Cooker and manufacturing method thereof
A non-stick layer with a mixed structure of solid solution and elemental particles, combined with an iron nitride-based layer formed by spraying, enhances the non-stick properties and corrosion resistance, ensuring effective and durable non-stick performance.
Patent Information
- Application Number
- CN202411181923.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-12-06
AI Technical Summary
Existing non-stick ceramic coatings on cookware lack initial non-stickiness and long-lasting non-stick properties, and are prone to corrosion, necessitating the development of materials with improved wear resistance and corrosion resistance.
A non-stick layer composed of a mixed layer of solid solution particles and elemental particles, including iron and non-metallic elements like boron, carbon, and selenium, with an amorphous structure, and an iron nitride corrosion-resistant layer formed by spraying, enhancing wear resistance and non-stick properties.
The combination of amorphous non-stick layer and iron nitride layer provides both initial and lasting non-stick properties, along with improved corrosion resistance, ensuring effective and durable non-stick performance.
Smart Images

Figure CN119073797A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of cookers, and in particular to a cooker and a method for manufacturing the cooker. Background Art
[0002] In the field of cookware, non-stick materials have always been a hot topic of research. With the development of non-stick industry technology, solid spray materials based on ceramics do not require the use of organic liquid coatings such as fluorine coatings or ceramic coatings. They can reduce the psychological burden of customers using cookware products and avoid various problems caused by atomized spray. They have broad development prospects and potential.
[0003] Specifically, solid spraying materials based on ceramics (e.g., titanium oxide, titanium nitride, titanium carbide, ferroferric oxide, ferrous oxide, ferrous oxide, aluminum oxide, chromium oxide, and nickel oxide, etc.) can form a non-stick layer, which is the so-called "coating-free non-stick technology". The coating-free here only means that it does not use organic coatings such as fluorine coatings or ceramic coatings.
[0004] However, although the coating formed by thermal spraying of the above-mentioned ceramic material is wear-resistant, its initial non-stickiness is poor and cannot meet the national standard requirements for initial non-stickiness. It is usually necessary to add grease or modify it with a material with good non-stickiness (such as modifying it with polysiloxanes or fluorinated materials) to improve its non-stick performance. Since the oil film or the modified material is easy to be damaged, it will affect the long-term non-stickiness of the cookware with the coating.
[0005] To this end, developing cookware that has both initial non-stick properties, long-lasting non-stick properties and corrosion resistance remains a problem that needs to be solved. Summary of the invention
[0006] Therefore, an object of the present application is to provide a cookware and a method for manufacturing the same, so as to solve the general problems of initial non-stickiness, long-lasting non-stickiness and corrosion resistance of the cookware in the prior art.
[0007] The purpose of the present application is to provide a cooker, wherein the cooker body, the iron nitride corrosion-resistant layer and the non-stick layer, the iron nitride corrosion-resistant layer is formed on the cooker body by spraying, and the non-stick layer is formed on the iron nitride corrosion-resistant layer, wherein the non-stick layer has an amorphous structure, and the non-stick layer is a mixed layer including solid solution particles and elemental particles, wherein the solid solution particles are solid solution particles formed by iron and a non-metallic elemental substance, and the non-metallic elemental substance includes one or more of boron, carbon, silicon and selenium, and the elemental particles are the same as the non-metallic elemental substance.
[0008] According to the cookware provided in the embodiment of the present application, the iron nitride corrosion-resistant layer is a dense layer, which can prevent the corrosive medium from entering between the cookware body and the iron nitride corrosion-resistant layer and affecting the bonding force between the two or causing corrosion of the cookware body, thereby ensuring the corrosion-resistant life of the cookware. The non-stick layer has an amorphous structure, so it can exert certain wear resistance and non-stick properties due to its amorphous nature. In addition, the non-stick layer is a mixed layer including solid solution particles and elemental particles. The solid solution particles can improve the wear resistance and corrosion resistance of the non-stick layer. The elemental particles have a good affinity with edible oil and can firmly lock the edible oil to form a uniform oil film layer. In this way, the possibility of food adhesion can be further reduced. In combination with the above, the cookware according to the present application can have both initial non-stickiness, lasting non-stickiness and corrosion resistance.
[0009] In some embodiments, an iron-containing compound is further dispersed in the mixed layer, and the iron-containing compound is an iron-containing compound formed by iron and a corresponding non-metallic element.
[0010] In these embodiments, the iron-containing compound can improve the wear resistance of the non-stick layer, thereby helping to improve the long-lasting non-stick performance of the cookware.
[0011] Specifically, the iron-containing compound is x-Fe5C2, θ-Fe3C, ε-Fe2C, ε'-Fe 2.2 One or more of C, Fe7C3, Fe2B, FeB, Fe2Si, Fe5Si3, FeSi, FeSi2, Fe3Se4, FeSe, and FeSe2.
[0012] In these embodiments, the iron-containing compound has multiple iron phases, and the composition of different phases represents the presence of more cavities and distortions inside the crystal, which can further enhance the amorphousness of the non-stick layer, thereby further optimizing the durable non-stick property.
[0013] In some embodiments, based on the total weight of the non-stick layer as 100%, the weight of the elemental particles accounts for 13%-33% of the total weight of the non-stick layer, and the remainder is solid solution particles; or based on the total weight of the non-stick layer as 100%, the weight of the solid solution particles accounts for 70%-80% of the total weight of the non-stick layer, the weight of the elemental particles accounts for 5%-15% of the total weight of the non-stick layer, and the remainder is iron-containing compounds.
[0014] In these embodiments, the non-stick layer has a preset amount of solid solution, has an amorphous form to reduce surface energy, and has non-stick and thermal stability. The non-stick layer has a preset amount of elemental particles to ensure the lipophilicity of the non-stick layer, has good affinity with edible oil during cooking, can firmly lock the edible oil to form a uniform oil film and enhance the non-stick property of the cookware. The non-stick layer has a preset amount of iron-containing compounds to improve the wear resistance of the cookware. Therefore, the non-stick layer in the above form can optimize the wear resistance, non-stick and thermal stability of the non-stick layer.
[0015] In some embodiments, the non-stick material is a material whose volume proportion of amorphous phase is in the range of 67%-75%, which can further optimize the non-stick performance of the formed non-stick layer. The particle size of the non-stick material is 300-500 mesh. During the plasma spraying process, the melting degree of the non-stick material is low, the deformation is small, and the non-stick layer can be formed in a densely packed manner. In this way, on the one hand, the formed non-stick layer has a pore structure that can store oil, ensuring the non-stick performance. On the other hand, the surface of the formed non-stick layer has a certain rough structure, which can serve as the main focus during the cooking process, protect the oil film, and improve the lasting non-stick property.
[0016] In some embodiments, the non-stick layer has a porous structure capable of storing oil, so that a stable oil film can be formed during use to make the cookware non-sticky. The surface of the non-stick layer has a rough structure. During the manufacturing process of the cookware, by controlling the particle size of the non-stick material, the surface of the non-stick layer with a rough structure can be formed by spraying. The hardness of the iron carbide particles themselves is extremely high, and the rough structure of the surface can serve as the main focus during the cooking process, which can protect the oil film and ensure long-lasting non-stick properties.
[0017] In some embodiments, the thickness of the non-stick layer is 40 microns to 80 microns. In this way, the properties of the cookware in various aspects such as non-stick, thermal conductivity and stress can be balanced, thereby obtaining a cookware with excellent comprehensive performance.
[0018] In some embodiments, the iron carbide particles include iron phases with different degrees of carburization. The composition of different phases represents the presence of more holes and distortions inside the crystals, which makes the non-stick layer as a whole appear amorphous, that is, has an amorphous structure, thus optimizing the long-lasting non-stick properties.
[0019] In some embodiments, the volume proportion of the amorphous phase of the amorphous structure is 67%-75%. In this way, the non-stick layer can optimize the non-stick performance due to its higher amorphousness.
[0020] In some embodiments, the iron nitride corrosion-resistant layer includes iron nitride particles and flaky graphite filled in the particle gaps of the iron nitride particles. In the iron nitride corrosion-resistant layer with such a structure, the flaky graphite can play a blocking role, reducing the number of through holes in the formed iron nitride corrosion-resistant layer and the probability of carburization of the corrosive medium.
[0021] In some embodiments, the iron nitride corrosion resistant layer is formed by granulated powder of iron nitride, and the granulated powder of iron nitride is obtained by drying, briquetting and crushing a mixed slurry including iron nitride particles, flaky graphite and a binder.
[0022] In these embodiments, the method of forming the granulated iron nitride powder is simple, and no spray drying step is required, which can simplify the overall process of the cooker.
[0023] In some embodiments, the particle size of the iron nitride particles is 800-1200 mesh. If the particle size of the iron nitride material is too coarse, for example, more than 800 mesh, the porosity of the iron nitride corrosion-resistant layer formed by spraying the iron nitride material is high, and the corrosive medium easily penetrates into the cookware substrate, causing corrosion of the substrate, resulting in the iron nitride corrosion-resistant layer and the cookware substrate falling off at the junction; if the particle size of the iron nitride material is too fine, for example, less than 500 mesh, the plasma equipment will not be able to spray normally.
