Antibacterial filter material, antibacterial filter composition, preparation method of antibacterial filter material and antibacterial filter composition, and application of antibacterial filter material and antibacterial filter composition in preparation of filter element

Through the combination of Cu-Ag bimetallic inorganic nanomaterial and honey slurry, antibacterial filter materials with oxygen-containing vacancies and Ti3+ active sites are formed, which solves the problem of low antibacterial material efficiency of existing filter elements in extreme environments, and achieves high efficiency. Long-lasting antibacterial and antivirus effects and reduce Ag dosage.

CN119075501APending Publication Date: 2024-12-06DONGGUAN AIR GUARD FILTER MANUFACTURING CO LTD

Patent Information

Application Number
CN202411174612.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing filter element has low sterilization efficiency, poor heat resistance, and complex extraction and purification process in extreme environments. Ag+ materials cannot maintain high levels for a long time. The Ag dosage is high and uneconomical, and organic antibacterial agents are highly toxic. TiO2 requires ultraviolet light. Only by activation can it be sterilized.

Method used

The Cu-Ag bimetallic inorganic nanomaterials are combined with honey slurry to prepare antibacterial filter materials, containing oxygen vacancies and Ti3+ active sites, and titanium dioxide supported by Cu nanoparticles and Ag nanoparticles are formed through heat treatment and specific gas treatment, combining with natural fibers The vine and honey slurry serve as a binder to form an antibacterial filtration composition.

Benefits of technology

Under natural conditions, no UV lamp activation is required, and it continues to effectively inhibit bacteria and virus, maintains high efficiency for more than one year, reduces Ag usage, improves antibacterial and filtration performance, and is suitable for a variety of bacteria and viruses.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005010370820000121
    Figure BDA0005010370820000121
  • Figure BDA0005010370820000131
    Figure BDA0005010370820000131
  • Figure BDA0005010370820000132
    Figure BDA0005010370820000132
Patent Text Reader

Abstract

The invention discloses an antibacterial filtering material, an antibacterial filtering composition, a preparation method of the antibacterial filtering composition and application of the antibacterial filtering composition in preparation of a filter element, and belongs to the technical field of filter elements, the antibacterial filtering material is titanium dioxide loaded with Cu nano particles and Ag nano particles, and the antibacterial filtering material contains oxygen vacancies and Ti < 3 + > active sites. The antibacterial filtering material contains oxygen vacancies and Ti < 3 + > active sites and is loaded with Cu nano particles and Ag nano particles, the oxygen vacancies and bimetals have a coordination effect, and the existence of the oxygen vacancies can effectively and continuously activate water molecules and oxygen molecules to generate free radicals and active oxygen species, so that the antibacterial filtering material has a good antibacterial effect. The Cu nano particles and the Ag nano particles are beneficial to electron transfer to activate oxygen molecules to generate active oxygen species besides self-coordination sterilization and disinfection effects. Therefore, under the actual application condition, efficient bacteriostasis and disinfection effects can be continuously achieved through in-situ generation, and excellent antibacterial effect and filtering effect are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of filter elements, and in particular to an antibacterial filtering material, an antibacterial filtering composition, a preparation method thereof, and an application thereof in preparing a filter element. Background Art

[0002] Existing filter elements generally use the following technologies for antibacterial and filtration: ① Silver ions or copper ions (Ag + , Cu 2+ ) as the representative of the inorganic material antibacterial technology with loaded type (such as porous molecular sieve), the representative products and technologies are Agion's Ag + or Cu 2+ The zeolite material slurry solution and Purafil Ag + / Cu 2+ ① Coated fiber composite filter material; ② Natural plant extract biological antibacterial technology represented by essential oils, the representative product is the non-woven filter element impregnated with citric acid plant extract from Freudenberg filtration; ③ Organic compound technology represented by organic amines and chlorine oxides; ④ Mechanical filtration technology represented by HEPA filter material; ⑤ Ultraviolet light (UV) sterilization technology.

[0003] In actual application environments, where temperature and humidity fluctuate with the change of seasons, in extremely humid environments, with fast air flow and continuous accumulation of particulate matter (dust), natural extracts (such as citric acid, polyphenols, etc.) antibacterial materials have low bactericidal efficiency, poor heat resistance, and cannot maintain high efficiency for a long time. In addition, the extraction and purification process is relatively complicated.

[0004] Ag + The representative material has the strongest bactericidal ability, but micron-level Ag + Composite materials (>1um) cannot maintain high levels for a long time. The high Ag dosage (>0.5wt.%) is not economical and environmentally friendly. The bactericidal slurry is not tightly bonded to the fiber substrate and is easy to fall off under high wind speed conditions. Organic antibacterial agents have poor heat resistance and high toxicity, which can cause pathogenic microorganisms to develop drug resistance. The bonding with the fiber substrate material is not uniform enough, affecting high efficiency. Inorganic bactericidal materials represented by TiO2 usually require ultraviolet light activation to have bactericidal ability.

