Gradient oxidation and etch of pvd metal as bottom liner in bottom-up gap fill
The gradient oxidation and erosion recovery process prioritizes the removal of metal on the side of the gap and retains the bottom seed layer, which solves the problem of incomplete metal gap filling in microelectronic devices, achieves efficient and seamless filling effect, and reduces manufacturing costs and defect risks .
Patent Information
- Application Number
- CN202380034539.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-07-19
- Filing Date
- 2023-03-20
- Publication Date
- 2024-12-03
AI Technical Summary
During the manufacturing process of microelectronic devices, the liner and seed layer may remain on the sides of the gap when the metal gap is filled, resulting in the inability to fully fill the fill material, and conventional removal methods can damage the bottom seed layer, increasing manufacturing costs and the risk of defects.
The gradient oxidation process is used to preferentially oxidize the field area of the substrate rather than the characteristic bottom surface. The oxidized part is removed in combination with the etchback process, retaining the seed layer on the bottom surface and side walls, and then bottom-up filling is used using gap fill material.
Seamless metal gap filling is achieved, reducing manufacturing costs, reducing defect risks, and improving process multiple cycle capabilities and wafer output.
Smart Images

Figure CN119072768A_ABST
Abstract
Description
Technical Field
[0001] Embodiments of the present invention relate to methods and apparatus for forming thin films. More particularly, the present disclosure relates to methods and apparatus for metal gap filling in semiconductor devices.
[0002] background
[0003] The manufacture of microelectronic devices typically involves a complex process sequence that requires hundreds of individual processes to be performed on semiconducting, dielectric, and conductive substrates. Examples of such processes include oxidation, diffusion, ion implantation, thin film deposition, cleaning, etching, photolithography, and other operations. Each operation is time-consuming and expensive.
[0004] As the critical dimensions of microelectronic devices continue to decrease, the design and manufacture of the devices on the substrate become increasingly complex. Control of critical dimensions and process uniformity becomes increasingly important. Complex multilayer stacks used to manufacture microelectronic devices involve precise process monitoring of critical dimensions of thickness, roughness, stress, density, and potential defects. The process recipe for forming the device has multiple incremental processes to ensure that the critical dimensions are maintained. Generally speaking, each incremental process may utilize one or more processing chambers, which increases the additional time for incrementally forming the device and also increases the chance of forming defects. Therefore, each process increases the overall manufacturing cost and the risk of defects in the finished microelectronic device.
[0005] In addition, as the critical dimensions of the devices shrink, past manufacturing techniques encounter new obstacles. For example, when the liner and / or seed layer is ready to grow the metal gap filler, the liner and / or seed layer may still exist on the sides of the gap, thereby potentially closing the gap before the bottom is completely filled with the fill material. Conventional methods for removing the seed layer from the sides and top surface of the gap also result in the removal of the seed layer at the bottom of the gap that was originally used to seed the fill material.
[0006] For at least the foregoing reasons, there continues to be a need for improved gapfill manufacturing methods.
[0007] Overview
[0008] The present disclosure relates to methods and apparatus for forming thin films. More particularly, the present disclosure relates to methods and apparatus for filling features on a substrate.
[0009] In one example, a method for filling a feature on a substrate is provided. The method includes forming a metal seed layer on an exposed surface of a substrate, wherein the substrate has a feature in the form of a trench or via formed in a top surface of the substrate, the feature having sidewalls and a bottom surface extending between the sidewalls. A gradient oxidation process is performed to oxidize the exposed portion of the metal seed layer to form a metal oxide, wherein the gradient oxidation process preferentially oxidizes a field region of the substrate rather than a bottom surface of the feature. An etch-back process removes or reduces an oxidized portion of the seed layer. A metal gap fill process fills or partially fills the feature with a gap fill material.
[0010] In another example, another method for filling features on a substrate is provided. The method includes depositing a molybdenum-containing layer on an exposed surface of a substrate, wherein the substrate includes a plurality of features formed in a top surface of the substrate, each of the plurality of features having a sidewall surface and a bottom surface, and the deposited molybdenum-containing layer is formed on the top surface of the substrate and on the sidewall surface and bottom surface of the plurality of features. The exposed surface of the substrate is exposed to a gradient oxidation process, wherein the gradient oxidation process forms an oxidized region containing molybdenum. The oxidized region preferentially etches the deposited molybdenum-containing layer, wherein after preferentially etching the oxidized region, a first portion of the deposited molybdenum-containing layer remains on the bottom surface of each of the plurality of features, and a second portion of the deposited molybdenum-containing layer remains on the sidewall surface of each of the plurality of features. Filling the features with a second molybdenum layer, wherein filling the features with a second molybdenum layer includes growing a second molybdenum layer in each feature from a second portion of the deposited molybdenum-containing layer on the sidewall surface and a first portion of the deposited molybdenum-containing layer on the bottom surface.