[0024] In some embodiments, in the mixed slurry, the weight ratios of the iron nitride particles, flake graphite and adhesive are (70-85):(3-8):(5-12) respectively. The iron nitride particles, flake graphite and adhesive have their own weight ratios, which can ensure the strength of the formed iron nitride material, thereby ensuring the quality of the iron nitride corrosion-resistant layer formed thereby.
[0025] In some embodiments, the thickness of the iron nitride corrosion-resistant layer is 30 microns to 60 microns. In this way, the properties of the cookware in various aspects such as corrosion resistance, thermal conductivity and stress can be balanced, thereby obtaining a cookware with excellent comprehensive performance.
[0026] In some embodiments, the porosity of the iron nitride corrosion-resistant layer is 0.5%-2%, and the pore size is 0.5 micrometers-1 micrometers. Such a pore structure can ensure the corrosion resistance of the cookware.
[0027] In some embodiments, an oil film layer formed by the combination of fatty acid anhydride groups and unsaturated fatty acid glycerides is disposed on the surface of the non-stick layer.
[0028] In these embodiments, grafting more lipophilic groups on the surface of the non-stick layer can ensure that the cookware can easily absorb grease during use and ensure the stability and continuity of the oil film layer, thereby further improving the non-stick performance of the cookware.
[0029] According to a second aspect of the present application, a method for manufacturing cookware is provided, wherein the method comprises: providing a cookware substrate; forming a non-stick layer on the cookware substrate by thermally spraying a non-stick material; wherein the non-stick material has an amorphous phase, the non-stick material comprises a solid solution and a single substance attached to the surface of the solid solution, the solid solution is a solid solution of iron and a non-metallic single substance, the non-metallic single substance comprises one or more of boron, carbon, silicon and selenium, and the single substance is the same as the non-metallic single substance.
[0030] According to the method for manufacturing cookware provided in the embodiment of the present application, the non-stick layer has an amorphous structure, so it can exert certain wear resistance and non-stick properties due to its amorphous nature. In addition, the non-stick layer is a mixed layer including solid solution particles and elemental particles. The solid solution particles can improve the wear resistance and corrosion resistance of the non-stick layer. The elemental particles have good affinity with edible oil and can firmly lock the edible oil to form a uniform oil film layer, thus further reducing the possibility of food adhesion. In combination with the above, the cookware according to the present application can have both initial non-stickiness and lasting non-stickiness.
[0031] In some embodiments, the non-stick material is formed by the following steps: ion implantation of iron with a single element is performed so that the single element is at least doped into the iron lattice, thereby forming a non-stick material having an amorphous phase and including a solid solution and a single element, wherein the single element is on the surface of the solid solution.
[0032] In these embodiments, the solid solution has low surface energy and high hardness, and the single substance has high hardness and a certain lipophilicity. The synergistic effect of the solid solution and the single substance can make the non-stick material have excellent non-stick properties and wear resistance, so that the coating of the non-stick cookware formed by the non-stick material has both excellent initial non-stick properties and long-lasting non-stick properties.
[0033] In some embodiments, the plasma implantation temperature is 200°C-300°C, and the ion implantation dose of the element on iron per square centimeter is 2.5×10 18 -3.0×10 19 ions, wherein in the step of forming the non-stick material, the non-stick material including the solid solution, the simple substance and the iron-containing compound is formed by increasing the dose of ion implantation and the temperature of ion implantation.
[0034] In these embodiments, iron-containing compounds are also dispersed in the non-stick material as a wear-resistant phase, which can further improve the wear resistance of the non-stick material and ensure the wear resistance of the non-stick layer.
[0035] In some embodiments, the method further comprises: before forming the non-stick layer, first using iron nitride to form an iron nitride corrosion-resistant layer on the cookware substrate by spraying, and then forming the non-stick layer on the surface of the iron nitride corrosion-resistant layer. In this way, adding the iron nitride corrosion-resistant layer to the cookware can ensure the corrosion resistance of the cookware, avoid the cookware from delaminating due to poor corrosion resistance, and thus to a certain extent extend the long-lasting non-stick life of the cookware.
[0036] In some embodiments, the method further comprises: after forming the non-stick layer, performing a hydroxylation treatment on the non-stick layer, immersing the hydroxylated non-stick layer in a fatty acid solution to connect fatty acid anhydride groups on the non-stick layer, and finally coating unsaturated fatty acid glyceride to react with the fatty acid anhydride groups to form an oil film layer. By modifying the non-stick layer, the non-stick layer has a good non-stick effect in an oil-free or low-oil environment in its initial state, so as to improve the user experience.
[0037] In some embodiments, the non-stick material is formed by ion implantation of carbon atoms into pure iron powder. In this way, the non-stick material that meets various requirements of the present application can be obtained.
[0038] In some embodiments, the particle size of the iron nitride material forming the iron nitride corrosion-resistant layer is smaller than the particle size of the non-stick material forming the non-stick layer. Since the iron nitride material is finer, it can be more tightly stacked together when forming the corrosion-resistant layer, reducing the gaps between the particles, thereby forming a denser iron nitride corrosion-resistant layer. The dense iron nitride corrosion-resistant layer can more effectively block the erosion of external corrosive media and improve the corrosion resistance of the material. The particle size of the non-stick material is relatively large, which can ensure the formation of a suitable rough structure and pore structure, and can ensure the stability of the subsequent oil film. And because it is arranged outside the iron nitride corrosion-resistant layer, it can act as a retaining wall, reduce the number of vents connecting the iron nitride corrosion-resistant layer with the outside world, and further optimize the corrosion resistance.
[0039] In some embodiments, the particle size of the non-stick material is 300-500 mesh; and / or the particle size of the iron nitride material is 500-800 mesh, which can balance the properties of the cookware in various aspects such as corrosion resistance, non-stick, thermal conductivity and stress, thereby obtaining cookware with excellent comprehensive performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] The above and other objects and features of the present application will become more apparent through the following description of the embodiments in conjunction with the accompanying drawings, in which:
[0041] Figure 1 is a schematic diagram of the structure of a cooker provided according to an embodiment of the present application;
[0042] Figure 2is a schematic diagram of the enlarged structure of the iron nitride corrosion-resistant layer of the cooker provided in an embodiment of the present application;
[0043] Figure 3 is an enlarged structural schematic diagram of a non-stick layer of a cooker provided according to an embodiment of the present application;
[0044] Figure 4 is a schematic structural diagram of a non-stick material provided according to an embodiment of the present application;
[0045] Figure 5 It is a schematic diagram of the structure of another non-stick material provided according to an embodiment of the present application.
[0046] Explanation of symbols
[0047] 100. Cookware; 110. Cookware body; 120. Iron nitride corrosion-resistant layer; 121. Iron nitride particles; 122. Flake graphite; 130. Non-stick layer; 200. Non-stick material; 201. Solid solution; 202. Simple substance; 203. Iron-containing compound. DETAILED DESCRIPTION
[0048] The inventive concept will be described more fully below in conjunction with exemplary embodiments, however, the inventive concept can be implemented in many different forms and should not be interpreted as being limited to the embodiments set forth herein. On the contrary, these embodiments are provided so that this disclosure will be thorough and complete, and will fully convey the scope of the inventive concept to those skilled in the art.
[0049] The initial non-stick properties and the lasting non-stick properties of the cookware in the prior art are average. Therefore, there is still an urgent need in the industry to develop new non-stick cookware with both initial non-stick properties and lasting non-stick properties.
[0050] In order to solve the problems in the above-mentioned prior art, the present application is committed to studying a variety of materials. The applicant has found that in the process of forming a non-stick material obtained by injecting iron ions into a non-metallic single substance (such as at least one of boron, carbon, silicon and selenium), a part of the non-metallic single substance atoms can diffuse into the lattice inside the iron powder under high-speed impact to form a solid solution, and lattice distortion occurs, resulting in the formation of a non-stick material with an amorphous phase, and another part of the non-metallic single substance does not enter the interior of the solid solution, but exists on the surface of the solid solution by accumulation, thereby forming a non-stick material including a solid solution and a single substance and having an amorphous phase. By thermally spraying the non-stick material obtained above, the various components in the non-stick material can be mostly retained, so that a mixed layer including solid solution particles and single substance particles can be formed. Among them, the solid solution particles are solid solution particles of iron and non-metallic single substances, and the non-metallic single substances include one or more of boron, carbon, silicon and selenium, and the single substance particles are the same as the non-metallic single substance. The solid solution particles have excellent surface properties and can ensure the non-stick properties of the cookware. The single-substance particles can make the cookware easy to be oleophilic during use and have high hardness and wear resistance. The appropriate amount of solid solution particles in the mixed layer can effectively resist wear and improve the non-stick properties. Therefore, the cookware according to the present application can have both initial non-stick properties and lasting non-stick properties.
[0051] According to the first aspect of the present application, a cooker is provided, wherein the cooker includes a cooker body and a non-stick layer, and the non-stick layer is formed by spraying a non-stick material on the cooker body. The non-stick layer has an amorphous structure, and the non-stick layer is a mixed layer including solid solution particles and elemental particles, wherein the solid solution particles are solid solution particles formed by iron and non-metallic elements, and the non-metallic elements include one or more of boron, carbon, silicon and selenium, and the elemental particles are the same as the non-metallic elements. That is to say, in the case where the non-metallic elements include one or more of boron, carbon, silicon and selenium, the elemental particles are the same as these non-metallic elements. As an example, when the non-metallic element is carbon, the elemental particles are carbon particles, and when the non-metallic element is boron, the elemental particles are boron particles.