[0005] In view of this, this application is filed. Summary of the invention

[0006] The purpose of the present invention is to overcome the shortcomings of the prior art and provide an antibacterial filter material, an antibacterial filter composition and a preparation method thereof and an application thereof in the preparation of a filter element. By combining Cu-Ag bimetallic inorganic nanomaterials and honey puree natural antibacterial agent, the antibacterial filter material has excellent antibacterial and filtering properties.

[0007] To achieve the above object, the technical solution adopted by the present invention is:

[0008] To achieve the above-mentioned object, the first aspect of the present application provides an antibacterial filter material, which is titanium dioxide loaded with Cu nanoparticles and Ag nanoparticles, wherein the antibacterial filter material contains oxygen vacancies and Ti 3+ Active site.

[0009] As an embodiment of the present application, the mass ratio of the Cu nanoparticles, the Ag nanoparticles, and the titanium dioxide is (0.1-0.5): (0.1-0.5): (99-99.8).

[0010] As an embodiment of the present application, the oxygen vacancies account for 5 to 20% of the antibacterial filter material, preferably 8.5 to 20%, and more preferably 10 to 20%.

[0011] As an embodiment of the present application, the average particle size of the Cu nanoparticles is ≤2 nm; and / or

[0012] The average particle size of the Ag nanoparticles is ≤2nm.

[0013] As an embodiment of the present application, the specific surface area of ​​the antibacterial filter material is 50 to 200 m 2 / g, and the average particle size is 15-25nm.

[0014] The second aspect of the present application provides a method for preparing an antibacterial filter material, comprising the following steps:

[0015] The titanium dioxide is dispersed in a solvent, copper salt and silver salt, stirred evenly, dried, and heat-treated under an inert gas or a reducing gas to obtain an antibacterial filter material.

[0016] As, the average particle size of the titanium dioxide is 15 to 25 nm; and / or

[0017] The specific surface area of ​​the titanium dioxide is 50 to 200 m 2 / g.

[0018] As an implementation scheme of the present application, at least one of the following (a) to (c) is satisfied:

[0019] (a) the copper salt comprises at least one of copper nitrate, copper sulfate, copper chloride and copper acetate;

[0020] (b) the silver salt comprises at least one of silver nitrate, silver sulfate, silver chloride and silver carbonate;

[0021] (c) The solvent includes at least one of water, acetone, ethanol, methanol, N,N-dimethylformamide, acetonitrile, dimethyl sulfoxide, cyclopentane, tetrahydrofuran, 2-methyltetrahydrofuran, ethylene nitrate, ethylene carbonate, 1,4-butyrolactone and dimethylacetamide.

[0022] As an embodiment of the present application, the mass ratio of titanium dioxide, copper salt and silver salt is (95-99.8): (x1×y1 / 63.5): (x2×y2 / 108);

[0023] Wherein, x1 = (0.1-0.5), y1 is the relative atomic mass of the copper salt;

[0024] x2=(0.1~0.5), y2 is the relative atomic mass of the silver salt.

[0025] As an embodiment of the present application, the inert gas includes at least one of nitrogen and helium, and the flow rate of the inert gas is 0.1 to 1 m / s; and / or

[0026] The reducing gas includes a mixture of hydrogen and inert gas, the volume ratio of the hydrogen to the inert gas is (2-10): (90-98), and the flow rate of the reducing gas is 0.1-1 m / s.

[0027] As an implementation scheme of the present application, the heat treatment temperature is 180 to 220° C., and the heat treatment time is 1 to 5 hours.

[0028] The third aspect of the present application provides an antibacterial filtration composition, comprising the following components in parts by weight: 10 to 30 parts of antibacterial filtration material, 1 to 3 parts of cellulose, 5 to 20 parts of honey puree, 2 to 10 parts of polyacrylic acid, and 37 to 82 parts of water;

[0029] The antibacterial filter material is the antibacterial filter material described above.

[0030] The fourth aspect of the present application provides a method for preparing an antibacterial filtration composition, comprising the following steps:

[0031] The antibacterial filtering material is dispersed in water, and cellulose, honey puree and polyacrylic acid are added and stirred evenly to obtain an antibacterial filtering composition.

[0032] The fifth aspect of the present application provides an application of an antibacterial filtration composition in the preparation of a filter element, wherein the filter element includes an air conditioning filter element, an automobile filter element, an air filter element or a filter element.

[0033] The sixth aspect of the present application provides a filter element, comprising a base layer and an antibacterial filter layer located on at least one surface of the base layer, wherein the antibacterial filter layer is prepared using the antibacterial filter composition described above.

[0034] As an embodiment of the present application, the base layer is micro glass fiber wool.

[0035] The beneficial effects of the present invention are as follows: the antibacterial filter material of the present invention contains oxygen vacancies and Ti 3+ Active sites are loaded with Cu nanoparticles and Ag nanoparticles. The oxygen vacancy defects and the bimetallic materials have a coordination effect. The presence of oxygen vacancies can effectively and continuously activate water molecules and oxygen molecules to produce free radicals and active oxygen species. In addition to their own coordinated bactericidal and antiviral effects, Cu nanoparticles and Ag nanoparticles can also be beneficial to electron transfer to activate oxygen molecules to produce active oxygen species. In this way, in-situ production under actual application conditions can continuously play a highly efficient antibacterial and antiviral role, with excellent antibacterial and filtering effects. Natural honey pulp and cellulose not only act as a binder to fix the CuAg / TiO2 inorganic material, but also have antibacterial efficiency themselves. DETAILED DESCRIPTION

[0036] In order to make the purpose, technical solutions and advantages of the embodiments of the present application clearer, the technical solutions in the embodiments of the present application are described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.

