High quantum computer components

By forming an oxygen-free interface between the aluminum layer and the silicon substrate, the problem of TLS defects in superconducting quantum computer components is solved, and the stability and computing performance of the quantum computer are improved.

CN119072767APending Publication Date: 2024-12-03APPLIED MATERIALS INC
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202380026528.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-08-30
Filing Date
2023-02-09
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existence of high-density two-stage system (TLS) defects in superconducting quantum computer components leads to instability of qubits and affects computing performance.

Method used

By forming an oxygen-free interface between the aluminum layer and the silicon substrate, oxygen sites are reduced, and multiple chambers in the treatment system are cleaned, deposited and cooled under vacuum conditions to prevent contact between oxygen and other contaminants and form a pattern The aluminium layer and alumina layer are melted to reduce TLS defects at the interface.

Benefits of technology

It significantly reduces the number of TLS defects that are unstable in qubits, improves the stability and computing performance of quantum computer components, and enhances the fault tolerance and scalability of quantum computing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119072767A_ABST
    Figure CN119072767A_ABST
Patent Text Reader

Abstract

Exemplary methods of manufacturing high quality quantum computing components are described. A method includes removing natural oxides from a deposition surface of a silicon substrate in a cleaning chamber of a processing system, and transferring the silicon substrate to a deposition chamber of the processing system under vacuum. The method further includes depositing an aluminum layer on the deposition surface of the silicon substrate in the deposition chamber, wherein an interface between the aluminum layer and the deposition surface of the silicon substrate is oxygen-free.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the benefit of and priority to U.S. Provisional Application No. 63 / 311,314, filed on February 17, 2022, the entire contents of which are incorporated herein by reference for all purposes. Technical Field

[0003] The present technology relates to high quality quantum computer components and methods of making the same. More specifically, the present technology relates to quantum computer components with reduced defect density, which enhances computing performance. Background Art

[0004] Integrated circuits may be made by processes that produce intricately patterned layers of material on a substrate surface. Producing patterned materials on a substrate requires controlled methods for forming and removing materials. Material properties can affect how the device operates, and can also affect how films are removed relative to each other. Plasma enhanced deposition can produce films with certain properties. Many of the films formed require additional processing to adjust or enhance the material properties of the film to provide suitable properties.

[0005] Therefore, there is a need for improved systems and methods that can be used to produce high quality devices and structures. These and other needs are addressed by the present technology. Summary of the invention

[0006] Embodiments of the present technology include a processing method for forming a device component. The method includes removing native oxide from a deposition surface of a silicon substrate in a cleaning chamber of a processing system, and transferring the silicon substrate to a deposition chamber of the processing system under vacuum. The method further includes depositing an aluminum layer on the deposition surface of the silicon substrate in the deposition chamber, wherein the interface between the aluminum layer and the deposition surface of the silicon substrate is oxygen-free.

[0007] In an additional embodiment, the method also includes providing the pre-processed silicon substrate to a degassing chamber of a processing system to form a degassed silicon substrate. The degassed silicon substrate is transferred to a cooling chamber of a processing system under vacuum to cool the silicon substrate, and is again transferred to a cleaning chamber of a processing system under vacuum. In a further embodiment, the method may also include forming a patterned photoresist layer on the aluminum layer, wherein the patterned photoresist layer includes a patterned opening, and the patterned opening provides access to the exposed portion of the aluminum layer. The exposed portion of the aluminum layer is removed downward to the underlying silicon substrate to form a patterned aluminum layer, and the patterned photoresist is removed from the patterned aluminum layer. In a further embodiment, the method includes forming the patterned aluminum layer into a device component, wherein the device component is a coplanar waveguide resonator. In an additional embodiment, the method includes providing a silicon substrate with a patterned aluminum layer to a cleaning chamber of a processing system to remove natural aluminum oxide from the exposed surface of the patterned aluminum layer, wherein removing the natural aluminum oxide forms an oxygen-free clean patterned aluminum layer on the exposed surface of the patterned aluminum layer. The silicon substrate with the cleaned patterned aluminum layer is transferred to a deposition chamber of a processing system under vacuum. The method further includes forming an aluminum oxide layer on the cleaned patterned aluminum layer in the deposition chamber. A second aluminum layer is formed on the aluminum oxide layer in the deposition chamber. The silicon substrate stays in the deposition chamber for both forming the aluminum oxide layer and forming the second aluminum layer. In more embodiments, the second aluminum layer is also formed directly on the silicon substrate, wherein the interface between the second aluminum layer and the silicon substrate is oxygen-free. In further embodiments, the method includes forming the silicon substrate with the second aluminum layer into a device component, wherein the device component is a Josephson Junction.

[0008] Embodiments of the present technology include additional processing methods for forming device components. These methods include removing native oxide from a deposition surface of a silicon substrate in a clean chamber of a processing system, and transferring the silicon substrate to a deposition chamber of a processing system under vacuum. The method also includes depositing a first aluminum layer on the deposition surface of the silicon substrate in the deposition chamber, wherein the interface between the first aluminum layer and the deposition surface of the silicon substrate is oxygen-free. The method still further includes patterning the first aluminum layer to form a first patterned aluminum layer, and forming and patterning a patterned dielectric layer on the first patterned aluminum layer and the silicon substrate. An aluminum oxide layer is formed on the first patterned aluminum layer, wherein the aluminum oxide layer is not formed on the first patterned aluminum layer covered by the patterned dielectric layer. A second aluminum layer is formed on the aluminum oxide layer and the patterned dielectric layer, wherein the silicon substrate stays in the deposition chamber for both forming the aluminum oxide layer and forming the second aluminum layer. The method additionally includes removing the patterned dielectric layer from the silicon substrate, wherein removing the patterned dielectric layer forms a second patterned aluminum layer from the second aluminum layer.

