Ceramic circuit board, semiconductor device, and method for using semiconductor device

By connecting the metal plates on both sides of the ceramic circuit substrate, the thickness and thermal conductivity of the ceramic substrate and the metal plate are optimized, and the problems of cooling efficiency and cost of the ceramic circuit substrate in the prior art are solved, thereby achieving high-efficiency cooling and small size .

CN119072780APending Publication Date: 2024-12-03SPECIAL CERAMIC MATERIALS CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202380034680.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-20
Filing Date
2023-04-17
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

While improving the cooling efficiency of semiconductor components, existing ceramic circuit substrates have led to the increase in the size of the heat sink and the cost increase, and are not suitable for the miniaturization of modules.

Method used

A ceramic circuit substrate is designed. By setting a cooling flow path section in the two-side bonding metal plate of the ceramic substrate, the number of radiator parts is reduced, and the thickness and thermal conductivity of the ceramic substrate and metal plate are optimized to improve heat dissipation and manufacturing. .

Benefits of technology

It realizes efficient cooling of semiconductor components, reduces the number of radiator components, is suitable for the miniaturization of modules, and at the same time reduces costs and improves the flatness and installation of ceramic circuit substrates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119072780A_ABST
    Figure CN119072780A_ABST
Patent Text Reader

Abstract

A ceramic circuit board according to an embodiment includes a ceramic substrate and metal plates bonded to both surfaces of the ceramic substrate. The metal plate bonded to at least one of the two surfaces of the ceramic substrate is a cooling flow path metal plate having a cooling flow path part. The thickness of the ceramic substrate is preferably smaller than the thickness of the cooling flow path metal plate. Furthermore, the ceramic substrate is preferably provided with a first ceramic substrate and a second ceramic substrate bonded to the metal plate bonded to the first ceramic substrate, one surface of the second ceramic substrate is bonded to the cooling flow path metal plate bonded to the first ceramic substrate, and the metal plate is bonded to the other surface of the second ceramic substrate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The embodiments described below generally relate to a ceramic circuit substrate, a semiconductor device, and a method of using the semiconductor device. Background Art

[0002] In recent years, with the improvement of the performance of industrial equipment, the power modules installed therein are becoming higher in output. Along with this, the semiconductor elements are becoming higher in output. The guaranteed operating temperature of semiconductor elements is 125°C to 150°C, but with the increase in output, it may rise to above 175°C in the future. As a circuit substrate for mounting semiconductor elements, a ceramic circuit substrate is used. A ceramic circuit substrate is formed by bonding a metal plate to a ceramic substrate. For example, in Japanese Patent Gazette No. 6789955 (Patent Document 1), there is an extension portion formed by a bonding layer extending from the end of a metal plate. In Patent Document 1, the TCT characteristics (heat cycle resistance characteristics) are improved by controlling the hardness and size of the extension portion of the bonding layer.

[0003] In order to improve the cooling efficiency of semiconductor elements as heat generating bodies, methods using cooling water are being studied. For example, in Japanese Patent Publication No. 2001-148451 (Patent Document 2), a water channel is provided in a heat sink on which a ceramic circuit substrate is mounted to dissipate the heat generated by the semiconductor element. In addition, in International Publication No. 2015 / 147071 (Patent Document 3), a water channel is provided in a ceramic substrate.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent No. 6789955

[0007] Patent Document 2: Japanese Patent Application Publication No. 2001-148451

[0008] Patent Document 3: International Publication No. 2015 / 147071 Summary of the invention

[0009] Technical problem to be solved by the invention

[0010] The devices of Patent Documents 2 and 3 can be water-cooled, thereby improving the cooling efficiency of semiconductor elements. However, Patent Document 2 leads to a large heat sink, and is therefore not suitable for miniaturization of modules. In addition, giving a three-dimensional shape to the ceramic substrate as in Patent Document 3 is a major cause of cost increase.

[0011] The present invention is to address such technical problems and to provide a ceramic circuit board that improves the cooling efficiency of semiconductor elements and has good manufacturability.

[0012] Means for solving technical problems

[0013] A ceramic circuit board of an embodiment includes a ceramic substrate and metal plates bonded to both surfaces of the ceramic substrate. The metal plate bonded to at least one of the both surfaces of the ceramic substrate is a cooling flow path metal plate having a cooling flow path portion. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 It is a side view showing an example of the ceramic circuit board according to the embodiment.

[0015] Figure 2 It is a side view showing another example of the ceramic circuit substrate according to the embodiment.

[0016] Figure 3 This is a diagram showing an example of a cooling flow path portion.

[0017] Figure 4 This is a diagram showing another example of the cooling flow path portion.

[0018] Figure 5 It is a side view showing an example of a semiconductor device according to an embodiment.

[0019] Figure 6 It is a side view showing another example of the semiconductor device according to the embodiment. DETAILED DESCRIPTION

[0020] Hereinafter, embodiments of a ceramic circuit substrate, a semiconductor device, and a method of using the semiconductor device will be described in detail with reference to the accompanying drawings.

[0021] The ceramic circuit board of the embodiment includes a ceramic substrate and metal plates bonded to both surfaces of the ceramic substrate. The metal plate bonded to at least one of the two surfaces of the ceramic substrate is a metal plate having a cooling flow path portion (hereinafter referred to as a "cooling flow path metal plate").

[0022] By providing the cooling flow path portion in the metal plate bonded to the ceramic substrate, the number of components such as a heat sink can be reduced.

[0023] In the ceramic circuit board of the embodiment, the thickness of the ceramic circuit board is preferably smaller than the thickness of the cooling flow path metal plate. That is, the ceramic circuit board preferably satisfies (thickness of the ceramic circuit board) < (thickness of the cooling flow path metal plate).

[0024] In addition, the ceramic circuit substrate of the embodiment comprises a first ceramic substrate and a second ceramic substrate joined to a metal plate joined to the first ceramic substrate. Furthermore, it is preferred that one surface of the second ceramic substrate is joined to a cooling flow path metal plate joined to the first ceramic substrate, and the metal plate is joined to another surface of the second ceramic substrate, and the thickness of the second ceramic substrate is less than the cooling flow path metal plate. In addition, the ceramic substrate is usually in the shape of a flat plate. The ceramic substrate may also have a three-dimensional structure with local projections and depressions. In the case of having a three-dimensional structure, the thickness of the ceramic substrate represents the thinnest part of the joint portion with the metal plate.

