Preparation method of potassium ion adsorbent for salt separation mother liquor of chemical high-salt wastewater

By performing multi-step modification of natural clinoptilolite, high-efficiency potassium ion adsorbent is prepared, which solves the problem of purification of high-salt wastewater salt mother liquor in chemical industry, reduces preparation costs and improves efficiency, and realizes effective potassium ions Use.

CN119075906AInactive Publication Date: 2024-12-06XIAN HENGXU TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411456602.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-18
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The prior art has failed to effectively simplify the preparation process of potassium ion adsorbent for chemical high-salt wastewater salt mother liquor, resulting in high cost, low efficiency and difficult product quality, and failure to effectively utilize potassium ion resources in chemical high-salt wastewater.

Method used

By crushing, calcining, adjusting the silicon-aluminum ratio and rare earth modification of natural clinoptilolite, combined with inorganic salt modification, efficient potassium ion adsorbent is prepared, simplifying the process flow, reducing costs, and improving preparation efficiency and purification effect.

Benefits of technology

It has achieved efficient purification of the salt mother liquor of high-salt wastewater in chemical industry, reduced preparation costs, improved process stability and quality control capabilities, and promoted the resource utilization of potassium ions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119075906A_ABST
    Figure CN119075906A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a potassium ion adsorbent for salt separation mother liquor of chemical high-salt wastewater, and belongs to the technical field of environment-friendly water treatment, namely the field of comprehensive utilization of water resources. Comprising the following steps: processing zeolite, namely crushing natural clinoptilolite, sieving, cleaning and drying to obtain treated natural clinoptilolite; roasting: introducing the treated natural clinoptilolite into a roasting device for roasting to obtain activated zeolite; adjusting and modifying the silica-alumina ratio, namely modifying the silica-alumina ratio of the obtained activated zeolite to obtain the silica-alumina ratio adjusted and modified zeolite; rare earth modification: carrying out rare earth modification on the obtained silica-alumina ratio adjusted modified zeolite to obtain rare earth modified zeolite; and preparing a potassium ion adsorbent product, firstly modifying the obtained rare earth modified zeolite with inorganic salt, and then sequentially boiling, cleaning, draining and drying to obtain the potassium ion adsorbent. The method has the advantages of reducing preparation cost and improving preparation efficiency; resource utilization is embodied; the preparation quality is ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of environmental protection water treatment technology and comprehensive utilization of water resources, and specifically relates to a technology for preparing a potassium ion adsorbent for salting mother liquor of chemical high-salt wastewater, especially a method for preparing an adsorbent for removing ions involved in resource utilization of coal chemical high-salt wastewater. Background Art

[0002] Chemical high-salt wastewater refers to: ① Chemical production, incomplete chemical reactions or chemical reaction by-products, especially a large amount of high-COD, high-salt toxic wastewater generated in the production process of chemical products such as coal chemical industry, petrochemical industry, metallurgy, fine chemicals, dyes, pesticides, etc.; ② Wastewater treatment, during the wastewater treatment process, the mineralization brought about by the addition of water treatment agents and acids and alkalis, as well as the concentrated liquid produced by the recovery of most of the "fresh water".

[0003] After the chemical high-salt wastewater passes through the "zero discharge system", concentrated water with a mass fraction of total dissolved solids (TDS) greater than 5% is obtained, which is difficult to biochemically treat; the concentrated water is further treated by a salt separation crystallization process to obtain recyclable by-product salts, namely sodium sulfate Na2SO4 and sodium chloride NaCl; the mother liquor produced by the aforementioned salt separation crystallization process has a salt content greater than 20wt%, mixed with monovalent salts such as potassium nitrate, potassium chloride, sodium chloride, sodium nitrate and other impurities. At present, the common practice in the chemical industry is to evaporate and crystallize the mother liquor to produce miscellaneous salts (i.e. hazardous waste, accounting for 15-20% of the total salt content), and the cost of miscellaneous salt disposal is 2,000-5,000 yuan / ton, which brings a large economic burden to chemical companies.

[0004] Potassium salt refers to natural potassium-containing minerals that are soluble, most of which are easily soluble in water, and their solubility is greater than that of other salts. Since potassium salts are variable (i.e., the potassium ions in the mother liquor of chemical high-salt wastewater are variable), special attention should be paid to changes in temperature and mother liquor composition. In addition, since the potassium salts in the mother liquor are resource-based, hidden, and have complex components, they often bring certain difficulties to separation during the recycling process, resulting in complex processes, high costs, and difficulty in product quality control.

[0005] There is basically no report on the method of separating potassium ions from the brine mother liquor of the above-mentioned chemical high-salt wastewater, while there are relatively more studies on the denitrification and phosphorus removal technology for industrial wastewater.