[0009] In additional embodiments, the second aluminum layer is also formed directly on the silicon substrate, wherein the interface between the second aluminum layer and the silicon substrate is oxygen-free. In further embodiments, the method may include forming the silicon substrate with the second aluminum layer into a device component, wherein the device component is a Josephson junction. In still further embodiments, the first aluminum layer and the second aluminum layer are formed by physical vapor deposition. In additional embodiments, patterning the first aluminum layer to form a first patterned aluminum layer includes reactive ion etching of the first aluminum layer. In yet additional embodiments, the dielectric layer includes a silicon oxide or silicon nitride layer formed on the first patterned aluminum layer by physical vapor deposition or flowable chemical vapor deposition. In more embodiments, patterning the first aluminum layer includes forming a photoresist layer on the first aluminum layer and patterning the first photoresist layer, wherein the photoresist layer includes a carbon-containing hard mask.

[0010] Embodiments of the present technology still further include a device component structure. The device component structure includes a silicon substrate and a first patterned aluminum layer positioned on the silicon substrate. The interface between the patterned aluminum layer and the silicon substrate is oxygen-free.

[0011] In additional embodiments, the silicon substrate comprises a silicon wafer having a volume resistivity greater than or about 3000 Ωcm. In further embodiments, the first patterned aluminum layer is characterized by a thickness of less than or about 100 nm. In still further embodiments, a first aluminum oxide layer is positioned over at least a portion of the first patterned aluminum layer, wherein the first aluminum oxide layer has a thickness of less than or about 2 nm. In still additional embodiments, the device component structure further comprises a second patterned aluminum oxide layer positioned over the first aluminum oxide layer and a portion of the silicon substrate, wherein a second interface between the second patterned aluminum layer and the silicon substrate is oxygen-free. In yet more embodiments, the device component structure forms at least a portion of a device component selected from the group consisting of a coplanar waveguide resonator and a Josephson junction.

[0012] Such techniques can provide several benefits over conventional manufacturing methods for making quantum computing components. Reducing the number of oxygen sites at the interface between the silicon substrate and the aluminum layer reduces the number of two-level-system (TLS) defects at the interface that can destabilize the quantum bit (qubit) during computation. These and other embodiments, along with many of the advantages and features of the embodiments, are described in more detail in conjunction with the following description and accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] A further understanding of the nature and advantages of the disclosed technology may be realized by reference to the remaining portions of the specification and the accompanying drawings.

[0014] Figure 1 A top plan view of an exemplary processing system is shown in accordance with an embodiment of the present technology.

[0015] Figure 2 A schematic cross-sectional view of an exemplary substrate treatment system according to an embodiment of the present technology is shown.

[0016] Figure 3 A schematic cross-sectional view of another exemplary substrate processing system in accordance with an embodiment of the present technology is shown.

[0017] Figure 4 A schematic cross-sectional view of an exemplary deposition system is shown in accordance with an embodiment of the present technology.

[0018] Figure 5 A flow chart illustrating selected operations of an exemplary method of fabricating quantum computer components in accordance with embodiments of the present technology.

[0019] FIG. 6A to FIG. 6C Shown is the development of a portion of an exemplary quantum computing component architecture in accordance with an embodiment of the present technology.

[0020] Figure 7 A bird's eye view showing an exemplary co-planar waveguide (CPW) resonator component of a quantum computer in accordance with embodiments of the present technology.

[0021] Figure 8 Graph showing the quality factor (Q-factor) of a CPW resonator component of a quantum computer in accordance with an embodiment of the present technology.

[0022] Fig. 9 A flow chart illustrating selected operations of another exemplary method of fabricating quantum computer components in accordance with embodiments of the present technology.

[0023] FIG. 10A to FIG. 10F Cross-sectional and bird's-eye views showing the development of a portion of another exemplary quantum computing component structure in accordance with embodiments of the present technology.

[0024] FIG. 11A to FIG. 11K Cross-sectional and bird's-eye views showing the development of a portion of yet another exemplary quantum computing component structure in accordance with embodiments of the present technology.

[0025] Several figures are included as schematic diagrams. It will be understood that the figures are for illustrative purposes and are not to be considered to scale unless specifically stated to be to scale. Furthermore, the figures are provided as schematic diagrams to aid understanding and may not include all aspects or information compared to realistic representations and may include exaggerated material for illustrative purposes.

[0026] In the drawings, similar components and / or features may have the same reference label. In addition, components of the same type may be distinguished by the reference label followed by a letter that distinguishes between similar components. If only the first reference label is used in this specification, the description applies to any of the similar components having the same first reference label, regardless of the letter. DETAILED DESCRIPTION

[0027] Quantum computers store and process information in the form of quantum bits, or "qubits." Keeping these qubits stable during computation is the main challenge that limits the use of quantum computers to solve complex computational problems. Qubit technology based on superconducting (SC) is considered one of the most promising and scalable ways to generate, maintain, and manipulate large numbers of stable qubits. The solid-state nature of SC-based qubit technology increases the number of qubits and qubit fidelity in quantum computers, and allows quantum computing to usher in a development milestone towards the goal of achieving fault-tolerant quantum computers.

[0028] SC-based qubit technology generates, stores, and manipulates superconducting qubits called transmons, which can be thought of as anharmonic oscillators that can be controlled and interrogated by external radio frequency signals. SC-based quantum computers can include device component structures such as Josephson junctions (JJs), coplanar waveguide (CPW) resonators, rf feeds, and quantum buses, among other components. Precision manufacturing of the structures and materials in these quantum computer components reduces the number of defects that can cause transmons to become unstable. In quantum computing terms, these defects can produce "two-level system" (TLS) defects that can redirect qubits from a stable state where they can perform computational tasks to a decoherent, unstable state where they lose computational information.

