Preparation method of iron-based nano-enzyme catalytic membrane
By optimizing raw material ratio and preparation process, an iron-based nanoenzyme catalytic film with stable performance and high catalytic efficiency was prepared, which solved the problems of complex and high cost in the existing technology, and achieved efficient removal of soluble organic pollutants and heavy metals Ion effects and suitable for large-scale production and environmentally friendly applications.
Patent Information
- Application Number
- CN202411183022.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-06
AI Technical Summary
The existing preparation methods of iron-based nanoenzymes are complex and costly, and it is difficult to produce on a large scale. The prepared iron-based nanoenzymes are usually in powder form and are difficult to directly apply to water treatment.
By optimizing the raw material ratio and preparation process, iron-based nanoenzyme catalytic films with stable performance and high catalytic efficiency are prepared, including the use of iron source substances, nanocarrier materials, reducing agents, stabilizers and membrane matrix materials, and reducing by stirring and heat The reaction forms nanoscale iron-based nanoenzyme particles and are uniformly coated on the membrane matrix material to form a catalytic film.
It significantly improves the catalytic efficiency and stability of the catalytic film, improves the removal effect of dissolved organic pollutants and heavy metal ions, is easy to recover and reuse, reduces the cost of wastewater treatment, is suitable for large-scale production, and has good mechanical strength. and durability.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of catalytic membrane preparation, and in particular to a method for preparing an iron-based nanozyme catalytic membrane. Background Art
[0002] Traditional water treatment technologies such as flocculation, sedimentation, and filtration can remove suspended solids and some pollutants in water to a certain extent, but the removal effect on some soluble organic pollutants and heavy metal ions is not ideal. Therefore, it is particularly important to develop new water treatment technologies that are efficient and environmentally friendly.
[0003] In recent years, the rise of nanotechnology has brought new hope to the field of water treatment. Nanomaterials have shown great application potential in catalysis, adsorption, separation, etc. due to their unique physical and chemical properties. In particular, nanozymes are nanomaterials with catalytic activity similar to that of natural enzymes. They can simulate the catalytic reaction of natural enzymes and have the advantages of low cost, good stability, and easy recycling. Therefore, they have broad application prospects in the field of wastewater treatment.
[0004] As a new type of nanozyme material, iron-based nanozymes mainly derive their catalytic activity from iron ions or iron-based nanoparticles. Iron-based nanozymes not only have good catalytic performance, but also have readily available raw materials and low cost, so they have broad application potential in wastewater treatment, organic synthesis, biosensors and other fields. However, how to prepare iron-based nanozyme catalytic membranes with stable performance and high catalytic efficiency is the focus and difficulty of current research.
[0005] At present, the preparation methods of iron-based nanozymes mainly include sol-gel method, hydrothermal synthesis method, microemulsion method, etc. Although these methods can prepare iron-based nanozymes with catalytic activity to a certain extent, there are problems such as complex preparation process, high cost, and difficulty in large-scale production. In addition, the prepared iron-based nanozymes often exist in the form of powder, which is difficult to directly apply in the actual water treatment process and needs to be further processed into a catalytic membrane form. Summary of the invention
[0006] The present invention proposes a method for preparing an iron-based nanozyme catalytic membrane. By optimizing the raw material ratio and the preparation process, an iron-based nanozyme catalytic membrane with stable performance and high catalytic efficiency is prepared. It not only has good catalytic activity, but is also easy to recycle and reuse, providing a new efficient and environmentally friendly technology for wastewater treatment.
[0007] The technical solution adopted by the present invention is: an iron-based nanozyme catalytic membrane, whose raw materials, counted by weight, include: 60-100 parts of iron source material, 20-40 parts of nanocarrier material, 5-20 parts of reducing agent, 2-5 parts of stabilizer, 40-80 parts of membrane matrix material, and 100-140 parts of solvent.
[0008] As a further improvement of the present invention, the iron source material is at least one of ferric chloride, ferric sulfate, ferric nitrate and ferric acetate.
[0009] As a further improvement of the present invention, the nanocarrier material is at least one of silica, alumina, carbon nanotubes, graphene, and activated carbon, which is used to support and disperse the iron-based nanozyme.
[0010] As a further improvement of the present invention, the reducing agent is at least one of sodium borohydride, ascorbic acid and hydrazine hydrate, which is used to reduce the iron ions into nanoparticles with catalytic activity.
