Preparation method and application of metal titanium-based composite piezoelectric catalytic membrane

By adopting the preparation method of metal titanium-based composite piezoelectric catalytic film in traditional membrane separation technology, the piezoelectric effect is used to produce reactive oxygen species, which solves the problems of membrane pollution and high energy consumption, and realizes the self-cleaning of the membrane and improves energy efficiency. Suitable for removal of micro-contaminants in water treatment.

CN119075968APending Publication Date: 2024-12-06DALIAN MARITIME UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411114981.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

There are problems of membrane pollution and high energy consumption in traditional membrane separation technology, which is difficult to expand on a large scale, and the energy consumption problems caused by existing electrocatalytic film processes have not been effectively solved.

Method used

The preparation method of metal titanium-based composite piezoelectric catalytic film is adopted to achieve the membrane by pretreatment of porous titanium-based film, growth of nano-titanium dioxide layer and formation of barium titanate layer by piezoelectric effect. Self-cleaning and energy efficiency improvement.

Benefits of technology

It realizes efficient removal of membrane pollution and reduces energy consumption, and provides a controllable and easy-to-scale water treatment solution, combining excellent water treatment capabilities and self-cleaning and anti-pollution function.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004993375400000011
    Figure HDA0004993375400000011
  • Figure HDA0004993375400000012
    Figure HDA0004993375400000012
Patent Text Reader

Abstract

The invention provides a preparation method and application of a metal titanium-based composite piezoelectric catalytic membrane, and the preparation method mainly comprises the following process steps: by taking a metal titanium membrane as a substrate, carrying out organic solvent cleaning and chemical reagent etching, and carrying out pretreatment on the surface and pore channels of the metal titanium-based composite membrane; and then, growing a titanium dioxide layer on the surface of the film in situ to obtain the titanium dioxide / titanium-based composite film. The titanium dioxide layer is converted into a barium titanate layer with a piezoelectric property through further chemical reaction, so that the barium titanate / titanium-based composite piezoelectric catalytic film is obtained. The coupling piezoelectric catalytic reaction is applied to water purification treatment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of novel membrane materials, and specifically relates to a preparation method and application of a metal titanium-based composite piezoelectric catalytic membrane. Background Art

[0002] Membrane separation technology is widely used in water treatment due to its high efficiency, energy saving and easy operation. However, the emergence of membrane fouling has become a key technical bottleneck in the development of membrane separation technology. With the accumulation of membrane fouling during operation, the flux and treatment efficiency of the membrane will decrease significantly, thereby affecting the overall performance of the membrane. The current membrane fouling mitigation methods are mainly physical backwashing and chemical cleaning. Although they can alleviate membrane fouling to a certain extent, they still need to introduce additional equipment and chemical reagents. This process will inevitably increase membrane loss, increase the operating cycle and economic cost.

[0003] In order to alleviate the membrane fouling problem in the membrane process, researchers have modified the membrane materials and further coupled advanced oxidation technology to improve the overall performance of the membrane. In recent years, electrocatalytic membrane technology has emerged, integrating membrane filtration with electrochemical advanced oxidation technology to achieve an integrated electrofiltration process. The active substances and electrical repulsion characteristics generated in the electrochemical process can effectively remove small molecule pollutants and alleviate membrane fouling. However, the electrochemical process introduced in the process inevitably caused researchers to think about energy consumption issues. If this problem can be effectively solved, it will provide support for the further development of membrane separation technology.

[0004] Based on the above problems, piezoelectric catalytic materials have attracted extensive attention from researchers because they can produce active substances only under the stimulation of external mechanical forces such as ultrasound. If piezoelectric catalytic materials can be prepared into membranes, the resulting piezoelectric catalytic membranes can generate piezoelectric voltages driven by the inherent water pressure in the membrane process, which is expected to alleviate both membrane pollution and energy consumption problems, thereby achieving the unification of membrane separation process and anti-membrane pollution process.

[0005] Titanium-based membranes have been widely commercialized. They have good electrical conductivity, high mechanical strength, acid and alkali resistance, and corrosion resistance, and are one of the excellent membrane carriers for constructing piezoelectric catalytic membranes. However, there are relatively few studies on modifying piezoelectric materials on titanium-based membranes and further applying them to water treatment. Summary of the invention

[0006] The purpose of the present invention is to provide a preparation method and application of a metal titanium-based composite piezoelectric catalytic membrane, aiming to overcome many problems in traditional membrane water treatment processes, including membrane pollution, high energy consumption, and difficulty in large-scale expansion.