[0029] The present technology solves the problem of high density TLS defects in SC-based quantum computer components. Embodiments of the present technology include methods for manufacturing SC-based quantum computer components with oxygen-free interfaces between metal layers such as aluminum layers and substrates. The lack of oxygen sites at these interfaces reduces the number of TLS defects in the components that can cause SC-based quantum bits to become unstable. Embodiments of the present technology also include a manufacturing system that can transport substrates and partially formed device components from one processing chamber to another processing chamber under vacuum. Transporting these components under vacuum prevents oxygen from reacting with clean oxygen-free surfaces before additional layers are formed on these surfaces. This provides an oxygen-free interface between the layers, reducing the number of TLS defects at the interface. Embodiments of the present technology also include performing two or more manufacturing operations in the same processing chamber without breaking the vacuum between operations. In an embodiment, a partially formed device component may stay in the same processing chamber for forming a first material layer, followed by forming a second material layer on the first material layer, without breaking the vacuum between the forming operations. In an additional embodiment, removing a portion of the first layer to form a patterned first layer may be followed by depositing a second layer on the patterned first layer, without breaking the vacuum between the removal and forming operations. In these and other embodiments, oxygen, particulates, and other contaminants are prevented from contacting device components between operations.

[0030] Figure 1 A top plan view of an embodiment of a processing system 100 is shown in accordance with an embodiment of the present technology. In an embodiment, the processing system 100 may include a processing chamber operable to perform one or more processing operations, such as cleaning, degassing, cooling, deposition, machining, etching, patterning, baking, and curing, among other processing operations. Figure 1 As shown in , a set of front-opening standard cabins 102a-102c supply substrates of various sizes, which are received by a robot 104 and placed in a low pressure holding area 106 before being placed in one of the processing chambers 108a-108gd. A second robot 111 can be used to transport substrate wafers from the holding area 106 to the processing chambers 108a-108f and back. Each processing chamber 108a-108g can be equipped to perform one or more processing operations, such as the processing operations described herein. In an embodiment, the processing chambers 108a-108g can be configured to perform one or more cleaning, degassing, cooling, deposition, processing, etching, patterning, baking, and curing operations, and other operations. In further embodiments, one or more of the processing operations may be configured to perform plasma enhanced chemical vapor deposition, atomic layer deposition, physical vapor deposition, etching, pre-cleaning, degassing, orientation, annealing, ashing, and other processing operations to form one or more portions of device components that can be integrated into an SC-based quantum computer. Figure 1The configuration of processing chambers 108a-108g shown in FIG. 1 represents an embodiment of a processing system 100 for fabricating device components. It should be appreciated that additional embodiments of the present technology contemplate additional configurations and arrangements of the location and functionality of the processing chambers.

[0031] Figure 2 An embodiment of a type of processing chamber 200 that may be included in the processing system 100 is shown. The processing chamber 200 is operable to perform one or more cleaning operations to remove oxide materials from the surface of a substrate integrated into a device component for an SC quantum computer. In an embodiment, the processing chamber 200 provides a cleaning gas mixture that reacts and sublimates silicon oxide from the surface of a silicon substrate to leave a substantially oxygen-free clean surface. In a further embodiment, the processing chamber 200 includes a substrate pedestal 202 on which a substrate 204 is placed. In an additional embodiment, the processing chamber 200 includes a port 206 through which one or more process gases can be supplied to a substrate processing region 208 in contact with the substrate 204. In a further embodiment, the processing chamber 200 includes a heating element 210 that is operable to heat the surface of the substrate 204. In a still further embodiment, the processing chamber 200 may include a substrate lift pin 212 that is operable to lift the substrate away from the substrate pedestal 202 toward the heating element 210.

[0032] In an embodiment, the substrate 204 placed in the processing chamber 200 may contain silicon. In further embodiments, the silicon-containing substrate may include crystalline silicon and may be characterized by a volume resistivity of greater than or about 3000 Ωcm or more, greater than or about 3000 Ωcm or more, greater than or about 3000 Ωcm, greater than or about 3500 Ωcm, greater than or about 4000 Ωcm, greater than or about 4500 Ωcm, greater than or about 5000 Ωcm, or more. The silicon-containing substrate may have a surface coating of silicon oxide resulting from exposure of the substrate to oxygen in air. The silicon oxide coating may be removed by a cleaning operation in the processing chamber 200, the cleaning operation comprising exposing the silicon oxide coating to a fluorine-containing gas mixture supplied to the processing region 208. In an embodiment, the fluorine-containing gas mixture reacts with the silicon oxide coating at a reduced temperature while the substrate is in contact with the cooled substrate pedestal 202. The reaction forms a solid containing silicon and fluorine that sublimates at a temperature greater than or about 100°C. In further embodiments, lift pins 212 lift the substrate 204 and the silicon- and fluorine-containing solid closer to the heating element 210. Positioning the substrate 204 closer to the heating element 210 raises the temperature of the silicon- and fluorine-containing solid above the sublimation temperature of the solid and removes the solid from the substrate surface. The clean surface of the substrate 204 is characterized by a reduced amount of oxygen. In embodiments, the clean surface is oxygen-free.

[0033] Figure 3 Another embodiment of a processing chamber 300 that may be included in the processing system 100 is shown. The processing chamber 300 is operable to perform one or more cleaning operations to remove oxide materials from the surface of a substrate integrated into a device component for an SC quantum computer. In an embodiment, the processing chamber 300 generates a cleaning plasma that removes oxide materials from the surface of the substrate to leave a substantially oxygen-free clean surface. In a further embodiment, the processing chamber 300 includes a substrate pedestal 302 having an electrostatic chuck 303. A substrate (not shown) may be fixed by the electrostatic chuck 303 in a substrate processing region 308 of the processing chamber 300. In a further embodiment, the substrate pedestal 302 may include a cooling base 305 for reducing the temperature of a substrate in contact with the substrate pedestal to a temperature below or about 25°C, below or about 20°C, below or about 15°C, below or about 10°C, below or about 5°C, below or about 0°C, or lower. In further embodiments, the substrate pedestal 302 may include a cathode assembly 305 operable to generate an electric field that can attract ions in the cleaning plasma to a substrate positioned on the substrate pedestal 302 .