[0011] As a further improvement of the present invention, the stabilizer is at least one of polyethylene glycol, polyvinyl pyrrolidone and chitosan, which is used to prevent the nanoparticles from agglomerating and improve the stability and durability of the catalytic film.
[0012] As a further improvement of the present invention, the membrane matrix material is at least one of polyvinyl alcohol, polyacrylic acid, cellulose acetate, and polysulfone polymer materials, which serves as a supporting skeleton of the catalytic membrane.
[0013] As a further improvement of the present invention, the solvent is at least one of water, ethanol, acetone, and dimethylformamide, which is used to dissolve and disperse the membrane matrix material and other components to ensure the uniformity and film-forming quality of the catalytic membrane.
[0014] A method for preparing an iron-based nanozyme catalytic membrane comprises the following steps:
[0015] Step 1, weighing raw materials: weighing iron source material, nanocarrier material, reducing agent, stabilizer, membrane matrix material, and solvent according to the above weight proportions;
[0016] Step 2: Mixing and stirring: Pour the solvent into the reaction kettle, add the iron source material and the nano-carrier material, and stir with a stirrer until a uniform suspension is formed;
[0017] Step 3, reduction reaction: heating the stirred suspension to between 40-60°C and maintaining this temperature, slowly adding a reducing agent while stirring to reduce the iron ions in the iron source material to nano-sized iron-based nanozyme particles;
[0018] Step 4, stabilization treatment: After the reduction reaction is completed, add a stabilizer to the suspension and continue stirring so that the nanozyme particles are evenly coated with the stabilizer to prevent agglomeration;
[0019] Step 5, film formation: the stabilized suspension is evenly coated on the membrane matrix material, and then dried to form a continuous film layer of the membrane matrix material, thereby obtaining an iron-based nanozyme catalytic membrane.
[0020] As a further improvement of the present invention, the stirring speed is 150-300 rpm.
[0021] As a further improvement of the present invention, the drying treatment is carried out by hot air drying, the drying temperature is controlled between 60-80° C., and the drying time is controlled between 1-3 hours.
[0022] Beneficial effects of the present invention: (1) The preparation method of the iron-based nanozyme catalytic membrane of the present invention significantly improves the catalytic efficiency and stability of the catalytic membrane by optimizing the raw material ratio and the preparation process, thereby showing a higher removal rate in the wastewater treatment process, especially for the removal of soluble organic pollutants and heavy metal ions.
[0023] (2) The iron-based nanozyme catalytic membrane of the present invention is easy to recycle and reuse, which greatly reduces the cost of wastewater treatment and reduces secondary pollution to the environment, meeting the requirements of sustainable development.
[0024] (3) The preparation method of the present invention is simple to operate, has mild reaction conditions, is easy to control, is suitable for large-scale production, and provides the possibility for industrial application.
[0025] (4) The iron-based nanozyme catalytic membrane prepared by the present invention by selecting suitable nanocarrier materials and membrane matrix materials has good mechanical strength and durability, ensuring long-term stable operation in practical applications.
[0026] (5) The iron-based nanozyme catalytic membrane of the present invention does not require complicated post-treatment during the preparation process and can be directly applied to water treatment equipment, thereby simplifying the wastewater treatment process and improving the treatment efficiency DETAILED DESCRIPTION
[0027] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0028] The invention provides an iron-based nanozyme catalytic membrane, whose raw materials include, by weight: 60-100 parts of iron source material, 20-40 parts of nanocarrier material, 5-20 parts of reducing agent, 2-5 parts of stabilizer, 40-80 parts of membrane matrix material and 100-140 parts of solvent.
[0029] The iron source material in the present invention is at least one of ferric chloride, ferric sulfate, ferric nitrate and ferric acetate.
[0030] The nano-carrier material in the present invention is at least one of silicon dioxide, aluminum oxide, carbon nanotubes, graphene and activated carbon, which is used to support and disperse the iron-based nanozyme.
[0031] The reducing agent in the present invention is at least one of sodium borohydride, ascorbic acid and hydrazine hydrate, which is used to reduce iron ions into nanoparticles with catalytic activity.
[0032] The stabilizer in the present invention is at least one of polyethylene glycol, polyvinyl pyrrolidone and chitosan, which is used to prevent the nanoparticles from agglomerating and improve the stability and durability of the catalytic film.
[0033] In the present invention, the membrane matrix material is at least one of polyvinyl alcohol, polyacrylic acid, cellulose acetate and polysulfone polymer materials, which serves as the supporting skeleton of the catalytic membrane.
