Polyvinylidene fluoride microporous filter membrane and preparation method thereof

The preparation of PVDF membranes was simplified by low-temperature and low-humidity non-solvent vapor-induced phase separation method, which solved the problems of complex process and poor protein transfer effect, and prepared a PVDF microporous filter membrane with excellent stiffness and protein transfer effect.

CN119075705AActive Publication Date: 2024-12-06MEMBRANE SOLUTIONS (NANTONG) CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411300828.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-12-06
Estimated Expiration
2044-09-18

AI Technical Summary

Technical Problem

The existing PVDF membrane preparation process is complex, not easy to industrialize, and the protein transfer effect is poor.

Method used

The low-temperature and low-humidity non-solvent vapor-induced phase separation method was used to form a metastable material liquid by cooling, and the spherical crystals and rod-shaped short fiber crystals were generated by steam induced, and the solvent was immersed in a solidification bath to exchange solvents to prepare a PVDF microporous filter membrane with excellent performance.

Benefits of technology

The preparation process is simplified and the controllability of the film formation process is improved. The prepared PVDF microporous filter membrane has excellent stiffness and support performance, which is suitable for protein transfer, and the effect is significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119075705A_ABST
    Figure CN119075705A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of microfiltration membranes, and provides a polyvinylidene fluoride microfiltration membrane and a preparation method thereof.The method comprises the steps that at the first temperature, polyvinylidene fluoride is dissolved in a solvent, an additive is added, mixing is conducted to obtain feed liquid, the feed liquid is cooled to the second temperature, and membrane casting liquid is obtained; preparing the membrane casting solution into a liquid membrane; and carrying out steam induced phase separation on the liquid membrane, and then immersing the liquid membrane into a coagulating bath for coagulating and forming to obtain the polyvinylidene fluoride microporous filter membrane. According to the preparation method disclosed by the invention, a complicated process is not needed, and the polyvinylidene fluoride (PVDF) microporous filter membrane with excellent performance can be prepared by adopting a simple low-temperature low-humidity non-solvent steam induced phase separation method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of microporous filter membranes, and in particular to a polyvinylidene fluoride microporous filter membrane and a preparation method thereof. Background Art

[0002] Polyvinylidene fluoride (PVDF) is one of the most commonly used polymers for making membranes due to its excellent chemical, thermal and mechanical stability. The prepared polyvinylidene fluoride membrane (PVDF membrane) can be widely used in wastewater treatment, microfiltration (MF), ultrafiltration (UF) and membrane bioreactor (MBR) for food and health applications. Since PVDF membrane has strong hydrophobicity and electrostatic adsorption, it has a strong nonspecific adsorption capacity for proteins. Therefore, PVDF membrane has broad application prospects in the biomedical field. At present, PVDF membrane has been used in Western-blotting (protein immunoblotting) in the laboratory. At the same time, due to the good physical strength and solvent tolerance of PVDF membrane, it has greater advantages than other transfer materials.

[0003] In addition, PVDF is easily dissolved in common organic solvents, such as N,N-dimethylacetamide (DMAc), N,N-dimethylformamide (DMF) and N,N-dimethyl sulfoxide (DMSO). Therefore, those skilled in the art can produce porous PVDF membranes by a simple phase inversion method.

[0004] The methods commonly used to prepare PVDF microporous membranes include non-solvent induced phase separation (NIPS) and non-solvent vapor induced phase separation (VIPS). For example, Chinese patent application document CN112495197A discloses a polyvinylidene fluoride filter membrane and its preparation method and use, and a PVDF microporous membrane is prepared by the VIPS method. European patent EP0037836 discloses a polyvinylidene fluoride hollow fiber microfiltration membrane and its manufacturing method, which adopts an immersion gel bath phase precipitation membrane to form an asymmetric membrane structure. Chinese patent application document CN 114849489A discloses a method for preparing a hydrophilic polyvinylidene fluoride microfiltration membrane, in which the liquid film is pre-evaporated under a constant temperature and humidity environment, and then immersed in a coagulation bath for phase separation precipitation to prepare a PVDF microfiltration membrane.

[0005] In addition, there have been related reports on using membranes as carriers for Western-blotting experiments. For example, Chinese patent CN1851462B discloses a method for preparing a cellulose adsorption and transfer membrane, which prepared a nitrocellulose membrane for protein adsorption. However, the adsorption capacity was small, the protein binding fastness was low, and the cellulose membrane was weak and easily broken.