[0034] In additional embodiments, the processing chamber 300 includes a port 306 through which one or more plasma precursors can be supplied to the substrate processing region 308. In further embodiments, the plasma precursor can include a fluorine-containing precursor, such as F 2 and NF 3 In yet more embodiments, the plasma precursor may include nitrogen trifluoride (NF 3 ) which may react with the silicon oxide layer on the substrate to produce a silicon, nitrogen and fluorine-containing precursor that may sublime. 3 ) and ammonia (NH 3 In additional embodiments, the plasma precursor may include one or more reducing gases, such as hydrogen (H 2 ). In embodiments, species generated by the reducing gas may react with oxygen in an oxide layer on the substrate to form reduced oxygen-containing compounds that may be removed from the oxide layer. In further embodiments, port 306 may be integrated into a cover 309 that holds a coil 311 operable to generate an inductively coupled plasma from a plasma precursor in substrate processing region 308. In further embodiments, the processing chamber may include a pump port 313 operable to remove clean plasma effluent from substrate processing region 308. In still more embodiments, a plasma screen 314 may be positioned between substrate processing region 308 and pump port 313 to prevent charged plasma species from entering the pump port from the substrate processing region.

[0035] In an embodiment, a silicon oxide layer formed on a processing surface of a silicon-containing substrate placed in the processing chamber 300 is exposed to a cleaning plasma formed in the substrate processing region 308. The cleaning plasma removes the silicon oxide layer from the surface of the silicon-containing substrate to leave a clean processing surface on the substrate with a reduced amount of oxygen. In an embodiment, the clean processing surface is oxygen-free.

[0036] Figure 4 1 shows another embodiment of a processing chamber 400 that can be included in the processing system 100. The processing chamber 400 is operable to perform one or more deposition operations to form a metal layer on a clean surface of a substrate 402 that is integrated into a device component for an SC quantum computer. In some embodiments, the processing chamber 400 is operable to perform physical vapor deposition and form a metal layer on the substrate 402. In additional embodiments, the processing chamber 400 is operable to perform plasma enhanced chemical vapor deposition and form a metal layer from a deposition plasma generated in a substrate processing region 408 of the processing chamber 400. Figure 4 In the embodiment shown in , the processing chamber 400 can be operated to generate a sputtering plasma 407 having one or more ion species, which are coulombically accelerated into a target 409, and the sputtering plasma sputters one or more materials from the target into a substrate 402. In embodiments, the sputtering plasma 407 can be generated by one or more sputtering plasma gases, such as helium, nitrogen, and argon, and other sputtering plasma gases. In further embodiments, the target can include at least one metal deposited as a metal layer on the substrate 402. In embodiments, the at least one metal can be aluminum, among other metals.

[0037] Figure 5 A flowchart showing selected operations of an exemplary method 500 for manufacturing a quantum computer component according to an embodiment of the present technology. The method 500 will be combined with FIG. 6A to FIG. 6C 600. In an embodiment, the component structure 600 forms part of a quantum computer component, such as a superconducting coplanar waveguide (CPW) resonator. FIG. 6A to FIG. 6C In the embodiment shown in FIG. 6 , component structure 600 includes a cross-sectional view of patterned metal layer 606 formed on substrate 602. It should be appreciated that additional layers may be formed below substrate 602 and above patterned metal layer 606.

[0038] In operation 505, method 500 includes removing from substrate 602 Fig. 6A601. In an embodiment, the substrate 602 may be a silicon-containing substrate and the natural oxide layer 601 may be a silicon oxide layer. In additional embodiments, the silicon-containing substrate may include crystalline silicon and may be characterized by a volume resistivity of greater than or about 3000 Ωcm or greater, greater than or about 3000 Ωcm or greater, greater than or about 3000 Ωcm or greater, greater than or about 3000 Ωcm, greater than or about 3500 Ωcm, greater than or about 4000 Ωcm, greater than or about 4500 Ωcm, greater than or about 5000 Ωcm, or greater. In still further embodiments, the natural oxide layer 601 may be removed by reacting the silicon oxide layer with a cleaning gas mixture, the cleaning gas mixture being formed of an oxide that may evaporate or sublime. In yet further embodiments, the natural oxide layer 601 may be removed by etching techniques such as wet chemical etching, dry chemical etching, or plasma enhanced etching, and other etching techniques. In embodiments, the removal operation 505 may be operable to remove greater than or about 90 wt%, greater than or about 92.5 wt%, greater than or about 95 wt%, greater than or about 97.5 wt%, greater than or about 99 wt%, greater than or about 99.5 wt%, greater than or about 99.9 wt%, or a greater percentage of the native oxide layer 601. In additional embodiments, the removal operation 505 removes all of the native oxide layer 601 to form a clean surface of the substrate 602 that is substantially free of oxygen.

[0039] At operation 510, the method 500 further includes depositing on the clean surface of the substrate 602 Figure 6B . In embodiments, the metal layer 604 may include one or more metals, such as aluminum. In additional embodiments, the metal layer 604 may be deposited to a thickness of greater than or about 25 nm, greater than or about 50 nm, greater than or about 75 nm, greater than or about 100 nm, or greater.

[0040] In an embodiment, between the removal operation 505 and the deposition operation 510, the substrate 602 is not exposed to an oxygen-containing environment. This prevents oxygen atoms and oxygen-containing molecules, free radicals, and ions from reacting with the clean surface of the substrate 602 to form oxygen-containing compounds on the clean surface. In additional embodiments, the metal layer 604 is deposited on the surface of the substrate 602, the substrate being characterized by a significantly reduced amount of oxygen compared to a starting substrate including a native oxide layer 601. In an embodiment, the number of defects generated by oxygen groups at the interface of the deposited metal layer 604 and the clean surface of the substrate 602 is reduced by greater than or about 90%, greater than or about 95%, greater than or about 99%, greater than or about 99.5%, greater than or about 99.9%, greater than or about 99.99%, greater than or about 99.999%, or greater than the starting substrate including the native oxide layer 601. The reduction in the number of defects generated by oxygen groups reduces the number of two-level systems, which can cause qubits to become unstable and drop out of the computing process in a quantum computer.