[0025] Figure 1 and Figure 2 An example of a ceramic circuit substrate according to an embodiment is shown. In the figure, reference numeral 1 is a ceramic circuit substrate, reference numeral 2 is a first ceramic substrate among ceramic substrates, reference numerals 3 and 8 are metal plates without a cooling flow path among metal plates (hereinafter referred to as "non-cooling flow path metal plates"), reference numeral 4 is a cooling flow path metal plate among metal plates, and reference numeral 5 ( Figure 3 , etc.) is a cooling flow path portion, reference numeral 5A is an inlet of the cooling flow path portion 5, reference numeral 5B is an outlet of the cooling flow path portion 5, and reference numeral 7 is a second ceramic substrate among the ceramic substrates.

[0026] Figure 1 The non-cooling flow path metal plate 3 is bonded to one surface of the first ceramic substrate 2, and the cooling flow path metal plate 4 is bonded to the other surface on the opposite side. Figure 2 The structure is that a non-cooling flow path metal plate 3 is joined to one surface of the first ceramic substrate 2, a cooling flow path metal plate 4 is joined to the other surface, one surface of the second ceramic substrate 7 is joined to the cooling flow path metal plate 4, and a non-cooling flow path metal plate 8 is joined to the other surface of the second ceramic substrate 7. In addition, although not shown in the figure, it is also possible to have a structure in which the cooling flow path metal plate 4 is provided on both surfaces of the first ceramic substrate 2. In this case, a through hole can also be provided in the first ceramic substrate 2, and the cooling flow path portions of the cooling flow path metal plates 4 on the front and back surfaces are connected to each other via the through hole.

[0027] Examples of the ceramic substrates 2 and 7 include silicon nitride substrates, aluminum nitride substrates, aluminum oxide substrates, zirconium oxide substrates, and aluminum zirconium substrates. The aluminum zirconium substrate is a ceramic sintered body obtained by mixing aluminum oxide and zirconium oxide.

[0028] The thickness T1 of the first ceramic substrate 2 and the thickness T3 of the second ceramic substrate 7 are preferably within the range of 0.2 mm to 4 mm. If the thickness T1 and T3 of the ceramic substrates 2 and 7 are less than 0.2 mm, the strength may be insufficient. In addition, if the thickness T1 and T3 of the ceramic substrates 2 and 7 exceed 4 mm, the heat dissipation may be reduced. Therefore, when the thickness T1 and T3 of the ceramic substrates 2 and 7 are 0.2 mm to 4 mm, and the ceramic substrates 2 and 7 are silicon nitride substrates or aluminum oxide substrates, the thickness T1 and T3 are preferably within the range of 0.2 mm to 1 mm. In addition, Figure 2 In the illustrated case, the thickness T1 of the first ceramic substrate 2 and the thickness T3 of the second ceramic substrate 7 may be the same or different.

[0029] The silicon nitride substrate used as the ceramic substrate 2, 7 preferably has a three-point bending strength of 600 MPa or more. In addition, the thermal conductivity is preferably 80 W / m·K or more. By increasing the strength of the silicon nitride substrate, the substrate thickness can be reduced. Therefore, the three-point bending strength of the silicon nitride substrate is preferably 600 MPa or more, and more preferably 700 MPa or more. The silicon nitride substrate can reduce the substrate thickness to less than 2 mm, and further to less than 0.40 mm.

[0030] The three-point bending strength of the aluminum nitride substrate as the ceramic substrates 2 and 7 is about 300 to 450 MPa. On the other hand, the thermal conductivity of the aluminum nitride substrate is 160 W / m·K or more. Since the strength of the aluminum nitride substrate is low, the substrate thickness is preferably 0.60 mm or more.

[0031] The three-point bending strength of an alumina substrate as the ceramic substrates 2 and 7 is about 300 to 450 MPa, but it is inexpensive. In addition, the three-point bending strength of an aluminum silicon substrate is as high as about 550 MPa, but the thermal conductivity is about 30 to 50 W / m·K.

[0032] The ceramic substrates 2 and 7 are preferably silicon nitride substrates. This is because silicon nitride substrates are strong and can be made thinner. In addition, by using silicon nitride substrates with a thermal conductivity of 80 W / m·K or more, heat dissipation can also be improved.

[0033] The metal plates, i.e., the non-cooling flow path metal plates 3, 8 and the cooling flow path metal plate 4, can be selected from one or more of copper plates, copper alloy plates, aluminum plates, and aluminum alloy plates. As the metal plate, a copper plate is preferred. In addition, the copper plate is further preferably an oxygen-free copper plate. As shown in JIS-H-3100, oxygen-free copper has a copper purity of 99.96wt% or more. The thermal conductivity of copper is about 400W / m·K, and the thermal conductivity of aluminum is about 240W / m·K. Compared with aluminum, copper has a high thermal conductivity, so the heat dissipation is improved. In addition, the aluminum plate is preferably pure aluminum. Pure aluminum is shown in JIS-H-4000. Aluminum plates are suitable for lightweighting. JIS-H-4000 corresponds to ISO6361. In addition, JIS-H-3100 corresponds to ISO197, etc.

[0034] By providing a cooling flow path portion 5 (at Figure 3 ), the number of components such as heat sinks used to dissipate heat generated from semiconductor elements can be reduced.

[0035] In addition, in the ceramic circuit substrate 1 of the embodiment, the thickness T1 of the first ceramic substrate 2 is smaller than the thickness T2 of the cooling flow path metal plate 4. That is, the ceramic circuit substrate 1 satisfies T1<T2. In addition, the ceramic circuit substrate 1 preferably has a thickness T3 of the second ceramic substrate 7 that is also smaller than the thickness T2 of the cooling flow path metal plate 4. That is, the ceramic circuit substrate 1 preferably satisfies T3<T2. In addition, the thickness of the first ceramic substrate 2 is set to T1, the thickness of the cooling flow path metal plate 4 is set to T2, and the thickness of the second ceramic substrate 7 is set to T3.