[0006] PVDF membranes are strong, have high protein binding strength, and have a large adsorption capacity, making them ideal membranes for immunoblotting. For example, the patent with publication number CN101850217B discloses a method for preparing a PVDF transfer membrane with a uniform structure without a skin layer, but the membrane has a large pore size and cannot retain small amounts of protein, and its protein transfer bands are relatively fuzzy.

[0007] Therefore, how to use a simple process to prepare a PVDF membrane with stable performance and effective application in protein transfer has become a research focus in this field. Summary of the invention

[0008] In view of the above-mentioned shortcomings of the prior art, the present invention provides a polyvinylidene fluoride microporous filter membrane and a preparation method thereof to solve the problems existing in the prior art such as complex PVDF membrane preparation process, difficulty in industrialization, and poor protein transfer effect of the prepared PVDF membrane.

[0009] To achieve the above-mentioned and related purposes, the present invention adopts the following technical means:

[0010] The first aspect of the present invention provides a method for preparing a polyvinylidene fluoride microporous filter membrane, comprising the following steps:

[0011] (1) dissolving polyvinylidene fluoride in a solvent at a first temperature and adding an additive, mixing to obtain a feed liquid, and cooling the feed liquid to a second temperature to obtain a casting solution;

[0012] (2) preparing the casting liquid to form a liquid film;

[0013] (3) After the liquid membrane is subjected to steam-induced phase separation, it is immersed in a coagulation bath for coagulation and molding to obtain a polyvinylidene fluoride microporous filter membrane.

[0014] In one embodiment of the present application, in step (1), the first temperature is 40-80° C.;

[0015] And / or, the second temperature is 30-60°C.

[0016] In one embodiment of the present application, in the feed solution of step (1), the mass fraction of polyvinylidene fluoride is 10 to 30 wt %;

[0017] and / or, the mass fraction of the solvent is 50 to 80 wt%;

[0018] And / or, the mass fraction of the additive is 0 to 20 wt%.

[0019] In one embodiment of the present application, the solvent in step (1) includes one or more of N,N-dimethylacetamide, N,N-methylformamide, N-methyl-2-pyrrolidone, triethyl phosphate, and 2-pyrrolidone.

[0020] In one embodiment of the present application, the additive in step (1) includes one or more of methanol, ethanol, glycerol, isopropanol, n-butanol, diethylene glycol, triethylene glycol, tetraethylene glycol, ethylene glycol methyl ether, ethylene glycol dimethyl ether, and water.

[0021] In one embodiment of the present application, step (3) includes: placing the liquid membrane in a low temperature and low humidity environment for steam-induced phase separation, wherein the temperature of the low temperature and low humidity environment is 10-30° C. and the relative humidity is 40-80 RH%.

[0022] In one embodiment of the present application, the steam induction time in step (3) is 120 to 600 seconds.

[0023] In one embodiment of the present application, the second temperature is more preferably 30-50°C.

[0024] In one embodiment of the present application, step (3) includes: immersing in a coagulation bath for coagulation, washing, and drying to obtain a polyvinylidene fluoride microporous filter membrane.

[0025] The second aspect of the present invention is a polyvinylidene fluoride microporous filter membrane prepared according to the above preparation method.

[0026] The beneficial technical effects of the present invention are:

[0027] The present invention does not require complicated processes, and can prepare a polyvinylidene fluoride (PVDF) microporous filter membrane with excellent performance by using a simple low-temperature and low-humidity non-solvent vapor-induced phase separation method. Specifically, the present invention first reduces the feed liquid temperature to ensure that the feed liquid system is in a metastable state; then, under low-temperature and low-humidity conditions, non-solvent vapor is used to induce the membrane to undergo crystallization phase separation to generate spherulites and rod-shaped short fiber crystals; finally, the membrane is immersed in a coagulation bath to exchange out other components such as the solvent, thereby preparing a polyvinylidene fluoride microporous filter membrane.

[0028] The present invention can effectively adjust the structure and performance of the final film by adjusting the components in the feed liquid and the parameters of the low-temperature and low-humidity non-solvent vapor induction environment.

[0029] The preparation method of the invention is simple, the film-forming process is highly controllable, and it is very easy to industrialize. The polyvinylidene fluoride microporous filter membrane prepared by the invention has excellent stiffness and supporting performance, and also has good protein transfer effect.