[0007] To achieve this goal, the technical solution provided by the present invention is as follows:

[0008] A method for preparing a metal titanium-based composite piezoelectric catalytic film comprises the following steps:

[0009] (1) First, a porous titanium-based membrane material is used as a substrate and pretreated by organic solvent cleaning and chemical reagent etching in sequence;

[0010] (2) Subsequently, a nano-titanium dioxide layer is grown on the surface of the pretreated porous titanium-based membrane to obtain a titanium dioxide / titanium-based composite membrane;

[0011] (3) After the catalytic film is fully dried, the titanium dioxide / titanium-based composite film prepared in step (2) is used as a substrate to react titanium dioxide to generate barium titanate, thereby obtaining the barium titanate / titanium-based composite piezoelectric catalytic film.

[0012] Furthermore, the organic solvent involved in step (1) can be selected from a mixture of one or more of acetone, methanol, ethanol, isopropanol and N,N-dimethylformamide. The cleaning time is 5 to 30 minutes. The purpose of this cleaning step is to remove impurities on the membrane surface.

[0013] Furthermore, the chemical reagent involved in the chemical reagent etching in step (1) is an alkaline reagent (one or a mixture of aqueous solutions of sodium hydroxide and potassium hydroxide) or an acidic reagent (a mixture of one or more of oxalic acid solution and citric acid solution), the solution concentration is 0.01mM to saturated concentration, and the etching time is 5 to 120min. The purpose of this step is to oxidatively etch the surface of the titanium-based film to increase its reaction activity.

[0014] Furthermore, in step (1), the configuration of the porous titanium-based membrane material involved includes one of a tubular, plate, hollow plate and hollow fiber membrane, wherein the pore size of the membrane is 0.2 to 10.0 μm, and the porosity is 20% to 60%.

[0015] Furthermore, in step (1), the pretreatment method used may be immersion and ultrasonic assisted cleaning.

[0016] Furthermore, in step (2), the growth method of the nano titanium dioxide is one of an anodic oxidation method, an electrolytic deposition method, a sol-gel method and a solvent (including water) thermal method. The process parameters of the anodic oxidation method are as follows: the electrolyte composition is a mixed solution of NH4F, water and ethanol, and the mass percentage is: NH4F is 0.25-5%, water is 0.1-30% and ethylene glycol is the balance; the oxidation voltage is 10-80V; the oxidation time is 1-300min; the process parameters of the electrolytic deposition method are: the current density is 1-50mA / cm 2, the electrolyte is one of titanium trichloride, potassium titanate and sodium titanate, the solvent is one of water, ethanol and ethylene glycol, the concentration is 0.01-0.5M, the reaction temperature is room temperature-80°C, the reaction time is 10min-2h, and the pH is 1-7; the sol-gel method is specifically as follows: the titanium dioxide / titanium-based composite film obtained in step (2) is immersed in a precursor solution for a certain period of time, dried, and then calcined in an air atmosphere; wherein the precursor in the precursor solution is one of titanium trichloride, potassium titanate and sodium titanate, the concentration of the precursor is 0.1-1M), the solvent is one of ethanol, acetone and isopropanol, and the precursor solution The method comprises the following steps: containing water, wherein the volume ratio of water to solvent is 1:1 to 1:100, the precursor solution contains a catalyst, wherein the catalyst is one of hydrochloric acid or nitric acid, and the concentration of the catalyst is 1 to 100 mM, the immersion temperature is room temperature to 80°C, the time is 10 min to 24 h, the calcination temperature is 300 to 700°C, and the calcination time is 1 to 5 h; the process parameters of the solvent (including water) thermal method are as follows: one of titanium trichloride, potassium titanate and sodium titanate is used as the reactant, the concentration of the reactant is 0.01 to 1 M, the solvent is one of water, ethanol and ethylene glycol, the solvent (including water) thermal temperature is 100 to 250°C, and the reaction time is 2 to 24 h.