[0052] According to the cookware provided in the embodiment of the present application, the non-stick layer has an amorphous structure, so it can exert certain wear resistance and non-stick properties due to its amorphous nature. In addition, the non-stick layer is a mixed layer including solid solution particles and elemental particles. The solid solution particles can improve the wear resistance and corrosion resistance of the non-stick layer. The elemental particles have good affinity with edible oil and can firmly lock the edible oil to form a uniform oil film layer, thus further reducing the possibility of food adhesion. In combination with the above, the cookware according to the present application can have both initial non-stickiness and lasting non-stickiness.
[0053] In some embodiments, the non-stick layer is formed by thermal spraying a non-stick material, and the non-stick material has an amorphous phase, so that the formed non-stick layer has an amorphous structure.
[0054] In some embodiments, based on the total weight of the non-stick layer being 100%, the weight of the single substance particles accounts for 13%-33% of the total weight of the non-stick layer, and the remainder is solid solution particles, so that the wear resistance, non-stickiness and thermal stability of the non-stick layer can be optimized. As an example, the non-stick layer has an amorphous structure, and the volume proportion of the amorphous phase of the non-stick layer is 65%-70%, which can further optimize the non-stick performance.
[0055] According to the present application, an iron-containing compound is also dispersed in the mixed layer, and the iron-containing compound is an iron-containing compound formed by iron and a corresponding non-metallic element, wherein the iron-containing compound has a plurality of iron phases. Specifically, when the non-metallic element is carbon, the non-stick layer is a mixed layer of solid solution particles of iron and carbon, carbon particles and iron-containing compounds, wherein the iron-containing compound includes iron phases with different degrees of carburization, for example, including x-Fe5C2, θ-Fe3C, ε-Fe2C, ε'-Fe 2.2 C and Fe7C3. In the case where the non-metallic element is boron, the non-stick layer is a mixed layer of solid solution particles of iron and boron, boron particles and iron-containing compounds, wherein the iron-containing compounds include iron phases with different degrees of boronization, for example, including Fe2B and FeB. In the case where the non-metallic element is silicon, the non-stick layer is a mixed layer of solid solution particles of iron and silicon, silicon particles and iron-containing compounds, wherein the iron-containing compounds include iron phases with different degrees of silicide, for example, including Fe2Si, Fe5Si3, FeSi, FeSi2. In the case where the non-metallic element is selenium, the non-stick layer is a mixed layer of solid solution particles of iron and selenium, selenium particles and iron-containing compounds, wherein, in the present application, the iron-containing compounds include iron phases with different degrees of selenization, for example, including Fe3Se4, FeSe and FeSe2.
[0056] In these embodiments, the iron-containing compound can improve the wear resistance of the non-stick layer, thereby helping to improve the long-lasting non-stick performance of the cookware. In addition, the iron-containing compound has a variety of iron phases, and the composition of different phases represents the presence of more cavities and distortions inside the crystal, which can further enhance the amorphousness of the non-stick layer, thereby further optimizing the long-lasting non-stick performance. As an example, the non-stick layer has an amorphous structure, and the volume proportion of the amorphous phase of the non-stick layer can be increased by 2%-4%, thereby further improving the non-stick performance.
[0057] According to the present application, the non-stick layer includes a mixed layer of solid solution particles and elemental particles, and also includes an iron-containing compound uniformly dispersed in the mixed layer. That is, in the non-stick layer, there is a mixed structure of solid solution particles, elemental particles and iron-containing compounds. In some embodiments, based on the total weight of the non-stick layer as 100%, the weight of the solid solution particles accounts for 70%-80% of the total weight of the non-stick layer, the weight of the elemental particles accounts for 5%-15% of the total weight of the non-stick layer, and the balance is the iron-containing compound.
[0058] In these embodiments, the non-stick layer has a preset amount of solid solution, has an amorphous form to reduce surface energy, and has non-stick and thermal stability. The non-stick layer has a preset amount of elemental particles to ensure the lipophilicity of the non-stick layer, has good affinity with edible oil during cooking, can firmly lock the edible oil to form a uniform oil film and enhance the non-stick property of the cookware. The non-stick layer has a preset amount of iron-containing compounds to improve the wear resistance of the cookware. Therefore, the non-stick layer in the above form can optimize the wear resistance, non-stick and thermal stability of the non-stick layer.
[0059] According to the present application, the non-stick layer is formed by plasma spraying a non-stick material on the cooker body. Specifically, the non-stick material is a material in which the volume proportion of the amorphous phase is 67%-75%, which can further optimize the non-stick performance of the formed non-stick layer. The particle size of the non-stick material is 300 mesh-500 mesh. During the plasma spraying process, the non-stick material has a low degree of melting and a small deformation, and can form a non-stick layer in a densely packed manner. In this way, on the one hand, the formed non-stick layer has a pore structure that can store oil, ensuring the non-stick performance. On the other hand, the surface of the formed non-stick layer has a certain rough structure, which can serve as the main focus during the cooking process, protect the oil film, and improve the lasting non-stick property.
[0060] According to the present application, the surface of the non-stick layer has a rough structure. During the manufacturing process of the cookware, by controlling the particle size of the non-stick material, the surface of the non-stick layer with a rough structure and a certain hardness can be formed by spraying. In this way, it can serve as the main focus during the cooking process, protect the oil film, and enhance the lasting non-stick properties.
[0061] According to the present application, the non-stick layer has a suitable thickness. In some embodiments, the thickness of the non-stick layer is 40 microns to 80 microns. In this way, the properties of the cookware in various aspects such as non-stick, thermal conductivity and stress can be balanced to obtain cookware with excellent comprehensive performance.
[0062] According to the present application, an oil film layer formed by combining fatty acid anhydride groups and unsaturated fatty acid glycerides is connected to the surface of the non-stick layer.
[0063] In these embodiments, grafting more lipophilic groups on the surface of the non-stick layer can ensure that the cookware can easily absorb grease during use and ensure the stability and continuity of the oil film layer, thereby further improving the non-stick performance of the cookware.
[0064] In the field of cookware manufacturing, it is usually adopted to form a non-coated non-stick layer by nitriding treatment first and then spraying. However, since the surface of the nitrided layer obtained by nitriding treatment is dense, hard and smooth, it is not easy to undergo metallurgical bonding and deformation, resulting in poor bonding strength of the subsequent non-coated non-stick layer. For this reason, in the prior art, a corrosion-resistant iron pot usually needs to first form a non-coated non-stick layer on the iron substrate by thermal spraying, and then undergo nitriding treatment. Most of the nitrogen atoms will act on the iron substrate through the pores of the non-coated non-stick layer, thereby forming a "white bright layer" with a corrosion-resistant effect, that is, a nitrided layer (iron nitride layer). However, the corrosion resistance life of an iron pan often depends on the thickness of the nitride layer, and the nitride layer formed by nitriding treatment is usually thin, generally 5 microns to 10 microns. This is because the nitriding treatment is subject to the nitriding temperature and time and the deformation of the substrate. If the thickness of the nitriding layer needs to be increased, it is difficult to achieve with existing processes. For example, blindly increasing the nitriding time may cause the cookware to deform and the uncoated non-stick layer to become brittle and collapse, resulting in a low yield in the manufacture of cookware.
[0065] The applicant has found that iron nitride has high corrosion resistance. Iron nitride particles with a particle size of 500-800 mesh can be used to form an iron nitride corrosion-resistant layer on the cookware substrate by spraying, rather than using a method of forming a corrosion-resistant layer by a nitriding process after the subsequent formation of a coating. This can control the thickness of the required corrosion-resistant layer to a certain extent. In addition, the iron nitride layer formed by spraying is not smooth and dense, but has a certain degree of roughness and porosity, and can form a mechanical bite with the subsequent non-stick layer, so there is no problem of insufficient bonding force. In addition, since the spraying process does not require the material to be completely melted, it is not necessary to set a too high temperature. In this case, deformation of the cookware substrate and collapse of the outer layer can be avoided, thereby ensuring the yield rate in the cookware manufacturing process.
[0066] In some embodiments, the cookware further comprises an iron nitride corrosion resistant layer, which is formed on the surface of the cookware body by spraying with an iron nitride material, wherein the non-stick layer is formed on the surface of the iron nitride corrosion resistant layer. As an example, the spraying method may be a plasma spraying method, and the thickness of the formed iron nitride corrosion resistant layer may be 30 microns to 60 microns, so that the properties of the cookware in various aspects such as corrosion resistance, thermal conductivity and stress can be balanced, thereby obtaining a cookware with excellent comprehensive performance.
[0067] like Figure 1 As shown, the cooker 100 includes a cooker body 110, an iron nitride corrosion-resistant layer 120 and a non-stick layer 130, wherein the iron nitride corrosion-resistant layer 120 is formed on the surface of the cooker body 110 by plasma spraying using an iron nitride material, and the non-stick layer 130 is formed on the cooker body by plasma spraying using a non-stick material, specifically, formed on the surface of the iron nitride corrosion-resistant layer 120.