[0036] The cooling flow path metal plate 4 allows a cooling medium such as cooling water to flow through the cooling flow path portion 5 ( Figure 3 The heat dissipation is improved by circulating or contacting the cooling path metal plate 4 (as shown in the figure). By setting T1 < T2, the heat dissipation of the cooling path metal plate 4 can be improved. In addition, by setting T3 < T2, the heat dissipation of the cooling path metal plate 4 can also be improved. As described later, the non-cooling path metal plate 3 or the non-cooling path metal plate 8 can be used for the circuit part for mounting semiconductor elements. If the ceramic substrate and the metal plate are compared, the thermal conductivity of the metal plate is high. By setting T1 < T2, the heat dissipation can be improved. In addition, the heat dissipation can also be improved for T3 < T2. In addition, at least one of the non-cooling path metal plate 3 and the non-cooling path metal plate 8 can be replaced with a cooling path metal plate, and the cooling path metal plate can be used for the circuit part for mounting semiconductor elements.

[0037] In addition, the thickness T2 of the cooling flow path metal plate 4 relative to the thickness T1 of the first ceramic substrate 2, that is, T2 / T1, is preferably within a range of 2 or more and 40 or less. In addition, the thickness T2 of the cooling flow path metal plate 4 relative to the thickness T3 of the second ceramic substrate 7, that is, T2 / T3, is preferably within a range of 2 or more and 20 or less. By satisfying one or both of 2≤T2 / T1≤40 or 2≤T2 / T3≤40, heat dissipation and warpage suppression can be achieved.

[0038] Conventionally, as in Patent Document 2, a ceramic circuit substrate and a heat sink having a cooling flow path are separately provided. Since the ceramic circuit substrate 1 of the embodiment has a cooling flow path structure provided on the metal plate 4 joined to the ceramic substrates 2 and 7, a structure without using a heat sink can be adopted. Therefore, as a semiconductor device, the number of components can be reduced.

[0039] In addition, the thickness T2 of the cooling flow path metal plate 4 is preferably 1 mm or more. If the thickness T2 of the cooling flow path metal plate 4 is 1 mm or more, it is easy to form the cooling flow path portion 5 on the metal plate 4. The upper limit of the thickness T2 of the cooling flow path metal plate 4 is not particularly limited, but is preferably 20 mm or less. If it exceeds 20 mm and is thicker, it is possible to increase the size of the ceramic circuit substrate 1. Therefore, when the thickness T2 is 1 mm or more and 20 mm or less, and the ceramic substrates 2 and 7 are silicon nitride substrates, the thickness T2 is preferably 3 mm or more and 10 mm or less.

[0040] In addition, let the thickness of the non-cooling flow path metal plate 3 be T4, and let the thickness of the non-cooling flow path metal plate 8 be T5. The thicknesses T4 and T5 of the non-cooling flow path metal plates 3 and 8 may be the same or different, but are preferably not less than 0.2 mm respectively. The non-cooling flow path metal plates 3 and 8 become the circuit parts for mounting semiconductor elements. In addition, the non-cooling flow path metal plates 3 and 8 are metal plates that do not have the cooling flow path part 5. By making the metal plate thicker, it is possible to have current carrying capacity and heat dissipation. In addition, the upper limit of the thickness of the non-cooling flow path metal plates 3 and 8 is not particularly limited, and is preferably not more than 10 mm. If the thickness of the non-cooling flow path metal plates 3 and 8 exceeds 10 mm, the ceramic circuit substrate 1 may be enlarged. In addition, it may become difficult to form the circuit shape. In Figure 1 and Figure 2 In the embodiment, a case where one non-cooling flow path metal plate 3 is bonded to one surface of the first ceramic substrate 2 and one non-cooling flow path metal plate 8 is bonded to one surface of the second ceramic substrate 7 is illustrated. However, the ceramic circuit substrate 1 of the embodiment is not limited to this mode, and a plurality of non-cooling flow path metal plates 3 (on one surface of the ceramic substrates 2 and 7) may be provided. Figure 4 3 shows the joining of three non-cooling flow path metal plates 3). That is, the non-cooling flow path metal plates 3 and 8 may be given a circuit shape.

[0041] In addition, the thickness T2 of the cooling flow path metal plate 4 relative to the thickness T4 of the non-cooling flow path metal plate 3, that is, T2 / T4, is preferably within a range of 0.5 to 50. By reducing the difference between the thickness T2 of the cooling flow path metal plate 4 and the thickness T4 of the non-cooling flow path metal plate 3 to a certain extent, such that 0.5≤T2 / T4≤50, the effect of suppressing the warping of the ceramic circuit board 1 can be obtained.

[0042] In addition, if Figure 2 As shown, the ceramic circuit substrate 1 is preferably provided with a second ceramic substrate 7 and a non-cooling flow path metal plate 8 . Figure 2 The ceramic circuit substrate 1 shown has a structure in which ceramic substrates are joined on both sides of a cooling flow path metal plate 4. By joining ceramic substrates 2 and 7 on both sides of the cooling flow path metal plate 4, the flatness of the ceramic circuit substrate 1 can be improved. The flatness of the ceramic circuit substrate 1 is expressed as the difference between the highest point and the lowest point on the surface of the non-cooling flow path metal plate 3. Similarly, it is expressed as the difference between the highest point and the lowest point on the surface of the non-cooling flow path metal plate 8. By adopting a structure in which ceramic substrates 2 and 7 are joined on both sides of the cooling flow path metal plate 4, the flatness can be made less than 1.0 mm. In addition, by using a silicon nitride substrate, the flatness can also be improved. The measurement of flatness can be measured by using a three-dimensional shape measuring machine. Flatness represents the difference between the highest point and the lowest point of the metal plate. For example, the highest point and the lowest point of the cooling flow path metal plate 4 are measured, and the difference is used as the flatness.