[0017] Furthermore, in step (3), the method for generating barium titanate by reaction includes a solid phase calcination synthesis method and a solvent thermal method. The solid phase calcination synthesis method is specifically as follows: the titanium dioxide / titanium-based composite film obtained in step (2) is immersed in a barium nitrate solution for 1 to 6 hours, the solvent is one of methanol, ethanol and acetone, and after drying, it is transferred to a crucible, and kept constant at 500 to 600°C in an air atmosphere for 1 to 10 hours, and then continued to calcine at 800 to 1200°C for 5 to 15 hours to obtain the barium titanate / titanium-based composite piezoelectric catalytic film; wherein the titanium dioxide / titanium-based composite film is immersed in a barium nitrate solution at a mass ratio of 1:1 to 1:100, and the concentration of the barium nitrate solution is 0.1 to 10M, preferably 0.1~1M; the specific solvent (including water) thermal method is: immersing the titanium dioxide / titanium-based composite film of step (2) in a barium source solution for 1-6h, the barium source is one of barium hydroxide or barium nitrate, the solvent is one of water, ethanol, and ethylene glycol, and the titanium dioxide / titanium-based composite film is immersed in the barium source solution at a mass ratio of 1:1 to 1:100, and the concentration of the barium source solution is 0.1~1M; then reacting at 150~300℃ for 5~20h, naturally cooling to room temperature and then taking out, washing with deionized water for 3~5 times, and drying to obtain the barium titanate / titanium-based composite piezoelectric catalytic film.

[0018] The present invention also relates to a metal titanium-based composite piezoelectric catalytic film prepared by the above preparation method.

[0019] The present invention also relates to the application of the above-mentioned metal titanium-based composite piezoelectric catalytic membrane in water treatment, including the deep purification of micro-pollutants in water bodies, and is particularly suitable for treating low-concentration organic wastewater such as 5-20 mg / L dyes, antibiotics, endocrine disruptors and pesticides to achieve their deep treatment.

[0020] Furthermore, during the treatment process, the catalytic membrane undergoes a piezoelectric catalytic reaction under the action of mechanical force, generating active oxygen species, which oxidatively degrade organic pollutants on the membrane surface and in the pores, achieving efficient removal of pollutants and achieving a self-cleaning and anti-pollution effect of the membrane.

[0021] Furthermore, the mechanical force includes periodic pulse water pressure, ultrasound, water flow impact, and swinging of the membrane in water (hollow fiber membrane).

[0022] Furthermore, the active oxygen species can be generated by direct piezoelectric catalysis, or by coupling persulfate activation, photocatalysis, catalytic ozone and catalytic Fenton processes.

[0023] The present invention provides an innovative method for preparing a metal titanium-based composite piezoelectric catalytic film, by cleaning with an organic solvent and etching with a chemical reagent, thereby pre-treating the surface and pores of the metal titanium-based composite film. Subsequently, a titanium dioxide layer is grown in situ to obtain a titanium dioxide / titanium-based composite film. After further chemical reactions, the titanium dioxide layer is converted into a barium titanate layer with piezoelectric properties, thereby obtaining a barium titanate / titanium-based composite piezoelectric catalytic film. The process of this method is controllable, ensuring good uniformity and orderliness, and it is also easier to prepare on a large scale, so it has significant industrial application prospects. In addition, without the coupling of additional technologies or the introduction of chemical reagents, active oxygen species are generated through the piezoelectric catalytic process to remove small molecular pollutants in the water body, thereby having both excellent water treatment capabilities and self-cleaning and anti-pollution functions, and being able to deeply remove micropollutants in the water body, providing strong support for the sustainable management of membrane pollution.

[0024] The beneficial effects of the present invention are

[0025] (1) The titanium-based composite piezoelectric catalytic film provided by the present invention is simple to prepare and has a controllable process. The piezoelectric catalytic layer formed is in-situ grown, has uniformity and order, and is easy to scale up for preparation and practical application;

[0026] (2) The titanium-based composite piezoelectric catalytic membrane provided by the present invention can effectively alleviate the membrane pollution problem and energy consumption problem in the traditional membrane separation process, and realize the membrane catalytic process without introducing additional technology or adding chemical reagents. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 Schematic diagram of the preparation process of the titanium-based composite piezoelectric catalytic film;

[0028] Figure 2 Schematic diagram of the piezoelectric catalytic process. DETAILED DESCRIPTION

[0029] The following non-limiting embodiments may enable a person skilled in the art to more fully understand the present invention, but are not intended to limit the present invention in any way.

