(gamma-MnO2) x / LaMnO3 catalyst for DMF (Dimethyl Formamide) catalytic combustion as well as preparation method and application thereof
The (γ-MnO2)x/LaMnO3 catalyst prepared by acid etching solves the problems of reduced activity and high by-products of existing catalysts during DMF catalytic combustion, improves the activity and selectivity of the catalyst, and realizes the DMF High efficiency oxidation and N2 selectivity, suitable for industrial applications.
Patent Information
- Application Number
- CN202411198354.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-06
AI Technical Summary
During the DMF catalytic combustion process, existing catalysts have problems such as reduced activity, high by-product concentration and low N2 selectivity, especially in high temperature and high concentration conditions, which are difficult to meet emission standards.
The (γ-MnO2)x/LaMnO3 catalyst was prepared by acid etching method. By etching LaMnO3 in nitric acid solution, the specific surface area and surface tetravalent manganese content of the catalyst are improved, and the synergy between oxygen vacancies and acidic sites is enhanced. effect, improve catalytic activity and selectivity.
The rapid adsorption and low-temperature oxidation of DMF are achieved, which significantly reduces the by-product concentration, improves the selectivity of N2, and maintains the stability of the catalyst at high temperatures, making it suitable for industrial applications.
Smart Images

Figure CN119075975A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of air pollution control, and in particular relates to a (γ-MnO2) x / LaMnO3 catalyst and its preparation method and application. Background Art
[0002] N,N-dimethylformamide (DMF) is a "universal solvent" and is widely used in chemical industries such as textiles, leather, pesticides, medicine, electronics, polymer synthesis and membrane manufacturing. Direct emissions will cause serious damage to nature and human health. At present, the commonly used treatment method for DMF waste gas is spray concentration treatment, but this type of treatment method has a complex process and consumes a lot of energy. In addition, the residual DMF concentration in the tail gas is much higher than the emission concentration limit of dimethylformamide specified in the "Comprehensive Emission Standards for Air Pollutants" (DB31 / 933-2023) (20mg / m 3 ). For low-concentration nitrogen-containing volatile organic compounds (NVOCs) tail gas, high-temperature thermal incineration technology or catalytic combustion technology is usually used for deep purification treatment to convert NVOCs into nitrogen, carbon dioxide and water. High-temperature thermal incineration technology requires the addition of auxiliary fuels such as natural gas, and has high operating costs. At the same time, the high processing temperature is very likely to produce nitrogen oxides (NO, NO2, etc.) and other gases that will cause secondary pollution to the environment. In addition, the high-temperature incinerator is a complex equipment that integrates combustion, cooling, and absorption. It has particularly stringent requirements on the equipment material, which often causes the incinerator to be unable to operate continuously for a long period of time. Catalytic combustion technology has the advantages of low operating temperature, high purification efficiency, recyclable heat generated, and no secondary pollution. It has better development prospects. The key is the development of high-performance purification catalysts.
[0003] In the process of catalytic combustion of NVOCs, the selective oxidation of nitrogen species and the deep oxidation of carbon species are technical difficulties. To achieve this goal, the catalyst must have suitable oxygen vacancies and acidic sites, which work synergistically to improve activity and selectivity. Currently, the commonly used catalysts for catalytic combustion reactions of NVOCs are metal oxide catalysts, molecular sieve catalysts and supported precious metal catalysts. For example, the Mn-based catalyst reported in the literature (Chem. Eng. J., 2018, 333: 402-413) found that the reaction path of HCN on the surface of MnOx has two forms: oxidation reaction at high temperature and hydrolysis reaction at low temperature. However, due to the change of the surface Mn valence state during the reaction and the coverage of the surface active sites by intermediate products, the N2 selectivity at high temperature is greatly reduced. There are abundant acid sites on the surface of molecular sieves, which can enhance the adsorption capacity of NVOCs, and the appropriate amount of loaded metal oxides can change the oxygen vacancies and acid sites on the catalyst surface, thereby effectively achieving the complete oxidation of NVOCs at low temperature. For example, the Cu-Mn / SAPO-45 catalyst reported in the literature (Appl. Catal. A: Gene., 2023, 665: 119354) has excellent catalytic combustion activity, but it will quickly produce high concentrations of N2O at high temperatures, causing secondary pollution. Precious metal-loaded rare earth metal catalysts have become a hot topic of research in recent years due to their excellent oxygen storage and release capacity, especially CeO2, such as the Ag / CeO2 catalyst reported in the literature (Appl. Catal. B: Environ., 2024, 341: 123268). The doping of precious metals improves the oxygen absorption and desorption ability of CeO2, promotes the reaction between surface oxygen species and NVOCs, and improves the thermal stability of the catalyst. However, excessive surface oxygen vacancies affect the selective catalytic oxidation ability of nitrogen species, thereby reducing the N2 selectivity during the catalytic reaction.