[0037] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0038] In this application, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values ​​of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0039] In the present application, there is no particular limitation on the specific dispersion and stirring treatment methods.

[0040] Unless otherwise specified, the components, raw materials or instruments used in the embodiments and comparative examples of the present invention are all commercially available raw materials or instruments, and the components and raw materials used in each parallel experiment are all of the same kind.

[0041] The present invention provides an antibacterial filter material, which is titanium dioxide loaded with Cu nanoparticles and Ag nanoparticles. The antibacterial filter material contains oxygen vacancies and Ti 3+ Active site.

[0042] The antibacterial filter material of the present invention contains oxygen vacancies and Ti 3+ Active sites are loaded with Cu nanoparticles and Ag nanoparticles. The oxygen vacancy defects and the bimetallic have a coordination effect. The presence of oxygen vacancies can effectively and continuously activate water molecules and oxygen molecules to produce free radicals and active oxygen species. In addition to their own coordinated bactericidal and antiviral effects, Cu nanoparticles and Ag nanoparticles can also be beneficial to electron transfer to activate oxygen molecules to produce active oxygen species. In this way, in-situ generation under actual application conditions can continuously play a highly efficient antibacterial and antiviral role, and has excellent antibacterial and filtration effects.

[0043] The Cu nanoparticles and Ag nanoparticles of the present invention are effectively combined, which not only exhibits high bactericidal activity but also greatly reduces the amount of Ag used. The titanium dioxide of the present invention contains abundant oxygen vacancies and Ti 3+ Active sites (gray-blue-black) can produce synergistic effects with Ag-Cu particles, without the need for special UV lamp activation, and can produce active oxygen species under natural conditions to achieve efficient sterilization and virus removal. The antibacterial filter material still maintains a high efficiency of >98% in an environment of alternating temperature and humidity, seasonal changes, and after long-term (>1 year) use.

[0044] In one embodiment, the mass ratio of the Cu nanoparticles, Ag nanoparticles, and titanium dioxide is (0.1-0.5): (0.1-0.5): (95-99.8). Especially when the mass ratio of the three is within this range, it has a more ideal synergistic effect and can more effectively improve the antibacterial effect and filtration performance.

[0045] In one embodiment, the oxygen vacancies account for 5-20% of the antibacterial filter material. The oxygen vacancies can be tested by XPS, EPR and oxygen adsorption and desorption methods. The present invention controls the content of oxygen vacancies within this range, which effectively improves the antibacterial performance and filtration performance. If the content is too low, the improvement effect cannot meet the requirements. If the content is too high, the stability of the material is reduced, resulting in a decrease in the effect.

[0046] In one embodiment, the average particle size of the Cu nanoparticles is ≤2 nm; and / or

[0047] The average particle size of the Ag nanoparticles is ≤2nm.

[0048] In one embodiment, the average particle size of the Cu nanoparticles is 0.1-2 nm.

[0049] In one embodiment, the average particle size of the Ag nanoparticles is 0.1-2 nm.

[0050] In one embodiment, the specific surface area of ​​the antibacterial filter material is 50 to 200 m 2 / g, and the average particle size is 15-25nm.

[0051] An embodiment of the present application provides a method for preparing an antibacterial filter material, comprising the following steps:

[0052] The titanium dioxide is dispersed in a solvent, copper salt and silver salt, stirred evenly, dried, and heat-treated under an inert gas or a reducing gas to obtain an antibacterial filter material.

[0053] As, the average particle size of the titanium dioxide is 15 to 25 nm; and / or

[0054] The specific surface area of ​​the titanium dioxide is 50 to 200 m 2 / g.

[0055] In one embodiment, at least one of the following (a) to (c) is satisfied:

[0056] (a) the copper salt comprises at least one of copper nitrate, copper sulfate, copper chloride and copper acetate;

[0057] (b) the silver salt comprises at least one of silver nitrate, silver sulfate, silver chloride and silver carbonate;

[0058] (c) The solvent includes at least one of water, acetone, ethanol, methanol, N,N-dimethylformamide, acetonitrile, dimethyl sulfoxide, cyclopentane, tetrahydrofuran, 2-methyltetrahydrofuran, ethylene nitrate, ethylene carbonate, 1,4-butyrolactone and dimethylacetamide.

[0059] In one embodiment, the mass ratio of titanium dioxide, copper salt and silver salt is (95-99.8): (x1×y1 / 63.5): (x2×y2 / 108);

[0060] Wherein, x1 = (0.1-0.5), y1 is the relative atomic mass of the copper salt;

[0061] x2=(0.1~0.5), y2 is the relative atomic mass of the silver salt.

[0062] In one embodiment, the inert gas includes at least one of nitrogen and helium, and the flow rate of the inert gas is 0.1 to 1 m / s; and / or

[0063] The reducing gas includes hydrogen and nitrogen, the volume ratio of the hydrogen to nitrogen is (2-10): (90-98), and the flow rate of the reducing gas is 0.1-1 m / s.