[0068] Figure 2 FIG. 1 is a schematic diagram of the enlarged structure of the iron nitride corrosion-resistant layer of the cooker provided in the embodiment of the present application. Figure 2 As shown, the iron nitride corrosion resistant layer 120 includes iron nitride particles 121 and flake graphite 122 filled in the particle gaps of the iron nitride particles 121. In a preferred embodiment, during the process of thermal spraying to form the iron nitride corrosion resistant layer, the flake graphite 122 is horizontally placed in the gaps between the plurality of iron nitride particles 121. In the iron nitride corrosion resistant layer with such a structure, the flake graphite can play a blocking role, reducing the number of through holes in the formed iron nitride corrosion resistant layer and the probability of carburization of the corrosive medium. .
[0069] Figure 3 Schematic diagram of the enlarged structure of the non-stick layer of the cooker provided in the embodiment of the present application. Figure 3 As shown, the non-stick layer 130 is formed by depositing a non-stick material 200 .
[0070] In these embodiments, the iron nitride corrosion-resistant layer is a dense layer, which can prevent the corrosive medium from entering between the cooker body and the iron nitride corrosion-resistant layer to affect the bonding strength between the two or cause corrosion of the cooker body, thereby ensuring the corrosion-resistant life of the cooker.
[0071] According to the present application, the iron nitride corrosion-resistant layer is located inside the cookware, and the non-stick layer is located outside the cookware, and the particle size of the iron nitride material forming the iron nitride corrosion-resistant layer is smaller than the particle size of the non-stick material forming the non-stick layer. Since the iron nitride material is finer, it can be more tightly stacked together when forming the corrosion-resistant layer, reducing the gaps between the particles, thereby forming a denser iron nitride corrosion-resistant layer. The dense iron nitride corrosion-resistant layer can more effectively block the erosion of external corrosive media and improve the corrosion resistance of the material. As an example, the porosity of the iron nitride corrosion-resistant layer (indicates the percentage of the pore volume in the iron nitride corrosion-resistant layer to the total volume) is 0.5%-2%, and the pore size is 0.5 microns-1 microns. Such a pore structure can ensure the corrosion resistance of the cookware. The particle size of the non-stick material is relatively large, which can ensure the formation of a suitable rough structure and pore structure, thereby ensuring the stability of the subsequent oil film. And because it is arranged outside the iron nitride corrosion-resistant layer, it can act as a retaining wall to reduce the number of vents connecting the iron nitride corrosion-resistant layer with the outside world, thereby further optimizing the corrosion resistance.
[0072] As an example, the particle size of the non-stick material is 300-500 mesh; and / or the particle size of the iron nitride is 500-800 mesh, which can balance the properties of the cookware in terms of corrosion resistance, non-stick, thermal conductivity and stress, thereby obtaining cookware with excellent comprehensive performance.
[0073] According to a second aspect of the present application, a method for manufacturing a cooker is provided, wherein the method comprises:
[0074] Step S101, providing a cooker base.
[0075] Step S102, a non-stick layer is formed on the cookware substrate by spraying a non-stick material, wherein the non-stick material includes a solid solution and a single substance attached to the surface of the solid solution, the solid solution is a solid solution of iron and a non-metallic single substance, the non-metallic single substance includes one or more of boron, carbon, silicon and selenium, and the single substance is the same as the non-metallic single substance. Correspondingly, the non-stick layer includes a mixed layer of solid solution particles and single substance particles, wherein the solid solution particles are solid solution particles of iron and a non-metallic single substance, the non-metallic single substance includes one or more of boron, carbon, silicon and selenium, and the single substance particles are single substances corresponding to the non-metallic single substance.
[0076] It should be noted that the non-stick layer formed as above can be obtained by ion implantation into an iron substrate. According to the present application, by using a non-stick material having a solid solution and a single substance to form a non-stick layer, the thermal effect and thermal damage to the cookware substrate can be reduced to a certain extent compared to the above-mentioned method. In addition, the uniformity of each component in the non-stick layer can be ensured to a certain extent, thereby improving the durability and stability of the non-stick layer.
[0077] According to the method for manufacturing cookware provided in the embodiment of the present application, the non-stick layer has an amorphous structure, so it can exert certain wear resistance and non-stick properties due to its amorphous nature. In addition, the non-stick layer includes a mixed layer of solid solution particles and elemental particles. The solid solution particles can improve the wear resistance and corrosion resistance of the non-stick layer. The elemental particles have good affinity with edible oil and can firmly lock the edible oil to form a uniform oil film layer, thereby further reducing the possibility of food adhesion. In combination with the above, the cookware according to the present application can have both initial non-stickiness and lasting non-stickiness.
[0078] Hereinafter, the method for manufacturing a cooker according to the present application will be described in conjunction with specific embodiments.
[0079] Provide cookware base
[0080] According to the present application, the cookware base can be made of commonly used metal materials. For example, the material can be stainless steel, titanium, aluminum, titanium alloy, aluminum alloy, and composite materials formed by the above materials. The cookware base can have a shape corresponding to the function. For example, when the non-stick cookware is a non-stick pan, the cookware base can have a conventional pan shape.
[0081] In some embodiments, the inner surface of the cookware base is a rough surface, which can be obtained by sanding the inner surface of the cookware base. As an example, the roughness of the rough surface is a Ra value in the range of 3 μm-6 μm.
[0082] Formation of iron nitride corrosion resistant layer
[0083] According to the present application, the step of forming the iron nitride corrosion resistant layer includes the step of selecting an iron nitride material, and then using the iron nitride material to form the iron nitride corrosion resistant layer by plasma spraying.
[0084] In some embodiments, the iron nitride material is in granular form, and the particle size of the iron nitride material is between 500 mesh and 800 mesh. If the particle size of the iron nitride material is too coarse, for example, more than 800 mesh, the porosity of the iron nitride corrosion-resistant layer formed by spraying the iron nitride material is high, and the corrosive medium easily penetrates into the cookware substrate, causing corrosion of the substrate, and causing the iron nitride corrosion-resistant layer and the cookware substrate to fall off at the junction; if the particle size of the iron nitride material is too fine, for example, less than 500 mesh, the plasma equipment will not be able to spray normally.
[0085] As some examples, the iron nitride material is iron nitride particles, wherein the particles are quasi-spherical or spherical particles, and the density of the formed iron nitride corrosion-resistant layer can be improved through spherical dense packing.
[0086] As some other examples, the iron nitride material is a granulated powder of iron nitride, wherein the granulated powder of iron nitride is obtained by drying, briquetting and crushing a mixed slurry including iron nitride powder, flaky graphite and a binder.
[0087] Specifically, the method for manufacturing the cookware also includes: a step of forming granulated powder of iron nitride, wherein the step of forming granulated powder of iron nitride includes: providing a mixed slurry of iron nitride powder, flaky graphite and an adhesive; drying, briquetting and crushing the mixed slurry to obtain granulated powder of iron nitride.
[0088] In some embodiments, the particle size of the iron nitride powder is 800-1200 mesh, and is spherical or quasi-spherical. Particles with such a structure can be dried and pressed into a densely packed structure, ensuring the density of the formed iron nitride granulated powder, and improving the corrosion resistance of the formed iron nitride corrosion-resistant layer.
[0089] In certain embodiments, the binder may include at least one of a cellulose binder and an alcohol binder. The cellulose binder may include at least one of a hydroxymethylcellulose binder, a hydroxyethylcellulose binder and a hydroxypropylcellulose binder. The alcohol binder may include at least one of polyethylene glycol, a polyvinyl alcohol binder, a polypropylene alcohol binder and other higher alcohol binders containing more than six carbon atoms. However, the application is not limited thereto, but may select a suitable binder according to actual needs.
[0090] According to the present application, flake graphite refers to graphite in a three-dimensional flake shape, having a unique grain orientation and a lamellar structure. In some embodiments, the particle size of the flake graphite can be 300 mesh to 400 mesh.
[0091] In these embodiments, flake graphite and iron nitride powder are selected to form a mixed slurry, wherein the flake graphite has excellent thermal conductivity, can quickly disperse and conduct heat, and helps to reduce the thermal stress caused by temperature changes in the iron nitride corrosion layer, thereby extending its service life. Graphite is chemically stable at room temperature and is not easy to react with other substances, which helps to protect the iron nitride corrosion layer from chemical corrosion. The lubricity of graphite can reduce the friction between the iron nitride corrosion layer and other components and reduce wear. The flaky structure of flake graphite can tightly fill the tiny pores and cracks in the corrosion layer, improving the compactness and corrosion resistance of the corrosion layer. It should be noted that according to the present application, other materials can also be used to replace the graphite according to the present application. For example, the filling material can be a nanomaterial, such as nano silicon dioxide, nano aluminum oxide, etc. These nanomaterials have extremely high specific surface area and surface activity, can more effectively fill the tiny pores in the corrosion layer, and provide better corrosion resistance.
[0092] According to the present application, in the mixed slurry, the weight ratios of iron nitride powder, flake graphite and adhesive are (70-85):(3-8):(5-12) respectively. Such weight ratios of the components can ensure the content of iron nitride as the main corrosion-resistant component in the iron nitride corrosion-resistant layer and the content of flake graphite formed between the iron nitride powders, thereby ensuring the corrosion resistance of the iron nitride corrosion-resistant layer formed by such materials.