[0030] It should be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] The drawings herein are incorporated into the specification and constitute a part of the specification, showing embodiments consistent with the present application, and together with the specification, are used to explain the principles of the present application. Obviously, the drawings described below are only some embodiments of the present application, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work. In the drawings:

[0032] Figure 1 This is an electron microscope photograph of the surface of the PVDF microporous filter membrane of Example 1;

[0033] Figure 2 This is an electron microscope photograph of the surface of the PVDF microporous filter membrane of Example 2;

[0034] Figure 3 This is an electron microscope photograph of the surface of the PVDF microporous filter membrane of Example 3;

[0035] Figure 4 This is an electron microscope photograph of the surface of the PVDF microporous filter membrane of Comparative Example 1;

[0036] Figure 5 This is an electron microscope photograph of the surface of the PVDF microporous filter membrane of Comparative Example 2;

[0037] Figure 6 This is an electron microscope photograph of the surface of the PVDF microporous filter membrane of comparative example 3. DETAILED DESCRIPTION

[0038] Unless otherwise defined, all technical and / or scientific terms used herein have the same meaning as the general understanding of a person of ordinary skill in the art to which the present invention belongs. It should be understood that certain features of the present invention (described in the context of separate embodiments for clarity) may also be provided in combination in a single embodiment. On the contrary, multiple features of the present invention (described in the context of a single embodiment for brevity) may also be provided separately or in any suitable combination or in any other described embodiment of the present invention when appropriate. Certain features described in the context of various embodiments will not be considered as essential features of those embodiments unless the embodiment is inoperable without those elements. The present invention is further described below by specific specific examples, but it should be noted that the specific process conditions and results described in the embodiments of the present invention are only used to illustrate the present invention, and the protection scope of the present invention cannot be limited thereto. All equivalent changes or modifications made according to the spirit and essence of the present invention should be included in the protection scope of the present invention.

[0039] First of all, it should be noted that the raw materials used in the technical solution of the present invention: polyvinylidene fluoride (PVDF for short), N,N-dimethylacetamide (DMAC for short), N,N-methylformamide (DMF for short), N-methyl-2-pyrrolidone (NMP for short), triethyl phosphate (TEP for short) and 2-pyrrolidone, methanol, ethanol, glycerol, isopropanol, n-butanol, diethylene glycol, triethylene glycol, tetraethylene glycol, ethylene glycol methyl ether, ethylene glycol dimethyl ether, etc. are all commercially available products.

[0040] The present invention provides a method for preparing a polyvinylidene fluoride microporous filter membrane, comprising the following steps:

[0041] (1) Dissolving polyvinylidene fluoride in a solvent at a first temperature and adding an additive, stirring and mixing the mixture to obtain a slurry, cooling the slurry to a second temperature and keeping the temperature to obtain a casting solution.

[0042] In this step, the first temperature is 40 to 80°C, preferably 50 to 80°C;

[0043] In this step, the second temperature is 30-60°C, preferably 30-50°C;

[0044] In this step, the mass fraction of polyvinylidene fluoride in the feed solution is 10 to 30 wt%, preferably 15 to 25 wt%;

[0045] In this step, the mass fraction of the solvent is 50 to 80 wt%, preferably 50 to 60 wt%;

[0046] In this step, the mass fraction of the additive is 0 to 20 wt%, preferably 10 to 20 wt%;

[0047] In this step, the solvent includes one or more of N,N-dimethylacetamide, N,N-methylformamide, N-methyl-2-pyrrolidone, triethyl phosphate, and 2-pyrrolidone;

[0048] In this step, the additive includes one or more of methanol, ethanol, glycerol, isopropanol, n-butanol, diethylene glycol, triethylene glycol, tetraethylene glycol, ethylene glycol methyl ether, ethylene glycol dimethyl ether, and water.

[0049] (2) The casting liquid is coated on the PES release film and scraped to form a liquid film. The scraping interval is 200 to 500 μm, preferably 200 to 300 μm.

[0050] (3) placing the liquid membrane in a low temperature and low humidity environment for steam-induced phase separation, wherein the temperature of the low temperature and low humidity environment is 10 to 30° C. and the relative humidity is 40 to 80 RH%.

[0051] In this step, the temperature is preferably 20 to 30°C;

[0052] In this step, the relative humidity is preferably 60-80 RH%;

[0053] In this step, the steam induction time is 120 to 600 seconds, preferably 180 to 300 seconds.

[0054] (4) immersing the liquid membrane after steam-induced phase separation in a coagulation bath, exchanging the solvent and additives, coagulating into a shape, washing, and drying to obtain a polyvinylidene fluoride microporous filter membrane.