[0006] Publication number CN112495340A discloses "a method for preparing modified clinoptilolite and a water purifier", which includes the following preparation steps: adding clinoptilolite to a NaCl aqueous solution for oscillation reaction for 3 hours, filtering and dehydrating, and drying; adding clinoptilolite to a lanthanum chloride aqueous solution for oscillation reaction for 3 hours, filtering and dehydrating, and drying; calcining clinoptilolite in a resistance furnace for 8 hours to obtain modified clinoptilolite. The adsorbent prepared by this method is suitable for denitrification and dephosphorization of water bodies. This method does not pay attention to the silicon-aluminum ratio (Si / Al) of clinoptilolite, while an appropriate silicon-aluminum ratio can effectively improve the ability of zeolite to adsorb potassium ions.

[0007] Publication number CN113477211A discloses "a rare earth composite salt-alkali modified zeolite and its preparation method", including the following steps: zeolite is crushed and sieved, mixed with a salt solution of a rare earth metal, filtered, washed and dried after ultrasonic vibration, and the dried zeolite is roasted to obtain a rare earth modified zeolite; the rare earth modified zeolite obtained in the previous step is mixed and soaked with an aqueous solution of alkali, then washed, and then immersed in a magnesium chloride solution, washed and dried to obtain a rare earth composite salt-alkali modified zeolite; the adsorbent prepared by this method is suitable for denitrification and dephosphorization of water bodies. This method also does not pay attention to the silicon-aluminum ratio (Si / Al) of clinoptilolite. In addition, the inorganic salt magnesium chloride is used for soaking and modification, and the adsorption effect on potassium ions is poor, because potassium is an alkali metal, and magnesium is an alkaline earth metal, and there are certain differences in the electronic configuration and chemical properties of the two.

[0008] Publication number CN103464095A discloses "an adsorbent capable of removing potassium ions from traditional Chinese medicine preparations and its application", comprising the following steps: taking clinoptilolite, soaking it in a 5% to 15% sodium chloride solution with a concentration of 5 to 100 times that of the clinoptilolite for 1 to 5 times, each time for 1 to 3 hours, taking out the clinoptilolite, rinsing it with purified water, and drying it to obtain a sodium-rich clinoptilolite; the adsorbent prepared by this method is suitable for adsorbing potassium ions in traditional Chinese medicine preparations, and this method only modifies the clinoptilolite with sodium chloride brine, and has a certain effect on the adsorption of potassium ions in the initial stage, but the adsorption capacity decreases rapidly after multiple regenerations.

[0009] Since there is no technical inspiration in the prior art for preparing potassium ion adsorbent for salting mother liquor of chemical high-salt wastewater with a simplified process flow, relatively low cost and no harsh process elements, the applicant has conducted persistent and beneficial exploration and formed the technical solution to be introduced below. Summary of the invention

[0010] The task of the present invention is to provide a method for preparing a potassium ion adsorbent for salting mother liquor of chemical high-salt wastewater. The method has a concise process flow and no harsh process elements, thereby reducing the preparation cost and improving the preparation efficiency, having a good purification effect on the mother liquor and thus well reflecting the significance of resource utilization, a stable and reliable preparation process and easy control of process elements, thereby ensuring the preparation quality and providing a beneficial channel for resource recycling.

[0011] The task of the present invention is accomplished by a method for preparing a potassium ion adsorbent for a chemical high-salt wastewater salt mother liquor, comprising the following steps:

[0012] A) zeolite processing, crushing the natural clinoptilolite, sieving it, washing it and drying it to obtain the treated natural clinoptilolite;

[0013] B) calcining, introducing the treated natural clinoptilolite obtained in step A) into a calcining device for calcining to obtain activated zeolite;

[0014] C) silicon-aluminum ratio adjustment and modification, modifying the activated zeolite obtained in step B) by silicon-aluminum ratio to obtain silicon-aluminum ratio adjusted modified zeolite;

[0015] D) rare earth modification, performing rare earth modification on the silicon-aluminum ratio-adjusted modified zeolite obtained in step C) to obtain a rare earth modified zeolite;

[0016] E) preparing a potassium ion adsorbent product, firstly modifying the rare earth modified zeolite obtained in step D) with an inorganic salt, then boiling, washing, draining and drying in sequence to obtain a potassium ion adsorbent.

[0017] In a specific embodiment of the present invention, the step A) of crushing the natural clinoptilolite and then sieving it is to crush the natural clinoptilolite and then pass it through a 40-120 mesh sieve, and the washing is to stir and wash the sieved natural clinoptilolite at room temperature, and then precipitate it, filter out the turbid liquid, and place it in an oven for drying until there are no visible suspended impurities, and then control the drying temperature of the oven and the water content of the natural clinoptilolite after drying.

[0018] In another specific embodiment of the present invention, the controlling of the drying temperature of the oven is to control the drying temperature of the oven to 60-100° C.; the controlling of the moisture content of the natural clinoptilolite after drying is to control the moisture content to less than 1%.