[0064] As an implementation scheme of the present application, the heat treatment temperature is 180 to 220° C., and the heat treatment time is 1 to 5 hours.

[0065] One embodiment of the present application provides an antibacterial filtration composition, comprising the following components in parts by weight: 10 to 30 parts of antibacterial filtration material, 1 to 3 parts of cellulose, 5 to 20 parts of honey puree, 2 to 10 parts of polyacrylic acid, and 37 to 82 parts of water;

[0066] The antibacterial filter material is the antibacterial filter material described above.

[0067] The inventors of the present invention have found that by combining the antibacterial filter material with the above-mentioned raw materials, an antibacterial filter composition with excellent antibacterial filtration performance is obtained. The antibacterial filter composition has excellent resistance to a variety of bacteria and viruses, and still maintains a high efficiency of >98% in an environment of alternating temperature and humidity and seasonal changes and after long-term (>1 year) use, and has broad application prospects.

[0068] The inventors of the present invention have creatively discovered that the antibacterial filter material has a significant synergistic effect when used in combination with honey puree. The honey puree contains peroxide compounds, polyphenolic acid compounds, methyldialdehyde and low pH, and exhibits good antibacterial and antiviral properties. In addition, the resources are abundant and can be used directly without any secondary processing and extraction. Combining natural cellulose and sugar compounds in honey can be used as an efficient binder to firmly fix the inorganic fungicide on the surface of the fiber cloth, thereby avoiding or reducing other organic solvents and cross-linking agents. The combination of the two promotes each other and significantly improves the antibacterial filtration performance and antibacterial filtration durability of the system.

[0069] An embodiment of the present application provides a method for preparing an antibacterial filtration composition, comprising the following steps:

[0070] The antibacterial filtering material is dispersed in water, and cellulose, honey puree and polyacrylic acid are added and stirred evenly to obtain an antibacterial filtering composition.

[0071] One embodiment of the present application provides an application of an antibacterial filtration composition in the preparation of a filter element, wherein the filter element includes an air conditioning filter element, an automobile filter element, an air filter element or a filter element.

[0072] One embodiment of the present application provides a filter element, comprising a base layer and an antibacterial filter layer located on at least one surface of the base layer, wherein the antibacterial filter layer is prepared using the antibacterial filter composition described above.

[0073] In one embodiment, the base layer is micro-glass fiber wool.

[0074] The following examples are provided to facilitate understanding of the present invention. These examples are not provided to limit the scope of the claims.

[0075] Example 1

[0076] A method for preparing an antibacterial filtration composition comprises the following steps:

[0077] (1) 99.8 parts of P25 titanium dioxide are dispersed in 300 parts of water and 100 parts of acetone, 0.43 parts of copper nitrate (pentahydrate) and 0.157 parts of silver nitrate are added, and the mixture is stirred uniformly at 25° C., and the mixture is transferred to a drying oven and dried at 80° C. to remove moisture and solvent, and the obtained powder is placed in a tubular rotary furnace, and heat-treated at 200° C. for 2 h in a 5% hydrogen / nitrogen mixed atmosphere at 0.5 m / s to obtain an antibacterial filter material, wherein the antibacterial filter material is titanium dioxide loaded with Cu nanoparticles and Ag nanoparticles, and the antibacterial filter material contains oxygen vacancies and Ti 3+ Active site;

[0078] (2) 20 parts of antibacterial filter material, 20 parts of honey puree, 2 parts of cellulose, 5 parts of polyacrylic acid and 53 parts of water were stirred uniformly to obtain an antibacterial filter composition.

[0079] Example 2

[0080] A method for preparing an antibacterial filtration composition comprises the following steps:

[0081] (1) 99.4 parts of P25 titanium dioxide are dispersed in 300 parts of water and 100 parts of acetone, 1.29 parts of copper nitrate (pentahydrate) and 0.47 parts of silver nitrate are added, and the mixture is stirred uniformly at 25° C., and the mixture is transferred to a drying oven and dried at 80° C. to remove moisture and solvent, and the obtained powder is placed in a tubular rotary furnace, and heat-treated at 200° C. for 2 h in a 5% hydrogen / nitrogen mixed atmosphere at 0.5 m / s to obtain an antibacterial filter material, wherein the antibacterial filter material is titanium dioxide loaded with Cu nanoparticles and Ag nanoparticles, and the antibacterial filter material contains oxygen vacancies and Ti 3+ Active site;

[0082] (2) 20 parts of antibacterial filter material, 20 parts of honey puree, 2 parts of cellulose, 5 parts of polyacrylic acid and 53 parts of water were stirred uniformly to obtain an antibacterial filter composition.