[0055] In this step, the coagulation bath temperature is 20 to 60°C, preferably 20 to 40°C;

[0056] In this step, the coagulation bath treatment time is 2 to 10 minutes, preferably 4 to 8 minutes;

[0057] In this step, the cleaning time is 5 to 20 minutes, preferably 10 to 20 minutes;

[0058] In this step, the drying temperature is 50-90°C, preferably 60-80°C;

[0059] In this step, the drying time is 1 to 10 minutes, preferably 2 to 8 minutes.

[0060] The present invention also provides a polyvinylidene fluoride microporous filter membrane prepared according to the preparation method.

[0061] The present invention is described in detail below by specific examples. It should also be understood that the following examples are only used to specifically illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are also only examples within a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description herein, and are not limited to the specific values ​​​​exemplified below.

[0062] Example 1

[0063] (1) dissolving 60 g of polyvinylidene fluoride in 180 g of N,N-dimethylacetamide, adding 60 g of ethylene glycol dimethyl ether, and stirring at 70° C. for 8 h until the polyvinylidene fluoride is uniformly dissolved to obtain a feed solution;

[0064] The material liquid was cooled to 30°C and kept warm to obtain a casting liquid.

[0065] (2) The casting liquid is coated onto the PES release film and scraped to form a liquid film with a scraping interval of 300 μm.

[0066] (3) The liquid film is placed in a low temperature and low humidity environment for steam-induced phase separation for 180 seconds, wherein the temperature of the low temperature and low humidity environment is 25° C. and the relative humidity is 80 RH%.

[0067] (4) immersing the liquid film after steam-induced phase separation in a coagulation bath at 25° C., wherein the coagulation bath is pure water, for 8 minutes to coagulate and form a gel film;

[0068] The gel membrane was washed with pure water for 10 minutes and then dried at 70° C. for 8 minutes to obtain a polyvinylidene fluoride microporous filter membrane.

[0069] Example 2

[0070] (1) dissolving 54 g of polyvinylidene fluoride in 216 g of N,N-dimethylacetamide, adding 27 g of ethylene glycol dimethyl ether and 3 g of water, stirring at 80° C. for 8 h until the polyvinylidene fluoride is uniformly dissolved to obtain a feed solution;

[0071] The material liquid was cooled to 40°C and kept warm to obtain a casting liquid.

[0072] (2) The casting liquid is coated onto the PES release film and the film is scraped to form a liquid film. The scraping interval is 350 μm.

[0073] (3) The liquid membrane is placed in a low temperature and low humidity environment for steam-induced phase separation for 240 seconds, wherein the temperature of the low temperature and low humidity environment is 20° C. and the relative humidity is 60 RH%.

[0074] (4) immersing the liquid film after steam-induced phase separation in a coagulation bath at 30° C., wherein the coagulation bath is pure water, for 5 minutes to coagulate and form a gel film;

[0075] The gel membrane was washed with pure water for 5 minutes and then dried at 80° C. for 5 minutes to obtain a polyvinylidene fluoride microporous filter membrane.

[0076] Example 3

[0077] (1) dissolving 60 g of polyvinylidene fluoride in 180 g of N,N-dimethylacetamide, adding 30 g of ethylene glycol dimethyl ether and 30 g of diethylene glycol, stirring at 70° C. for 8 h until the polyvinylidene fluoride is uniformly dissolved to obtain a feed solution;

[0078] The material liquid was cooled to 30°C and kept warm to obtain a casting liquid.

[0079] (2) The casting liquid is coated onto the PES release film and the film is scraped to form a liquid film. The scraping interval is 350 μm.

[0080] (3) The liquid membrane is placed in a low temperature and low humidity environment for steam-induced phase separation for 240 seconds, wherein the temperature of the low temperature and low humidity environment is 20° C. and the relative humidity is 70 RH%.

[0081] (4) immersing the liquid film after steam-induced phase separation in a coagulation bath at 40° C., wherein the coagulation bath is pure water, for 10 min to coagulate and form a gel film;

[0082] The gel membrane was washed with pure water for 10 min and then dried at 80° C. for 10 min to obtain a polyvinylidene fluoride microporous filter membrane.

[0083] Comparative Example 1

[0084] The difference between this comparative example and Example 1 is:

[0085] (1) Dissolve 60 g of polyvinylidene fluoride in 180 g of N,N-dimethylacetamide, add 60 g of ethylene glycol dimethyl ether, and stir at 70° C. for 8 h until the polyvinylidene fluoride is evenly dissolved to obtain a casting solution.

