] Prepare example 2.1 to example 2.16 as described above and mold them into test parts (or plates). Carry out UL 94 vertical burning test (under normal conditions) and measure the limiting oxygen index value of each example in these examples, and measure the notched Izod impact of example 2.13, example 2.14 and example 2.16. Composition and normal UL test results and notched Izod impact values are listed below in Table 7 and Table 8. Also carry out UL 94 vertical burning test (under aging conditions) to each example in these examples. Aging UL test results are listed below in Table 9 and Table 10.
[0188] The UL94 vertical burning test was performed on Example 2 as follows:
[0189] Normal testing was performed on a test bar with a thickness of 3.2 mm, a width of 12.7 mm and a length of 152 mm. Before testing, the test bar was cured at 23C and 50% RH for 40 hours. For the aging test, the test bar was cured at 70C for 168 hours and then cured at 23C and less than 20% RH for 40 hours. The following results were measured:
[0190] TAF - Total Afterflame (t1 + t2). TAF is measured according to the UL 94 test procedure.
[0191] RIC - Repeated Ignition Cotton (DIC). PIC is measured according to the UL 94 test procedure.
[0192] UL94 classification.
[0193] FD - Total number of flame test drops.
[0194] MFT - Maximum Flame Time (seconds). MFT is measured according to the UL 94 test procedure.
[0195] TF / GT - Total Flame and Glow Time (seconds). TF / GT is measured according to the UL 94 test procedure.
[0196] AFT(t1) - measures the afterflame time t1 according to the UL 94 test procedure.
[0197] AFT(t2) - The afterflame time t2 is measured according to the UL 94 test procedure.
[0198] LOI - The Limiting Oxygen Index value is measured by ASTM D2863.
[0199] Table 7 - Examples 2.1 to 2.8 Components / UL Normal Test Results
[0200]
[0201] Table 8 - Examples 2.9 to 2.16 Components / UL Normal Test Results
[0202]
[0203]
[0204] Table 9 - Composition / UL Aging Test Results of Examples 2.1 to 2.8
[0205]
[0206] Table 10 - Examples 2.9 to 2.16 Composition / UL Aging Test Results
[0207]
[0208] A review of Tables 7 to 10 shows that the formulations of Examples 2.13, 2.14, and 2.16 all achieve a V0 rating at 3.2 mm thickness under normal and aging tests, and that Examples 2.1 to 2.3 and 2.9 to 2.16 all achieve an afterflame time of 1 to 2 seconds. This indicates that the formulations with polyphosphonate and poly(phosphonate-co-carbonate) additives rapidly extinguish the flame, with HM1100, HM9000, and AVG-4 being the most effective, especially at 50% loading levels of the additives. The limiting oxygen index of Tritan TX1000 is about 25%. The data from Tables 7 and 8 above indicate that the limiting oxygen index values for all formulations are higher, indicating that the flame retardancy of the composition is stronger.
[0209] In addition, examples 2.13, 2.14, and 2.16 were tested for notched Izod impact strength (ASTM D256). Tritan copolyesters typically have a notched Izod impact strength of about 1000 J / m. All compositions showed a decrease in impact strength, but example 2.16 containing NofiaAVG-4 and XiBond 920 maintained a higher level of impact resistance.
[0210] The invention has been described in detail with reference to the embodiments disclosed herein, but it will be understood that variations and modifications can be effected within the spirit and scope of the invention.
Claims
1. A copolyester composition comprising: (a) from about 50% to about 95% by weight of a copolyester comprising: (i) a diacid component comprising 70 mol % to 100 mol % of terephthalic acid residues, 0 to 30 mol % of a modified aromatic diacid residue having 8 to 12 carbon atoms, and 0 to 10 mol% of aliphatic dicarboxylic acid residues; and (ii) a diol component comprising 45 mol % to 95 mol % of cyclohexanedimethanol (CHDM) residues, 5 to 65 mol% of 2,2,4,4-tetramethylcyclobutane-1,3-diol (TMCD) residues, and 0 to 10 mol% of a modifying diol having 2 to 20 carbon atoms; wherein the copolyester has an intrinsic viscosity of 0.5 dL / g to 1.2 dL / g, as measured at 25°C in 60 / 40 (wt / wt) phenol / tetrachloroethane at a concentration of 0.5 g / 100 ml, and wherein the weight % is based on the weight of the copolyester, wherein the total mole % of the dicarboxylic acid components is 100 mole % and the total mole % of the diol components is 100 mole %; and (b) a flame retardant additive comprising a polyphosphonate compound, the flame retardant additive being present in an amount from about 5 wt % to about 55 wt %; (c) at least one of: a flame retardant synergist present in an amount of 10 wt % to 40 wt %, and / or a multifunctional chain extender in an amount of about 0.1 wt % to about 5 wt %; and (d) 0 wt % to about 0.5 wt % of a drip suppressant additive; The copolyester composition has a UL 94 V-0 rating or higher.