[0034] The solvent in the present invention is at least one of water, ethanol, acetone and dimethylformamide, which is used to dissolve and disperse the membrane matrix material and other components to ensure the uniformity and film-forming quality of the catalytic membrane.
[0035] A method for preparing an iron-based nanozyme catalytic membrane comprises the following steps:
[0036] Step 1, weighing raw materials: weighing iron source material, nanocarrier material, reducing agent, stabilizer, membrane matrix material, and solvent according to the above weight proportions;
[0037] Step 2: Mixing and stirring: Pour the solvent into the reaction kettle, add the iron source material and the nano-carrier material, and stir with a stirrer until a uniform suspension is formed;
[0038] Step 3, reduction reaction: heating the stirred suspension to between 40-60°C and maintaining this temperature, slowly adding a reducing agent while stirring to reduce the iron ions in the iron source material to nano-sized iron-based nanozyme particles;
[0039] Step 4, stabilization treatment: After the reduction reaction is completed, add a stabilizer to the suspension and continue stirring so that the nanozyme particles are evenly coated with the stabilizer to prevent agglomeration;
[0040] Step 5, film formation: the stabilized suspension is evenly coated on the membrane matrix material, and then dried to form a continuous film layer of the membrane matrix material, thereby obtaining an iron-based nanozyme catalytic membrane.
[0041] The stirring speed in the present invention is 150-300 rpm.
[0042] The drying method of the present invention is hot air drying, the drying temperature is controlled between 60-80° C., and the drying time is controlled between 1-3 hours.
[0043] Embodiment 1:
[0044] This embodiment provides a method for preparing an iron-based nanozyme catalytic membrane, and the specific steps are as follows.
[0045] (I) Weighing raw materials: weigh 65 parts of ferric chloride as an iron source, 30 parts of silicon dioxide as a nanocarrier, 10 parts of sodium borohydride as a reducing agent, 3 parts of polyethylene glycol as a stabilizer, 50 parts of polyvinyl alcohol as a membrane matrix material, and 120 parts of water as a solvent;
[0046] (ii) mixing and stirring: pouring water into a reaction kettle, adding ferric chloride and silicon dioxide, and stirring with a stirrer at a speed of 200 rpm until a uniform suspension is formed;
[0047] (iii) Reduction reaction: The stirred suspension is heated to 50°C and maintained at this temperature, and sodium borohydride is slowly added under stirring to reduce the iron ions in the ferric chloride to nano-sized iron-based nanozyme particles;
[0048] (iv) Stabilization treatment: After the reduction reaction is completed, polyethylene glycol is added to the suspension and stirring is continued for 30 minutes to allow the nanozyme particles to be evenly coated with the stabilizer to prevent agglomeration;
[0049] (V) Film formation: The stabilized suspension is evenly coated on the polyvinyl alcohol film matrix material, and then hot air drying is performed. The drying temperature is controlled at 70°C and the drying time is controlled at 2 hours, so that the film matrix material forms a continuous film layer, thereby obtaining an iron-based nanozyme catalytic membrane.
[0050] Embodiment 2:
[0051] This embodiment provides a method for preparing an iron-based nanozyme catalytic membrane, and the specific steps are as follows.
[0052] (I) Weighing raw materials: weighing 70 parts of iron source material ferric sulfate, 25 parts of nanocarrier material carbon nanotubes, 15 parts of reducing agent ascorbic acid, 4 parts of stabilizer chitosan, 60 parts of membrane matrix material cellulose acetate, and 110 parts of solvent ethanol by weight;
[0053] (ii) Mixing and stirring:
[0054] Pour ethanol into the reaction kettle, add iron sulfate and carbon nanotubes, and stir with a stirrer at a speed of 250 rpm until a uniform suspension is formed;
[0055] (iii) Reduction reaction: heating the stirred suspension to 45°C and maintaining this temperature, slowly adding ascorbic acid under stirring to reduce the iron ions in the iron sulfate to nano-sized iron-based nanozyme particles;
[0056] (IV) Stabilization treatment:
[0057] After the reduction reaction was completed, chitosan was added to the suspension and stirring was continued for 40 minutes to allow the nanozyme particles to be evenly coated by the stabilizer to prevent agglomeration;
[0058] (V) Film formation:
[0059] The stabilized suspension is evenly coated on the cellulose acetate membrane matrix material, and then hot air drying is performed. The drying temperature is controlled at 65°C and the drying time is controlled at 2.5 hours, so that the membrane matrix material forms a continuous membrane layer to obtain an iron-based nanozyme catalytic membrane.