[0083] Example 3

[0084] A method for preparing an antibacterial filtration composition comprises the following steps:

[0085] (1) 99.0P25 titanium dioxide is dispersed in 300 parts of water and 100 parts of acetone, 2.15 parts of copper nitrate (pentahydrate) and 0.78 parts of silver nitrate are added, and the mixture is stirred uniformly at 25°C, and the mixture is transferred to a drying oven and dried at 80°C to remove moisture and solvent. The obtained powder is placed in a tubular rotary furnace, and heat-treated at 200°C for 2 hours in a 5% hydrogen / nitrogen mixed atmosphere at 0.5 m / s to obtain an antibacterial filter material, wherein the antibacterial filter material is titanium dioxide loaded with Cu nanoparticles and Ag nanoparticles, and the antibacterial filter material contains oxygen vacancies and Ti 3+ Active site;

[0086] (2) 20 parts of antibacterial filter material, 20 parts of honey puree, 2 parts of cellulose, 5 parts of polyacrylic acid and 53 parts of water were stirred uniformly to obtain an antibacterial filter composition.

[0087] Example 4

[0088] A method for preparing an antibacterial filtration composition comprises the following steps:

[0089] (1) 99.4 parts of P25 titanium dioxide are dispersed in 300 parts of water and 100 parts of acetone, 1.29 parts of copper nitrate (pentahydrate) and 0.47 parts of silver nitrate are added, and the mixture is stirred uniformly at 25°C, and the mixture is transferred to a drying oven and dried at 80°C to remove moisture and solvent. The obtained powder is placed in a tubular rotary furnace, and heat-treated at 180°C for 1 hour in a nitrogen atmosphere at a flow rate of 0.1 m / s to obtain an antibacterial filter material, wherein the antibacterial filter material is titanium dioxide loaded with Cu nanoparticles and Ag nanoparticles, and the antibacterial filter material contains oxygen vacancies and Ti 3+ Active site;

[0090] (2) 20 parts of antibacterial filter material, 20 parts of honey puree, 2 parts of cellulose, 5 parts of polyacrylic acid and 53 parts of water were stirred uniformly to obtain an antibacterial filter composition.

[0091] Example 5

[0092] A method for preparing an antibacterial filtration composition comprises the following steps:

[0093] (1) 99.4 parts of P25 titanium dioxide are dispersed in 300 parts of water and 100 parts of acetone, 1.29 parts of copper nitrate (pentahydrate) and 0.47 parts of silver nitrate are added, and the mixture is stirred uniformly at 25° C., and the mixture is transferred to a drying oven and dried at 80° C. to remove moisture and solvent, and the obtained powder is placed in a tubular rotary furnace, and heat-treated at 220° C. for 5 h in a 10% hydrogen / nitrogen mixed atmosphere at a speed of 1 m / s to obtain an antibacterial filter material, wherein the antibacterial filter material is titanium dioxide loaded with Cu nanoparticles and Ag nanoparticles, and the antibacterial filter material contains oxygen vacancies and Ti 3+ Active site;

[0094] (2) 20 parts of antibacterial filter material, 20 parts of honey puree, 2 parts of cellulose, 5 parts of polyacrylic acid and 53 parts of water were stirred uniformly to obtain an antibacterial filter composition.

[0095] Example 6

[0096] A method for preparing an antibacterial filtration composition comprises the following steps:

[0097] (1) 99.4 parts of P25 titanium dioxide are dispersed in 300 parts of water and 100 parts of acetone, 1.29 parts of copper nitrate (pentahydrate) and 0.47 parts of silver nitrate are added, and the mixture is stirred uniformly at 25° C., and the mixture is transferred to a drying oven and dried at 80° C. to remove moisture and solvent, and the obtained powder is placed in a tubular rotary furnace, and heat-treated at 200° C. for 2 h in a 5% hydrogen / nitrogen mixed atmosphere at 0.5 m / s to obtain an antibacterial filter material, wherein the antibacterial filter material is titanium dioxide loaded with Cu nanoparticles and Ag nanoparticles, and the antibacterial filter material contains oxygen vacancies and Ti 3+ Active site;

[0098] (2) 15 parts of antibacterial filter material, 15 parts of honey puree, 3 parts of cellulose, 2 parts of polyacrylic acid, and 65 parts of water were stirred uniformly to obtain an antibacterial filter composition.

[0099] Example 7

[0100] A method for preparing an antibacterial filtration composition comprises the following steps:

[0101] (1) 99.4 parts of P25 titanium dioxide are dispersed in 300 parts of water and 100 parts of acetone, 1.29 parts of copper nitrate (pentahydrate) and 0.47 parts of silver nitrate are added, and the mixture is stirred uniformly at 25° C., and the mixture is transferred to a drying oven and dried at 80° C. to remove moisture and solvent, and the obtained powder is placed in a tubular rotary furnace, and heat-treated at 200° C. for 2 h in a 5% hydrogen / nitrogen mixed atmosphere at 0.5 m / s to obtain an antibacterial filter material, wherein the antibacterial filter material is titanium dioxide loaded with Cu nanoparticles and Ag nanoparticles, and the antibacterial filter material contains oxygen vacancies and Ti 3+Active site;

[0102] (2) 30 parts of antibacterial filter material, 5 parts of honey puree, 1 part of cellulose, 10 parts of polyacrylic acid, and 54 parts of water were stirred uniformly to obtain an antibacterial filter composition.