[0093] Specifically, the step of forming iron nitride granulated powder includes mechanically mixing 800-1200 mesh iron nitride powder and flaky graphite evenly, adding polyvinyl alcohol aqueous solution, stirring evenly, and then drying the water, pressing it into larger blocks in a press, and then crushing and screening it into a suitable particle size, and screening 500 mesh-800 mesh iron nitride granulated powder as the material for forming the iron nitride corrosion-resistant layer.
[0094] In the case where the cookware of the present application includes an iron nitride corrosion-resistant layer, according to the present application, the method for manufacturing the cookware further includes, before forming the non-stick layer, using iron nitride to form the iron nitride corrosion-resistant layer on the cookware substrate by spraying, and then forming the non-stick layer on the iron nitride corrosion-resistant layer. In this way, adding the iron nitride corrosion-resistant layer to the cookware can ensure the corrosion resistance of the cookware, avoid the cookware from delaminating due to poor corrosion resistance, and thus to a certain extent extend the long-lasting non-stick life of the cookware.
[0095] As an example, the spraying method for forming the iron nitride corrosion-resistant layer is plasma spraying, and the specific parameters of plasma spraying include: current of 550A-650A; voltage of 60V-90V: main gas (argon) flow rate of 2000L / h-2500L / h; hydrogen flow rate of 100L / h-150L / h: powder feeding gas flow rate of 600L / h-800L / h: powder feeding rate of 10g / min-20g / min; spraying (distance from gun nozzle to workpiece) distance of 10cm-12cm; spraying angle of 45°-80°. After spraying, an iron nitride corrosion-resistant layer with a thickness of 30 microns to 60 microns can be formed, which can achieve the purpose of a corrosion-resistant layer with controllable thickness.
[0096] Forming non-stick material
[0097] According to the present application, the non-stick material includes a solid solution and a single substance, wherein the solid solution is a solid solution of iron and a non-metallic single substance, the non-metallic single substance includes one or more of boron, carbon, silicon and selenium, and the single substance is a single substance corresponding to the non-metallic single substance, wherein the single substance is on the surface of the solid solution. Correspondingly, the step of forming the non-stick material includes ion implantation of iron using a non-metallic single substance, so that the non-metallic single substance is at least doped into the iron lattice, thereby forming a non-stick material having an amorphous phase and including a solid solution and a single substance that does not form a solid solution but is attached to the surface of the solid solution, wherein the solid solution is a solid solution of iron and a non-metallic single substance, the non-metallic single substance includes one or more of boron, carbon, silicon and selenium, and the single substance is the same as the non-metallic single substance.
[0098] In these embodiments, the solid solution has low surface energy and high hardness, and the single substance has high hardness and a certain lipophilicity. The synergistic effect of the solid solution and the single substance can make the non-stick material have excellent non-stick properties and wear resistance, so that the coating of the non-stick cookware formed by the non-stick material has both excellent initial non-stick properties and long-lasting non-stick properties.
[0099] In some embodiments, the non-stick material is a material in which the volume proportion of the amorphous phase is in the range of 67%-75%. In this way, a non-stick layer with corresponding amorphous properties can be formed, so that the non-stick layer exhibits excellent performance in terms of non-stickiness, stability, hardness and wear resistance.
[0100] According to the present application, the dose of ion implantation and the temperature of the iron powder during the ion implantation are controlled, so that a non-stick material having a solid solution and a single substance or a non-stick material having a solid solution, a single substance and an iron-containing compound can be formed.
[0101] According to the present application, during the ion implantation process, the non-metallic ions to be implanted are in a high-speed and high-energy state, impacting the iron surface, entering the iron crystal lattice, colliding with iron atoms, causing the iron atoms to shift, and the displaced atoms may also transfer energy to other atoms, resulting in a series of vacancy-interstitial atom pairs and other types of lattice disordered distribution. This phenomenon is called lattice damage. Due to the influx of too many "atoms" in a short period of time, the interior of the iron crystal is actually very messy, making the material amorphous.
[0102] In the following, two embodiments will be described in more detail.
[0103] According to the first embodiment of the present application, the non-stick layer is a mixed layer of solid solution particles and elemental particles. Correspondingly, the non-stick material has a shell structure, including a solid solution 201 and an elemental substance 202 attached to the surface of the solid solution 201. Accordingly, the method for preparing the non-stick material includes: placing iron in an ion implanter, and at a certain temperature, implanting one or more elemental elements (such as boron, carbon, silicon and selenium) at a density of 2.5×10 18 -3.0×10 19 ions are implanted into iron to form a non-stick material containing solid solution particles and elemental particles. Specifically, 300-500 mesh iron powder is placed in an ion implanter, and one or more elemental elements (such as boron, carbon, silicon and selenium) are implanted at a density of 2.5×10 per square centimeter of iron. 18 -3.0×10 19 The ion implantation dose of each ion is injected into the iron, vacuumed to 5Pa-10Pa, and then ion implantation is performed at 200℃-300℃, and finally cooled to room temperature with the furnace to obtain a non-stick material. Among them, the non-stick material is composed of a solid solution and a single substance, and the single substance is on the surface of the solid solution. As for the proportion of each component in the mixture, as an example, the weight of the solid solution accounts for 70%-90% of the total weight of the non-stick material, and the balance is the single substance, that is, the weight of the single substance accounts for 10%-30% of the total weight of the non-stick material.
[0104] In these embodiments, iron powder of 300-500 mesh is selected to ensure the uniformity and a certain surface area of the iron powder, which is beneficial to the sufficiency and uniformity of ion implantation. Vacuuming to 5Pa-10Pa can reduce the occurrence of oxidation reaction and facilitate the diffusion of the injected ions. In an environment of 200°C-300°C, a non-stick material having a solid solution and a single substance is formed. In addition, the presence of a solid solution in a non-stick material can significantly affect the properties of the material, including bonding force, surface energy and wear resistance. The presence of a single substance can provide additional lipophilicity, hardness or chemical stability, etc., so that the mixed layer formed by the non-stick material containing solid solution particles and single substance particles has a lower surface energy and can have excellent initial non-stickiness, long-lasting non-stickiness, durability and stability.
[0105] According to the second embodiment of the present application, the non-stick layer is a mixed layer of solid solution particles, elemental particles and iron-containing compounds. Correspondingly, the non-stick material includes a solid solution, an elemental substance and an iron-containing compound, wherein the iron-containing compound is an iron-containing compound formed by iron and a corresponding non-metallic elemental substance, the elemental substance is attached to the surface of the solid solution, and the iron-containing compound is dispersed inside the solid solution. Correspondingly, the method for preparing the non-stick material includes: in the step of forming the non-stick material, by increasing the dose of ion implantation and the temperature of ion implantation, the solid solution in the first embodiment can be quickly approached to saturation, so that the saturated solid solution can precipitate to obtain an iron-containing compound, thereby forming a non-stick material including a solid solution, an elemental substance and an iron-containing compound. In some embodiments, iron powder is placed in an ion implanter, and at a certain temperature, one or more elemental elements (such as boron, carbon, silicon and selenium) are implanted at a density of 3.0×10 18 -3.8×10 19 The ion implantation dose of ions is implanted into the iron powder to form a non-stick material containing a solid solution and a single substance. Specifically, 300-500 mesh iron powder is placed in an ion implanter, and one or more single elements (such as boron, carbon, silicon and selenium) are implanted at a density of 3.0×10 per square centimeter of iron. 18 -3.8×10 19The ion implantation dose of each ion is injected into the iron powder, vacuumed to 5Pa-10Pa, and then ion implantation is performed at 400℃-600℃, and finally cooled to room temperature with the furnace, thereby obtaining a non-stick material including a solid solution, an iron-containing compound and a single substance. Among them, the single substance is on the surface of the solid solution, and the iron-containing compound is dispersed in the solid solution. For the proportion of each component in the non-stick material, as an example, the weight of the solid solution accounts for 72%-82% of the total weight of the non-stick material, the weight of the iron-containing compound accounts for 10%-20% of the total weight of the non-stick material, and the weight of the single substance accounts for 2%-12% of the total weight of the non-stick material. The sum of the weight proportions of the solid solution, the single substance and the iron-containing compound is 100%. It should be noted that here, the solid solution is a saturated solid solution of iron and the corresponding non-metallic single substance. The saturated solid solution of iron and the corresponding non-metallic single substance indicates that the solubility of the non-metallic single substance in iron has reached the limit, and the iron-containing compound is the above-mentioned compound precipitated and generated from the saturated solid solution of iron and the corresponding non-metallic single substance.
[0106] In these embodiments, iron-containing compounds are also dispersed in the non-stick material as a wear-resistant phase, which can further improve the wear resistance of the non-stick material, ensure the wear resistance of the non-stick layer, and thus improve the long-lasting non-stick property.
[0107] In these embodiments, during the process of preparing the non-stick material, various iron-containing compound phases are formed, for example, various carbide phases (Fe5C2, Fe7C3, Fe 2.2 C and Fe3C, etc.), various boride phases (Fe2B and FeB), various silicide phases (Fe2Si, Fe5Si3, FeSi, FeSi2), and various selenide phases (Fe3Se4, FeSe, FeSe2). These phases are all composed of iron phases with different chemical combinations, which makes the non-stick material amorphous. In addition, the color of the non-stick material is black or gray-black, and the non-stick layer formed by it also presents the corresponding color. In this case, it can avoid affecting the user experience due to dirt.