[0041] At operation 515, the method 500 still further includes patterning the aluminum layer 604 to form Figure 6C 604. In an embodiment, the patterning of the aluminum layer 604 may include forming and patterning a mask layer (not shown) on a surface of the aluminum layer 604 opposite to a surface that interfaces with the substrate 602. In further embodiments, an etching technique may be used to etch a portion of the aluminum layer that is exposed to the etchant through the patterned mask layer. In further embodiments, the etching technique used to etch the exposed aluminum and form the patterned aluminum layer 606 may include reactive ion etching. After forming the patterned aluminum layer 606, the patterned mask layer may be removed from the component structure 600.

[0042] In an embodiment, the formation and patterning of the mask layer may be accomplished in a photomasking chamber included in the processing system 100. In a further embodiment, the substrate 602 with the aluminum layer 604 may be moved from a deposition chamber for deposition of the aluminum layer to a photomasking chamber in a low oxygen environment to reduce oxygen contact on the surface of the deposited aluminum layer. In still further embodiments, the deposition of the aluminum layer 604 and the deposition and patterning of the mask layer may be accomplished in the same chamber, and the chamber may be maintained under vacuum during both operations.

[0043] In additional embodiments, the patterned aluminum layer 606 may include one or more grooves formed in the aluminum layer. In further embodiments, the bottom side of the one or more grooves 608a-608b may be formed by the surface of the substrate 602. In still further embodiments, the width of the grooves including the substrate surface 610 in the bottom side may be characterized by a width greater than or about 1 μm, greater than or about 2 μm, greater than or about 3 μm, greater than or about 4 μm, greater than or about 5 μm, or greater. In still further embodiments, the bottom surface 610 of the groove formed by the substrate surface and the sidewall surfaces 612a-612b of the groove formed by the patterned aluminum layer 606 may be substantially oxygen-free during the patterning operation 515.

[0044] Figure 7 A bird's eye view of an exemplary coplanar waveguide (CPW) resonator component 700 of a quantum computer according to embodiments of the present technology is shown. In the illustrated embodiment, the CPW component 700 includes an rf coplanar feed line 702 and a coplanar waveguide resonator 704. In further embodiments, the coplanar waveguide resonator 704 may be a λ / 4 CPW operable to produce a resonant frequency greater than or about 5 GHz (e.g., ~5.08 GHz). In still further embodiments, the coplanar waveguide resonator 704 may have open and short circuits that terminate the ends of the CPW path.

[0045] Figure 8 is a graph depicting S11 and S12 lines of photons generated by a CPW resonator according to an embodiment of the present technology at frequencies ranging from 5.078 GHz to 5.088 GHz. The S11 line shows a sharp drop at the maximum of the S12 line, indicating a robust resonator capability to store rf energy of a qubit. The robust resonator capability to store rf energy is due, at least in part, to a reduction in the number of defects at the interface of the patterned aluminum layer and the silicon substrate in the CPW resonator. The reduction in the number of defects is due to the present processing method, which removes oxides from the substrate and forms a metal layer on a clean substrate in the absence of oxygen and other species that create a lossy interface between the metal layer and the substrate. In an embodiment, the reduction in the number of defects at the interface of the metal layer and the substrate increases the quality factor of the CPW resonator. In additional embodiments, the CPW resonator may be characterized by a quality factor greater than or about 3000, greater than or about 4000, greater than or about 5000, or greater.

[0046] Fig. 9 A flowchart showing selected operations of another exemplary method 900 for manufacturing a quantum computer component according to an embodiment of the present technology. The method 900 will be combined with FIG. 10A to FIG. 10F1000 is described with reference to the development of a portion of an exemplary quantum computing component structure 1000 shown in FIG. In an embodiment, the component structure 1000 forms part of a quantum computer component, such as a superconducting Josephson junction (JJ). FIG. 10A to FIG. 10F In the embodiment shown in FIG. 1 , component structure 1000 includes a cross-sectional view of a first patterned metal layer 1006 and a second patterned metal layer 1016 formed on substrate 1002. It should be appreciated that additional layers may be formed below substrate 1002 and above patterned metal layers 1006 and 1016.

[0047] In operation 905, method 900 includes removing a native oxide layer (not shown) from substrate 1002. In an embodiment, substrate 1002 may be a silicon-containing substrate and the native oxide layer may be a silicon oxide layer. In additional embodiments, silicon-containing substrate 1002 may include crystalline silicon and may be characterized by a volume resistivity of greater than or about 3000 Ωcm or greater, greater than or about 3000 Ωcm or greater, greater than or about 3000 Ωcm or greater, greater than or about 3000 Ωcm, greater than or about 3500 Ωcm, greater than or about 4000 Ωcm, greater than or about 4500 Ωcm, greater than or about 5000 Ωcm, or greater. In still further embodiments, the native oxide layer may be removed by reacting the silicon oxide layer with a cleaning gas mixture consisting of an oxide-forming material that may evaporate or sublime. In yet further embodiments, the native oxide layer may be removed by an etching technique, such as wet chemical etching, dry chemical etching, or plasma enhanced etching, and other etching techniques.

[0048] At operation 910, the method 900 further includes depositing on the clean surface of the substrate 1002 Fig. 10A . In an embodiment, the metal layer 1004 may include one or more metals, such as aluminum. In additional embodiments, the metal layer 1004 may be deposited to a thickness of greater than or about 25 nm, greater than or about 50 nm, greater than or about 75 nm, greater than or about 100 nm, or greater.

[0049] In an embodiment, between the removal operation 905 and the deposition operation 910, the substrate 1002 is not exposed to an oxygen-containing environment. This prevents oxygen atoms and oxygen-containing molecules, free radicals, and ions from reacting with the clean surface of the substrate 1002 to form oxygen-containing compounds on the clean surface. In additional embodiments, the metal layer 1004 is deposited on a surface of the substrate 1002, the substrate being characterized by a significantly reduced amount of oxygen compared to a starting substrate comprising a native oxide layer. In an embodiment, the number of defects generated by oxygen groups at the interface of the deposited metal layer 1004 and the clean surface of the substrate 1002 is reduced by greater than or about 90%, greater than or about 95%, greater than or about 99%, greater than or about 99.5%, greater than or about 99.9%, greater than or about 99.99%, greater than or about 99.999%, or greater than the starting substrate comprising a native oxide layer. The reduction in the number of defects generated by oxygen groups reduces the number of two-level systems, which can cause qubits to become unstable and fall out of the computational process in a quantum computer.