[0004] Although the various catalysts reported in the above literature can improve the catalytic oxidation activity of DMF, the catalysts are limited to the types of reactants and reaction conditions, and a lot of NO will be generated. x Or CO, so the emission requirements cannot be met during the catalytic combustion of DMF.
[0005] Mn-based catalysts have been widely studied in the catalytic combustion of NVOCs in recent years due to their variable chemical valence and excellent redox properties. However, manganese oxide is easily subject to phase change due to the increase in reaction temperature during the reaction, which results in the deactivation of the catalyst and reduced stability. Although LaMnO3 perovskite can well control the Mn species in the B position, making it difficult for the Mn species to undergo phase change during the reaction, the performance of the LaMnO3 perovskite catalyst is not ideal due to its small specific surface area, low content of mobile oxygen species and weak acidity. Therefore, it is essential to treat the LaMnO3 perovskite catalyst based on it. Summary of the invention
[0006] The purpose of the present invention is to provide a (γ-MnO2) for DMF catalytic combustion with high activity, high stability and strong water resistance in order to overcome the defects of the above-mentioned prior art. x / LaMnO3 catalyst and its preparation method and application.
[0007] The object of the present invention can be achieved by the following technical scheme: a (γ-MnO2) for DMF catalytic combustion x / LaMnO3 catalyst, the catalyst comprising the following composition in weight percentage:
[0008] La 28~30%,
[0009] Mn 47~49%.
[0010] Furthermore, (γ-MnO2) x The γ-MnO2 in the / LaMnO3 catalyst is obtained by etching LaMnO3 in a nitric acid solution for 30-120 minutes.
[0011] The present invention also provides a (γ-MnO2) for DMF catalytic combustion reaction x / The preparation method of LaMnO3 catalyst comprises the following steps:
[0012] Dissolve hydrated lanthanum nitrate and manganese nitrate solution in deionized water, then continue to add a certain amount of monohydrated citric acid, stir in an oil bath at 50-100°C for 1-6 hours, then dry at 90-110°C for 8-14 hours, and roast in an air atmosphere at 600-800°C for 2-6 hours. Place the resulting solid in a dilute nitric acid solution, stir, filter, dry at 110-130°C for 8-14 hours, and roast in an air atmosphere at 400-500°C for 2-6 hours to obtain (γ-MnO2) x / LaMnO3 catalyst.
[0013] The present invention also provides a (γ-MnO2) for DMF catalytic combustion x / Application of LaMnO3 catalyst, using the catalyst for catalytic treatment of gas containing DMF.
[0014] Furthermore, the conditions for the catalytic combustion reaction are: the concentration of DMF is 1500 ppm, the reaction space velocity is 60000 mL·g -1 ·h -1 .