[0019] In another specific embodiment of the present invention, the natural clinoptilolite in step A) and step B) is a zeolite having a chemical formula of Na(AlSi5O 12 )·4H2O and the cation is Na + , K + Mainly Ca 2+Next is natural clinoptilolite, whose crystal structure is monoclinic.

[0020] In another specific embodiment of the present invention, the roasting time in step B) is 120-240 minutes, and the roasting temperature is 200-400°C; the roasting device is a roasting furnace, and the roasting furnace is an electric heating furnace, a gas furnace, a coal-fired furnace or an oil-fired furnace.

[0021] In another specific embodiment of the present invention, the silicon-aluminum ratio modification in step C) is a silicon-aluminum molar ratio modification, and the silicon-aluminum molar ratio is SiO2:Al2O3=3-6.

[0022] In a more specific embodiment of the present invention, the silicon-aluminum ratio modification of the activated zeolite obtained in step B) described in step C) is carried out under the action of ultrasound, and the activated zeolite is immersed in an aluminum salt aqueous solution prepared by an aluminizing agent solution in an ultrasonic reaction tank, the ultrasonic reaction time is controlled to be 90-180 min, the ultrasonic reaction temperature is 150-200°C, and the pH value of the aluminum salt aqueous solution is pH=13-14; the aluminum salt aqueous solution is sodium aluminate (NaAlO2), aluminum chloride (AlCl3), aluminum sulfate [Al2(SO4)3] or aluminum nitrate [Al(NO3)3] aqueous solution and has a concentration of 1-2 mol / L, and the frequency of the ultrasonic reaction tank is controlled to be 30-50KHz.

[0023] In a further specific embodiment of the present invention, the rare earth modification described in step D) refers to improvement using a rare earth compound solution, and during the modification process, the silicon-aluminum ratio adjusted modified zeolite is completely immersed in the rare earth compound solution, and is soaked and reacted at 20-30°C for 120-240 minutes; the rare earth compound is a compound containing a rare earth element, and the compound containing a rare earth element is a rare earth chloride, a rare earth nitrate or a rare earth sulfate.

[0024] In yet another specific embodiment of the present invention, the rare earth chloride is a single rare earth salt, which is lanthanum chloride, cerium chloride, praseodymium chloride, neodymium chloride, promethium chloride, yttrium chloride or scandium chloride, and the mass fraction of the single rare earth chloride aqueous solution at room temperature (25°C) is 0.5-1%; the rare earth nitrate is a single rare earth salt, which is lanthanum nitrate, cerium nitrate, praseodymium nitrate, neodymium nitrate, promethium nitrate, yttrium nitrate or scandium nitrate, and the mass fraction of the single rare earth nitrate aqueous solution at room temperature (25°C) is 0.5-1%; the rare earth sulfate is a single rare earth sulfate, which is lanthanum sulfate, cerium sulfate, praseodymium sulfate, neodymium sulfate, yttrium sulfate or scandium sulfate, and the mass fraction of the rare earth sulfate aqueous solution at room temperature (25°C) is 0.5-1%;

[0025] In yet another specific embodiment of the present invention, the inorganic salt modification of the rare earth modified zeolite obtained in step D) in step E) is performed by immersing the rare earth modified zeolite in an inorganic salt solution and boiling the zeolite, wherein the inorganic salt is sodium chloride, ammonium chloride, barium chloride or strontium chloride; the inorganic salt solution is a nearly saturated solution of inorganic salt; the pH value of the nearly saturated solution of inorganic salt is 6-9; the boiling time is 30-60 minutes, and the boiling is cooled to room temperature after boiling, and the boiling and cooling cycles are alternated three times; the cleaning is performed by using a cleaning tank and stirring and cleaning at room temperature; the drying is performed by placing the drained inorganic salt-modified clinoptilolite in an oven and drying it at 60-100°C until the moisture content is less than 1%.

[0026] The technical effects of the technical scheme provided by the present invention are as follows: first, the process flow is very concise and there are no harsh process elements such as high temperature and high pressure reaction, so the preparation cost can be reduced and the preparation efficiency can be improved; second, since the characteristics of the salt mother liquor of chemical high-salt wastewater are comprehensively considered, the purification effect of the mother liquor is good and the significance of resource utilization can be well reflected; third, since the preparation process is stable and reliable and the process elements involved in each step are easy to control, the preparation quality can be guaranteed; fourth, since clinoptilolite is widely available and cheap, and all materials involved in the process also have the advantage of wide sources, it can meet the requirements of industrial scale-up preparation; fifth, since the silicon-aluminum ratio is used for adjustment and modification, for the same type of zeolite, the exchange of potassium ions can be made more efficient through a reasonable silicon-aluminum ratio, thereby improving the ability of the zeolite to adsorb potassium ions; sixth, since the zeolite modified by rare earths coordinates with water in an aqueous solution to form a hydroxylated surface, it is easy to form a surface coordination complex with metal cations, so the adsorption amount can be significantly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 The present invention is a flowchart of the steps for preparing a potassium ion adsorbent for desalting mother liquor of chemical high-salt wastewater. DETAILED DESCRIPTION

[0028] In order to make the purpose, technical solution and advantages of the present invention more clear, the present invention is further described in detail below. However, it should be understood that the description herein is only used to explain the present invention and is not used to limit the scope of the present invention.