[0011] In yet another example, another cluster tool for filling features on a substrate is provided. The cluster tool includes an oxygen source fluidly coupled to a processing region of a first processing chamber, wherein the oxygen source is configured to deliver an oxygen-containing gas to the processing region. The cluster tool has a first flow control valve configured to control the flow of the oxygen-containing gas provided from the oxygen source to the processing region; an etching gas source fluidly coupled to the processing region of the first processing chamber, wherein the etching gas source is configured to deliver the etching gas to the processing region; a third flow control valve configured to control the flow of the etching gas provided from the etching gas source to the processing region; an inductively coupled plasma source configured to generate a plasma in the processing region, wherein the plasma includes an oxygen-containing gas; and a controller. The controller is configured to form a metal seed layer on an exposed surface of a substrate, wherein the substrate has a feature in the form of a trench or a through hole formed in a top surface of the substrate, the feature having sidewalls and a bottom surface extending between the sidewalls. The controller is further configured to perform a gradient oxidation process to oxidize an exposed portion of the metal seed layer to form a metal oxide, wherein the gradient oxidation process preferentially oxidizes a field region of the substrate rather than a bottom surface of the feature. The controller performs an etch-back process to remove or reduce an oxidized portion of the seed layer and performs a molybdenum gapfill process to fill or partially fill the feature with a gapfill material.
[0012] BRIEF DESCRIPTION OF THE DRAWINGS
[0013] In order to facilitate a detailed understanding of the above-mentioned features of the present disclosure, the aspects briefly summarized above may be described in more detail with reference to the embodiments, some of which are illustrated in the accompanying drawings. However, it should be noted that the drawings only illustrate typical embodiments of the present disclosure and are therefore not to be considered as limiting the scope thereof, as the present disclosure may admit to other equally effective embodiments.
[0014] Figure 1 A schematic top view of one example of a multi-chamber processing tool according to one or more embodiments of the present disclosure is shown.
[0015] FIG. 2A to FIG. 2E Views of a semiconductor device at various stages of fabrication are shown in accordance with one or more embodiments of the disclosure.
[0016] Figure 3 A flow chart is shown of a method for filling features on a substrate according to one or more embodiments of the present disclosure.
[0017] To facilitate understanding, identical reference numerals have been used, where possible, to designate identical elements in the figures. It is contemplated that elements and features of one embodiment may be beneficially incorporated in other embodiments without further recitation.
[0018] Specific description
[0019] In the above summary of the invention, the embodiments, the following claims and the accompanying drawings, reference is made to specific features (including method operations) of the present disclosure. It should be understood that the disclosure in this specification includes all possible combinations of the specific features. For example, if a specific feature or claim is disclosed in the context of a specific aspect or implementation of this specification, then the feature may also be used in combination and / or context of other specific aspects and implementations of this specification, as well as in general in this specification. For example, if a specific feature is disclosed in the context of a specific aspect or implementation of the present disclosure or a specific claim, then the feature may also be combined with other specific aspects and embodiments of the present disclosure, and / or used in the context of other specific aspects and embodiments of the present disclosure, and generally used in the present disclosure.
[0020] As used herein, the term "comprising" and its grammatical equivalents mean that other components, ingredients, operations, etc. may be present as appropriate. For example, an article "comprising" (or "which comprises") components A, B, and C may consist of (i.e., only comprise) components A, B, and C, or may not comprise only components A, B, and C but may also comprise one or more other components.
[0021] When this document refers to a method comprising two or more specified operations, the specified operations may be performed in any order or simultaneously (unless the context excludes that possibility), and the method may include one or more other operations performed before any specified operation, between two specified operations, or after all specified operations (unless the context excludes that possibility).
[0022] Embodiments of the present disclosure relate to methods and apparatus for filling features on a substrate. For example, the method can perform highly selective gradient oxidation and etching of physical vapor deposition (PVD) metals to form a bottom seed layer in a bottom-up gap fill. The metal gap fill process can be used to deposit different metals, such as tungsten (W), molybdenum (Mo), ruthenium (Ru), and other metals. The present disclosure includes separate process sequences, including metal oxidation (e.g., WO x 、MoO x ) process and selective removal process of metal oxides.
[0023] PVD metal deposition typically forms a thicker film in the area around the via (or trench) and a thinner film at the bottom of the via. The oxidation and etching gradient process selectively removes the field metal. The metal in the field around the via is "selectively" oxidized 7 times faster than the metal at the bottom of the via. Selective oxidation allows the subsequent etching process to remove the field metal oxide while leaving a small bottom metal layer as a seed for the metal fill. The etching removal of the oxidized metal in the field is very selective relative to the bottom (unoxidized) metal, which results in a thin metal seed layer remaining at the bottom of the via. The oxidation process uses an inductively coupled (ICP) oxygen (O2) plasma with low power, low O2 flow and high temperature reaction, which produces a high ion ratio at low ion energy, which improves the selectivity of preferentially oxidizing the metal in the field rather than the metal at the bottom of the via. Using this method, the field metal can be completely removed while leaving a high-quality metal seed layer at the bottom of the structure for seamless bottom-up gap filling.