[0030] Example 1

[0031] A three-hole hollow plate titanium membrane with a length of 10 cm, a width of 5 cm, and a thickness of 3 cm was selected. At the same time, the diameter of the hollow channel was 1 cm, the membrane pore size was 2.2 μm, and the porosity was 28.6%. First, the membrane was placed in methanol for ultrasonic cleaning for 15 minutes, and then immersed in a 10mM citric acid solution for 5 minutes. Further, titanium dioxide was deposited on the surface of the hollow plate titanium membrane by an electrodeposition process. The deposition liquid was a 0.1M titanium trichloride aqueous solution. The pH value was adjusted to 3 using hydrochloric acid and sodium bicarbonate. The deposition voltage was 10 mA / cm 2 , the deposition time is 15min, and a titanium film material with a titanium dioxide layer on the surface is obtained. Further, barium titanate is grown in situ by combining the hydrothermal method to prepare a barium titanate / titanium-based composite piezoelectric catalytic membrane, wherein barium nitrate is used as a reactant, and the titanium film material with a titanium dioxide layer on the surface is immersed in a barium nitrate aqueous solution for 1h, and then transferred to a polytetrafluoroethylene reactor for hydrothermal reaction. After the reaction, it is naturally cooled to room temperature and taken out, washed with deionized water 5 times, and dried to obtain the barium titanate / titanium-based composite piezoelectric catalytic membrane; wherein the mass ratio of the hollow plate titanium dioxide / titanium-based membrane material to the barium nitrate aqueous solution is 1:20, the concentration of barium nitrate is 0.5M, the hydrothermal temperature is 180°C, and the hydrothermal time is 16h. Driven by the pressure of a peristaltic pump (100kPa), the piezoelectric catalytic process of the obtained membrane achieves a removal effect of more than 95% of 250mL of phenol (5mg / L) within 60min, and its flux can reach 1660.2L / m 2 In addition, the membrane still maintained a removal capacity of more than 85% after 7 days of long-term operation, showing good piezoelectric catalytic performance.

[0032] Example 2

[0033] A hollow fiber titanium membrane with a length of 15 cm was selected, with an outer diameter of 2 mm, an inner diameter of 1 mm, a membrane pore size of 1.4 μm, and a porosity of 34.8%. First, the membrane was placed in acetone for ultrasonic cleaning for 10 min, and then immersed in a 5 mM oxalic acid solution for 20 min. Further, the hollow fiber titanium membrane was immersed in an isopropanol solution of 0.2 M potassium titanate (water and hydrochloric acid were added to the isopropanol solution, the volume ratio of water to solvent isopropanol was 2:10, and the concentration of hydrochloric acid was 50 mM) for 20 min, taken out and dried, and then placed in a muffle furnace for calcination at 500 ° C for 3 h, forming a hollow fiber titanium membrane with a titanium dioxide layer on the surface. The composite membrane prepared above was further immersed in a mixed solution of barium nitrate and acetone (barium nitrate concentration is 0.8M) for 3 hours, wherein the mass ratio of the composite membrane to the mixed solution of barium nitrate and acetone was 1:15, and then transferred to a crucible after rotary evaporation at room temperature until completely dry, and kept constant temperature in air atmosphere at 500°C for 3 hours, and then continued to calcine at 1000°C for 3 hours to obtain a barium titanate / titanium-based composite piezoelectric catalytic membrane. Under the action of an ultrasonic cleaning machine with a power of 180W and a frequency of 40kHz, the piezoelectric catalytic process of the obtained membrane achieved a 100% removal effect on 100mL of methylene orange (10mg / L) within 30 minutes. Moreover, under the same operating conditions, even in the presence of 10mg / L humic acid, the removal rate of methylene orange by the membrane piezoelectric catalytic process remained above 80%, and its flux changed little, only from 2450.3L / m 2 h bar dropped to 2320.5L / m 2 h bar, showing good anti-pollution ability.