[0108] Figure 4 is a schematic structural diagram of a non-stick material provided according to an embodiment of the present application, Figure 5 Schematic diagram of another non-stick material provided according to an embodiment of the present application. Figure 4 As shown, the non-stick material is composed of a solid solution 201 and a single substance 202, and the single substance 202 is distributed on the surface of the solid solution 201. Figure 5 As shown, the non-stick material includes a solid solution 201 , an iron-containing compound 203 and a simple substance 202 , wherein the simple substance 202 is distributed on the surface of the solid solution 201 , and the iron-containing compound 203 is dispersed in the solid solution 201 .
[0109] Forming a non-stick layer
[0110] According to the present application, the non-stick layer is formed by spraying a non-stick material on the iron nitride corrosion-resistant layer or the cookware substrate. As an example, the method of spraying the non-stick material is plasma spraying. The specific parameters of the plasma spraying method include a current of 450A-550A, a voltage of 50V-70V, a main gas (argon) flow rate of 1000L / h-1200L / h, a hydrogen flow rate of 150L / h-200L / h, a powder feeding gas flow rate of 400L / h-600L / h, a powder feeding amount of 20g / min-30g / min, a spraying distance (distance between the gun nozzle and the workpiece) of 10cm-12cm, and a spraying angle of 45°-80°.
[0111] According to the present application, controlling the spraying process can enable the non-stick layer to retain the properties of the non-stick material, for example, amorphousness. As an example, controlling the spraying process includes certain interventions in the process of forming the non-stick layer. Specifically, the cookware substrate includes a first surface and a second surface opposite to each other. Controlling the spraying process includes: cooling the second surface of the substrate, spraying a non-stick material on the first surface of the substrate, thereby forming a non-stick layer with an amorphous structure on the first surface of the substrate. It should be noted that the first surface here can be an inner surface, and the second surface can be an outer surface. Of course, the present application does not make too many restrictions on this. It can be understood that those skilled in the art can, under the guidance of the present application, according to actual use requirements, the first surface can be an outer surface and the second surface can be an inner surface.
[0112] In an exemplary embodiment, cooling the second surface of the substrate includes placing the second surface of the substrate in an environment of cooling gas, wherein the cooling gas temperature is -5°C to 0°C and the flow rate is 2500L / h to 3500L / h.
[0113] Under the action of the above spraying parameters, the non-stick layer retains the properties of the non-stick material, such as amorphous, solid solution, single substance, etc. In addition, in the process of forming the non-stick layer, part of the solid solution can decompose to form more single substances, thereby further improving the lipophilicity of the non-stick layer. As an example, the solid solution includes a solid solution of iron and boron, a solid solution of iron and carbon, a solid solution of iron and silicon, and a solid solution of iron and selenium, etc. In the process of forming the non-stick layer, part of the solid solution can decompose to form more single substances, such as boron, carbon, silicon and selenium, thereby further improving the lipophilicity of the non-stick layer. It should be noted that the solid solution according to the present application can also be a solid solution of a plurality of non-metallic single substances. In the case of a solid solution of a plurality of amorphous single substances, it can be obtained by corresponding ion implantation into iron.
[0114] In some embodiments, the formed non-stick layer includes iron carbide particles having iron phases with different carburization degrees. For example, x-Fe5C2, θ-Fe3C, ε-Fe2C, ε'-Fe 2.2C and Fe7C3. The different phase compositions represent the presence of more cavities and distortions inside the crystals, which makes the non-stick layer more amorphous, thus further optimizing the long-lasting non-stick properties of the cookware.
[0115] Modification of the non-stick layer
[0116] According to the present application, the method for manufacturing the cookware further includes the step of modifying the surface of the non-stick layer after the non-stick layer is formed. By modifying the non-stick layer, the non-stick layer has a good non-stick effect even in an oil-free or oil-less environment in its initial state, thereby improving the user experience.
[0117] In some embodiments, modifying the surface of the non-stick layer includes hydroxylating the non-stick layer, immersing the hydroxylated non-stick layer in a fatty acid solution to connect fatty acid anhydride groups to the non-stick layer, and finally, coating unsaturated fatty acid glyceride to react with the fatty acid anhydride groups to form an oil film layer.
[0118] Specifically, modifying the surface of the non-stick layer comprises the following steps:
[0119] S200, hydroxylation treatment.
[0120] Specifically, the hydroxylation treatment of the non-stick layer includes placing the cookware with the non-stick layer in a modification solution to hydroxylate the non-stick layer. As an example, the non-stick layer is soaked in the modification solution for 3min-10min to remove organic and inorganic impurities on the surface and form hydroxyl (-OH) groups on the surface. Subsequently, rinse with clean water to remove the residual modification solution for standby use. Among them, the modification solution is a mixed solution formed by mixing 98% concentrated sulfuric acid and 30% hydrogen peroxide in a volume ratio of 3:1.
[0121] S201, fatty acid grafting.
[0122] The non-stick layer after hydroxylation is immersed in a fatty acid solution. Wherein, the fatty acid molecule contains a long hydrocarbon chain and a carboxyl group (-COOH). In a preferred embodiment, the selected fatty acid is an unsaturated fatty acid, and further, a polyunsaturated fatty acid. As above, the fatty acid contains multiple double bonds, which makes them more likely to react with hydroxyl groups and form a more complex cross-linked structure on the surface.
[0123] Specifically, the non-stick layer after hydroxylation treatment is immersed in a fatty acid solution for 5-10 minutes. During this process, the fatty acid reacts with the hydroxyl groups on the surface of the non-stick layer to form fatty acid anhydride groups, thereby grafting a layer of fatty acid anhydride on the surface of the iron carbide. Then, rinse with clean water to remove unreacted fatty acids and other impurities for standby use.
[0124] According to the present application, the non-stick layer comprises iron carbide particles, elemental carbon and iron dispersed in the iron carbide particles, and fatty acid anhydride groups are mainly grafted on the iron carbide particles.
[0125] S202, unsaturated fatty acid glyceride coating.
[0126] Specifically, a layer of unsaturated fatty acid glyceride (i.e., edible oil) is coated on the non-stick layer grafted with fatty acid anhydride. In a preferred embodiment, the unsaturated fatty acid glyceride is a polyunsaturated fatty acid glyceride, such as linseed oil, sunflower seed oil, etc. These unsaturated fatty acid glycerides contain more double bonds, which is conducive to subsequent cross-linking and curing.
[0127] S203, drying process.
[0128] Specifically, the non-stick layer coated with unsaturated fatty acid glyceride is placed in an environment of 150° C. to 300° C. for drying. At this temperature, the double bonds in the glyceride will rapidly undergo a cross-linking reaction to form a stable polymer network structure.
[0129] In these embodiments, through the above steps, a stable oil film layer can be formed on the surface of the non-stick layer to further improve the non-stick performance of the cookware.
[0130] In some embodiments, the thickness of the oil film layer is between 1 micrometer and 3 micrometers.
[0131] The method for manufacturing a cooker and the cooker of the present invention are described in detail above in combination with exemplary embodiments. In the following, the beneficial effects of the present invention will be described in more detail in combination with specific embodiments, but the protection scope of the present invention is not limited to the embodiments.
[0132] Example 1
[0133] The cookware according to Example 1 was manufactured by the following method.
[0134] Step S10, providing a cookware base made of low carbon steel with a thickness of 1.2 mm.
[0135] Step S20, placing the outer surface of the cookware base in a circulating cooling air gas environment, wherein the temperature of the cooling gas is -5°C. Loading a non-stick material of 300-500 mesh into a powder feeder, wherein the non-stick material is a material in which the volume of the amorphous phase accounts for 70%, and the non-stick material is a solid solution and carbon, wherein the carbon is attached to the surface of the solid solution, and the solid solution is a solid solution of iron and carbon. Wherein, based on the total weight of the non-stick material being 100%, the weight of the solid solution of iron and carbon accounts for 85% of the total weight of the non-stick material, and the weight of carbon accounts for 15% of the total weight of the non-stick material. Then, the spraying parameters of plasma spraying are set as follows: current is 500A, voltage is 60V, main gas (argon) flow rate is 1100L / h, hydrogen flow rate is 180L / h, powder feeding gas flow rate is 500L / h, powder feeding amount is 25g / min, spraying (distance between gun nozzle and workpiece) distance is 11cm, spraying angle is 60°, and non-stick material is formed on the inner surface of the pot substrate by plasma spraying to obtain a non-stick layer with a thickness of 50μm, thereby completing the manufacture of the pot of Example 1. Among them, the non-stick layer is a mixed layer of solid solution particles of iron and carbon and carbon particles, and the weight of the solid solution particles of iron and carbon accounts for 80% of the total weight of the non-stick layer, and the weight of the carbon particles accounts for 20% of the total weight of the non-stick layer, based on the weight percentage of 100%.
[0136] Example 2
[0137] The cookware of Example 2 is manufactured by the same method as Example 1, except that in step S20, the thickness of the non-stick layer is set to 80 μm.
[0138] Example 3
[0139] The cookware of Example 3 was manufactured by the same method as Example 1, except that in step S20, the thickness of the non-stick layer was set to 40 μm.