[0024] Examples of processing systems that may be appropriately modified in accordance with the teachings provided herein include integrated processing systems, or other suitable processing systems available from Applied Materials, Inc. located in Santa Clara, Calif. It is contemplated that other processing systems, including systems from other manufacturers, may also be adapted to benefit from the aspects described herein.
[0025] Figure 1 A schematic top view of an exemplary multi-chamber processing system 100 or cluster tool is shown, which can be used to perform gradient oxidation and etching of PVD metals according to embodiments of the present disclosure. The processing system 100 includes a plurality of processing chambers 102 coupled to a first transfer chamber 104. The first transfer chamber 104 is also coupled to a first pair of through chambers 106. The first transfer chamber 104 has a centrally disposed transfer robot (not shown) for transferring substrates between the through chamber 106 and the processing chamber 102. The through chamber 106 is coupled to a second transfer chamber 110, which is coupled to a processing chamber 114 configured to perform a pre-cleaning process and a processing chamber 116 configured to perform a PVD deposition process, or alternatively, an epitaxial growth process or an atomic deposition chamber. The second transfer chamber 110 has a centrally disposed transfer robot (not shown) for transferring substrates between a set of load lock chambers 112 and the processing chamber 114 or the processing chamber 116. The factory interface 120 is connected to the second transfer chamber 110 via the load lock chamber 112. The factory interface 120 is coupled to one or more wafer pods 130 on the opposite side of the load lock chamber 112. The wafer pod 130 may be a front opening unified pod (FOUP) or a similar device for storing and transporting substrates.
[0026] Prior to various operations, a substrate may first be transferred from one of the wafer transfer boxes 130 to the processing chamber 114 where a pre-cleaning process is performed to remove contaminants such as carbon or oxide contaminants on exposed surfaces of source / drain regions of transistors to be formed on the substrate.
[0027] The substrate is then transferred to one or more of the processing chambers 102. In some embodiments, the processing chamber 102 may etch a through hole or trench in a dielectric material layer of the substrate. In some embodiments, the substrate is provided to an etching chamber that is not part of the processing system 100 to perform a trench formation process. In other operations, the substrate has a trench formed therein. Once the trench is formed in the dielectric material, the substrate is transferred to the processing chamber 114 for cleaning.
[0028] The substrate is then transferred to the processing chamber 116 and / or at least one of the processing chambers 102, where one or more operations are performed. For example, the substrate is transferred to one of the processing chambers 102, where a metal deposition operation is performed to form a seed layer. The metal can be deposited in any suitable chamber, such as a PVD chamber, an atomic layer deposition (ALD) chamber, an epitaxial (EPI) chamber, or other suitable chamber.
[0029] After depositing the seed layer, the substrate can be transferred to one of the processing chambers 102, in which a gradient oxidation operation can be performed. The gradient oxidation can be performed in an inductively coupled plasma (ICP) reactor or other suitable plasma processing chamber. The gradient oxidation operation is configured to oxidize unwanted portions of a metal layer formed on the substrate. For example, metal formed in the bottom and sidewalls of a trench or via can be oxidized together with metal disposed on a field region (i.e., top side) of the substrate.
[0030] The substrate is transferred to one of the processing chambers 102, where an etching operation is performed to selectively remove the oxidized portion of the deposited metal layer. For example, the etching operation can be performed in an etching chamber. Alternatively, the etching operation can be performed in an ICP reactor where a gradient oxidation is performed.
[0031] After the etching operation, a portion of the deposited metal layer (e.g., seed material) will remain along the bottom surface of the through hole or trench. In some embodiments, the seed material may additionally be present along the sidewalls of the feature. Subsequently, the substrate may be transferred to one of the processing chambers 102 or 116, in which a gap fill operation is performed. The gap fill operation may be performed in a CVD chamber, an ALD chamber, or other suitable chamber. For example, the processing chamber 102 or 116 may deposit a metal such as tungsten (W), molybdenum (Mo), ruthenium (Ru), or other suitable material grown on a seed layer disposed on the bottom of the trench or feature for forming a portion of a microelectronic device.
[0032] The system controller 180 is coupled to the processing system 100 for controlling the processing system 100 or components thereof. For example, the system controller 180 may control the operation of the processing system 100 using direct control of the processing chambers 102, 104, 106, 110, 112, 114, 116, 120, 130 of the processing system 100 or by controlling controllers associated with the processing chambers 102, 104, 106, 110, 112, 114, 116, 120, 130, 160. In operation, the system controller 180 enables data collection and feedback from the various chambers to coordinate the execution of the processing system 100.
[0033] The system controller 180 generally includes a central processing unit (CPU) 182, a memory 184, and support circuits 186. The CPU 182 may be one of any form of general purpose processor that may be used in an industrial environment. The memory 184, a non-transitory computer readable medium, or a machine readable storage device may be accessed by the CPU 182 and may be one or more of a memory such as a random access memory (RAM), a read-only memory (ROM), a floppy disk, a hard disk, or any other form of local or remote digital storage. The support circuits 186 are coupled to the CPU 182 and may include caches, clock circuits, input / output subsystems, power supplies, etc. The various embodiments disclosed in the present disclosure may generally be implemented, for example as a computer program product or software routine, by executing computer instruction codes stored in the memory 184 (or the memory of a particular processing chamber) under the control of the CPU 182. That is, the computer program product is tangibly embodied on the memory 184 (or a non-transitory computer readable medium or a machine readable storage device). When the CPU 182 executes the computer instruction code, the CPU 182 controls the chamber to perform operations according to various embodiments.