[0103] Example 8

[0104] A method for preparing a filter element comprises the following steps:

[0105] Select 1m*1m micro glass wool fibers (fiber diameter is 0.4-3μm), and apply the antibacterial filtration composition of each of the above Examples 1-7 on the surface of the micro glass wool fibers, with a coating amount of 15g / m 2 , dried, cut, folded and edged to obtain a filter element product of a certain size (20cm x 20cm x 2cm).

[0106] Comparative Example 1

[0107] Compared with Example 2, Comparative Example 1 controls the loading amount of Cu nanoparticles and Ag nanoparticles by controlling the added amount of copper nitrate and silver nitrate.

[0108] A method for preparing an antibacterial filtration composition comprises the following steps:

[0109] (1) 99.9 parts of P25 titanium dioxide are dispersed in 300 parts of water and 100 parts of acetone, 0.21 parts of copper nitrate (pentahydrate) and 0.07 parts of silver nitrate are added, and the mixture is stirred uniformly at 25° C., and the mixture is transferred to a drying oven and dried at 80° C. to remove moisture and solvent, and the obtained powder is placed in a tubular rotary furnace, and heat-treated at 200° C. for 2 h in a 5% hydrogen / nitrogen mixed atmosphere at 0.5 m / s to obtain an antibacterial filter material, wherein the antibacterial filter material is titanium dioxide loaded with Cu nanoparticles and Ag nanoparticles, and the antibacterial filter material contains oxygen vacancies and Ti 3+ Active site;

[0110] (2) 20 parts of antibacterial filter material, 20 parts of honey puree, 2 parts of cellulose, 5 parts of polyacrylic acid and 53 parts of water were stirred uniformly to obtain an antibacterial filter composition.

[0111] Comparative Example 2

[0112] Comparative Example 2 Compared with Example 2, Comparative Example 2 controls the loading amount of Cu nanoparticles and Ag nanoparticles by controlling the added amount of copper sulfate and silver sulfate.

[0113] A method for preparing an antibacterial filtration composition comprises the following steps:

[0114] (1) 96 parts of P25 titanium dioxide are dispersed in 300 parts of water and 100 parts of acetone, 8.3 parts of copper nitrate (pentahydrate) and 3.02 parts of silver nitrate are added, and the mixture is stirred uniformly at 25° C., and the mixture is transferred to a drying oven and dried at 80° C. to remove moisture and solvent, and the obtained powder is placed in a tubular rotary furnace, and heat-treated at 200° C. for 2 h under a 5% hydrogen / nitrogen mixture at a flow rate of 0.5 m / s to obtain an antibacterial filter material, wherein the antibacterial filter material is titanium dioxide loaded with Cu nanoparticles and Ag nanoparticles, and the antibacterial filter material contains oxygen vacancies and Ti 3+ Active site;

[0115] (2) 20 parts of antibacterial filter material, 20 parts of honey puree, 2 parts of cellulose, 5 parts of polyacrylic acid and 53 parts of water were stirred uniformly to obtain an antibacterial filter composition.

[0116] Comparative Example 3

[0117] Comparative Example 3 Compared with Example 2, Comparative Example 3 is heat-treated in an air atmosphere.

[0118] The loading amount of Cu nanoparticles and Ag nanoparticles can be controlled by controlling the added amount of copper nitrate and silver nitrate.

[0119] A method for preparing an antibacterial filtration composition comprises the following steps:

[0120] (1) 99.4 parts of P25 titanium dioxide are dispersed in 300 parts of water and 100 parts of acetone, 1.29 parts of copper nitrate (pentahydrate) and 0.47 parts of silver nitrate are added, and the mixture is stirred uniformly at 25°C, and the mixture is transferred to a drying oven and dried at 80°C to remove moisture and solvent. The obtained powder is placed in a tubular rotary furnace, and heat-treated at 200°C for 2 hours in an air atmosphere of 0.5 m / s to obtain an antibacterial filter material, wherein the antibacterial filter material is titanium dioxide loaded with Cu nanoparticles and Ag nanoparticles, and the antibacterial filter material does not contain oxygen vacancies and Ti 3+ Active site;

[0121] (2) 20 parts of antibacterial filter material, 20 parts of honey puree, 2 parts of cellulose, 5 parts of polyacrylic acid and 53 parts of water were stirred uniformly to obtain an antibacterial filter composition.

[0122] Comparative Example 4

[0123] Compared with Example 2, the heat treatment temperature of Comparative Example 4 is 160° C. and the nitrogen flow rate is 0.5 m / s.

[0124] A method for preparing an antibacterial filtration composition comprises the following steps:

[0125] (1) 99.4 parts of P25 titanium dioxide are dispersed in 300 parts of water and 100 parts of acetone, 1.29 parts of copper nitrate (pentahydrate) and 0.47 parts of silver nitrate are added, and the mixture is stirred uniformly at 25°C, and the mixture is transferred to a drying oven and dried at 80°C to remove moisture and solvent. The obtained powder is placed in a rotary furnace and heat-treated at 160°C for 3 hours in a nitrogen atmosphere at a flow rate of 0.5 m / s to obtain an antibacterial filter material, wherein the antibacterial filter material is titanium dioxide loaded with Cu nanoparticles and Ag nanoparticles, and the antibacterial filter material contains oxygen vacancies and Ti 3+ Active site;

[0126] (2) 20 parts of antibacterial filter material, 20 parts of honey puree, 2 parts of cellulose, 5 parts of polyacrylic acid and 53 parts of water were stirred uniformly to obtain an antibacterial filter composition.