[0060] Embodiment 3:
[0061] This embodiment provides a method for preparing an iron-based nanozyme catalytic membrane, and the specific steps are as follows.
[0062] (I) Weighing raw materials: weigh 80 parts of iron source material ferric nitrate, 35 parts of nano-carrier material graphene, 12 parts of reducing agent hydrazine hydrate, 5 parts of stabilizer polyvinyl pyrrolidone, 65 parts of membrane matrix material polysulfone, and 130 parts of solvent acetone by weight;
[0063] (ii) mixing and stirring: pouring acetone into a reaction kettle, adding ferric nitrate and graphene, and stirring with a stirrer at a speed of 220 rpm until a uniform suspension is formed;
[0064] (iii) Reduction reaction: The stirred suspension is heated to 55°C and maintained at this temperature, and hydrazine hydrate is slowly added under stirring to reduce the iron ions in the ferric nitrate to nano-sized iron-based nanozyme particles;
[0065] (iv) Stabilization treatment: After the reduction reaction is completed, polyvinyl pyrrolidone is added to the suspension and stirring is continued for 35 minutes to allow the nanozyme particles to be evenly coated with the stabilizer to prevent agglomeration;
[0066] (V) Film formation: The stabilized suspension is evenly coated on the polysulfone membrane matrix material, and then hot air drying is performed. The drying temperature is controlled at 75°C and the drying time is controlled at 1.5 hours to allow the membrane matrix material to form a continuous film layer, thereby obtaining an iron-based nanozyme catalytic membrane.
[0067] Performance Testing
[0068] In order to verify the performance of the iron-based nanozyme catalytic membrane, the following performance tests were performed on Examples 1-3:
[0069] (I) Catalytic activity test: The catalytic activity of the catalytic membrane was determined by using the hydrogen peroxide decomposition reaction as a model reaction. The iron-based nanozyme catalytic membrane obtained in Examples 1-3 was placed in a solution containing hydrogen peroxide, and the catalytic activity was evaluated by measuring the decomposition rate of hydrogen peroxide in the solution.
[0070] The test results show that the catalytic membranes of Examples 1-3 all exhibit high catalytic activity, indicating that the iron-based nanozyme catalytic membrane prepared by the present invention has a significant catalytic effect in the hydrogen peroxide decomposition reaction. In particular, the iron-based nanozyme catalytic membrane of Example 2 has a decomposition rate slightly higher than that of Examples 1 and 3 under the same test conditions, showing the best catalytic performance.
[0071] (ii) Stability test: The iron-based nanozyme catalytic membrane obtained in Examples 1-3 was immersed in deionized water at room temperature for 7 consecutive days, and the catalytic activity of the catalytic membrane was measured every day.
[0072] The test results show that the catalytic activity of the catalytic membranes of Examples 1-3 decreased by less than 10% within 7 days, indicating that the iron-based nanozyme catalytic membrane prepared by the present invention has good stability.
[0073] (III) Durability test: The iron-based nanozyme catalytic membrane obtained in Examples 1-3 was subjected to a cyclic test during continuous use. After each use, it was rinsed with deionized water and dried. The catalytic activity was measured after repeated use for 100 times.
[0074] The test results show that the catalytic activity of the catalytic membranes of Examples 1-3 only decreases by about 15% after 100 cycles of use, indicating that the iron-based nanozyme catalytic membranes prepared by the present invention have excellent durability.
[0075] (IV) Anti-pollution performance test: The catalytic activity of the iron-based nanozyme catalytic membrane obtained in Examples 1-3 was tested in a solution containing a certain concentration of organic pollutants (such as methyl orange) to evaluate its anti-pollution performance.
[0076] The test results show that the catalytic activity of the catalytic membranes of Examples 1-3 decreases slightly after treating solutions containing organic pollutants, indicating that the iron-based nanozyme catalytic membranes prepared by the present invention have good anti-pollution properties.
[0077] In summary, the performance test results of Examples 1-3 show that the iron-based nanozyme catalytic membrane prepared by the present invention exhibits excellent performance in catalytic activity, stability, durability and anti-pollution performance, and has broad application prospects.
[0078] The preparation method of an iron-based nanozyme catalytic membrane of the present invention not only provides an efficient and stable catalytic material, but also has wide application potential in the fields of environmental protection, energy and biomedicine. By optimizing the raw material ratio and preparation process, an iron-based nanozyme catalytic membrane with high catalytic activity, good stability and excellent durability is successfully prepared. These catalytic membranes show significant advantages in decomposing harmful substances, improving energy conversion efficiency and promoting biological reactions.