[0050] At operation 915, the method 900 still further includes patterning the aluminum layer 1004 to form Fig. 10B 1004. In an embodiment, the patterning of the aluminum layer 1004 may include forming and patterning a mask layer (not shown) on a surface of the aluminum layer 1004 opposite to a surface that interfaces with the substrate 1002. In further embodiments, an etching technique may be used to etch portions of the aluminum layer that are exposed to an etchant through the patterned mask layer. In further embodiments, the etching technique used to etch the exposed aluminum and form the patterned aluminum layer 1006 may include reactive ion etching. After forming the patterned aluminum layer 1006, the patterned mask layer may be removed from the component structure 1000.

[0051] At operation 920, the method 900 further includes forming a FIG. 10B to FIG. 10C1004. In an embodiment, the aluminum oxide layer 1008 may be formed by exposing the substrate 1002 and the patterned aluminum layer 1006 to an oxygen-containing environment in a processing chamber that is part of the system 100. In a further embodiment, the aluminum oxide layer 1008 may be formed by physical vapor deposition of an oxygen-containing gas or plasma on the patterned aluminum layer 1006. In still further embodiments, the substrate 1002 and the patterned aluminum layer 1006 may be cleaned to remove any oxide material formed on the exposed surfaces of the layers after patterning of the aluminum layer 1004. In still more embodiments, the aluminum oxide layer 1008 may be characterized by a thickness of less than or about 5 nm, less than or about 4 nm, less than or about 3 nm, less than or about 2 nm, less than or about 1 nm, or less. In still further embodiments, any silicon oxide formed on the exposed surface of the substrate 1002 during the formation of the aluminum oxide layer 1008 may be removed before forming an additional aluminum layer on the exposed surface of the substrate.

[0052] At operation 925, the method 900 further includes depositing on the substrate 1002 and the aluminum oxide layer 1008 FIG. 10D to FIG. 10E . In an embodiment, the second metal layer 1012 may include aluminum. In a further embodiment, the second metal layer 1012 may have the same composition as the first aluminum layer 1004. In a further embodiment, the second metal layer 1012 may be a patterned metal layer deposited on a portion of the substrate 1002 and the aluminum oxide layer 1008, such as Fig. 10E In additional embodiments, the second metal layer 1012 can be patterned by depositing and patterning a photoresist layer on the substrate 1002 and the aluminum oxide layer 1008, blanketing the second metal layer on the patterned photoresist layer, and removing portions of the second metal that are not in direct contact with the substrate 1002 or the aluminum oxide layer 1008. In yet additional embodiments, the removed portions of the second metal layer can be removed by reactive ion etching to form a patterned metal layer shown as the second metal layer 1012.

[0053] In further embodiments, the second metal layer 1012 can be characterized by a patterned metal layer having a thickness of greater than or about 25 nm, greater than or about 50 nm, greater than or about 75 nm, greater than or about 100 nm, or greater. In still further embodiments, the second metal layer 1012 can be a patterned metal layer that overlaps the aluminum oxide layer 1008 and a portion of the patterned aluminum layer 1006 to form a portion of a Josephson junction on the substrate 1002. In more embodiments, the second metal layer 1012 can be characterized by a width across the aluminum oxide layer 1008 of greater than or about 250 nm, greater than or about 300 nm, greater than or about 350 nm, greater than or about 400 nm, greater than or about 450 nm, greater than or about 500 nm, or greater.

[0054] In operation 930, the method 900 further includes forming the second metal layer 1012 as follows: Fig.10F , a portion of the aluminum oxide layer 1008 is removed. In an embodiment, the removed portion of the aluminum oxide layer 1008 may include a portion of the layer that has not been covered by forming the second metal layer 1012. In further embodiments, the removal of the portion of the aluminum oxide layer 1008 may be accomplished by one or more metal oxide cleaning techniques, including dry etching using plasma.

[0055] FIG. 11A to FIG. 11K A development of a portion of yet another exemplary quantum computing component structure 1100 is shown in accordance with an embodiment of the present technology. In an embodiment, the component structure 1100 may be part of a superconducting Josephson junction (JJ). Fig.11A A first metal layer 1104 is shown formed on a silicon substrate 1102. In additional embodiments, the first metal layer 1104 may be formed on a surface of the silicon substrate 1102 with a reduced amount of silicon oxide or no silicon oxide. In further embodiments, the interface between the deposited first metal layer 1104 and the silicon substrate 1102 has significantly fewer defects that can cause two-level system defects in the quantum computing component structure 1100. In additional embodiments, the interface formed where the surface of the first metal layer 1104 contacts the surface of the substrate 1102 may be oxygen-free. In further embodiments, the first metal layer 1104 may include aluminum.

[0056] FIG. 11B to FIG. 11CA cross-sectional view and a bird's-eye view are respectively shown of a patterned first metal layer 1106 on a substrate 1102. In an embodiment, the first metal layer 1004 may be patterned by depositing and patterning a photoresist layer on the substrate 1102, covering the first metal layer on the patterned photoresist layer, and removing portions of the first metal that are not in direct contact with the substrate 1002. In yet additional embodiments, the removed portions of the first metal may be removed by reactive ion etching to form a patterned metal layer, shown as patterned first metal layer 1106.