[0034] System controller 180 is configured to execute methods stored in memory 184, such as method 300 (described below).
[0035] In some embodiments, the first processing chamber 102 includes an oxygen source 132 fluidly coupled to a processing region 140 of the first processing chamber 102, wherein the oxygen source 132 is configured to deliver an oxygen-containing gas to the processing region 140. The first processing chamber 102 may further include a first flow control valve 133 configured to control a flow rate of the oxygen-containing gas provided from the oxygen source 132 to the processing region 140. The first processing chamber 102 may further include an etching gas source 136 fluidly coupled to the processing region 140 of the first processing chamber 102, wherein the etching gas source 136 is configured to deliver an etching gas to the processing region 140. The first processing chamber 102 may further include a third flow control valve 137 configured to control a flow rate of the etching gas provided from the etching gas source 136 to the processing region 140. The first processing chamber 102 may further include an inductively coupled plasma source 138 configured to generate a plasma in the processing region 140, wherein the plasma includes a hydrogen-containing gas and an oxygen-containing gas.
[0036] In some embodiments, the system controller 180 is configured to control the first flow control valve 133 so that a certain amount of oxygen-containing gas is provided to the surface of the substrate disposed in the processing region 140 of the first processing chamber 102. The oxygen-containing gas preferentially oxidizes one or more metal-containing layers disposed on the field region and sidewalls of features formed in the substrate. The system controller 180 is additionally configured to control the third flow control valve 137 so that a certain amount of etching gas provided to the surface of the substrate preferentially etches oxidized portions of the one or more metal-containing layers disposed on the field region and the sidewalls of features formed in the substrate.
[0037] Will discuss together Figure 2A To Figure 2F and Figure 3 . FIG. 2A to FIG. 2E Cross-sectional views of some embodiments of device structures for semiconductor devices at different stages of fabrication are provided to illustrate Figure 3 Method 300. Method 300 may be used to fill various features, such as trenches or vias, with gap fill metal. Although described with respect to method 300 FIG. 2A to FIG. 2E , but it should be understood that FIG. 2A to FIG. 2E The structure disclosed in is not limited to the method 300, but can exist as a structure independent of the method 300. Similarly, although the method 300 is relative to FIG. 2A to FIG. 2E However, it should be understood that method 300 is not limited to FIG. 2A to FIG. 2E The structure disclosed in FIG. 2A to FIG. 2E The structure disclosed in .
[0038] For the sake of clarity, some reference numerals describing subsequent stages are omitted in the following figures. When discussing features that are called up in the following figures, the reference numerals can be collected from the previous figures. For example, Figure 2A Certain features disclosed in the disclosure are omitted Figure 2B The reference numerals in .
[0039] The method 300 begins at operation 310 where a substrate having a trench or a via formed in a top surface is provided. The substrate may be a device substrate or a semiconductor substrate as described herein. Figure 2A A cross-sectional view of a semiconductor device structure 200 is shown, in accordance with some embodiments, during an intermediate stage of fabrication corresponding to operation 310. The semiconductor device structure 200 includes a body 210 having a dielectric layer 220 formed thereon.
[0040] The body 210 of the semiconductor device structure 200 may be or include a monolithic semiconductor substrate, a semiconductor-on-insulator (SOI) substrate, etc., which may be doped (e.g., with a p-type dopant or an n-type dopant) or undoped. In some embodiments, the semiconductor material of the body 210 may include an elemental semiconductor, such as silicon (Si) or germanium (Ge); a compound semiconductor, including, for example, silicon carbide, gallium arsenide, gallium phosphide, indium phosphide, indium arsenide, and / or indium antimonide; an alloy semiconductor, including, for example, SiGe, GaAsP, AllnAs, GalnAs, GalnP, and / or GalnAsP; a combination of the above, etc. The body 210 may include additional materials, such as a silicide layer, a metal silicide layer, a metal layer, a dielectric layer, or a combination of the above.
[0041] The dielectric layer 220 may include a plurality of layers. The dielectric layer 220 includes a top surface 229. In some embodiments, the dielectric layer 220 is silicon oxide, silicon oxynitride, silicon nitride, or a combination thereof. In some embodiments, the dielectric layer 220 consists essentially of silicon oxide. Note that the foregoing descriptors (e.g., silicon oxide) should not be construed as disclosing any particular stoichiometric ratio. Thus, "silicon oxide" and the like will be understood by those skilled in the art as a material consisting essentially of silicon and oxygen, without disclosing any particular stoichiometric ratio.