[0015] The present invention adopts acid etching method to prepare (γ-MnO2) x / LaMnO3 catalyst, although Mn has good stability in LaMnO3, it needs to be acid-etched due to its small specific surface area, low content of mobile oxygen species and weak acidity. During the preparation process of acid etching, the LaMnO3 perovskite catalyst is added to the nitric acid solution and stirred, gradually completing the transformation from LaMnO3 to γ-MnO2, increasing the specific surface area and the content of tetravalent manganese on the surface, which is beneficial to the adsorption of DMF on the catalyst surface. At the same time, the formed γ-MnO2 further promotes the formation of acid and oxygen vacancies, which is beneficial to the catalytic combustion of DMF and the selective oxidation of nitrogen species, achieving high activity and high selectivity. In addition, since La and part of the Mn element are gradually etched away from the bulk phase, a strong interaction between the metal oxide and the carrier will be formed between the formed γ-MnO2 and LaMnO3, so that the surface γ-MnO2 has excellent high-temperature stability, effectively avoiding the reduction of activity caused by phase change of manganese oxide after high-temperature calcination.
[0016] Compared with the prior art, the present invention has the following beneficial effects:
[0017] (1) The abundant oxygen vacancies on the catalyst surface can achieve rapid adsorption and elimination of DMF, and can quickly oxidize DMF under low temperature conditions. Moreover, the catalyst can still maintain excellent performance after high-temperature calcination.
[0018] (2) (γ-MnO2) prepared by acid etching x / LaMnO3 catalyst can significantly reduce the concentration of by-products during the combustion of DMF catalyst, while improving the selectivity of N2 in the reaction process, and the preparation method is simple and easy to implement industrialization. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 (γ-MnO2) x / Activity diagram of LaMnO3 series catalysts for DMF catalytic combustion;
[0020] Figure 2 (γ-MnO2)x / LaMnO3 series catalysts for the by-product concentration changes during the catalytic combustion of DMF;
[0021] Figure 3 (γ-MnO2) x / LaMnO3 series catalysts for N2 selectivity changes during DMF catalytic combustion;
[0022] Figure 4 (γ-MnO2) 50 / Activity diagram of LaMnO3 catalyst for catalytic combustion of DMF at different concentrations;
[0023] Figure 5 (γ-MnO2) 50 / Activity diagram of LaMnO3 catalyst for DMF catalytic combustion at different space velocities;
[0024] Figure 6 (γ-MnO2) x / Activity diagram of LaMnO3 series catalysts for catalytic combustion of DMF under water addition conditions;
[0025] Figure 7 (γ-MnO2) 50 / LaMnO3 catalyst in T 100 Long-range stability of DMF catalytic combustion under low temperature conditions;
[0026] Figure 8 (γ-MnO2) x / Raman characterization diagram of LaMnO3 series catalysts. DETAILED DESCRIPTION
[0027] The present invention will be described in detail below with reference to specific embodiments, but this does not limit the protection scope of the present invention.
[0028] Example 1
[0029] (γ-MnO2) 50 Preparation of LaMnO3 catalyst: 4.33 g La(NO3)3·6H2O, 3.58 g Mn(NO3)2 solution (mass fraction 50%) and 4.2 g C6H8O7·6H2O were dissolved in 40 mL deionized water, stirred for 30 minutes, and then stirred in an oil bath at 80°C for 4 hours to form a yellow sol, which was dried at 100°C for 12 hours and calcined in an air atmosphere at 700°C for 4 hours. 1 g of the obtained solid was placed in 20 mL of 3M nitric acid solution and stirred for 50 minutes, then filtered, dried at 120°C for 12 hours, and calcined in an air atmosphere at 450°C for 4 hours.
[0030] The etching time during the acid etching process is changed to increase the proportion of γ-MnO2 in the bulk phase. In this embodiment, the acid etching time is 50 minutes.
[0031] Example 2
[0032] The acid etching time was changed to 40 minutes, and the rest was the same as in Example 1 to obtain (γ-MnO2) 40 / LaMnO3 catalyst.
[0033] Example 3
[0034] The acid etching time was changed to 60 minutes, and the rest was the same as in Example 1 to obtain (γ-MnO2) 60 / LaMnO3 catalyst.
[0035] Example 4
[0036] The acid etching time was changed to 90 minutes, and the rest was the same as in Example 1 to obtain (γ-MnO2) 90 / LaMnO3 catalyst.
[0037] Example 5
[0038] The acid etching time was changed to 120 minutes, and the rest was the same as in Example 1 to obtain (γ-MnO2) 120 / LaMnO3 catalyst.