[0057] FIG. 11D to FIG. 11E A cross-sectional view and a bird's-eye view of a sacrificial dielectric layer 1110 formed on a portion of a patterned first metal layer 1106 and a substrate 1102 are shown, respectively. The dielectric layer 1110 can be patterned by depositing and patterning a photoresist layer on the substrate 1102 and the patterned first metal layer 1106, covering the dielectric layer on the patterned photoresist layer, and removing portions of the dielectric material that are not in direct contact with the substrate 1002 and the patterned first metal layer 1106. In an embodiment, the blanket dielectric layer can be formed by a dielectric deposition technique, such as flowable chemical vapor deposition, and plasma enhanced chemical vapor deposition, and other dielectric deposition techniques. In additional embodiments, the dielectric material can include silicon oxide or silicon nitride, and other types of dielectric materials. In still further embodiments, the dielectric layer 1110 can be characterized by a thickness greater than or about 50 nm, greater than or about 100 nm, greater than or about 150 nm, greater than or about 200 nm, greater than or about 250 nm, or greater.

[0058] FIG. 11F to FIG. 11GA cross-sectional view and a bird's-eye view of a metal oxide layer 1108 formed on portions of the patterned first metal layer 1106 not covered by the dielectric layer 1110 are shown, respectively. In an embodiment, the metal oxide layer 1108 may be formed by exposing the uncovered portions of the patterned first metal layer 1106 to an oxygen-containing environment in a processing chamber that is part of the system 100. In a further embodiment, the metal oxide layer 1108 may be formed by physical vapor deposition of an oxygen-containing gas or plasma on the patterned first metal layer 1106. In still further embodiments, the substrate 1102 and the uncovered portions of the patterned first metal layer 1106 may be cleaned to remove any oxide material formed on the exposed surface of the layer after patterning of the aluminum layer 1104. In additional embodiments, the metal oxide layer 1108 may include aluminum oxide. In yet more embodiments, the metal oxide layer 1108 may be characterized by a thickness of less than or about 5 nm, less than or about 4 nm, less than or about 3 nm, less than or about 2 nm, less than or about 1 nm, or less. In still further embodiments, any silicon oxide formed on the exposed surface of the substrate 1102 during the formation of the dielectric layer 1110 and the metal oxide layer 1108 may be removed prior to forming an additional metal layer on the exposed surface of the substrate.

[0059] FIG. 11H to FIG. 11I A cross-sectional view and a bird's-eye view are respectively shown of a second metal layer 1112 formed on portions of the patterned first metal layer 1106 not covered by the dielectric layer 1110 and may also be formed on a portion of the substrate 1102. In an embodiment, the second metal layer 1112 may include aluminum. In further embodiments, the second metal layer 1112 may have the same composition as the first aluminum layer 1104. In still further embodiments, the second metal layer 1112 may be a patterned metal layer deposited on the metal oxide layer 1108 and a portion of the substrate 1102, such as Fig.11I. In yet more embodiments, a portion of the second metal layer 1112 may also extend between the dielectric layer 1110 and the metal oxide layer 1108 to be in direct contact with the patterned first metal layer 1106. In additional embodiments, the second metal layer 1112 may be patterned by depositing and patterning a photoresist layer on the substrate 1102 and the patterned metal oxide layer 1108, covering the second metal layer on the patterned photoresist layer, and removing portions of the second metal that are not in direct contact with the substrate 1102 or the metal oxide layer 1108. In yet additional embodiments, the removed portions of the second metal layer may be removed by reactive ion etching to form a patterned metal layer shown as the second metal layer 1112. In further embodiments, the interface where the second metal layer 1112 contacts the substrate 1102 may be oxygen-free. In still more embodiments, the interface between the second metal layer 1112 and the patterned first metal layer 1106 may be oxygen-free.

[0060] Figures 11J to 11K A cross-sectional view and a bird's-eye view of the component structure 1100 are shown, respectively, after the sacrificial dielectric layer 1110 is removed from the structure. In an embodiment, the dielectric layer 1110 can be removed by a removal technique, such as wet etching, or dry etching, and other removal techniques for dielectric materials. The portion of the component structure 1100 formed after removing the dielectric layer 1110 can be a portion of a high-quality Josephson junction (JJ), which is characterized by significantly fewer two-level system (TLS) defects at the interface of the patterned first metal layer 1106 and the second metal layer 1112 with the oxide layer 1108. Reducing the number of TLS defects reduces the impact of significant decoherence mechanisms of quantum bits in quantum computer systems that include current JJs.

[0061] Embodiments of the present technology provide quantum computing components with a reduced number of two-level system (TLS) defects that cause decoherence of qubits in a quantum computer. The present technology achieves these more stable quantum computing components by forming interfaces under controlled conditions between the surface of a substrate, a metal layer, and an oxide layer. In embodiments, these interfaces have fewer TLS defects caused by contaminants on the surface, such as oxygen groups at the interface of the substrate and the metal layer. Among other benefits, the processing methods of the present technology allow for the manufacture of quantum computing components with increased fault tolerance and more scalable computing power.

[0062] In the foregoing description, for the purpose of explanation, several details have been set forth to provide an understanding of various embodiments of the present technology. However, it is apparent to one skilled in the art that certain embodiments may be practiced without some of these details or with additional details.

[0063] Where several embodiments have been disclosed, those skilled in the art will recognize that various modifications, alternative configurations, and equivalents may be used without departing from the spirit of the embodiments. In addition, a variety of well-known processes and elements have not been described to avoid unnecessarily obscuring the present technology. Accordingly, the above description should not be considered to limit the scope of the technology.

[0064] Where a range of values ​​is provided, it will be understood that unless the context clearly indicates otherwise, each intermediate value between the upper and lower limits of this range will also be specifically disclosed to the smallest fraction of the lower limit unit. Any narrower range between any mentioned value or intermediate value not mentioned in the mentioned range and any other mentioned value or intermediate value in the mentioned range is included. The upper and lower limits of these smaller ranges may be independently included or excluded in the range, and each range (where any limit, no limit, or two limits are included in the smaller range) is also included in the technology, subject to any specifically excluded limits in the mentioned range. Where the mentioned range includes one or two limits, the range excluding any one or two of these included limits is also included.

[0065] As used herein and in the appended claims, the singular forms "a," "an," and "the" include plural references unless the context clearly dictates otherwise. Thus, for example, reference to "a material" includes a plurality of such materials and reference to "the precursor" includes reference to one or more precursors and equivalents of the precursor known to those skilled in the art, and so forth.