[0042] The dielectric layer 220 is patterned with one or more features 222. In some embodiments, the features 222 may be selected from trenches, vias, holes, or combinations thereof. In a particular embodiment, the features 222 are vias.
[0043] In operation 320, a liner layer 225 is formed on the surface of one or more features. The liner layer 225 may be formed by a PVD process, an ALD process, an epitaxial process, or other suitable deposition process. The liner layer 225 may be formed of titanium silicon (nitride) or other suitable materials. The liner layer 225 may be formed on the exposed surface of the substrate. Figure 2A As shown, liner layer 225 is disposed in feature 222 and along top surface 229 of dielectric layer 220. When feature 222 is a trench structure, liner layer 225 can be disposed inside feature 222. Alternatively, liner layer 225 can be optional when feature 222 is a through hole. Liner layer 225 can be disposed on top surface 229 of dielectric layer 220 including upper surface or field region 227. In the discussion below, when liner layer 225 is absent, field region 227 corresponds to top surface 229 of dielectric layer 220.
[0044] The liner layer 225 may have an initial thickness of about 1 angstrom to about 100 angstroms, for example, an initial thickness of about 20 angstroms to about 50 angstroms. In some embodiments, the liner layer 225 may be discontinuous along, for example, the sidewall surface 223 and / or the bottom surface 224. Any suitable metal deposition process may be used to deposit the liner layer 225. In one example, a PVD process is used to deposit the liner layer 225.
[0045] Feature 222 has a first depth measured from field region 227 to bottom surface 224 and a width defined between two sidewall surfaces 223. In some embodiments, the depth is in a range of about 2 nm to 200 nm, 3 nm to 200 nm, 5 nm to 100 nm, 2 nm to 100 nm, or 50 nm to 100 nm. In some embodiments, the width is in a range of about 10 nm to 100 nm, 10 nm to 20 nm, 10 nm to 50 nm, or 50 nm to 100 nm. In some embodiments, the aspect ratio (depth / width) of feature 222 is in a range of about 1:20, 5:20, 10:20, or 15:20.
[0046] In some embodiments, feature 222 extends downward from field region 227 into body 210. Feature 222 includes sidewall surfaces 223 and a bottom surface 224 extending between sidewall surfaces 223. Sidewall surfaces 223 and bottom surface 224 are formed by exposed liner layer 225 when a liner is present, and are formed on dielectric layer 220 when liner layer 225 is not present. In some embodiments, sidewall surfaces 223 are tapered.
[0047] In operation 330 , a seed layer 230 is formed on a surface of one or more features, such as on a surface of the liner layer 225 . Figure 2BA cross-sectional view of semiconductor device structure 200 is shown during an intermediate stage of fabrication corresponding to operation 330, according to some embodiments. Seed layer 230 may be formed on exposed surfaces of the substrate, namely, on sidewall surfaces 223 and bottom surface 224 of feature 222 and on field region 227.
[0048] The seed layer 230 is a metal material suitable for use as a seed layer for the subsequent deposition of a metal gap filler. The seed layer 230 may be molybdenum (Mo) or a molybdenum-containing layer, tungsten (W) or a tungsten-containing layer, or ruthenium (Ru) or a ruthenium-containing layer. In one example, the seed layer 230 is molybdenum (Mo) or a molybdenum-containing layer. The seed layer 230 may be formed on the sidewall surface 223 and the bottom surface 224 of one or more features 222 and on the field area 227. The seed layer 230 may be a conformal layer. The seed layer 230 may be deposited using any suitable deposition process 232. In one example, the seed layer 230 is deposited using a physical vapor deposition (PVD) process. Alternatively, the seed layer 230 may be formed using a low temperature and low pressure CVD process. The seed layer 230 may be used to repair any damage or discontinuity in the liner layer. In one example, the deposition process 232 may be cycled and repeated for 3 to 5 cycles.
[0049] Seed layer 230 may create an overhang 234 in field region 227 that obstructs or blocks a top opening of one or more features 222. The overhang reduces the width of the top opening at the top of feature 222 from a first, larger width to a second, narrower width.
[0050] In operation 340 , the seed layer is exposed to a gradient oxidation process. Figure 2C A cross-sectional view of the semiconductor device structure 200 is shown during an intermediate stage of fabrication corresponding to operation 340 , in accordance with some embodiments. The gradient oxidation process oxidizes portions of the seed layer 230 to form an oxidized seed layer 240 .
[0051] In some embodiments, the gradient oxidation process includes using an O2 inductively coupled plasma (ICP) including a confined gas flow to produce an oxygen-deficient reaction mode on the exposed metal seed layer 230 (e.g., Mo layer). The O2 ICP provides a low-power O2 plasma with a high ion / radical ratio, which enhances field oxidation and deactivates reactive species before reaching the molybdenum-containing seed layer 230 on the bottom surface 224. In this mode, the oxidation field region 227 and the overhanging portion 234 are oxidized, or more severely oxidized, which allows preferential etching of the oxidized region of the oxidation seed layer 240 while maintaining the seed layer 230 along the bottom surface 224 of the feature 222. In one example, the oxidation of the seed layer 230 is seven times more selective at the field region 227 than at the bottom surface 224. Therefore, the oxidation seed layer 240 is preferentially formed in the field region 227. In one example, the gradient oxidation of the Mo seed layer 230 results in MoO x The oxidation seed layer 240 is formed.