[0043] In addition, similarly to the thickness T2 of the cooling flow path metal plate 4 relative to the thickness T4 of the non-cooling flow path metal plate 3, the thickness T2 of the cooling flow path metal plate 4 relative to the thickness T5 of the non-cooling flow path metal plate 8, that is, T2 / T5, is preferably within the range of 0.5 to 50. By reducing the difference between the thickness T2 of the cooling flow path metal plate 4 and the thickness T5 of the non-cooling flow path metal plate 8 to a certain extent, such that 0.5≤T2 / T5≤50, the effect of suppressing the warping of the ceramic circuit board 1 can be obtained.

[0044] The cooling flow path metal plate 4 is provided with the cooling flow path portion 5, and thus has a hollow portion. Therefore, deformation is easily generated in the cooling flow path metal plate 4. Therefore, by providing the ceramic substrates 2 and 7 and the metal plates 3 and 8 on both sides of the cooling flow path metal plate 4, deformation of the cooling flow path metal plate 4 can be suppressed. By suppressing deformation of the cooling flow path metal plate 4, the mountability of the semiconductor element 11 can be improved.

[0045] In addition, the cooling flow path metal plate 4 can provide the inlet 5A and the outlet 5B of the cooling flow path portion 5 on the same side surface of the cooling flow path metal plate 4 ( Figure 3As shown), it can also be set on different sides of the cooling flow path metal plate 4 ( Figure 4 The positions of the inlet 5A and the outlet 5B of the cooling flow path portion 5 are determined according to the location where the semiconductor device 12 is installed and the mechanism for introducing cooling water. In addition, the cooling flow path portion 5 of the cooling flow path metal plate 4 preferably has a plurality of bends (for example, the folded portion 9). In particular, when the inlet 5A and the outlet 5B of the cooling flow path portion 5 are provided on the same side of the cooling flow path metal plate 4 ( Figure 3 As shown), preferably having a folded portion 9.

[0046] Figure 3 and Figure 4 In the figure, reference numeral 4 is a cooling flow path metal plate, reference numeral 5 is a cooling flow path portion, reference numeral 5A is an inlet of the cooling flow path portion 5, reference numeral 5B is an outlet of the cooling flow path portion 5, reference numeral 9 is a folding portion, and reference numeral 10 is a cover portion. Figure 3 and Figure 4 It is a schematic diagram showing a cutout model for explaining the structure of the cooling flow path portion 5 .

[0047] The shape of the flow path of the cooling flow path portion 5 can be various shapes. Figure 3 The curvilinear flow path may be as shown in FIG. Figure 3 The structure of bending through a plurality of folded portions 9 as shown in FIG. 1 may also be a structure having a U-shaped, V-shaped, W-shaped, L-shaped or other bending portion. Figure 4 It is a straight line as shown. In addition, a plurality of cooling flow path sections 5 may be provided. In addition, a combination of a curved line and a straight line may be provided. In addition, the cooling flow path section 5 may also be a structure in which a plurality of cooling flow paths intersect. In addition, when observing the structure of one cooling flow path section 5, it is not limited to a straight line, and may also be a wave shape. In addition, the cooling flow path section 5 may have a fin structure, or may adopt a heat spreader method.

[0048] The cooling flow path portion 5 may also be configured to pass through a region of the cooling flow path metal plate 4 close to the semiconductor element 11 mounted on the non-cooling flow path metal plates 3 and 8, for example, a region directly below the semiconductor element 11. This can effectively cool the heat from the semiconductor element 11 and improve the cooling efficiency.

[0049] The cooling flow path metal plate 4 may also be configured such that the inlet 5A and the outlet 5B of the cooling flow path portion 5 are disposed on the same side of the cooling flow path metal plate 4. In the configuration in which the inlet 5A and the outlet 5B are disposed on the same side of the cooling flow path metal plate 4, when the cooling flow path portion 5 is spread over the entire cooling flow path metal plate 4, the cooling flow path portion 5 also becomes a continuous structure in which one inlet 5A is connected to one outlet 5B. This makes it easy to manage the cooling medium. For example, Figure 4 As shown in FIG. 1 , if a plurality of linear cooling flow path portions 5 are provided, a plurality of inlets 5A and a plurality of outlets 5B are required. Therefore, when a plurality of inlets 5A and outlets 5B are formed, the load of managing the cooling medium increases. In addition, when the cooling flow path portion 5 is provided directly below the mounting position of a plurality of semiconductor elements, if Figure 4 The linear cooling flow path portion 5 shown requires a plurality of cooling flow path portions 5 .

[0050] If Figure 3 As shown in the figure, a cooling flow path 5 having a curved shape with an inlet 5A and an outlet 5B connected to each other can facilitate the management of the cooling medium and increase the degree of freedom of the mounting position of the semiconductor element. Therefore, it is preferable to use a cooling flow path 5 having a folded portion 9. Figure 3 In the figure, the left side of the paper is set as the entrance 5A, and the right side of the paper is set as the exit 5B, but it is not limited to this. Figure 4 In the example, the front of the paper is set as the entrance 5A, and the back of the paper is set as the exit 5B, but the invention is not limited thereto. Figure 3 and Figure 4 In the example, the case where the cross section of the inlet 5A and the outlet 5B is circular is illustrated. However, the cross section near the inlet 5A and the outlet 5B is not limited to the case where the cross section is circular, and may have a quadrilateral or elliptical shape, or may have various shapes such as a U-shaped groove or a V-shaped groove formed from one side or both sides. Figure 4 As shown, the inlet 5A and the outlet 5B of the cooling flow path portion 5 may be provided on different side surfaces of the cooling flow path metal plate 4 .

[0051] The cooling flow path portion 5 formed in the cooling flow path metal plate 4 may be formed by any one or two or more of one surface, both surfaces, or the inside of the cooling flow path metal plate 4 . Figure 3 The cooling flow path portion 5 shown is formed in a circular cross-section in the vicinity of the inlet 5A and the outlet 5B, and a U groove (a groove having a quadrilateral cross section or a quadrilateral groove with rounded corners in the deep part) is formed on one side of the main body portion other than this. Figure 4 The cooling flow path portion 5 shown is formed inside in a circular cross-section. Figure 4 In the example of FIG. 4 , the cooling flow path portion 5 is formed by digging a hole (tunnel) from a circular cutout on the side surface of the cooling flow path metal plate 4 in the flow path direction.