[0079] In the field of environmental protection, iron-based nanozyme catalytic membranes can be used for sewage treatment, effectively decomposing organic pollutants in water, improving water quality, and reducing environmental pollution. In the field of energy, the catalytic membrane can be used in fuel cells and solar cells to improve energy conversion efficiency and promote the development of new energy technologies. At the same time, in the field of biomedicine, iron-based nanozyme catalytic membranes can be used in biosensors and drug delivery systems to improve detection sensitivity and drug efficacy.
[0080] In addition, the preparation method of the present invention is simple to operate, low in cost, and easy to achieve large-scale production, which provides the possibility for the commercial application of iron-based nanozyme catalytic membrane. With the deepening of research and the improvement of technology, iron-based nanozyme catalytic membrane is expected to play an important role in more fields and contribute to the sustainable development of human society.
[0081] Therefore, the preparation method of the iron-based nanozyme catalytic membrane of the present invention has significant technical advantages and broad application prospects. Its innovation and practicality will bring new development opportunities to related industries and have important social and economic value.
[0082] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features thereof may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. An iron-based nanozyme catalytic membrane, It is characterized in that The raw materials include, by weight: 60-100 parts of iron source material, 20-40 parts of nanometer carrier material, 5-20 parts of reducing agent, 2-5 parts of stabilizer, 40-80 parts of membrane matrix material and 100-140 parts of solvent.
2. The iron-based nanozyme catalytic membrane according to claim 1, It is characterized in that The iron source material is at least one of ferric chloride, ferric sulfate, ferric nitrate and ferric acetate.
3. The iron-based nanozyme catalytic membrane according to claim 1, It is characterized in that The nano-carrier material is at least one of silicon dioxide, aluminum oxide, carbon nanotubes, graphene, and activated carbon, and is used to support and disperse the iron-based nanozyme.
4. The iron-based nanozyme catalytic membrane according to claim 1, It is characterized in that The reducing agent is at least one of sodium borohydride, ascorbic acid and hydrazine hydrate, and is used to reduce iron ions into nanoparticles with catalytic activity.
5. The iron-based nanozyme catalytic membrane according to claim 1, It is characterized in that The stabilizer is at least one of polyethylene glycol, polyvinyl pyrrolidone and chitosan, and is used to prevent the nanoparticles from agglomerating and improve the stability and durability of the catalytic film.
6. The iron-based nanozyme catalytic membrane according to claim 1, It is characterized in that The membrane matrix material is at least one of polyvinyl alcohol, polyacrylic acid, cellulose acetate and polysulfone polymer materials, which serves as a supporting skeleton of the catalytic membrane.
7. The iron-based nanozyme catalytic membrane according to claim 1, It is characterized in that The solvent is at least one of water, ethanol, acetone and dimethylformamide, and is used to dissolve and disperse the membrane matrix material and other components to ensure the uniformity and film-forming quality of the catalytic membrane.
8. A method for preparing an iron-based nanozyme catalytic membrane, It is characterized in that The following steps are involved: Step 1, weighing raw materials: weighing iron source material, nanocarrier material, reducing agent, stabilizer, membrane matrix material, and solvent according to the above weight proportions; Step 2: Mixing and stirring: Pour the solvent into the reaction kettle, add the iron source material and the nano-carrier material, and stir with a stirrer until a uniform suspension is formed; Step 3, reduction reaction: heating the stirred suspension to between 40-60°C and maintaining this temperature, slowly adding a reducing agent while stirring to reduce the iron ions in the iron source material to nano-sized iron-based nanozyme particles; Step 4, stabilization treatment: After the reduction reaction is completed, add a stabilizer to the suspension and continue stirring so that the nanozyme particles are evenly coated with the stabilizer to prevent agglomeration; Step 5, film formation: the stabilized suspension is evenly coated on the membrane matrix material, and then dried to form a continuous film layer of the membrane matrix material, thereby obtaining an iron-based nanozyme catalytic membrane.
9. The method for preparing an iron-based nanozyme catalytic membrane according to claim 1, It is characterized in that The stirring speed is 150-300 rpm.
10. The method for preparing an iron-based nanozyme catalytic membrane according to claim 1, It is characterized in that The drying treatment method is hot air drying, the drying temperature is controlled between 60-80° C., and the drying time is controlled between 1-3 hours.