[0052] In some embodiments, the gradient oxidation process includes a reduction process followed by an oxidation process. In some embodiments, the gradient oxidation process includes an oxidation process without a reduction process. The reduction process includes exposing the substrate to a reducing gas, such as hydrogen. The oxidation process includes exposing the substrate to an oxidizing gas, such as oxygen. In some embodiments, during the reduction process, the processing area is maintained at a pressure of less than about 120 mTorr, such as in a range of about 50 mTorr to about 110 mTorr, in a range of about 60 mTorr to about 100 mTorr, or, for example, in a range of about 70 mTorr to about 90 mTorr. Exposing the semiconductor device structure 200 to a reducing gas includes causing the reducing gas to flow into the processing area at a flow rate of about 200 sccm or less, such as in a range of about 100 sccm to about 170 sccm, or in a range of about 120 sccm to about 80 sccm. Exposing the semiconductor device structure 200 to the reducing agent may also include flowing a carrier gas, such as an inert gas such as argon, into the processing region at a flow rate of about 300 sccm or less, such as in a range from about 100 sccm to about 200 sccm, or in a range from about 120 sccm to about 150 sccm. During the reduction process, the semiconductor device structure 200 may be maintained at a temperature of about 450 degrees Celsius or less, such as in a range from about 200 degrees Celsius to about 450 degrees Celsius, in a range from about 250 degrees Celsius to about 400 degrees Celsius, or such as in a range from about 300 degrees Celsius to about 350 degrees Celsius. During the reduction process, an ICP plasma power of 2000 watts or less is applied to maintain the plasma, such as in a range from about 500 watts to 1500 watts, or such as in a range from about 850 watts to about 1000 watts. The reduction process may be performed for 60 seconds or less, such as in a range from about 10 seconds to about 40 seconds, or for example in a range from about 10 seconds to about 30 seconds.
[0053] In some embodiments, during the oxidation process, the processing region is maintained at a pressure of less than about 10 mTorr, such as about 1 mTorr to about 5 mTorr, or, for example, about 1 mTorr to about 2 mTorr. Exposing the seed layer 240 to the oxidizing gas includes flowing the oxidizing gas into the processing region at a flow rate of about 20 sccm or less, such as in a range of about 1 sccm to about 10 sccm, or in a range of about 1 sccm to about 5 sccm. Exposing the seed layer 240 to the reducing agent may further include flowing a carrier gas, such as an inert gas such as argon, into the processing region at a flow rate of about 100 sccm or less, such as in a range of about 50 sccm to about 100 sccm, or in a range of about 50 sccm to about 100 sccm. During the oxidation process, the semiconductor device structure 200 may be maintained at a temperature of about 450 degrees Celsius or less, such as in a range from about 200 degrees Celsius to about 450 degrees Celsius, in a range from about 250 degrees Celsius to about 400 degrees Celsius, or, for example, in a range from about 300 degrees Celsius to about 350 degrees Celsius. During the oxidation process, the ICP plasma power is 300 watts or less, such as in a range from about 100 watts to 300 watts, or, for example, in a range from about 180 watts to about 210 watts. The oxidation process may be performed for 60 seconds or less, such as in a range from about 10 seconds to about 40 seconds, or, for example, in a range from about 12 seconds to about 30 seconds.
[0054] In some embodiments, the oxidation process is performed at a pressure in a range of about 2 mTorr to about 7 mTorr, an ICP power in a range of about 210 Watts to about 350 Watts, argon gas entering the processing region at a flow rate in a range of about 900 sccm to about 1000 sccm, oxygen gas entering the processing region at a flow rate in a range of from about 5 sccm to about 10 sccm, a temperature in a range of from about 300 degrees Celsius to about 400 degrees Celsius, and a duration of from about 90 seconds to about 180 seconds.
[0055] In operation 350 , the oxide seed layer 240 is exposed to an etch-back process. Figure 2D A cross-sectional view of semiconductor device structure 200 is shown during an intermediate stage of fabrication corresponding to operation 350 , in accordance with some embodiments. The etch-back process selectively targets oxidation seed layer 240 relative to seed layer 230 .
[0056] The etch-back process includes flowing an etching gas and an optional inert gas into the processing region. The etching gas may include a chlorine-containing or fluorine-containing gas or a combination thereof, wherein the etchant is selected to be reactive to metal oxides (i.e., oxidized seed layer 240) and not reactive to non-oxide metals (i.e., seed layer 230). In some embodiments, the etch-back process is performed under the following conditions: a pressure in the range of about 5 mTorr to about 20 mTorr, an ICP power in the range of about 300 Watts to about 400 Watts, argon gas entering the processing region at a flow rate in the range of about 450 sccm to about 500 sccm, WF6 gas entering the processing region at a flow rate in the range of about 5 sccm to about 10 sccm, a temperature in the range of about 300 degrees Celsius to about 400 degrees Celsius, and a duration of about 15 seconds to about 30 seconds.