[0127] Comparative Example 5

[0128] Compared with Example 2, the heat treatment temperature of Comparative Example 5 is 300° C. and the nitrogen flow rate is 0.5 m / s.

[0129] A method for preparing an antibacterial filtration composition comprises the following steps:

[0130] (1) 99.4 parts of P25 titanium dioxide are dispersed in 300 parts of water and 100 parts of acetone, 1.29 parts of copper nitrate (pentahydrate) and 0.47 parts of silver nitrate are added, and the mixture is stirred uniformly at 25°C, and the mixture is transferred to a drying oven and dried at 80°C to remove moisture and solvent. The obtained powder is placed in a rotary furnace and heat-treated at 300°C for 3 hours in a nitrogen atmosphere at a flow rate of 0.5 m / s to obtain an antibacterial filter material, wherein the antibacterial filter material is titanium dioxide loaded with Cu nanoparticles and Ag nanoparticles, and the antibacterial filter material contains oxygen vacancies and Ti 3+ Active site;

[0131] (2) 20 parts of antibacterial filter material, 20 parts of honey puree, 2 parts of cellulose, 5 parts of polyacrylic acid and 53 parts of water were stirred uniformly to obtain an antibacterial filter composition.

[0132] Comparative Example 6

[0133] Compared with Example 2, Comparative Example 6 uses an equal amount of honey puree to replace the antibacterial filter material.

[0134] A method for preparing an antibacterial filtration composition comprises the following steps:

[0135] (1) 99.4 parts of P25 titanium dioxide are dispersed in 300 parts of water and 100 parts of acetone, 1.29 parts of copper nitrate (pentahydrate) and 0.47 parts of silver nitrate are added, and the mixture is stirred uniformly at 25° C., and the mixture is transferred to a drying oven and dried at 80° C. to remove moisture and solvent, and the obtained powder is placed in a tubular rotary furnace, and heat-treated at 200° C. for 2 h in a 5% hydrogen / nitrogen atmosphere at 0.5 m / s to obtain an antibacterial filter material, wherein the antibacterial filter material is titanium dioxide loaded with Cu nanoparticles and Ag nanoparticles, and the antibacterial filter material contains oxygen vacancies and Ti 3+ Active site;

[0136] (2) 40 parts of honey puree, 2 parts of cellulose, 5 parts of polyacrylic acid, and 53 parts of water were stirred uniformly to obtain an antibacterial filtration composition.

[0137] Comparative Example 7

[0138] Compared with Example 2, Comparative Example 7 uses an equal amount of antibacterial filtration material to replace the honey puree.

[0139] A method for preparing an antibacterial filtration composition comprises the following steps:

[0140] (1) 99.4 parts of P25 titanium dioxide are dispersed in 300 parts of water and 100 parts of acetone, 1.29 parts of copper nitrate (pentahydrate) and 0.47 parts of silver nitrate are added, and the mixture is stirred uniformly at 25° C., and the mixture is transferred to a drying oven and dried at 80° C. to remove moisture and solvent, and the obtained powder is placed in a tubular rotary furnace, and heat-treated at 200° C. for 2 h in a 5% hydrogen / nitrogen atmosphere at 0.5 m / s to obtain an antibacterial filter material, wherein the antibacterial filter material is titanium dioxide loaded with Cu nanoparticles and Ag nanoparticles, and the antibacterial filter material contains oxygen vacancies and Ti 3+ Active site;

[0141] (2) 40 parts of antibacterial filter material, 2 parts of cellulose, 5 parts of polyacrylic acid and 53 parts of water were stirred uniformly to obtain an antibacterial filter composition.

[0142] Among them, the indicators of the antibacterial filter materials of Examples 1 to 8 and Comparative Examples 1 to 7 are as follows:

[0143] The mass ratio of titanium dioxide, Cu nanoparticles, and Ag nanoparticles is denoted as A

[0144] The mass ratio of the antibacterial filter material, honey puree, cellulose, polyacrylic acid and water is marked as B.

[0145] Table 1 Relative concentration of oxygen vacancies in antibacterial materials, average size of metal nanoparticles and mass ratio of each component

[0146]

[0147]

[0148] Performance Testing

[0149] The antibacterial filtration compositions of Examples 1 to 7 and Comparative Examples 1 to 7 were prepared into filter elements for testing according to the method of Example 8.

[0150] 1. Sterilization test

[0151] Antiviral test: ISO 18184:2014 (E) Test method for antiviral performance of textiles (test strains are influenza A virus H3N2 and influenza A virus H1N1).

[0152] Antibacterial (inhibitory) test: GB / T 20944.3-2008 oscillation method (test bacteria are Escherichia coli and Staphylococcus aureus).

[0153] The same filter element is used in the embodiment and the comparative example. After one year of use, the new filter element is installed in the air conditioning system of the car for air filtration. After one year of actual filtration, the filter element is taken out and then tested for antibacterial and antiviral activity, particle removal and wind resistance.