[0029] Unless otherwise defined, all technical terms and scientific terms used herein have the same meanings as those generally understood by those skilled in the art of the present invention. The terms used in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The characterization means involved in this article can refer to the relevant descriptions in the prior art and will not be repeated herein.

[0030] In order to further understand the present invention, the following is a detailed description of the high-salt wastewater salt crystallization mother liquor produced by a coal chemical enterprise as a treatment object and combined with specific embodiments.

[0031] The water quality of the salt crystallization mother liquor (i.e. "crystallization mother liquor") of a coal chemical high-salt wastewater is as follows: inert organic matter (inert COD) is 11200 mg / L, TDS is 205600 mg / L, total hardness (calculated as CaCO3) is 1330 mg / L, potassium ion is 3470 mg / L, nitrate is 2860 mg / L, chloride ion is 70840 mg / L, sulfate ion is 49600 mg / L, pH value is 12.7, and total silicon (calculated as SiO2) is 477 mg / L.

[0032] The water quality of the above-mentioned coal chemical wastewater salt crystallization mother liquor contains inert COD, Na + , K + , Ca 2+ Mg 2+ 、NO3 - , Cl - 、SO4 2- In order to eliminate the influence of inert organic matter and nitrate ions on the adsorption and separation effect of potassium ions in a multi-component complex system, the applicant has separately filed a patent application for removing inert organic matter and nitrate ions from the mother liquor.

[0033] Embodiment 1:

[0034] See also Figure 1 , a method for preparing a potassium ion adsorbent for salting mother liquor of chemical high-salt wastewater, the method comprising the following steps:

[0035] A) Zeolite processing, the chemical formula is Na(AlSi5O 12 )·4H2O and the cation is Na + and K + Mainly Ca 2+ The natural clinoptilolite with a second-rate and monoclinic crystal structure is crushed and then passed through an 80-mesh sieve (i.e., "screening", the same below), then repeatedly washed with stirring at room temperature, and then precipitated and filtered in sequence after stirring and washing, so as to remove the turbid liquid by filtering, and then allowed to stand until there are no visible suspended impurities, and finally drained and placed in an oven to dry until the water content of the natural clinoptilolite is less than 1%, and the oven temperature is controlled at 80° C., to obtain the treated natural clinoptilolite;

[0036] B) calcining, introducing the treated natural clinoptilolite obtained in step A) into a calcining furnace such as an electric heating furnace as a calcining device and calcining for 120 minutes at a calcining temperature of 400° C., wherein the heating method of the above calcination is continuous operation and indirect heating, to obtain an activated zeolite;

[0037] C) silicon-aluminum ratio adjustment and modification, the activated zeolite obtained in step B) is modified in silicon-aluminum ratio, and the silicon-aluminum molar ratio is SiO2:Al2O3=6, the silicon-aluminum ratio modification of the activated zeolite is carried out under the action of ultrasound, and the activated zeolite is immersed (i.e., "immersed", the same below) in an aluminum salt aqueous solution prepared by an aluminizing agent solution in an ultrasonic reaction tank, the ultrasonic reaction time is controlled to be 180min, the ultrasonic reaction temperature is 150°C, the pH value of the aluminum salt aqueous solution is Ph=13, the aluminum salt aqueous solution is a sodium aluminate (NaAlO2) aqueous solution with a concentration of 1 mol / L, and the frequency of the ultrasonic reaction tank is controlled to be 30KHz, to obtain a silicon-aluminum ratio adjusted modified zeolite;

[0038] D) rare earth modification, the silicon-aluminum ratio adjusted modified zeolite obtained in step C) is subjected to rare earth modification using a rare earth compound solution to obtain a rare earth modified zeolite, specifically: during the modification process, the silicon-aluminum ratio adjusted modified zeolite is completely immersed (soaked) in the aforementioned rare earth compound solution, and the soaking reaction is carried out at 25° C. for 120 minutes. The rare earth compound used in this embodiment is a compound containing a rare earth element, and the rare earth element-containing compound is a rare earth chloride, and the rare earth chloride is a single rare earth chloride salt. In this embodiment, a lanthanum chloride rare earth chloride salt aqueous solution with a mass fraction of 0.5-1% at room temperature (25° C.) is selected, but any one of the other rare earth chloride salt aqueous solutions listed in the above list by the applicant can also be used;