[0140] Example 4
[0141] The cookware of Example 4 is manufactured by the same method as Example 1, except that in the non-stick layer, the weight of the solid solution particles of iron and carbon accounts for 87% of the total weight of the non-stick layer, and the weight of the carbon particles accounts for 13% of the total weight of the non-stick layer, based on the weight percentage of 100% (the corresponding method adjusts the temperature and the dose of ion implantation to form a non-stick material composed of solid solution and carbon).
[0142] Example 5
[0143] The cookware of Example 5 is manufactured by the same method as Example 1, except that in the non-stick layer, the weight of the solid solution particles of iron and carbon accounts for 67% of the total weight of the non-stick layer, and the weight of the carbon particles accounts for 33% of the total weight of the non-stick layer, based on the weight percentage of 100% (the corresponding method adjusts the temperature and the dose of ion implantation to form a non-stick material composed of solid solution and carbon).
[0144] Example 6
[0145] In addition to adding step S30 between steps S10 and S20, using iron nitride particles to form an iron nitride corrosion-resistant layer on the cookware substrate by plasma spraying (in this embodiment, the outer surface of the cookware substrate is placed in a circulating cooling air gas environment, wherein the temperature of the cooling gas is -5°C. 500-800 mesh iron nitride is loaded into the powder feeder, and the spraying parameters of the plasma spraying are set as follows: the current is 500A, the voltage is 80V, and the main gas (argon) flow rate is 2200L / h; hydrogen flow rate is 140L / h: powder feeding gas flow rate is 500L / h: powder feeding amount is 25g / min; spraying (distance from gun nozzle to workpiece) distance is 11cm; spraying angle is 60°, iron nitride particles are formed on the inner surface of the cookware substrate by plasma spraying to obtain an iron nitride corrosion-resistant layer with a thickness of 40μm, and then, a non-stick layer of Example 1 is formed on the surface of the iron nitride corrosion-resistant layer), and the cookware of Example 6 is manufactured by the same method as Example 1.
[0146] Example 7
[0147] The cookware of Example 7 is manufactured by the same method as Example 6, except that in step S30, the thickness of the iron nitride corrosion-resistant layer is set to 60 μm.
[0148] Example 8
[0149] The cookware of Example 8 is manufactured by the same method as Example 6, except that in step S30, the thickness of the iron nitride corrosion-resistant layer is set to 30 μm.
[0150] Example 9
[0151] The cookware of Example 9 is manufactured by the same method as Example 1, except that in step S10, a different material is used to form the cookware base (the material of this embodiment is a stainless steel base material).
[0152] Example 10
[0153] The cookware of Example 10 is manufactured by the same method as Example 1, except that in step S10, a different material is used to form the cookware base (the material of this embodiment is an aluminum substrate).
[0154] Embodiment 11
[0155] The cookware of Example 11 is manufactured by the same method as Example 1, except that in step S20, non-stick materials with different particle sizes are used to form the non-stick layer (the particle size of the non-stick material in this embodiment is 400 mesh-500 mesh).
[0156] Example 12
[0157] The cookware of Example 12 is manufactured by the same method as Example 1, except that in step S20, non-stick materials with different particle sizes are used to form the non-stick layer (the particle size of the non-stick material in this embodiment is 300 mesh-400 mesh).
[0158] Embodiment 13
[0159] In addition to using different non-stick materials to form the non-stick layer in step S20 (the non-stick materials in this embodiment are solid solution, carbon and iron carbide, wherein the solid solution is a solid solution of iron and carbon, wherein, based on the total weight of the non-stick material as 100%, the weight of the solid solution of iron and carbon accounts for 75% of the total weight of the non-stick material, the weight of carbon accounts for 10% of the total weight of the non-stick material, and the remainder is iron carbide. Correspondingly, the formed non-stick layer is a mixed layer of solid solution particles, carbon particles and iron carbide, wherein the carbon particles are elemental particles, and iron carbide is an iron-containing compound, the weight of the solid solution particles accounts for 73% of the total weight of the non-stick layer, the weight of the elemental particles accounts for 12% of the total weight of the non-stick layer, and the remainder is an iron-containing compound), the cookware of Example 13 is manufactured using the same method as Example 1.
[0160] Embodiment 14
[0161] In addition to using different non-stick materials to form the non-stick layer in step S20 (the non-stick material is a solid solution and boron, wherein the solid solution is a solid solution of iron and boron, wherein, based on the total weight of the non-stick material being 100%, the weight of the solid solution of iron and boron accounts for 85% of the total weight of the non-stick material, and the weight of boron accounts for 15% of the total weight of the non-stick material. Correspondingly, the formed non-stick layer is a mixed layer of solid solution particles and boron particles, wherein the boron particles are single particles, the weight of the solid solution particles accounts for 80% of the total weight of the non-stick layer, and the weight of the single particles accounts for 20% of the total weight of the non-stick layer), the cookware of Example 14 is manufactured using the same method as Example 1.
[0162] Embodiment 15
[0163] Except that in step S20, different non-stick materials are used to form the non-stick layer (the non-stick material is a solid solution, boron and iron boride, wherein the solid solution is a solid solution of iron and boron, wherein, based on the total weight of the non-stick material being 100%, the weight of the solid solution of iron and boron accounts for 75% of the total weight of the non-stick material, the weight of boron accounts for 10% of the total weight of the non-stick material, and the remainder is iron boride. Correspondingly, the formed non-stick layer is a mixed layer of solid solution particles, carbon particles and iron boride, wherein the carbon particles are elemental particles, the iron boride is an iron-containing compound, the weight of the solid solution particles accounts for 73% of the total weight of the non-stick layer, the weight of the elemental particles accounts for 12% of the total weight of the non-stick layer, and the remainder is iron-containing compounds), the cookware of Example 15 is manufactured using the same method as Example 1.
[0164] Example 16
[0165] In addition to using different non-stick materials to form the non-stick layer in step S20 (the non-stick material is a solid solution and silicon, wherein the solid solution is a solid solution of iron and silicon, wherein, based on the total weight of the non-stick material being 100%, the weight of the solid solution of iron and silicon accounts for 85% of the total weight of the non-stick material, and the weight of silicon accounts for 15% of the total weight of the non-stick material. Correspondingly, the formed non-stick layer is a mixed layer of solid solution particles and silicon particles, wherein the silicon particles are single particles, the weight of the solid solution particles accounts for 80% of the total weight of the non-stick layer, and the weight of the single particles accounts for 20% of the total weight of the non-stick layer), the cookware of Example 16 is manufactured using the same method as Example 1.
[0166] Embodiment 17
[0167] In addition to using different non-stick materials to form the non-stick layer in step S20 (the non-stick materials are solid solution, silicon and iron silicide, wherein the solid solution is a solid solution of iron and silicon, wherein, based on the total weight of the non-stick material being 100%, the weight of the solid solution of iron and silicon accounts for 75% of the total weight of the non-stick material, the weight of silicon accounts for 10% of the total weight of the non-stick material, and the remainder is iron silicide. Correspondingly, the formed non-stick layer is a mixed layer of solid solution particles, silicon particles and iron silicide, wherein the silicon particles are elemental particles, the iron silicide is an iron-containing compound, the weight of the solid solution particles accounts for 73% of the total weight of the non-stick layer, the weight of the elemental particles accounts for 12% of the total weight of the non-stick layer, and the remainder is iron-containing compounds), the cookware of Example 17 is manufactured using the same method as Example 1.
[0168] Embodiment 18
[0169] Except that in step S20, different non-stick materials are used to form the non-stick layer (the non-stick material is a solid solution and selenium, wherein the solid solution is a solid solution of iron and selenium, wherein, based on the total weight of the non-stick material being 100%, the weight of the solid solution of iron and selenium accounts for 85% of the total weight of the non-stick material, and the weight of selenium accounts for 15% of the total weight of the non-stick material. Correspondingly, the formed non-stick layer is a mixed layer of solid solution particles and selenium particles, wherein the selenium particles are single particles, the weight of the solid solution particles accounts for 80% of the total weight of the non-stick layer, and the weight of the single particles accounts for 20% of the total weight of the non-stick layer), the cookware of Example 18 is manufactured using the same method as Example 1.
[0170] Embodiment 19
[0171] Except that in step S20, different non-stick materials are used to form the non-stick layer (the non-stick materials are solid solution, selenium and iron selenide, wherein the solid solution is a solid solution of iron and selenium, wherein, based on the total weight of the non-stick material being 100%, the weight of the solid solution of iron and selenium accounts for 75% of the total weight of the non-stick material, the weight of selenium accounts for 10% of the total weight of the non-stick material, and the remainder is iron selenide. Correspondingly, the formed non-stick layer is a mixed layer of solid solution particles, selenium particles and iron selenide, wherein the selenium particles are elemental particles, and the iron selenide is an iron-containing compound, the weight of the solid solution particles accounts for 73% of the total weight of the non-stick layer, the weight of the elemental particles accounts for 12% of the total weight of the non-stick layer, and the remainder is an iron-containing compound), the cookware of Example 19 is manufactured by the same method as Example 1.
[0172] Embodiment 20
[0173] The cookware of Example 20 was manufactured in the same manner as in Example 1, except that after step S30, a 2-micron oil film layer was provided on the non-stick layer.
[0174] Comparative Example 1
[0175] The cookware of Comparative Example 1 was manufactured in the same manner as in Example 1, except that in step S20, the non-stick layer was formed by a different material (the non-stick material of Example 1 was replaced by commercially available 300-500 mesh iron carbide). The iron carbide layer was obtained in this comparative example.