[0052] The cooling flow path portion 5 formed on a single surface of the cooling flow path metal plate 4 is formed by forming a groove from a single surface side of the cooling flow path metal plate 4. The cooling flow path portion 5 formed on both surfaces of the cooling flow path metal plate 4 is formed by forming grooves from both sides. In the case where grooves are provided on both surfaces of the cooling flow path metal plate 4, the front and back surfaces may be of the same shape or of different shapes. In addition, the cooling flow path portion 5 formed inside the cooling flow path metal plate 4 is formed by digging a hole (tunnel) from the side surface of the cooling flow path metal plate 4 along the flow path direction. If the cooling flow path portion 5 is dug out in this way, the front and back surfaces are not open, so that the cooling medium can be prevented from leaking out of the cooling flow path portion 5.

[0053] On the other hand, in the case where a cooling flow path portion 5 formed by a groove excavated from one side or both sides of the cooling flow path metal plate 4 is provided, since the front and back sides are not sealed, the cooling medium may easily leak out of the cooling flow path portion 5. Therefore, as required, the metal plate may be joined to the cooling flow path metal plate 4 as a cover portion 10 covering the groove formed in the cooling flow path metal plate 4. In order to provide a cooling flow path portion 5 having a folding portion 9, it is effective to perform groove processing on one side or both sides of the cooling flow path metal plate 4. In the cooling flow path metal plate 4, the bonding area with the ceramic substrate 2 may be insufficient. In addition, by providing the cover portion 10, the flatness of the non-cooling flow path metal plates 3 and 8 can be improved. The portion of the non-cooling flow path metal plates 3 and 8 located directly above the portion where the cooling flow path portion 5 is provided is easily recessed. Therefore, the flatness of the non-cooling flow path metal plates 3 and 8 may be reduced. By using the cover portion 10, the flatness of the non-cooling flow path metal plates 3 and 8 can be improved.

[0054] In addition, by providing the cover 10 on the cooling flow path metal plate 4, it is possible to ensure a bonding area with the ceramic substrate 2. In other words, when the bonding area with the ceramic substrate 2 can be ensured, the cover 10 may not be used. Figure 3 This is an example in which a cover portion 10 is provided. Figure 4 This is an example in which the cover portion 10 is not provided. When the cover portion 10 is provided, the thickness T2 is the sum of the thickness of the cooling flow path metal plate 4 and the thickness of the cover portion 10 .

[0055] In addition, the ratio of the volume of the cavity of the cooling flow path portion 5 to the overall volume of the cooling flow path metal plate 4 is preferably in the range of 10% to 80%. If the ratio of the volume of the cooling flow path portion 5 is less than 10%, the effect of providing the cooling flow path portion may be insufficient. In addition, if the ratio of the volume of the cooling flow path portion 5 exceeds 80%, the strength of the cooling flow path metal plate 4 may be reduced. In addition, there is a possibility that the bonding area between the ceramic substrates 2, 7 and the cooling flow path metal plate 4 is insufficient. Therefore, the ratio of the volume of the cooling flow path portion 5 to the overall volume of the cooling flow path metal plate 4 is preferably in the range of 10% to 80%, and more preferably in the range of 20% to 60%. In addition, in the case where a plurality of cooling flow path portions 5 are provided on the cooling flow path metal plate 4, the ratio of the volume using the total value thereof is set.

[0056] In addition, the width in the cross section of the cooling flow path portion 5 is preferably greater than 1 mm. When the cross section of the cooling flow path portion 5 is circular, the width of the cross section of the cooling flow path portion 5 refers to the length of the diameter of the cross section of the cooling flow path portion 5. When the cross section of the cooling flow path portion 5 is other shapes, the width in the cross section of the cooling flow path portion 5 refers to the shortest length of the lengths of the relative points in the cross section of the cooling flow path portion 5. If the width of the cooling flow path portion 5 is less than 1 mm, the flow of the cooling medium may deteriorate. In addition, if the width of the cooling flow path portion 5 is too thin, a load will be applied during processing or the manufacturability will be reduced. In addition, the upper limit of the width of the cooling flow path portion 5 is not particularly limited, and is preferably less than 10 mm. If the width of the cooling flow path portion 5 exceeds 10 mm, the flatness may be impaired. Therefore, the width of the cooling flow path portion 5 is preferably greater than 1 mm and less than 10 mm, and more preferably in the range of greater than 2 mm and less than 8 mm.

[0057] In addition, the creepage distance of the cooling flow path portion 5 is preferably more than 1mm. The creepage distance of the cooling flow path portion 5 is the shortest distance between the cooling flow path portion 5 and the end of the cooling flow path metal plate 4. If the creepage distance of the cooling flow path portion 5 is less than 1mm, if the cooling flow path portion 5 is slightly expanded, it will reach the end of the cooling flow path metal plate 4 and reduce the bonding area, so it may become the cause of water leakage. For example, the ceramic substrate 2 and the cooling flow path metal plate 4 are bonded using an active metal bonding method. If the creepage distance is short, then in the case of an unbonded portion (gap, etc.) in the bonding layer, it may become the cause of water leakage. In addition, the unbonded portion is sometimes formed when thermal stress is loaded as in the TCT test. In other words, by making the creepage distance more than 1mm, durability can be improved. Therefore, the creepage distance of the cooling flow path portion is preferably more than 1mm, and more preferably more than 2mm.

[0058] In addition, the first ceramic substrate 2 is preferably joined to the metal plates 3 and 4, and the second ceramic substrate 7 is preferably joined to the metal plates 4 and 8 using an active metal joining method. The active metal joining method refers to a joining method using one or more active metals selected from Ti (titanium), Zr (zirconium), and Hf (hafnium). An active metal solder having copper (Cu) or silver (Ag) as a main component and containing an active metal is used. The main component mentioned here is the component that contains the most in the metal components of the solder. In addition, if the active metal joining method is used, the ceramic substrate 2 is joined to the metal plates 3 and 4 via an active metal joining layer, and the second ceramic substrate 7 is joined to the metal plates 4 and 8.