[0034] Example 3

[0035] A tubular titanium membrane with a length of 20 cm was selected, with an outer diameter of 10 mm, an inner diameter of 5 mm, a membrane pore size of 4.2 μm, and a porosity of 54.8%. First, the membrane was placed in ethanol for ultrasonic cleaning for 5 min, and then treated with a 1 mM sodium hydroxide aqueous solution at room temperature for 10 min. Further, by an anodic oxidation method, with the titanium membrane as the anode and the titanium plate as the cathode, the electrolyte composition was 5% NH4F, 10% water and 85% ethylene glycol, the oxidation voltage was 60 V, and the oxidation time was 60 min, a titanium dioxide layer was formed on the surface of the titanium membrane, and a titanium membrane material with a titanium dioxide layer on the surface was obtained. The barium titanate / titanium-based composite piezoelectric catalytic film was further coupled with the hydrothermal growth method, wherein the barium hydroxide aqueous solution was used as the reactant, the titanium film material with a titanium dioxide layer on the surface was immersed in a barium nitrate aqueous solution for 2 hours, and then transferred to a polytetrafluoroethylene reactor for hydrothermal reaction, and after the reaction was completed, it was naturally cooled to room temperature and then taken out, washed with deionized water for 3 to 5 times, and dried to obtain the barium titanate / titanium-based composite piezoelectric catalytic film; wherein the mass ratio of the titanium dioxide / titanium composite film to the barium hydroxide aqueous solution was 1:40, the barium hydroxide concentration was 0.5M, the hydrothermal reaction temperature was 200°C, and the reaction time was 20 hours. The piezoelectric catalytic process of the obtained film under the action of an ultrasonic machine with a power of 1000W and a frequency of 40kHz achieved a 100% removal effect on 100mL of sulfamethoxazole (5mg / L) within 60 minutes. At the same time, the membrane that had been running for more than one week was backwashed continuously with 0.1M sodium hydroxide solution for 2 hours, and the performance of the membrane was evaluated under the same conditions. The removal effect of sulfamethoxazole was restored to 90%, showing good membrane regeneration ability.

Claims

1. A method for preparing a titanium-based composite piezoelectric catalytic film, characterized in that: The preparation method comprises: (1) Using a porous titanium-based membrane material as a substrate, pre-treating the substrate by sequentially using an organic solvent cleaning method and a chemical reagent etching method; (2) growing a nano-titanium dioxide layer on the surface of the pretreated porous titanium-based membrane to obtain a titanium dioxide / titanium-based composite membrane; (3) Using the titanium dioxide / titanium-based composite film obtained in step (2) as a substrate, the titanium dioxide is reacted to generate barium titanate to obtain the barium titanate / titanium-based composite piezoelectric catalytic film.

2. The preparation method according to claim 1, characterized in that: In step (1), the configuration of the porous titanium-based membrane is one of tubular, plate, hollow plate and hollow fiber membrane; the pore size of the porous titanium-based membrane is 0.2-10.0 μm, and the porosity is 20%-60%.

3. The preparation method according to claim 1, characterized in that: In step (1), the organic solvent is a mixture of one or more of acetone, methanol, ethanol, isopropanol, and N,N-dimethylformamide; the chemical reagent is an alkaline reagent or an acidic reagent, the alkaline reagent is a mixture of one or two of sodium hydroxide and potassium hydroxide aqueous solutions, and the acidic reagent is a mixture of one or more of oxalic acid solution and citric acid solution, the concentration is 0.01mM to saturation concentration, and the etching time is 5 to 120min.

4. The preparation method according to claim 1, characterized in that: In step (2), the growth method of nano titanium dioxide includes anodization, electrodeposition, sol-gel and solvent thermal method.

5. The preparation method according to claim 1, characterized in that: In step (3), the barium titanate growth method includes a solid phase calcination synthesis method and a solvent thermal method.

6. The metal titanium-based composite piezoelectric catalytic film prepared by the preparation method according to any one of claims 1 to 5.

7. Use of the metal titanium-based composite piezoelectric catalytic membrane according to claim 6 in water treatment.

8. The use according to claim 7, characterized in that: During the treatment process, the catalytic membrane undergoes a piezoelectric catalytic reaction under the action of mechanical force, generating active oxygen species, which oxidize and degrade organic pollutants on the membrane surface and in the pores, thereby removing pollutants and achieving a self-cleaning and anti-pollution effect of the membrane.

9. The use according to any one of claims 7 to 8, characterized in that: The mechanical force action includes one or more of periodic pulse water pressure, ultrasound, water flow impact, and swing of the membrane in water.

10. The use according to any one of claims 7 to 9, characterized in that: The active oxygen species are generated by direct piezoelectric catalysis, or by coupling persulfate activation, photocatalysis, catalytic ozone or catalytic Fenton process.