[0039] E) preparing a potassium ion adsorbent product, firstly modifying the rare earth modified zeolite obtained by step D) with an inorganic salt, then boiling, washing, draining and drying in sequence to obtain a potassium ion adsorbent, that is, obtaining a potassium ion adsorbent of a chemical high-salt wastewater salt mother liquor, wherein the inorganic salt modification described in this step is to immerse the rare earth modified zeolite obtained by step D) in an inorganic salt solution for boiling, wherein the inorganic salt is sodium chloride, and the inorganic salt solution is an inorganic salt nearly saturated solution, and the pH value of the inorganic salt nearly saturated solution is 6; the aforementioned boiling time is 60 minutes, and the boiling is cooled to room temperature after boiling, and then boiled and cooled again after boiling, so that the boiling and cooling cycles are alternated three times, and of course, if more than three alternations or only two alternations, then it is undoubtedly still within the scope of the technical connotation disclosed in the present invention. The washing described in this step is to stir and wash at room temperature, and the drying described in this step is to place the inorganic salt-modified clinoptilolite after draining in an oven and dry it at 80°C until the moisture content is less than 1%.

[0040] Embodiment 2:

[0041] See also Figure 1 , a method for preparing a potassium ion adsorbent for salting mother liquor of chemical high-salt wastewater, the method comprising the following steps:

[0042] A) Zeolite processing, the chemical formula is Na(AlSi5O 12 )·4H2O and the cation is Na + and K + Mainly Ca 2+ The natural clinoptilolite with a second-rate and monoclinic crystal structure is crushed and then passed through a 40-mesh sieve (i.e., "screening", the same below), then repeatedly stirred and washed at room temperature, and then precipitated and filtered in sequence after stirring and washing, so as to remove the turbid liquid by filtering, and then allowed to stand until there are no visible suspended impurities, and finally drained and placed in an oven to dry until the water content of the natural clinoptilolite is less than 1%, and the oven temperature is controlled at 60° C., to obtain the treated natural clinoptilolite;

[0043] B) calcination, introducing the treated natural clinoptilolite obtained in step A) into a calcination furnace such as a gas furnace as a calcination device and calcining for 180 minutes at a temperature of 300° C., wherein the heating method of the calcination is continuous operation and indirect heating, to obtain an activated zeolite;

[0044] C) silicon-aluminum ratio adjustment and modification, the activated zeolite obtained in step B) is modified in silicon-aluminum ratio, and the silicon-aluminum molar ratio is SiO2:Al2O3=5, the silicon-aluminum ratio modification of the activated zeolite is carried out under the action of ultrasound, and the activated zeolite is immersed (i.e., "immersed", the same below) in an aluminum salt aqueous solution prepared by an aluminizing agent solution in an ultrasonic reaction tank, the ultrasonic reaction time is controlled to be 135min, the ultrasonic reaction temperature is 180°C, the pH value of the aluminum salt aqueous solution is Ph=14, the aluminum salt aqueous solution is an aluminum chloride (AlCl3) aqueous solution with a concentration of 2mol / L, and the frequency of the ultrasonic reaction tank is controlled to be 40KHz, to obtain a silicon-aluminum ratio adjusted modified zeolite;

[0045] D) rare earth modification, the silicon-aluminum ratio adjusted modified zeolite obtained in step C) is subjected to rare earth modification using a rare earth compound solution to obtain a rare earth modified zeolite, specifically: during the modification process, the silicon-aluminum ratio adjusted modified zeolite is completely immersed (soaked) in the aforementioned rare earth compound solution, and the soaking reaction is carried out at 20° C. for 240 min. The rare earth compound used in this embodiment is a compound containing a rare earth element, and the rare earth element-containing compound is a rare earth nitrate, and the rare earth nitrate is a single rare earth nitrate. In this embodiment, a lanthanum nitrate rare earth nitrate aqueous solution with a mass fraction of 0.5-1% at room temperature (25° C.) is selected, but any one of the other rare earth nitrate aqueous solutions listed in the above list by the applicant can also be used;

[0046] E) preparing a potassium ion adsorbent product, firstly modifying the rare earth modified zeolite obtained by step D) with an inorganic salt, then boiling, washing, draining and drying in sequence to obtain a potassium ion adsorbent, that is, obtaining a potassium ion adsorbent of a chemical high-salt wastewater salt mother liquor, wherein the inorganic salt modification described in this step is to immerse the rare earth modified zeolite obtained by step D) in an inorganic salt solution for boiling, wherein the inorganic salt is ammonium chloride, and the inorganic salt solution is an inorganic salt nearly saturated solution, and the pH value of the inorganic salt nearly saturated solution is 9; the aforementioned boiling time is 50 minutes, and the boiling is cooled to room temperature after boiling, and then boiled and cooled again after boiling, so that the boiling and cooling cycles are alternated three times, and of course, if more than three alternations or only two alternations, then it is undoubtedly still within the scope of the technical connotation disclosed in the present invention. The washing described in this step is to stir and wash at room temperature, and the drying described in this step is to place the inorganic salt-modified clinoptilolite after draining in an oven and dry it at 60°C until the moisture content is less than 1%.