[0059] In addition, the active metal solder composition preferably contains Ag (silver) of 0 mass % or more and 60 mass % or less, Cu (copper) of 15 mass % or more and 70 mass % or less, Ti (titanium) or TiH2 (titanium hydride) of 1 mass % or more and 15 mass %. In addition, when both Ti and TiH2 are used, the total is set to be within the range of 1 mass % or more and 15 mass % or less. In addition, when both Ag and Cu are used, it is preferred that Ag is within the range of 20 mass % or more and 60 mass % or less, and Cu is within the range of 15 mass % or more and 40 mass % or less.

[0060] In addition, as required, it is also possible to contain one or two of Sn (tin) or In (indium) in an amount of more than 1 mass % and less than 50 mass %. In addition, the content of Ti or TiH2 is preferably in the range of more than 1 mass % and less than 15 mass %. In addition, it is also possible to contain C (carbon) in an amount of more than 0.1 mass % and less than 2wt % as required. In addition, the active metal solder may also be added with one or more of tungsten (W), molybdenum (Mo), and rhenium (Re) in an amount of more than 0.1 mass % and less than 10 mass %. Carbon, tungsten, molybdenum, and rhenium can control the fluidity of the active metal solder.

[0061] The ratio of the active metal solder composition is calculated based on the total of the mixed raw materials being 100 mass %. For example, in the case of being composed of three kinds of Ag, Cu, and Ti, Ag+Cu+Ti=100 mass %. In addition, in the case of being composed of four kinds of Ag, Cu, TiH2, and In, Ag+Cu+TiH2+In=100 mass %. In addition, in the case of being composed of five kinds of Ag, Cu, Ti, Sn, and C, Ag+Cu+Ti+Sn+C=100 mass %.

[0062] Ag or Cu is a component of the base material of the solder. In addition, Sn or In has the effect of lowering the melting point of the solder. In addition, C (carbon) has the effect of controlling the fluidity of the solder or reacting with other components to control the structure of the bonding layer. Therefore, as the components of the solder, Ag-Cu-Ti, Ag-Cu-Sn-Ti, Ag-Cu-Ti-C, Ag-Cu-Sn-Ti-C, Ag-Ti, Cu-Ti, Ag-Sn-Ti, Cu-Sn-Ti, Ag-Ti-C, Cu-Ti-C, Ag-Sn-Ti-C, Cu-Sn-Ti-C can be cited. In addition, In can also be used instead of Sn. In addition, both Sn and In can also be used.

[0063] The above-mentioned active metal solder is effective for joining copper plates. In addition, it is preferred that the metal part is a copper component, and the ceramic substrates 2 and 7 are joined to the copper component via a bonding layer that does not contain Ag. A bonding layer that does not contain Ag refers to the use of an active metal solder to which no Ag is added. As an inevitable impurity, the amount of Ag may be less than 0.01 mass % (including zero). By using a bonding layer that does not contain Ag, the occurrence of Ag ion migration can be suppressed. Ag ion migration refers to the phenomenon that when a voltage is applied in an environment with high humidity, the Ag in the bonding layer is ionized and moves. Ag ions move and precipitate elsewhere. As a result, it becomes a cause of poor insulation. Among active metal solders, Ag is most susceptible to ion migration. By not using Ag in the bonding layer, Ag ion migration can be suppressed.

[0064] When the metal plates 3, 4, 8 are aluminum plates, Al-Si or AlMg based brazing materials are preferably used as active metal brazing materials. The content of one or both of Si and Mg in the active metal brazing materials is preferably within a range of 0.1 mass % to 20 mass %.

[0065] The active metal bonding method can improve the bonding strength between the ceramic substrates 2 and 7 and the metal plates 3, 4 and 8. Therefore, airtightness can be ensured when the cooling flow path metal plate 4 and the ceramic substrates 2 and 7 are bonded on one side or both sides.

[0066] The ceramic circuit board 1 as described above can be used for a semiconductor device having a semiconductor element mounted thereon. Figure 5 An example of a semiconductor device according to an embodiment is shown. Figure 5 The semiconductor device of the embodiment shown in the figure illustrates a case where the inlet 5A and the outlet 5B are provided on the same side of the cooling flow path metal plate 4. The case where the inlet 5A and the outlet 5B are provided on different sides of the cooling flow path metal plate 4 is not illustrated, but due to the Figure 5 In the figure, reference numeral 1 is a ceramic circuit substrate, reference numeral 11 is a semiconductor element, and reference numeral 12 is a semiconductor device. Figure 5In the example, the semiconductor element 11 is mounted on both sides, but the semiconductor element 11 may be mounted on only one side. In addition, a plurality of semiconductor elements 11 may be mounted on one side. In addition, wire bonding, a lead frame, etc., which are not shown in the figure, may be provided.

[0067] A cooling medium is introduced from the inlet 5A of the cooling flow path portion 5 of the semiconductor device 12. Examples of the cooling medium include cooling water, cooling gas, and the like. By introducing the cooling medium from the inlet 5A to the outlet 5B of the cooling flow path portion 5, a semiconductor device 12 with high cooling efficiency can be formed. In addition, since the cooling flow path metal plate 4 is provided on the back surface of the ceramic substrate 2, the semiconductor device 12 can also be made thinner. Therefore, cooling efficiency and thinness can be achieved at the same time.

[0068] In addition, if the ceramic circuit substrate 1 of the embodiment is assembled in a power module, it can be installed without using a heat sink. That is, a structure in which the ceramic circuit substrate 1 is directly mounted on a mounting plate (or a base plate) can also be adopted. Since a heat sink is not required, it is effective in reducing the number of components.

[0069] In addition, in the past, the ceramic circuit substrate was provided on the cooler provided on the power module side via a TIM (Thermal Interface Material) layer. In the case of the ceramic circuit substrate 1 of the embodiment, it is possible to install it without providing a TIM layer on the cooling flow path metal plate 4. The TIM layer may include thermal grease, etc. That is, it is also possible to install it without providing grease between the ceramic circuit substrate and the mounting plate. It is also possible not to use a TIM layer, which is effective in reducing the number of components.