[0176] Comparative Example 2
[0177] The cookware of Comparative Example 2 was manufactured in the same manner as in Example 1, except that in step S20, the non-stick layer was formed by a different material (the non-stick material of Example 1 was replaced by commercially available 300-500 mesh iron boride). The iron boride layer was obtained in this comparative example.
[0178] Comparative Example 3
[0179] The cookware of Comparative Example 3 was manufactured in the same manner as in Example 1, except that in step S20, the non-stick layer was formed by a different material (the non-stick material of Example 1 was replaced by commercially available 300-500 mesh iron silicide). The iron silicide layer was obtained in this comparative example.
[0180] Comparative Example 4
[0181] The cookware of Comparative Example 4 was manufactured in the same manner as in Example 1, except that in step S20, the non-stick layer was formed by a different material (the non-stick material of Example 1 was replaced by commercially available 300-500 mesh iron selenide). The iron selenide layer was obtained in this comparative example.
[0182] Comparative Example 5
[0183] The cookware of Comparative Example 5 was manufactured in the same manner as in Example 1, except that a non-stick layer was formed by a different material in step S20 (a commercially available multi-component alloy solid solution of (Ti, W, Nb, Al) (Cx, Ny) with a mesh size of 300-500 was used to replace the non-stick material of Example 1). The cookware of Comparative Example 5 was manufactured in the same manner as in Example 1. The cookware obtained in this Comparative Example was a multi-component alloy solid solution layer.
[0184] Performance index test
[0185] The performance of the cookware of Examples 1-20 and Comparative Examples 1-5 was tested using the following test methods, and the results are recorded in Table 1 below.
[0186] The corrosion resistance, initial non-stickiness and long-lasting non-stickiness of the cookware prepared in the examples and comparative examples were tested.
[0187] (1) Corrosion resistance
[0188] Refer to the corrosion resistance test method 6.17 in GBT 32432-2015 Household Steel Cookware, mix 95% by weight of distilled water and 5% by weight of analytical grade sodium chloride. During the boiling process, distilled water needs to be continuously added to a constant water surface to ensure that the concentration in the solution remains unchanged. Boil it in a pot and keep it slightly boiling. Record the time when rust appears in the pot. According to the project requirements, the corrosion resistance should not be less than 1h. If it is less than 1h, it is unqualified.
[0189] (2) Initial non-stick test method
[0190] Initial non-stickiness test method: GB / T32095.2-2015 fried egg non-stickiness test method. This method is an initial non-stickiness test, which is divided into levels Ⅰ, Ⅱ, and Ⅲ. Level Ⅰ has the best non-stickiness and level Ⅲ has the worst non-stickiness.
[0191] (3) Test method for long-lasting non-stick properties
[0192] Long-lasting non-stick test method: Long-lasting non-stick test method in GB / T32388-2015, the unit is the number of times, the higher the number, the longer the life, the non-stick result is evaluated once every 500 times, and the number of times when it is used to level III is recorded.
[0193] (4) Adhesion test method
[0194] The test was carried out according to the method specified in G / T8642-2002 to determine the bonding strength (i.e., bonding force) of the samples. Here, the samples refer to the coatings of the embodiments and comparative examples.
[0195] For the bonding strength of the thermal spray coating, according to the project expectations, the final measured value should not be less than 10MPa. If it is less than 10MPa, the thermal spray coating is prone to fall off or even collapse.
[0196] Table 1 Performance index test data of the embodiments of the present application and the comparative examples
[0197]
[0198]
[0199] In summary, according to the cookware of the embodiments of the present application, it can be seen from the comparison of Embodiment 1, Embodiment 4 and Embodiment 5 that the higher the carbon content, the better the non-stickiness. It can be understood that the single substance according to the present application can greatly affect the lasting non-stickiness.
[0200] From the comparison between Example 1 and Example 13, it can be seen that the added compound can affect the lasting non-stickiness.
[0201] From the comparison among Example 6, Example 7 and Example 8, it can be seen that the thickness of the iron nitride corrosion-resistant layer is within the scope of the present application, and improved corrosion resistance can be obtained.
[0202] Although the embodiments of the present application have been described in detail above, those skilled in the art may make various modifications and variations to the embodiments of the present application without departing from the spirit and scope of the present application. However, it should be understood that, in the opinion of those skilled in the art, these modifications and variations will still fall within the spirit and scope of the embodiments of the present application defined by the claims.
Claims
1. A cooking utensil, characterized in that: The cooker comprises: Cooker body; An iron nitride corrosion-resistant layer is formed on the cooker body by spraying; A non-stick layer is formed on the iron nitride corrosion-resistant layer, wherein the non-stick layer has an amorphous structure and is a mixed layer including solid solution particles and elemental particles, wherein the solid solution particles are solid solution particles formed by iron and a non-metallic elemental substance, the non-metallic elemental substance includes one or more of boron, carbon, silicon and selenium, and the elemental particles are the same as the non-metallic elemental substance.
2. The cooker according to claim 1, characterized in that: Taking the total weight of the non-stick layer as 100%, the weight of the single substance particles accounts for 13%-33% of the total weight of the non-stick layer, and the remainder is solid solution particles.
3. The cooker according to claim 1, characterized in that: The mixed layer also contains dispersed iron-containing compounds, which are formed by iron and corresponding non-metallic elements.
4. The cooker according to claim 3, characterized in that: The iron-containing compound is x-Fe5C2, θ-Fe3C, ε-Fe2C, ε'-Fe 2.2 One or more of C, Fe7C3, Fe2B, FeB, Fe2Si, Fe5Si3, FeSi, FeSi2, Fe3Se4, FeSe, and FeSe2.
5. The cooker according to claim 3, characterized in that: Taking the total weight of the non-stick layer as 100%, the weight of the solid solution particles accounts for 70%-80% of the total weight of the non-stick layer, the weight of the elemental particles accounts for 5%-15% of the total weight of the non-stick layer, and the remainder is iron-containing compounds.
6. The cooker according to claim 1, characterized in that: The non-stick layer has a pore structure capable of storing oil; and / or the surface of the non-stick layer has a rough structure; and / or the volume proportion of the amorphous phase of the amorphous structure is 67%-75%.
7. The cooker according to claim 1, characterized in that: The iron nitride corrosion-resistant layer comprises iron nitride particles and flake graphite filled in gaps between the iron nitride particles.
8. The cooker according to claim 1, characterized in that: The iron nitride corrosion-resistant layer is formed by granulated iron nitride powder, which is obtained by drying, briquetting and crushing a mixed slurry including iron nitride particles, flake graphite and a binder.
9. The cooker according to claim 8, characterized in that: The particle size of the iron nitride particles is 800 mesh-1200 mesh; and / or in the mixed slurry, the weight ratio of the iron nitride particles, flake graphite and adhesive is (70-85):(3-8):(5-12) respectively.
10. The cooker according to claim 1, characterized in that: The thickness of the iron nitride corrosion resistant layer is 30 microns to 60 microns; and / or the thickness of the non-stick layer is 40 microns to 80 microns; and / or the porosity of the iron nitride corrosion resistant layer is 0.5% to 2%, and the pore size is 0.5 microns to 1 micron.
11. The cooker according to any one of claims 1 to 10, characterized in that: An oil film layer formed by the combination of fatty acid anhydride groups and unsaturated fatty acid glycerides is arranged on the surface of the non-stick layer.
12. A method for manufacturing a cooker, characterized in that: The method comprises: providing a cookware base; forming a non-stick layer on the cookware substrate by thermally spraying a non-stick material; Among them, the non-stick material has an amorphous phase, and the non-stick material includes a solid solution and a single substance attached to the surface of the solid solution. The solid solution is a solid solution of iron and a non-metallic single substance. The non-metallic single substance includes one or more of boron, carbon, silicon and selenium, and the single substance is the same as the non-metallic single substance.
13. The method according to claim 12, characterized in that The non-stick material is formed by the following steps: ion implantation of a single element into iron is performed, so that the single element is at least doped into the iron lattice, thereby forming a non-stick material having an amorphous phase and including the solid solution and the single element.
14. The method according to claim 13, characterized in that The ion implantation temperature is 200°C-300°C, and the ion implantation dose of the element per square centimeter of iron is 2.5×10 18 -3.0×10 19 ions, In the step of forming the non-stick material, the non-stick material including the solid solution, the simple substance and the iron-containing compound is formed by increasing the dose of ion implantation and the temperature of ion implantation.
15. The method according to claim 12, characterized in that The method further comprises: before forming the non-stick layer, firstly using an iron nitride material to form an iron nitride corrosion-resistant layer on the cookware substrate by spraying, and then forming the non-stick layer on the surface of the iron nitride corrosion-resistant layer.
16. The method according to claim 12, characterized in that The method further comprises: after forming the non-stick layer, performing a hydroxylation treatment on the non-stick layer, immersing the hydroxylated non-stick layer in a fatty acid solution to connect fatty acid anhydride groups on the non-stick layer, and finally, coating unsaturated fatty acid glyceride to react with the fatty acid anhydride groups to form an oil film layer.
17. The method according to claim 15, characterized in that The particle size of the non-stick material is 300-500 mesh; and / or the particle size of the iron nitride material is 500-800 mesh.