[0057] The etch-back process exposes the oxidized seed layer 240 to an etchant process to selectively remove the oxidized seed layer 240 while minimizing the removal of the underlying seed layer 230. The gradient oxidation process and the etch-back process may be cyclic processes. For example, one cycle may include a gradient oxidation process followed by an etch-back process. The gradient oxidation and etch-back processes may be repeated for a plurality of cycles sufficient to reduce the thickness of the seed layer 230 from an initial thickness to a target reduced thickness. For example, the gradient oxidation and etch-back processes may be repeated for two to four cycles, such as two cycles. The gradient oxidation process of operation 340 and the etch-back process of operation 350 may be repeated until the thickness of the molybdenum-containing layer (e.g., the seed layer 230) is reduced, such as Figure 2D As shown, and completely removed from the field region 227 of the dielectric layer 220 .
[0058] The thickness of the molybdenum-containing layer formed on the field region decreases at a greater rate than the thickness of the molybdenum-containing layer formed on the sidewall surface and the bottom surface of the feature 222. In addition, the thickness of the molybdenum-containing seed layer 230 formed on the sidewall surface 223 decreases at a greater rate than the thickness of the molybdenum-containing seed layer 230 formed on the bottom surface 224.
[0059] The gradient oxidation process (operation 340) and the etch-back process (operation 350) substantially suppress the formation of seams and voids that occur in conventional processes by removing metal from field regions 227 while retaining seed metal along sidewall surfaces 223 and bottom surface 224 of feature 222. Thus, substantially seamless metal gap filling can be achieved.
[0060] In operation 360 , one or more features are filled with a metallic material. Figure 2EA cross-sectional view of a semiconductor device structure 200 during an intermediate stage of manufacturing corresponding to operation 360 is shown according to some embodiments. A metal may be formed on the seed layer 230 to fill the feature 222, thereby forming a gap fill layer 250. The gap fill layer 250 may be deposited using any suitable metal deposition process. The gap fill layer 250 may be deposited via a chemical vapor deposition (CVD) gap fill process. The gap fill layer 250 may partially or completely fill one or more features. The gap fill layer 250 is formed of a metal such as tungsten (W), molybdenum (Mo), or ruthenium (Ru). In one example, the gap fill layer 250 is formed of molybdenum (Mo).
[0061] In some embodiments, the gap-fill layer 250 is formed using a chemical vapor deposition (CVD) process that includes simultaneously flowing (co-flowing) a molybdenum-containing precursor gas and a reducing agent into a processing region and exposing the semiconductor device structure 200 to the precursor gas and the reducing agent.
[0062] In another embodiment, the gap fill layer 250 is deposited using an atomic layer deposition (ALD) process in operation 360. The Mo gap fill ALD process includes repeated cycles of alternating exposures of the semiconductor device structure 200 to a Mo-containing precursor gas and a reducing agent, and purging the processing area between the alternating exposures.
[0063] In other embodiments, the gap-fill layer 250 is deposited using a pulsed CVD method that includes repeatedly exposing the semiconductor device structure 200 to cycles of alternating molybdenum-containing precursor gas and reducing gas without purging the process area.
[0064] The foregoing embodiments of the present disclosure have many advantages, including that the metal oxidation process and the selective metal oxide removal process can be completed in two processing chambers or a single processing chamber, thereby reducing manufacturing time and the possibility of handling induced defects. The method uses an inductively coupled plasma (ICP) O2 plasma to produce an oxygen-deficient reaction, which plasma includes a diffusion-limited gas flow formed in a feature (e.g., a trench or a via) on a substrate. In one embodiment, an ICP O2 plasma (a low-energy O2 plasma with a high ion / radical ratio) is manufactured to enhance field oxidation and deplete reactive oxygen species before reaching the bottom of the trench structure or gap. This gives good selectivity (>7) in the trench structure and achieves field top metal removal while seed material remains at the bottom of the trench structure or in the gap for bottom-up growth of metal fill. The method achieves multiple cycle capabilities with high wafer output. The method solves the difficulties of seams and voids during conventional metal gap filling by removing metal from the field area and sidewalls while retaining seed metal at the bottom of the gap or trench. In this manner, a substantially seamless bottom-up metal gap fill may be performed.
[0065] While the foregoing is directed to embodiments of the present disclosure, other and further embodiments of the present disclosure may be devised without departing from the basic scope thereof, the scope of which is determined by the claims that follow.
Claims
1. A method of filling a feature on a substrate, the method comprising the steps of: forming a metal seed layer on an exposed surface of the substrate, wherein the substrate has a feature in the form of a trench or via formed in a top surface of the substrate, the feature having sidewalls and a bottom surface extending between the sidewalls; performing a gradient oxidation process to oxidize the exposed portion of the metal seed layer to form a metal oxide, wherein the gradient oxidation process preferentially oxidizes the field region of the substrate rather than the bottom surface of the feature, performing an etch-back process to remove or reduce the oxidized portion of the seed layer; and A metal gapfill process is performed to fill or partially fill the features with a gapfill material.