[0070] Figure 6 The structure in which a ceramic circuit substrate 1 is mounted on a mounting board is illustrated. In the figure, reference numeral 1 is a ceramic circuit substrate, reference numeral 8 is a metal plate (rear metal plate), reference numeral 11 is a semiconductor element, reference numeral 12 is a semiconductor device, reference numeral 13 is a mounting board, and reference numeral 14 is a power module. The ceramic circuit substrate 1 with the semiconductor element 11 mounted thereon becomes a semiconductor device 12. In addition, if the semiconductor device 12 is mounted on the mounting board 13, it becomes a power module 14.

[0071] In the past, a thermal grease layer was provided between the ceramic circuit substrate and the heat sink or between the ceramic circuit substrate and the mounting plate. Thermal grease is made by adding fillers to silicone resin or the like. Its thermal conductivity is about 1 to 2 W / m·K. By using grease having a lower thermal conductivity than the ceramic substrate and the metal plate, it is difficult to release the heat of the semiconductor element. The ceramic circuit substrate 1 of the embodiment is provided with a cooling flow path portion 5, so the ceramic circuit substrate 1 itself has good heat dissipation properties. Therefore, it can be installed even without using thermally conductive grease between the non-cooling flow path metal plate 8 and the mounting plate 13. In addition, a structure that does not use a heat sink is sometimes referred to as a heat sink-free structure. In addition, a structure that does not use grease is sometimes referred to as a grease-free structure. The mounting plate 13 can also be installed by screw fixing, etc. as needed. In addition, a molded resin can also be provided as needed.

[0072] The above example shows a structure without a heat sink or grease, but it can also be used as needed. This means that it can be used even without a heat sink or grease. Figure 1 In the case of such a shape, the cooling flow path metal plate 4 can also be mounted on the mounting plate 13 .

[0073] In addition, the method of using the semiconductor device 12 of the embodiment is to control the temperature by allowing the cooling medium to flow through or contact the cooling flow path portion 5. This can effectively release the heat generated when the semiconductor element is operating.

[0074] (Example)

[0075] (Examples 1 to 8)

[0076] As ceramic substrates 2 for the ceramic circuit substrates 1 of Examples 1 to 8, silicon nitride substrates, aluminum oxide substrates, and aluminum nitride substrates are prepared. The silicon nitride substrate uses a substrate with a thermal conductivity of 90 W / m·K, a 3-point bending strength of 650 MPa, and a length of 100 mm × a width of 90 mm. In addition, the aluminum oxide substrate uses an aluminum oxide substrate with a thermal conductivity of 20 W / m·K, a 3-point bending strength of 430 MPa, and a length of 100 mm × a width of 90 mm. The aluminum nitride substrate uses an aluminum nitride substrate with a thermal conductivity of 170 W / m·K, a 3-point bending strength of 400 MPa, and a length of 100 mm × a width of 90 mm. In addition, a copper plate is prepared as a metal plate. The copper plate is an oxygen-free copper plate. The ceramic circuit substrates 1 of Examples 1 to 7 are as follows Figure 2 As shown in FIG. 1 , the second ceramic substrate 7 is provided. On the other hand, the ceramic circuit substrate 1 of Example 8 is as shown in FIG. Figure 1 The second ceramic substrate 7 and the non-cooling flow path metal plate 8 are not provided.

[0077] The ceramic substrate 2 and the copper plate were bonded together using an active metal bonding method. Ag-Cu-Sn-Ti based solder was used as the active metal solder.

[0078] In the ceramic circuit substrates 1 of Examples 1 to 7, the thickness of the copper plate corresponding to the non-cooling flow path metal plate 3, the cooling flow path metal plate 4, and the non-cooling flow path metal plate 8 and the thickness of the ceramic substrate 2 are shown in Table 1. In addition, the vertical and horizontal dimensions of the non-cooling flow path metal plate 3, the cooling flow path metal plate 4, and the non-cooling flow path metal plate 8 are shown in Table 2. In addition, the non-cooling flow path metal plate 3 is described as the front metal plate, and the non-cooling flow path metal plate 8 is described as the back metal plate. In addition, the shape of the cooling flow path portion 5 provided on the copper plate corresponding to the cooling flow path metal plate 4 is shown in Table 3.

[0079] In addition, the ceramic circuit substrates 1 of Examples 1 to 7 refer to Figure 2 structure.

[0080] In addition, as the ceramic circuit substrate 1 of Example 8, Figure 1 The front metal plate is bonded to the front surface of the silicon nitride substrate as the ceramic circuit substrate 1, and the cooling flow path metal plate 4 is bonded to the back surface by an active metal bonding method. In addition, the non-cooling flow path metal plate 3 is expressed as the front metal plate. The front metal plate and the cooling flow path metal plate 4 are copper plates (oxygen-free copper plates).

[0081] [Table 1]

[0082]

[0083] [Table 2]

[0084]

[0085] [Table 3]

[0086]

[0087] The vertical and horizontal dimensions of the front and back metal plates shown in Table 2 represent vertical mm × horizontal mm. In addition, the cooling flow path metal plate 4 is a shape in which a groove is formed from a single side. The cover portion 10 uses a copper plate with a thickness of 0.3 mm. In addition, the cooling flow path portion 5 is a curved cooling flow path portion, each of which is provided with an inlet 5A and an outlet 5B. In addition, the cooling flow path portion 5 is a linear component, and a plurality of them are arranged in such a way that the volume ratio becomes a specified value. In addition, the width of the cooling flow path portion 5 is within the range of more than 1 mm and less than 10 mm. In addition, the surface distance of the cooling flow path portion 5 is set to be more than 1 mm.

[0088] The flatness of the ceramic circuit substrate 1 of Examples 1 to 8 was investigated. The flatness of the front metal plate and the back metal plate was measured. In the ceramic circuit substrate 1 of Examples 1 to 7, the flatness of the non-cooling flow path metal plate 3 as the front metal plate and the non-cooling flow path metal plate 8 as the back metal plate was measured. On the other hand, in the ceramic circuit substrate 1 of Example 8, the flatness of the non-cooling flow path metal plate 3 as the front metal plate and the cooling flow path metal plate 4 was measured. The difference between the highest point and the lowest point on the front side of the front metal plate was measured using a three-dimensional shape measuring machine. The back metal plate was measured in the same manner. The results are shown in Table 4.