[0047] Embodiment 3:

[0048] See also Figure 1 , a method for preparing a potassium ion adsorbent for salting mother liquor of chemical high-salt wastewater, the method comprising the following steps:

[0049] A) Zeolite processing, the chemical formula is Na(AlSi5O 12 )·4H2O and the cation is Na + and K + Mainly Ca 2+ The natural clinoptilolite with a second-rate and monoclinic crystal structure is crushed and then passed through a 120-mesh sieve (i.e., "screening", the same below), then repeatedly washed with stirring at room temperature, and then precipitated and filtered in sequence after stirring and washing, so as to remove the turbid liquid by filtering, and then allowed to stand until there are no visible suspended impurities, and finally drained and placed in an oven to dry until the water content of the natural clinoptilolite is less than 1%, and the oven temperature is controlled at 100° C., to obtain the treated natural clinoptilolite;

[0050] B) calcination, introducing the treated natural clinoptilolite obtained in step A) into a calcination furnace such as an oil-fired furnace as a calcination device and calcining for 240 minutes at a temperature of 200° C., wherein the heating method of the calcination is continuous operation and indirect heating, to obtain an activated zeolite;

[0051] C) silicon-aluminum ratio adjustment and modification, the activated zeolite obtained in step B) is modified in silicon-aluminum ratio, and the silicon-aluminum molar ratio is SiO2:Al2O3=3, the silicon-aluminum ratio modification of the activated zeolite is carried out under the action of ultrasound, and the activated zeolite is immersed (i.e., "immersed", the same below) in an aluminum salt aqueous solution prepared by an aluminizing agent solution in an ultrasonic reaction tank, the ultrasonic reaction time is controlled to be 90 minutes, the ultrasonic reaction temperature is 200°C, the pH value of the aluminum salt aqueous solution is Ph=13, the aluminum salt aqueous solution is an aluminum nitrate [Al(NO3)3] aqueous solution with a concentration of 1.5 mol / L, the frequency of the ultrasonic reaction tank is controlled to be 50KHz, and the silicon-aluminum ratio adjusted modified zeolite is obtained;

[0052] D) rare earth modification, the silicon-aluminum ratio adjusted modified zeolite obtained in step C) is subjected to rare earth modification using a rare earth compound solution to obtain a rare earth modified zeolite, specifically: during the modification process, the silicon-aluminum ratio adjusted modified zeolite is completely immersed (soaked) in the aforementioned rare earth compound solution, and the soaking reaction is carried out at 22° C. for 200 min. The rare earth compound used in this embodiment is a compound containing a rare earth element, and the rare earth element-containing compound is a rare earth sulfate, and the rare earth sulfate is a single rare earth sulfate. In this embodiment, a lanthanum sulfate rare earth sulfate aqueous solution with a mass fraction of 0.5-1% at room temperature (25° C.) is selected, but any one of the other rare earth sulfate aqueous solutions listed in the above list by the applicant can also be used;

[0053] E) preparing a potassium ion adsorbent product, firstly modifying the rare earth modified zeolite obtained by step D) with an inorganic salt, then boiling, washing, draining and drying in sequence to obtain a potassium ion adsorbent, that is, obtaining a potassium ion adsorbent of a chemical high-salt wastewater salt mother liquor, wherein the inorganic salt modification described in this step is to immerse the rare earth modified zeolite obtained by step D) in an inorganic salt solution for boiling, wherein the inorganic salt is barium chloride, and the inorganic salt solution is an inorganic salt nearly saturated solution, and the pH value of the inorganic salt nearly saturated solution is 7; the aforementioned boiling time is 40 minutes, and the boiling is cooled to room temperature after boiling, and then boiled and cooled again after boiling, so that the boiling and cooling cycles are alternated three times, and of course, if more than three alternations or only two alternations, then it is undoubtedly still within the scope of the technical connotation disclosed in the present invention. The washing described in this step is to stir and wash at room temperature, and the drying described in this step is to place the inorganic salt-modified clinoptilolite after draining in an oven and dry it at 75°C until the moisture content is less than 1%.

[0054] Embodiment 4:

[0055] See also Figure 1 , a method for preparing a potassium ion adsorbent for salting mother liquor of chemical high-salt wastewater, the method comprising the following steps:

[0056] A) Zeolite processing, the chemical formula is Na(AlSi5O 12 )·4H2O and the cation is Na + and K + Mainly Ca 2+ The natural clinoptilolite with a second-order and monoclinic crystal structure is crushed and passed through a 100-mesh sieve (i.e., "screening", the same below), and then repeatedly washed with stirring at room temperature, and then precipitated and filtered in sequence after stirring and washing, so as to remove the turbid liquid by filtering, and then allowed to stand until there are no visible suspended impurities, and finally drained and placed in an oven to dry until the water content of the natural clinoptilolite is less than 1%, and the oven temperature is controlled at 90° C., to obtain the treated natural clinoptilolite;