[0039] Comparative Example 1
[0040] Preparation of LaMnO3 catalyst: Dissolve 4.33 g La(NO3)3·6H2O, 3.58 g Mn(NO3)2 solution (mass fraction of 50%) and 4.2 g C6H8O7·6H2O in 40 mL deionized water. Stir for 30 minutes, then continue stirring in an oil bath at 80°C for 4 hours to form a yellow sol. Dry at 100°C for 12 hours and calcine at 700°C in an air atmosphere for 4 hours.
[0041] Performance Evaluation
[0042] (I) Activity evaluation
[0043] 1.1 Catalytic combustion performance of gas containing dimethylformamide
[0044] The catalytic performance evaluation conditions are as follows: 0.1 g of the catalysts prepared in Examples 1-5 and Comparative Example were placed in a quartz tube fixed bed reactor, air was used as an oxidant, the concentration of dimethylformamide was 1500 ppm and the reaction space velocity was 60000 mL·g -1 ·h -1 The catalytic combustion reaction was carried out under the conditions of , and the reaction exhaust gas was detected by capillary gas chromatograph.
[0045] Activity test results such as Figure 1 As shown, from Figure 1 It can be seen that acid etching significantly improves the activity of LMO in catalytic oxidation of DMF. Gradually increasing the etching time can significantly improve the activity. After 60 minutes of etching, the activity of the catalyst has been increased to the maximum, and continued etching no longer increases the reaction activity. Examples 1-5 can achieve complete conversion of DMF before 200°C.
[0046] Byproduct test results are as follows Figure 2 As shown, from Figure 2 It can be seen that the comparative example produces a large amount of DMA during the reaction process, while the concentration of DMA after acid etching drops to 1 / 20 of the original, and can disappear at a lower temperature. In addition, when the acid etching time is 60 minutes, the concentration of DMA is the lowest. If the etching time is increased, the DMA concentration will increase again. But in general, Examples 1-5 can control the concentration of DMA produced during the reaction process to less than 40ppm.
[0047] N2 selectivity results are as follows Figure 3 As shown, from Figure 3 It can be seen that the acid etching treatment improves the selectivity of N2. When the acid etching time is 90 minutes, the selectivity of N2 reaches the highest, reaching 94% at 400°C. In general, Examples 1-5 can control the selectivity of N2 to above 90% at 400°C.
[0048] 1.2 Catalytic combustion performance of dimethylformamide gas with different concentrations
[0049] The concentration of dimethylformamide was changed from 500 ppm to 5000 ppm. The other catalytic performance evaluation conditions were the same as those in Example 1. The activity test results were as follows: Figure 4 As shown, from Figure 4 It can be seen that Example 1 not only exhibits excellent catalytic performance for low concentration of dimethylformamide (500ppm), but also has excellent performance for high concentration of dimethylformamide (5000ppm). In addition, when the concentration of the reactant exceeds 1500ppm, the catalytic activity of Example 1 for dimethylformamide remains basically unchanged when the concentration of the reactant is further increased. In general, Example 1 can achieve complete catalytic combustion of dimethylformamide within 5000ppm at 250°C.
[0050] 1.3 Catalytic combustion performance of dimethylformamide gas at different space velocities
[0051] Changing the reaction space velocity of dimethylformamide from 30000 mL g -1 ·h -1 To 120000mL·g -1·h -1 The rest of the catalytic performance evaluation conditions were the same as those in Example 1. The activity test results were as follows: Figure 5 As shown, from Figure 5 It can be seen that Example 1 not only has a good effect on the low space velocity of dimethylformamide (30000mL·g -1 ·h -1 ) showed excellent catalytic performance, and for high space velocity dimethylformamide (120000mL·g -1 ·h -1 ) also has excellent performance. In addition, when the reaction space velocity exceeds 60000mL·g -1 ·h -1 After that, the reaction space velocity was increased, and the catalytic activity of Example 1 for dimethylformamide remained basically unchanged. In general, Example 1 can achieve 120000 mL·g -1 ·h -1 Complete catalytic combustion of dimethylformamide within .