[0089] [Table 4]

[0090]

[0091] As shown in Table 4, in the ceramic circuit substrates 1 of Examples 1 to 8, the flatness of the metal plate is less than 1.5 mm, so sufficient flatness can be ensured. In Examples 1 to 8, in the ceramic circuit substrates 1 of Examples 1 to 6, the flatness of the front metal plate and the back metal plate is less than 1.0 mm. In addition, in the ceramic circuit substrates 1 of Examples 2, 3, and 5 using the cover 10, the flatness of the front metal plate and the back metal plate is relatively small, less than 0.4 mm. In addition, in the ceramic circuit substrates 1 of Examples 2 and 3 using a silicon nitride substrate and the cover 10, the flatness of the front metal plate and the back metal plate is further reduced to less than 0.2 mm.

[0092] On the other hand, in Example 7, the flatness of the front metal plate and the back metal plate both exceed 1.0 mm. In the ceramic circuit substrate 1 of Example 7, since the thickness of the cooling flow path metal plate 4 is thin, the deformation of the ceramic circuit substrate 1 becomes larger. In addition, the ceramic circuit substrate 1 of Example 8 has a structure that does not use the second ceramic substrate 7. In this case, the flatness of the front metal plate is good. On the other hand, the flatness of the cooling flow path metal plate 4 exceeds 1.0 mm. Therefore, it can be seen that the flatness of the metal plate is good when the second ceramic substrate is used.

[0093] Next, the cooling efficiency was investigated. A semiconductor device 12 was produced in which a semiconductor element 11 was mounted on the ceramic circuit substrate 1 of Examples 1 to 8. Next, a device was produced in which the semiconductor device 12 of Examples 1 to 8 was mounted on a mounting plate via grease (hereinafter referred to as semiconductor device A). In addition, the grease was set to a thickness of 0.7 mm. In addition, a device was produced in which the semiconductor device 12 of Examples 1 to 8 was mounted on a mounting plate without grease (hereinafter referred to as semiconductor device B).

[0094] Each semiconductor device A and B was energized, and the temperature rising from the steady state was measured. In addition, the temperature was measured while cooling water as a cooling medium flowed through the cooling flow path 5. Five samples were made to show the lower limit value to the upper limit value of the rising temperature. The results are shown in Table 5.

[0095] [Table 5]

[0096]

[0097] As can be seen from Table 5, the ceramic circuit substrates 1 of Examples 1 to 8 are provided with a cooling flow path portion 5, so the cooling efficiency is improved. In addition, the ceramic circuit substrates 1 of Examples 1 to 8 do not need to use a radiator heat sink or a water-cooled water tank portion as in Patent Document 2. Therefore, the semiconductor device can be made thinner. In addition, a heat sink or a water-cooled water tank portion may not be provided separately, so the thermal resistance can be reduced. In addition, it can be used even without grease. Therefore, the ceramic circuit substrates of Examples 1 to 8 can improve the cooling efficiency.

[0098] As described above, according to the ceramic circuit board 1 of the embodiment, it is possible to provide a ceramic circuit board that improves the cooling efficiency of the semiconductor element 11 and has excellent manufacturability.

[0099] Several embodiments of the present invention are illustrated above, but these embodiments are presented as examples and are not intended to limit the scope of the invention. These new embodiments can be implemented in various other ways, and various omissions, substitutions, changes, etc. can be made without departing from the scope of the main purpose of the invention. Modifications of these embodiments are included in the scope and main purpose of the invention, and are included in the invention described in the claims and the scope of their equivalents. In addition, the above-mentioned embodiments can be implemented in combination with each other.

Claims

1. A ceramic circuit substrate, comprising a ceramic substrate and metal plates bonded to both surfaces of the ceramic substrate, characterized in that: The metal plate bonded to at least one of the two surfaces of the ceramic substrate is a cooling flow path metal plate having a cooling flow path portion.

2. The ceramic circuit substrate according to claim 1, characterized in that: The thickness of the ceramic substrate is smaller than the thickness of the cooling flow path metal plate.

3. The ceramic circuit substrate according to claim 1 or 2, characterized in that: The ceramic substrate includes a first ceramic substrate and a second ceramic substrate joined to a metal plate joined to the first ceramic substrate. One surface of the second ceramic substrate is joined to the cooling flow path metal plate joined to the first ceramic substrate, The metal plate is bonded to the other surface of the second ceramic substrate.

4. The ceramic circuit substrate according to any one of claims 1 to 3, characterized in that: An inlet and an outlet of the cooling flow path portion of the cooling flow path metal plate are provided on the same side surface of the cooling flow path metal plate.

5. The ceramic circuit substrate according to any one of claims 1 to 3, characterized in that: The cooling flow path portion of the cooling flow path metal plate has a plurality of folded portions.

6. The ceramic circuit substrate according to any one of claims 1 to 5, characterized in that: The ceramic substrate is a silicon nitride substrate.

7. The ceramic circuit substrate according to any one of claims 1 to 6, characterized in that: The metal plate is a copper plate.

8. The ceramic circuit substrate according to any one of claims 1 to 7, characterized in that: The ceramic substrate and the metal plate are bonded via an active metal bonding layer.

9. The ceramic circuit substrate according to any one of claims 1 to 8, characterized in that: The metal plate bonded to one of the two surfaces of the ceramic substrate is the cooling flow path metal plate, and the metal plate bonded to the other surface is a non-cooling flow path metal plate that does not have the cooling flow path portion.

10. A semiconductor device, characterized in that: A semiconductor element is mounted on the non-cooling flow path metal plate of the ceramic circuit substrate according to claim 9 .

11. The method for using a semiconductor device according to claim 10, wherein: The temperature is controlled by causing a cooling medium to flow through or contact the cooling flow path portion of the cooling flow path metal plate.

Citation Information

Cited By

  • Manufacturing method of ceramic substrate, ceramic substrate and power module

    CN120767205A