[0057] B) calcination, introducing the treated natural clinoptilolite obtained in step A) into a calcination furnace such as a coal-fired furnace as a calcination device and calcining for 210 minutes at a temperature of 250° C., wherein the heating method of the calcination is continuous operation and indirect heating, to obtain an activated zeolite;

[0058] C) silicon-aluminum ratio adjustment and modification, the activated zeolite obtained in step B) is modified in silicon-aluminum ratio, and the silicon-aluminum molar ratio is SiO2:Al2O3=4, the silicon-aluminum ratio modification of the activated zeolite is carried out under the action of ultrasound, and the activated zeolite is immersed (i.e., "immersed", the same below) in an aluminum salt aqueous solution prepared by an aluminizing agent solution in an ultrasonic reaction tank, the ultrasonic reaction time is controlled to be 160 min, the ultrasonic reaction temperature is 165°C, the pH value of the aluminum salt aqueous solution is Ph=14, the aluminum salt aqueous solution is an aluminum sulfate [Al2(SO4)3] aqueous solution with a concentration of 1 mol / L, and the frequency of the ultrasonic reaction tank is controlled to be 50KHz, to obtain a silicon-aluminum ratio adjusted modified zeolite;

[0059] D) rare earth modification, the silicon-aluminum ratio adjusted modified zeolite obtained in step C) is subjected to rare earth modification using a rare earth compound solution to obtain a rare earth modified zeolite, specifically: during the modification process, the silicon-aluminum ratio adjusted modified zeolite is completely immersed (soaked) in the aforementioned rare earth compound solution, and the soaking reaction is carried out at 28° C. for 150 minutes. The rare earth compound used in this embodiment is a compound containing a rare earth element, and the rare earth element-containing compound is a rare earth chloride, and the rare earth chloride is a single rare earth chloride salt. In this embodiment, a yttrium chloride rare earth chloride salt aqueous solution with a mass fraction of 0.5-1% at room temperature (25° C.) is selected, but any one of the other rare earth chloride salt aqueous solutions listed in the above list by the applicant can also be used;

[0060] E) preparing a potassium ion adsorbent product, firstly modifying the rare earth modified zeolite obtained by step D) with an inorganic salt, then boiling, washing, draining and drying in sequence to obtain a potassium ion adsorbent, that is, obtaining a potassium ion adsorbent of a chemical high-salt wastewater salt mother liquor, wherein the inorganic salt modification described in this step is to immerse the rare earth modified zeolite obtained by step D) in an inorganic salt solution for boiling, wherein the inorganic salt is strontium chloride, and the inorganic salt solution is an inorganic salt nearly saturated solution, and the pH value of the inorganic salt nearly saturated solution is 8; the aforementioned boiling time is 30 minutes, and the boiling is cooled to room temperature after boiling, and then boiled and cooled again after boiling, so that the boiling and cooling cycles are alternated three times, and of course, if more than three alternations or only two alternations, then it is undoubtedly still within the scope of the technical connotation disclosed in the present invention. The washing described in this step is to stir and wash at room temperature, and the drying described in this step is to place the inorganic salt-modified clinoptilolite after draining in an oven and dry it at 100°C until the moisture content is less than 1%.

[0061] The potassium ion adsorbent prepared in the above Examples 1 to 4 has the technical effects shown in the following table on the treatment of the salt crystallization mother liquor of a coal chemical high-salt wastewater.

[0062]

[0063] The above description is only a preferred embodiment of the present invention. It should be pointed out that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as within the scope of protection of the present invention.

Claims

1. A method for preparing a potassium ion adsorbent for salting mother liquor of chemical high-salt wastewater, characterized in that: The following steps are involved: A) zeolite processing, crushing the natural clinoptilolite, sieving it, washing it and drying it to obtain the treated natural clinoptilolite; B) calcining, introducing the treated natural clinoptilolite obtained in step A) into a calcining device for calcining to obtain activated zeolite; C) silicon-aluminum ratio adjustment and modification, modifying the activated zeolite obtained in step B) by silicon-aluminum ratio to obtain silicon-aluminum ratio adjusted modified zeolite; D) rare earth modification, performing rare earth modification on the silicon-aluminum ratio-adjusted modified zeolite obtained in step C) to obtain a rare earth modified zeolite; E) preparing a potassium ion adsorbent product, firstly modifying the rare earth modified zeolite obtained in step D) with an inorganic salt, then boiling, washing, draining and drying in sequence to obtain a potassium ion adsorbent.

2. The method for preparing a potassium ion adsorbent for salting mother liquor of chemical high-salt wastewater according to claim 1, characterized in that: The step A) of crushing the natural clinoptilolite and then sieving it is to crush the natural clinoptilolite and then pass it through a 40-120 mesh sieve, and the cleaning is to stir and clean the sieved natural clinoptilolite at room temperature, then precipitate it, filter out the turbid liquid, and let it stand until there are no visible suspended impurities, and then place it in an oven for drying, and control the drying temperature of the oven and the water content of the dried natural clinoptilolite.