[0086] Comparative Example 2

[0087] The difference between this comparative example and Example 1 is:

[0088] (3) The liquid film is placed in a high temperature and high humidity environment (relative conditions) for steam-induced phase separation for 180 seconds, wherein the temperature of the high temperature and high humidity environment is 35° C. and the relative humidity is 85 RH%.

[0089] Comparative Example 3

[0090] The difference between this comparative example and Example 1 is:

[0091] (1) dissolving 60 g of polyvinylidene fluoride in 180 g of N,N-dimethylacetamide, stirring at 70° C. for 8 h, until the polyvinylidene fluoride is evenly dissolved to obtain a feed solution;

[0092] The material liquid was cooled to 30°C and kept warm to obtain a casting liquid.

[0093] Performance Testing

[0094] Bubble point pressure and flux: The bubble point pressure (test liquid is anhydrous ethanol) and flux (test liquid is anhydrous ethanol) of the membranes prepared in Examples 1 to 3 and Comparative Examples 1 to 3 were tested according to "GB / T32361-2015 Separation membrane pore size test method bubble point and average flow method". The test results are shown in Table 1.

[0095] Protein adsorption capacity: The protein adsorption capacity of the membranes prepared in Examples 1 to 3 and Comparative Examples 1 to 3 was detected by the following method:

[0096] The cross section of the film is a sample fractured in liquid nitrogen, and the surface to be observed is gold-plated by a sputtering coater in a vacuum environment. After treatment, the sample is scanned and imaged at an accelerating voltage of 10 kV. The dried transfer film is placed in a protein solution of a certain concentration and statically adsorbed for 24 hours. The change in the absorbance of the solution before and after adsorption is detected, and the amount of protein adsorbed by the film is calculated. The test results are shown in Table 1.

[0097] Microstructure: The microstructure of the membranes prepared in Examples 1 to 3 and Comparative Examples 1 to 3 was observed using an electron scanning microscope. Figures 1 to 6 shown.

[0098] The experimental data and analysis are as follows:

[0099] Table 1 Properties of the films prepared in Examples 1 to 3 and Comparative Examples 1 to 3

[0100]

[0101] It can be seen from Table 1 that the bubble point pressures of the PVDF microporous membranes of Examples 1 to 3 of the present application are all lower than those of the PVDF membranes of Comparative Examples 1 to 3, which indicates that the pore size of the PVDF microporous membrane of the present application is relatively large and it is not easy to form a dense structure on its membrane-forming surface.

[0102] The flux of the PVDF microporous filter membranes of Examples 1 to 3 of the present application is greater than that of the PVDF membranes of Comparative Examples 1 to 3, which indicates that the pore size of the PVDF microporous filter membranes of the present application is relatively large and uniform.

[0103] The protein adsorption amount of the PVDF microporous filter membranes of Examples 1 to 3 of the present application is greater than that of the PVDF membranes of Comparative Examples 1 to 3, which indicates that the PVDF microporous filter membranes of the present application can be used for protein immunoblotting and have a good protein transfer effect.

[0104] In the comparative example 1, when preparing the casting liquid, the material liquid is not subjected to cooling and heat preservation treatment. Due to the high temperature of the material liquid, liquid-liquid phase separation occurs to form the film. Therefore, the final film surface is dense, the membrane has a high bubble point pressure, and the flux is low.

[0105] In comparative example 2, the liquid membrane is subjected to non-solvent vapor induction in a high temperature and high humidity (relative conditions) environment, which accelerates the phase separation of the membrane, causing liquid-liquid phase separation of the membrane, and finally the bubble point pressure of the membrane is relatively high and the flux is low.

[0106] In Comparative Example 3, no additives were added to the casting liquid, resulting in only polyvinylidene fluoride and solvent in the slurry, wherein DMAc is a good solvent for PVDF. Therefore, the state of the casting liquid is very stable relative to that of the casting liquid in Example 1. Furthermore, when induced by low-temperature and low-humidity non-solvent vapor, the liquid membrane cannot undergo phase separation in a short period of time. After the liquid membrane is placed in a coagulation bath, violent liquid-liquid phase separation occurs, resulting in a dense membrane surface, a relatively high bubble point pressure, and a low flux.

[0107] Further, if Figure 1 As shown, spherulites and rod-shaped short fiber crystals are generated on the surface of the PVDF microporous filter membrane in Example 1 of the present application, and there is no dense cortex, so it can be used for protein transfer and the protein transfer effect is better.