[0066] Furthermore, when used in this specification and the appended claims, the words “comprise(s)”, “comprising”, “contain(s)”, “containing”, “include(s)”, and “including” are intended to specify the presence of stated features, integers, components, or operations, but these words do not exclude the presence or addition of one or more other features, integers, components, operations, actions, or groups.

Claims

1. A processing method for forming a device component, the processing method comprising: removing native oxide from a deposition surface of a silicon substrate in a clean chamber of a processing system; transferring the silicon substrate to a deposition chamber of the processing system under vacuum; and An aluminum layer is deposited on the deposition surface of the silicon substrate in the deposition chamber, wherein an interface between the aluminum layer and the deposition surface of the silicon substrate is oxygen-free.

2. The processing method according to claim 1, wherein the method further comprises: providing a pre-processed silicon substrate to a degassing chamber of the processing system to form a degassed silicon substrate; transferring the degassed silicon substrate to a cooling chamber of the processing system under vacuum to cool the silicon substrate; and The silicon substrate is transferred to the clean chamber of the processing system under vacuum.

3. The processing method of claim 1, wherein the method further comprises: forming a patterned photoresist layer on the aluminum layer, wherein the patterned photoresist layer includes patterned openings that provide access to exposed portions of the aluminum layer; removing the exposed portion of the aluminum layer down to the silicon substrate to form a patterned aluminum layer; and The patterned photoresist layer is removed from the patterned aluminum layer.

4. The processing method of claim 3, wherein the method further comprises: forming the patterned aluminum layer into the device component, wherein the device component is a coplanar waveguide resonator.

5. The processing method of claim 3, wherein the method further comprises: providing the silicon substrate having the patterned aluminum layer to the cleaning chamber of the processing system to remove native aluminum oxide from an exposed surface of the patterned aluminum layer, wherein the removal of the native aluminum oxide forms an oxygen-free, clean patterned aluminum layer on the exposed surface of the patterned aluminum layer; transferring the silicon substrate with the cleaned patterned aluminum layer to the deposition chamber of the processing system under vacuum; forming an aluminum oxide layer on the cleaned patterned aluminum layer in the deposition chamber; and A second aluminum layer is formed on the aluminum oxide layer in the deposition chamber, wherein the silicon substrate remains in the deposition chamber for both the forming of the aluminum oxide layer and the forming of the second aluminum layer.

6. The processing method of claim 5, wherein the second aluminum layer is also formed directly on the silicon substrate, and wherein the interface between the second aluminum layer and the silicon substrate is oxygen-free.

7. The processing method of claim 5, wherein the method further comprises: forming the silicon substrate with the second aluminum layer into the device component, wherein the device component is a Josephson junction.

8. A processing method for forming a device component, the processing method comprising: removing native oxide from a deposition surface of a silicon substrate in a clean chamber of a processing system; transferring the silicon substrate to a deposition chamber of the processing system under vacuum; depositing a first aluminum layer on the deposition surface of the silicon substrate in the deposition chamber, wherein an interface between the first aluminum layer and the deposition surface of the silicon substrate is oxygen-free; patterning the first aluminum layer to form a first patterned aluminum layer; forming and patterning a patterned dielectric layer on the first patterned aluminum layer and the silicon substrate; forming an aluminum oxide layer on the first patterned aluminum layer, wherein the aluminum oxide layer is not formed on the first patterned aluminum layer covered by the patterned dielectric layer; forming a second aluminum layer on the aluminum oxide layer and the patterned dielectric layer, wherein the silicon substrate remains in the deposition chamber for both the forming of the aluminum oxide layer and the forming of the second aluminum layer; and The patterned dielectric layer is removed from the silicon substrate, wherein the removal of the patterned dielectric layer forms a second patterned aluminum layer from the second aluminum layer.

9. The processing method of claim 8, wherein a second aluminum layer is also formed directly on the silicon substrate, and wherein an interface between the second aluminum layer and the silicon substrate is oxygen-free.

10. The processing method of claim 8, wherein the method further comprises: forming the silicon substrate with the second aluminum layer into the device component, wherein the device component is a Josephson junction.

11. The method of claim 8, wherein the first aluminum layer and the second aluminum layer are formed by physical vapor deposition.

12. The processing method of claim 8, wherein said patterning said first aluminum layer to form said first patterned aluminum layer comprises reactive ion etching of said first aluminum layer.

13. The process of claim 8, wherein the dielectric layer comprises a silicon oxide or silicon nitride layer formed on the first patterned aluminum layer by physical vapor deposition or flowable chemical vapor deposition.

14. The processing method of claim 8, wherein patterning the first aluminum layer comprises: A photoresist layer is formed on the first aluminum layer and patterned, wherein the photoresist layer includes a carbon-containing hardmask.

15. A device component structure, comprising: a silicon substrate; and A first patterned aluminum layer is positioned on the silicon substrate, wherein an interface between the patterned aluminum layer and the silicon substrate is oxygen-free.

16. The device component structure of claim 15, wherein the silicon substrate comprises a silicon wafer having a volume resistivity greater than or about 3000 Ωcm.

17. The device component structure of claim 15, wherein the first patterned aluminum layer is characterized by a thickness of less than or about 100 nm.

18. The device component structure of claim 15, wherein the structure further comprises a first aluminum oxide layer positioned on at least a portion of the first patterned aluminum layer, wherein the first aluminum oxide layer has a thickness of less than or approximately 2 nm.

19. The device component structure of claim 18, wherein the structure further comprises the first aluminum oxide layer and a second patterned aluminum oxide layer positioned on a portion of the silicon substrate, wherein a second interface between the second patterned aluminum layer and the silicon substrate is oxygen-free.

20. The device component structure of claim 15, wherein the device component structure forms a portion of a device component selected from the group consisting of a coplanar waveguide resonator and a Josephson junction.

Citation Information

Cited By

  • Manufacturing process and equipment of high-performance long-service-life cold working die

    CN121629313A