[0154] The particle removal and wind resistance test tests the particle removal efficiency and wind resistance of the automotive air conditioning filter in accordance with the national standard GB / T 32085-1.

[0155] Table 2 Antibacterial performance of the antibacterial compositions of the embodiments and comparative examples configured into filter cartridges before and after use

[0156]

[0157]

[0158] Table 3 Removal efficiency of 0.3um particles and wind resistance (300m 3 / h wind speed)

[0159]

[0160] It can be seen from Table 2 and Table 3 that the material described in the present invention has excellent antibacterial filtration performance.

[0161] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. An antibacterial filter material, characterized in that: It is titanium dioxide loaded with Cu nanoparticles and Ag nanoparticles, and the antibacterial filter material contains oxygen vacancies and Ti 3+ Active site.

2. The antibacterial filter material according to claim 1, characterized in that: The mass ratio of the Cu nanoparticles, the Ag nanoparticles and the titanium dioxide is (0.1-0.5): (0.1-0.5): (99-99.8).

3. The antibacterial filter material according to claim 1, characterized in that: The oxygen vacancies account for 5-20% of the antibacterial filter material, preferably 8.5-20%.

4. The antibacterial filter material according to claim 1, characterized in that: The average particle size of the Cu nanoparticles is ≤2nm; and / or The average particle size of the Ag nanoparticles is ≤2nm.

5. The antibacterial filter material according to claim 1, characterized in that: The specific surface area of ​​the antibacterial filter material is 50 to 200 m 2 / g, and the average particle size is 15-25nm.

6. The method for preparing the antibacterial filter material according to any one of claims 1 to 5, characterized in that: The following steps are involved: The titanium dioxide is dispersed in a solvent, copper salt and silver salt, stirred evenly, dried, and heat-treated under an inert gas or a reducing gas to obtain an antibacterial filter material.

7. The method for preparing the antibacterial filter material according to claim 6, characterized in that: The average particle size of the titanium dioxide is 15 to 25 nm; and / or The specific surface area of ​​the titanium dioxide is 50 to 200 m 2 / g.

8. The method for preparing the antibacterial filter material according to claim 6, characterized in that: Satisfy at least one of the following (a) to (c): (a) the copper salt comprises at least one of copper nitrate, copper sulfate, copper chloride and copper carbonate; (b) the silver salt comprises at least one of silver nitrate, silver sulfate, silver chloride and silver carbonate; (c) The solvent includes at least one of water, acetone, ethanol, methanol, N,N-dimethylformamide, acetonitrile, dimethyl sulfoxide, cyclopentane, tetrahydrofuran, 2-methyltetrahydrofuran, ethylene nitrate, ethylene carbonate, 1,4-butyrolactone and dimethylacetamide.

9. The method for preparing the antibacterial filter material according to claim 6, characterized in that: The mass ratio of the titanium dioxide, copper salt and silver salt is (95-99.8): (x1×y1 / 63.5): (x2×y2 / 108); Wherein, x1 = (0.1-0.5), y1 is the relative atomic mass of the copper salt; x2=(0.1~0.5), y2 is the relative atomic mass of the silver salt.

10. The method for preparing the antibacterial filter material according to claim 6, characterized in that: The inert gas includes at least one of nitrogen and helium, and the flow rate of the inert gas is 0.1-1 m / s; and / or The reducing gas includes hydrogen and nitrogen, the volume ratio of the hydrogen to nitrogen is (2-10): (90-98), and the flow rate of the reducing gas is 0.1-1 m / s.

11. The method for preparing the antibacterial filter material according to claim 6, characterized in that: The heat treatment temperature is 180-220° C., and the heat treatment time is 1-5 hours.

12. An antibacterial filtration composition, characterized in that: The invention comprises the following components in parts by weight: 10 to 30 parts of antibacterial filter material, 1 to 3 parts of cellulose, 5 to 20 parts of honey puree, 2 to 10 parts of polyacrylic acid, and 37 to 82 parts of water; The antibacterial filter material is the antibacterial filter material according to any one of claims 1 to 5.

13. The method for preparing the antibacterial filtration composition according to claim 12, characterized in that: The following steps are involved: The antibacterial filtering material is dispersed in water, and cellulose, honey puree and polyacrylic acid are added and stirred evenly to obtain an antibacterial filtering composition.

14. Use of the antibacterial filtration composition according to claim 12 in preparing a filter element, characterized in that: The filter element includes an air conditioning filter element, an automobile filter element, an air filter element or a filter element.

15. A filter element, characterized in that: It comprises a base layer and an antibacterial filter layer located on at least one surface of the base layer, wherein the antibacterial filter layer is prepared by using the antibacterial filter composition according to claim 12.

16. The filter element according to claim 15, characterized in that The base layer is micro glass fiber wool.

Citation Information

Patent Citations

  • Preparation method for medical honey dressing

    CN101569761A

  • Preparation method of sterile honey dressing

    CN102406958A

Cited By

  • High-stability nano titanium dioxide, preparation method thereof and application of high-stability nano titanium dioxide in modified coating

    CN119978851A