[0108] like Figure 2 As shown, spherulites and rod-shaped short fiber crystals are generated on the surface of the PVDF microporous filter membrane in Example 2 of the present application, and there is no dense cortical structure, so it can be used for protein transfer and the protein transfer effect is better.

[0109] like Figure 3 As shown, spherulites and rod-shaped short fiber crystals are generated on the surface of the PVDF microporous filter membrane in Example 3 of the present application, and there is no dense cortical structure, so it can be used for protein transfer and the protein transfer effect is better.

[0110] like Figure 4 As shown, due to the high temperature of the feed liquid, liquid-liquid phase separation occurred to form a film. Therefore, the final film of Comparative Example 1 had less crystals and a denser film surface, which was not suitable for protein transfer.

[0111] like Figure 5 As shown, high temperature and high humidity induction will accelerate the phase separation of the membrane, causing liquid-liquid phase separation of the membrane. The surface of the membrane of Comparative Example 2 does not form a typical crystalline spherical structure, the surface is dense, and is not suitable for protein transfer.

[0112] like Figure 6 As shown, the casting liquid state of Comparative Example 3 is stable. When steam induction is performed, the liquid film cannot be phase-separated in a short time. When the liquid film is placed in a coagulation bath, a violent liquid-liquid phase separation occurs, resulting in a dense membrane surface, which is not suitable for protein transfer.

[0113] In summary, the present invention controls the process conditions such as non-solvent vapor induction temperature and time through appropriate raw material ratios, suitable film-forming temperature, and a simple induction method, so that the film-forming process is controlled, and then a PVDF microporous filter membrane with excellent performance is prepared. The performance is stable and can be effectively applied in the field of protein transfer with good protein transfer effect.

[0114] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A method for preparing a polyvinylidene fluoride microporous filter membrane, characterized in that: The steps include: (1) dissolving polyvinylidene fluoride in a solvent at a first temperature and adding an additive, mixing to obtain a feed liquid, and cooling the feed liquid to a second temperature to obtain a casting liquid; (2) preparing the casting solution to form a liquid film; (3) After the liquid membrane is subjected to steam-induced phase separation, it is immersed in a coagulation bath for coagulation and molding to obtain the polyvinylidene fluoride microporous filter membrane.

2. The preparation method according to claim 1, characterized in that: In the step (1), the first temperature is 40 to 80° C. And / or, the second temperature is 30-60°C.

3. The preparation method according to claim 1, characterized in that: In the feed solution of step (1), the mass fraction of polyvinylidene fluoride is 10 to 30 wt %; and / or, the mass fraction of the solvent is 50 to 80 wt%; And / or, the mass fraction of the additive is 0 to 20 wt%.

4. The preparation method according to claim 1, characterized in that: The solvent in step (1) includes one or more of N,N-dimethylacetamide, N,N-methylformamide, N-methyl-2-pyrrolidone, triethyl phosphate, and 2-pyrrolidone.

5. The preparation method according to claim 1, characterized in that: The additive in step (1) includes one or more of methanol, ethanol, glycerol, isopropanol, n-butanol, diethylene glycol, triethylene glycol, tetraethylene glycol, ethylene glycol methyl ether, ethylene glycol dimethyl ether, and water.

6. The preparation method according to claim 1, characterized in that: The step (3) comprises: placing the liquid membrane in a low temperature and low humidity environment for steam-induced phase separation, wherein the temperature of the low temperature and low humidity environment is 10 to 30° C. and the relative humidity is 40 to 80 RH%.

7. The preparation method according to claim 1, characterized in that: The steam induction time in step (3) is 120 to 600 seconds.

8. The preparation method according to claim 2, characterized in that: The second temperature is 30-50°C.

9. The preparation method according to claim 1, characterized in that: The step (3) comprises: immersing in a coagulation bath for coagulation, washing, and drying to obtain the polyvinylidene fluoride microporous filter membrane.

10. The polyvinylidene fluoride microporous filter membrane obtained according to the preparation method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Polyvinylidene fluoride filter membrane as well as preparation method and application thereof

    CN112495197A

  • Application of symmetric polyvinylidene fluoride micro-filtration membrane and western blotting method

    CN117074665A

  • Preparation method of symmetric polyvinylidene fluoride micro-filtration membrane and micro-filtration membrane prepared by same

    CN117298869A

  • Microfiltration membrane preparation method

    CN117323835A

  • Macroporous polyvinylidene fluoride (PVDF) membranes

    US20190262777A1