3. The method for preparing a potassium ion adsorbent for salting mother liquor of chemical high-salt wastewater according to claim 2, characterized in that: The controlling of the drying temperature of the oven is to control the drying temperature of the oven to 60-100° C.; the controlling of the moisture content of the natural clinoptilolite after drying is to control the moisture content to less than 1%.

4. The method for preparing a potassium ion adsorbent for salting mother liquor of chemical high-salt wastewater according to claim 1, characterized in that: The natural clinoptilolite described in step A) and step B) is a zeolite having a chemical formula of Na(AlSi5O 12 )·4H2O and the cation is Na + , K + Mainly Ca 2+ Next is natural clinoptilolite, whose crystal structure is monoclinic.

5. The method for preparing a potassium ion adsorbent for salting mother liquor of chemical high-salt wastewater according to claim 1, characterized in that: The roasting time in step B) is 120-240 minutes, and the roasting temperature is 200-400° C. The roasting device is a roasting furnace, and the roasting furnace is an electric heating furnace, a gas furnace, a coal-fired furnace or an oil-fired furnace.

6. The method for preparing a potassium ion adsorbent for salting mother liquor of chemical high-salt wastewater according to claim 1, characterized in that: The silicon-aluminum ratio modification described in step C) is a silicon-aluminum molar ratio modification, and the silicon-aluminum molar ratio is SiO2:Al2O3=3-6.

7. The method for preparing a potassium ion adsorbent for salting mother liquor of chemical high-salt wastewater according to claim 1, characterized in that: The silicon-aluminum ratio modification of the activated zeolite obtained in step B) in step C) is carried out under the action of ultrasound, and the activated zeolite is immersed in an aluminum salt aqueous solution prepared from an aluminizing agent solution in an ultrasonic reaction tank, the ultrasonic reaction time is controlled to be 90-180 minutes, the ultrasonic reaction temperature is 150-200° C., the pH value of the aluminum salt aqueous solution is pH=13-14; the aluminum salt aqueous solution is sodium metaaluminate, aluminum chloride, aluminum sulfate or aluminum nitrate aqueous solution and has a concentration of 1-2 mol / L, and the frequency of the ultrasonic reaction tank is controlled to be 30-50 KHz.

8. The method for preparing a potassium ion adsorbent for salting mother liquor of chemical high-salt wastewater according to claim 1, characterized in that: The rare earth modification described in step D) refers to the improvement using a rare earth compound solution, and during the modification process, the silicon-aluminum ratio adjusted modified zeolite is completely immersed in the rare earth compound solution and soaked for reaction at 20-30°C for 120-240 minutes; the rare earth compound is a compound containing a rare earth element, and the compound containing a rare earth element is a rare earth chloride, a rare earth nitrate or a rare earth sulfate.

9. The method for preparing a potassium ion adsorbent for salting mother liquor of chemical high-salt wastewater according to claim 8, characterized in that: The rare earth chloride is a single rare earth salt, which is lanthanum chloride, cerium chloride, praseodymium chloride, neodymium chloride, promethium chloride, yttrium chloride or scandium chloride, and the mass fraction of the single rare earth chloride aqueous solution at room temperature is 0.5-1%; the rare earth nitrate is a single rare earth salt, which is lanthanum nitrate, cerium nitrate, praseodymium nitrate, neodymium nitrate, promethium nitrate, yttrium nitrate or scandium nitrate, and the mass fraction of the single rare earth nitrate aqueous solution at room temperature is 0.5-1%; the rare earth sulfate is a single rare earth sulfate, which is lanthanum sulfate, cerium sulfate, praseodymium sulfate, neodymium sulfate, yttrium sulfate or scandium sulfate, and the mass fraction of the rare earth sulfate aqueous solution at room temperature is 0.5-1%.

10. The method for preparing a potassium ion adsorbent for salting mother liquor of chemical high-salt wastewater according to claim 1, characterized in that: The step E) of modifying the rare earth modified zeolite obtained in step D) with an inorganic salt comprises immersing the rare earth modified zeolite in an inorganic salt solution and boiling the solution, wherein the inorganic salt is sodium chloride, ammonium chloride, barium chloride or strontium chloride; and the inorganic salt solution is a nearly saturated solution of the inorganic salt; The pH value of the inorganic salt nearly saturated solution is 6-9; the boiling time is 30-60 minutes, and the solution is cooled to room temperature after boiling, and the boiling and cooling cycles are alternated three times; the cleaning is performed in a cleaning tank and stirred at room temperature; the drying is performed by placing the drained inorganic salt-modified clinoptilolite in an oven and drying it at 60-100°C until the moisture content is less than 1%.