2. The copolyester composition of claim 1, wherein the flame retardant additive is present in an amount of about 5 wt% to about 20 wt%.
3. The copolyester composition according to claim 2, wherein the copolyester composition comprises the synergist in an amount of 10 wt% to 40 wt%.
4. The copolyester composition of claim 3, wherein the synergist comprises melamine cyanurate, aluminum phosphinate compounds, melamine polyphosphate (MPP), liquid phosphorus compounds (such as PhireGuard RDP and PhireGuard BDP), other organic phosphorus compounds (e.g., compounds containing phosphorus (V) with a double bond between P and N), or combinations thereof.
5. The copolyester composition of claim 4, wherein the synergist comprises melamine cyanurate.
6. The copolyester composition of claim 1, wherein the flame retardant additive is present in an amount of about 20 wt% to about 55 wt%.
7. The copolyester composition of claim 6, wherein the copolyester composition comprises a multifunctional chain extender in an amount of about 0.1 wt% to about 2 wt%.
8. The copolyester composition according to any one of claims 1 to 7, wherein the copolyester composition comprises a drip inhibitor in an amount of 0.01 wt% to 0.5 wt%.
9. The copolyester composition of any one of claims 1 to 8, wherein the copolyester composition further comprises: (e) from about 1 wt% to about 10 wt% of an impact modifier component.
10. The copolyester composition of any one of claims 1 to 9, wherein the copolyester composition further comprises: (f) from about 0.1 wt% to about 5 wt% of a compatibilizer.
11. The copolyester composition according to any one of claims 1 to 10, wherein the diol component comprises: 60 mol % to 95 mol % of cyclohexanedimethanol residues and 5 to 40 mol % of 2,2,4,4-tetramethylcyclobutane-1,3-diol residues.
12. The copolyester composition of claim 11, wherein the diol component comprises: 70 mol % to 95 mol % of cyclohexanedimethanol residues and 5 to 30 mol%, or 10 to 30 mol%, or 15 to 30 mol%, or 20 to 30 mol%, or 15 to 25 mol% of 2,2,4,4-tetramethylcyclobutane-1,3-diol residues.
13. The copolyester composition of claim 11, wherein the diol component comprises: 60 to 75 mol % of cyclohexanedimethanol residues and 25 mol % to 40 mol % or 30 mol % to 40 mol % of 2,2,4,4-tetramethylcyclobutane-1,3-diol residues.
14. The copolyester composition of any one of claims 1 to 13, wherein the intrinsic viscosity of the copolyester is 0.55 dL / g to 0.85 dL / g, or 0.55 dL / g to 0.65 dL / g, or 0.65 dL / g to 0.80 dL / g, or 0.65 dL / g to 0.75 dL / g.
15. The copolyester composition of any one of claims 1 to 5 and 8 to 14, wherein the flame retardant additive is present in an amount of 6 to 15 wt% or 7 to 12 wt% of the copolyester composition.
16. The copolyester composition according to any one of claims 1 to 3 and 6 to 15, wherein the copolyester composition comprises a flame retardant synergist additive selected from the group consisting of ammonium polyphosphate, melamine phosphate, melamine pyrophosphate, melamine polyphosphate, zinc melamine polyphosphate, aluminum melamine polyphosphate, DOPO and DOPO derivatives, p-methylphenyl phosphate, or combinations thereof.
17. The copolyester composition according to any one of claims 1 and 6 to 16, wherein the copolyester composition further comprises a multifunctional epoxide chain extender selected from the group consisting of glycidyl methacrylate modified epoxides, random copolymers of styrene and glycidyl methacrylate, or combinations thereof.
18. The copolyester composition of any one of claims 1 to 17, wherein the copolyester composition has a notched Izod impact strength of 30 J / m, or 50 J / m, or 100 J / m, or 150 J / m, or 200 J / m, or 250 J / m, or 300 J / m, or 500 J / m or more measured according to ASTM D256.
19. The copolyester composition according to any one of claims 1 to 18, wherein the copolyester composition further comprises one or more additional additives selected from the group consisting of colorants, dyes, mold release agents, additional flame retardants, plasticizers, processing aids, rheology modifiers, nucleating agents, antioxidants, light stabilizers, fillers and reinforcing materials.
20. An article comprising the copolyester composition according to any one of claims 1 to 19, wherein the article is in the form of a film, sheet, molded part or profile, and wherein the article is selected from the group consisting of medical device housings or components, electronic device or peripheral device housings, personal electronic device components, television or monitor housings or components, power tool housings or components, power adapter housings or components, home automation device components, gaming device housings or components, building and construction materials and components, furniture and home furnishing components, wiring and connector housings or components, and automotive structural or decorative components.