[0052] (II) Water resistance evaluation
[0053] 5 vol.% H2O was added to the reaction atmosphere to investigate the effect of water introduction on the activity of Examples 1, 5 and the comparative example. The rest was the same as in Performance Evaluation 1.1. The activity test results are shown in Figure 6 As shown, from Figure 6 It can be seen that after acid etching, the catalytic performance of Examples 1 and 5 under humid conditions is improved, while the catalytic performance of the comparative example under humid conditions is reduced. Therefore, the catalyst after acid etching has improved water resistance stability.
[0054] (III) Water resistance evaluation
[0055] Example 1 was placed in a quartz tube fixed bed reactor, with air as the oxidant, at a DMF concentration of 1500 ppm and a reaction space velocity of 60000 mL·g -1 ·h -1 and T 100 The DMF catalytic combustion reaction was carried out for 120 hours under the conditions of , and the long-term catalytic stability of the catalyst was investigated. The stability test results are shown in Figure 7 As shown, from Figure 7 It can be seen that within the reaction time of 120 hours, the conversion rate of dimethylformamide remained at 100%, and no nitrogen-containing organic by-products were produced. Therefore, the acid-etched catalyst has excellent long-term catalytic stability.
[0056] from Figure 1-7It can be seen that the acid etching treatment of the comparative example can effectively improve the performance of the catalyst, not only can the complete conversion of dimethylformamide be achieved at a lower temperature, but also the concentration of the byproduct DMA during the reaction is reduced, and the N2 selectivity of the sample at high temperature is improved. In addition, the catalyst treated with acid etching has excellent catalytic performance for dimethylformamide at different concentrations, different space velocities and humid conditions.
[0057] Figure 8 The Raman graphs of Examples 1-5 and the comparative catalysts show that acid etching gradually reduces the Raman wavenumber of the Mn-O bond, from 666 cm-1 of LaMnO3 to 1. -1 The wavelengths of 616 and 553 cm-1 belonging to MnO2 -1 , which corresponds to the disappearance of LaMnO3 and the generation of MnO2 on the surface. Therefore, the acid etching treatment can expose more MnO2 on the catalyst surface, and with the increase of etching time, the exposed MnO2 also increases significantly, thereby improving the catalytic performance of dimethylformamide.
Claims
1. Used for DMF catalytic combustion reaction (γ-MnO2) x / LaMnO3 catalyst, characterized in that The catalyst comprises the following compositions in weight percentage: La 28~30%, Mn 47~49%.
2. (γ-MnO2) for DMF catalytic combustion reaction according to claim 1 x / LaMnO3 catalyst, characterized in that (γ-MnO2) x The etching time of the / LaMnO3 catalyst in the nitric acid solution is 30-120 minutes.
3. (γ-MnO2) for DMF catalytic combustion reaction according to claim 1 x / A method for preparing a LaMnO3 catalyst, characterized in that: (γ-MnO2) x / LaMnO3 catalyst was prepared by the following method: Dissolve hydrated lanthanum nitrate and manganese nitrate solution in deionized water, then continue to add a certain amount of monohydrated citric acid, stir in an oil bath at 50-100°C for 1-6 hours, then dry at 90-110°C for 8-14 hours, and roast in an air atmosphere at 600-800°C for 2-6 hours. Place the resulting solid in a dilute nitric acid solution, stir, filter, dry at 110-130°C for 8-14 hours, and roast in an air atmosphere at 400-500°C for 2-6 hours to obtain (γ-MnO2) x / LaMnO3 catalyst.
4. (γ-MnO2) for DMF catalytic combustion reaction according to any one of claims 1 to 3 x / Application of LaMnO3 catalyst, characterized in that, The catalyst is used for treating gas containing DMF by catalytic combustion method.
5. (γ-MnO2) for DMF catalytic combustion reaction according to claim 4 x / Application of LaMnO3 catalyst, characterized in that, The conditions for the catalytic combustion reaction are: DMF concentration is 500-5000ppm, reaction space velocity is 30000-120000mL·g -1 ·h -1 .