2. The method of claim 1, wherein the seed layer is a molybdenum-containing layer, the metal oxide is molybdenum oxide, and the metal gap-fill material comprises molybdenum.
3. The method of claim 2, wherein an overhanging portion of the seed layer extends into an opening of one or more features formed along the field region of the substrate, and the overhanging portion is preferentially oxidized relative to the metal seed layer. 4 . The method of claim 2 , wherein the gradient oxidation process and the etch-back process are performed in two separate chambers.
5. The method of claim 2, further comprising: A liner layer is formed on the exposed surface of the substrate, wherein the seed layer is formed on the liner layer and the liner layer extends into the feature.
6. The method of claim 3, further comprising: The oxidation process and the etch-back process are repeated on the substrate.
7. The method of claim 3, wherein: The seed layer is removed from the field region and the overhanging portion.
8. A method of filling a feature formed on a substrate, the method comprising the steps of: A molybdenum-containing layer is deposited on the exposed surface of the substrate, wherein the substrate comprising a plurality of features formed in a top surface of the substrate, Each of the plurality of features has a sidewall surface and a bottom surface, and The deposited molybdenum-containing layer is formed on the top surface of the substrate and the sidewall surfaces and the bottom surfaces of the plurality of features; exposing the exposed surface of the substrate to a gradient oxidation process, wherein the gradient oxidation process forms the molybdenum-containing oxidized region; Preferentially etching the oxidized regions of the deposited molybdenum-containing layer, wherein after preferentially etching the oxidized regions, a first portion of the deposited molybdenum-containing layer remains on the bottom surface in each of the plurality of features, and a second portion of the deposited molybdenum-containing layer remains on the sidewall surface in each of the plurality of features; and Filling the features with a second molybdenum layer, wherein filling the features with the second molybdenum layer includes growing the second molybdenum layer in each feature from the second portion of the deposited molybdenum-containing layer on the sidewall surface and the first portion of the deposited molybdenum-containing layer on the bottom surface.
9. The method of claim 8, wherein an overhanging portion of the seed crystal extends into an opening of one or more features formed along the top surface of the substrate, and the overhanging portion is preferentially oxidized relative to the metal seed crystal layer.
10. The method of claim 8, wherein the gradient oxidation process and the etch-back process are performed in two separate chambers.
11. The method of claim 8, further comprising: A liner layer is formed on the exposed surface of the substrate, wherein the liner layer is formed on the seed layer and the liner layer extends into the feature.
12. The method of claim 8, further comprising: The oxidation process and the etching back process are repeated on the substrate.
13. The method of claim 12, wherein the seed layer is removed from the top surface and the overhanging portion.
14. A cluster tool for filling a feature on a substrate, the cluster tool comprising: The first processing chamber comprises: an oxygen source fluidly coupled to a processing region of the first processing chamber, wherein the oxygen source is configured to deliver an oxygen-containing gas to the processing region; a first flow control valve configured to control a flow rate of the oxygen-containing gas provided from the oxygen source to the processing region; an etching gas source fluidly coupled to the processing region of the first processing chamber, wherein the etching gas source is configured to deliver an etching gas to the processing region; a third flow control valve configured to control a flow rate of the etching gas provided from the etching gas source to the processing region; and an inductively coupled plasma source configured to generate a plasma in the processing region, wherein the plasma includes the oxygen-containing gas; and A controller, the controller being configured to: forming a metal seed layer on an exposed surface of the substrate, wherein the substrate has a feature in the form of a trench or via formed in a top surface of the substrate, the feature having sidewalls and a bottom surface extending between the sidewalls; performing a gradient oxidation process to oxidize the exposed portion of the metal seed layer to form a metal oxide, wherein the gradient oxidation process preferentially oxidizes the field region of the substrate rather than the bottom surface of the feature, performing an etch-back process to remove or reduce the oxidized portion of the seed layer; and A molybdenum gapfill process is performed to fill or partially fill the feature with a gapfill material.
15. The cluster tool of claim 14, wherein the seed layer is a molybdenum-containing layer and the metal oxide is molybdenum oxide.
16. The cluster tool of claim 15, wherein an overhanging portion of the seed layer obstructs or blocks a top opening of one or more features formed along the field region of the substrate, and the overhanging portion is preferentially oxidized.
17. The cluster tool of claim 16, wherein the gradient oxidation process and the etch-back process are performed in two separate chambers.
18. The cluster tool of claim 17, wherein the controller is further configured to: A liner layer is formed on the exposed surface of the substrate, wherein the seed layer is formed on the liner layer and the liner layer extends into the feature.
19. The cluster tool of claim 18, wherein the controller is further configured to: The oxidation process and the etching back process are repeated on the substrate.
20. The cluster tool of claim 19, wherein the seed layer is removed from the field region and the overhanging portion.